Catalyst for synthesis ammonia reaction as well as preparation method and application of catalyst
By using the co-precipitation method in the synthesis ammonia reaction, combined with the alternating magnetic field, the problems of high energy consumption and difficulty in activation of N2 are solved, and the synthesis of ammonia in low temperature and normal pressure is achieved, and the catalytic activity is significantly improved. 能量效率提升。
Patent Information
- Application Number
- CN202411145823.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The existing synthetic ammonia reactions have problems such as high energy consumption and difficulty in activating N2 molecules under low temperature and normal pressure, resulting in low yields of synthetic ammonia and poor energy efficiency.
The ferromagnetic catalyst was prepared by co-precipitation method, and the alternating magnetic field and the Prussian blue analog precursor were calcined under an inert gas to generate Fe-Co alloy and FeCoOx oxide, which not only acts as a magnetic induction heating center, but also activates N2 and H2 molecules to achieve low temperature Efficient synthesis of ammonia at normal pressure.
It significantly reduces the apparent activation energy of the reaction of synthetic ammonia, improves the reaction rate of synthetic ammonia under normal temperature and pressure, has high catalytic activity and has nearly ten times increased energy efficiency, avoiding the high energy consumption and uneven heating problems of traditional thermal catalysis.
Smart Images

Figure CN119034819A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy chemical industry, and specifically relates to a catalyst for synthetic ammonia reaction, a preparation method and an application thereof. Background Art
[0002] According to statistics, about 1-2% of fossil energy is used for ammonia synthesis every year. In recent years, ammonia synthesis has attracted wide attention due to its huge potential in clean energy. However, due to the strong N≡N covalent bond and high kinetic barrier in the N2 molecule, industrial ammonia synthesis is usually carried out using iron-based catalysts (HB process) or ruthenium-based catalysts (Kellogg advanced ammonia synthesis process) at high temperature (400-500℃) and high pressure (10-30MPa). Therefore, green ammonia synthesis at low temperature and low pressure is very attractive.
[0003] In recent years, with the rapid development of renewable energy power generation technology, there is great potential for developing electricity as the main energy supply in long-term catalytic processes. In industrial catalytic reactions, energy efficiency, suitable reaction conditions and intermittent energy supply have become increasingly important parameters. However, the ammonia synthesis reaction usually has a low yield, which is caused by the contradiction between thermodynamics (NH3 generation requires low temperature) and kinetics (N2 activation requires high temperature) for the reaction temperature. In order to obtain a high NH3 yield, a feasible solution is to achieve N2 activation at a lower temperature. In this case, magnetic induction heating (MIH) provides the possibility of directly heating magnetic materials. Compared with traditional heating methods, magnetic induction heating can achieve in-situ heat supply without heating the entire reactor. These characteristics make magnetic induction heating faster and more energy-efficient than traditional heating, greatly reducing heat loss and improving energy efficiency. Therefore, magnetic induction heating for ammonia synthesis not only reduces the reaction temperature and pressure, but also greatly reduces the reaction energy consumption in the ammonia synthesis process. Therefore, it is of great significance to use electromagnetic induction system and catalyst to achieve green ammonia synthesis.
[0004] In addition, ammonia has a wide range of uses. In addition to being used in fertilizers, it is also widely used in pharmaceuticals, chemicals, refrigeration, military products, etc. At present, synthetic ammonia mainly adopts the Haber-Bosch process, which is considered to be the greatest invention of the 20th century and was once called "air alchemy" by American popular science writer Thomas Haig. However, after more than a century of development, artificial synthesis of ammonia still needs to be carried out under harsh reaction conditions of high temperature and high pressure. With the increasingly serious global environment and the increasing depletion of energy, the development of new synthetic ammonia technology under mild conditions has been a long-term unremitting pursuit of scientific researchers and a very challenging research topic.
[0005] N2 is a highly stable chemical molecule with a bond energy of up to 945 kJ / mol. Therefore, it is very difficult to activate N2 and convert it into other nitrogen-containing compounds. Generally, high temperatures are applied to accelerate molecular motion, which weakens the N≡N bond. Therefore, the activation of N2 requires high energy consumption. In the electromagnetic induction system, when a magnetic field is applied, the unpaired electrons in the ferromagnetic material are arranged in a specific direction. When the magnetic field is reversed, the arranged magnetic moment is deflected, and the magnetization curve shows "hysteresis behavior", converting electromagnetic energy into heat energy through hysteresis loss. Therefore, it is very promising to use the alternating magnetic field to directional arrange the electrons of ferromagnetic catalysts and the characteristics of in-situ heat supply to achieve low-temperature and normal-pressure synthesis of ammonia.
[0006] The ammonia synthesis reaction is an exothermic entropy reduction process. From a thermodynamic point of view, low temperature and high pressure are conducive to the formation of ammonia. However, the kinetic resistance of this reaction is large, and high temperature and high pressure reaction conditions are required to achieve a faster reaction rate. In recent decades, researchers have conducted extensive research on the ammonia synthesis process and developed a series of ammonia synthesis catalysts. In the thermal catalytic synthesis of ammonia, iron-based and ruthenium-based catalysts are mainly used. Iron-based catalysts are currently the only widely used catalysts and are an ideal ammonia synthesis catalyst. Compared with iron-based catalysts, ruthenium-based catalysts can catalyze the synthesis of ammonia under relatively mild conditions (temperature: 370-400°C, pressure: 5-10MPa). The disadvantage is that the cost is high and H2 has a strong inhibitory effect on the surface of metal ruthenium. However, thermal catalytic synthesis of ammonia has problems such as high energy consumption, slow heating process, low energy utilization efficiency, and serious environmental pollution. Therefore, researchers have explored alternative ways to synthesize green ammonia under other conditions. In electrochemical synthesis of ammonia, the activation degree of N2 molecules can be controlled by controlling the electrode potential, and the ammonia synthesis process can be regulated by controlling the transport rate of N2 and ions. However, the main challenges faced by electrochemical ammonia synthesis are low ammonia synthesis activity and poor selectivity. In photocatalytic ammonia synthesis, the band gap of the photocatalyst must not only meet the redox barrier of the N2 molecule, but also be as narrow as possible to increase the photon absorption efficiency. At the same time, it is necessary to further regulate the catalytic sites to promote the transfer of photogenerated electrons from the catalyst to the adsorbed N2 in order to improve the activation ability of N2. However, most materials cannot meet the above conditions required for photocatalytic ammonia synthesis. It can be seen that achieving low-energy green ammonia synthesis at low temperature and normal pressure is still a major challenge. Summary of the invention
[0007] In order to overcome the problems of high energy consumption in the prior art ammonia synthesis reaction and difficulty in activating N2 molecules at low temperature and normal pressure, the purpose of the present invention is to provide a catalyst for ammonia synthesis reaction and a preparation method and application thereof. The catalyst can realize green ammonia synthesis at room temperature and normal pressure. The catalyst acts as both an active center and a heating center in an alternating magnetic field, so it can greatly reduce heat loss and improve energy efficiency.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a catalyst for ammonia synthesis reaction comprises the following steps:
[0010] The solution containing an iron source, a surfactant, water and ethanol is uniformly mixed with the solution containing a cobalt salt, water and ethanol, and then crystallized at 30-40° C. for 24-36 hours to obtain a Prussian blue analog precursor;
[0011] The Prussian blue analog precursor is calcined at 500-700° C. for 2-3 hours to obtain a catalyst for ammonia synthesis reaction.
[0012] A further improvement of the present invention is that the iron source is one or more of Fe(NO3)3, FeCl3, FeC6H5O7 and K3[Fe(CN)6].
[0013] A further improvement of the present invention is that the surfactant is one or more of terephthalic acid, trimesic acid, urea and polyvinyl pyrrolidone.
[0014] A further improvement of the present invention is that the usage ratio of the iron source to the surfactant is 5-10 mmol:5-10 g.
[0015] A further improvement of the present invention is that in the solution containing the iron source, the surfactant, water and ethanol, the volume ratio of water to anhydrous ethanol is 1:1.
[0016] A further improvement of the present invention is that the usage ratio of the iron source to deionized water is 5-10 mmol:60-70 mL.
[0017] A further improvement of the present invention is that the cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt acetate and cobalt citrate dihydrate.
[0018] A further improvement of the present invention is that in the solution containing cobalt salt, water and ethanol, the dosage ratio of cobalt salt to water is 5-10mmol:60-70mL, and the volume ratio of water to ethanol is 1:1.
[0019] The inert gas is Ar or N2;
[0020] 2-10℃·min -1 The heating rate is increased to 500-700°C.
[0021] A catalyst for ammonia synthesis reaction, comprising a metal and a surface oxide, wherein the metal comprises Fe1Co3, Fe or Co; the surface oxide comprises FeCoO x ,FeO x or CoO x .
[0022] A catalyst for ammonia synthesis reaction is used in ammonia synthesis reaction. The catalyst is used for ammonia synthesis reaction under alternating magnetic field conditions, the pressure is normal pressure, and the magnetic field strength is 14-58 mT.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention adopts a coprecipitation method to prepare a ferromagnetic catalyst. Prussian blue is calcined at 500-700°C under an inert gas to remove cyanide and generate a ferromagnetic material containing Fe-Co alloy and FeCoOx oxide, i.e., a catalyst. The Fe-Co alloy serves as both a magnetic induction heating center and an active center for activating N2 and H2 molecules, and cooperates with an alternating magnetic field to achieve low-temperature and normal-pressure efficient synthesis of ammonia.
[0025] Furthermore, in the present invention, PVP acts as a binder to allow the carbonyl group in the pyrrolidone ring to interact with the nitrogen atom in the metal salt, and acts as a stabilizer to prevent ion aggregation during the synthesis process. In the present invention, the catalytic activity of the material can be significantly improved by converting Prussian blue Fe-Co / PBAs into corresponding derivatives.
[0026] The catalyst prepared by the present invention is subjected to the temperature range of 100°C to 300°C and 0.1 MPa, and the apparent activation energy (E a =4.558 kJ mol -1 ) and traditional thermal catalysis (E a =7.604 kJ mol -1 ) is much smaller than that of the catalyst. These results show that the alternating magnetic field significantly reduces the apparent activation energy of the reaction of synthesizing ammonia, thereby increasing the reaction rate of synthesizing ammonia at room temperature and pressure. The catalyst prepared by the present invention has high ammonia synthesis activity and can synthesize ammonia greenly at room temperature and pressure. The reaction rate of ammonia synthesis catalyzed by magnetic induction is nearly ten times higher than that of ordinary thermal catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Fe-Co@FeCoO at 300K x 、Fe@FeO x 、Co@CoO x and FeCoO x VSM diagram;
[0028] Figure 2 Fe-Co@FeCoO x 、Fe@FeO x 、Co@CoO x and FeCoO x XRD pattern of
[0029] Figure 3 It is a structural schematic diagram of a magnetic induction catalytic reaction device;
[0030] In the figure, 1 is a nitrogen cylinder, 2 is a hydrogen cylinder, 3 is a first mass flow controller, 4 is a second mass flow controller, 5 is an MIH fixed bed reactor, 6 is an infrared camera, and 7 is a container. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0032] Since the ammonia synthesis reaction is an exothermic process, low temperature is conducive to the reaction, while the N≡N bond needs to be activated at high temperature (400-500°C). This contradiction leads to a generally low yield in the ammonia synthesis reaction. In order to obtain a high NH3 yield, a feasible solution is to activate N2 at a lower temperature. This invention is the first to use ferromagnetic catalysts for magnetic induction catalytic synthesis of ammonia under an alternating magnetic field, and prepare a series of ferromagnetic materials (Fe-Co@FeCoO x 、Fe@FeO x 、Co@CoO x 、FeCoO x ), where Fe-Co@FeCoO x The maximum reaction rate of the catalyst at normal pressure and low temperature (220°C) can reach 1257 μmol g -1 h -1 Compared with thermal catalysis at the same NH3 synthesis rate, magnetic induction catalysis can reduce the bed temperature by about 500°C. Compared with thermal catalysis under the same conditions, magnetic induction catalysis can increase the ammonia synthesis reaction rate by nearly ten times.
[0033] The present invention provides a method for preparing a catalyst for ammonia synthesis reaction, comprising the following steps:
[0034] 1) First, a certain amount of iron source and surfactant are dissolved in a mixed solution of deionized water and anhydrous ethanol, and stirred until the solid is completely dissolved to form solution A;
[0035] The iron source is one or more of Fe(NO3)3, FeCl3, FeC6H5O7 and K3[Fe(CN)6], preferably K3[Fe(CN)6] or Fe(NO3)3;
[0036] The surfactant is one or more of terephthalic acid (H2DBC), trimesic acid (H3BTC), urea and polyvinyl pyrrolidone (PVP), preferably polyvinyl pyrrolidone (PVP) or urea.
[0037] The dosage ratio of the iron source to the surfactant is 5-10 mmol:5-10 g. The volume ratio of deionized water to anhydrous ethanol is 1:1.
[0038] The usage ratio of iron source to deionized water is 5-10mmol:60-70mL.
[0039] 2) Dissolve the cobalt salt in a mixed solution of deionized water and anhydrous ethanol in a volume ratio of 1:1, and stir until the solid is completely dissolved to form solution B.
[0040] The cobalt salts are Co(NO3)2, CoCl2, (CH3COO)2Co and cobalt citrate dihydrate (C 12 H 14 Co3O 16 ), preferably Co(NO3)2 or CoCl2.
[0041] The dosage ratio of cobalt salt to deionized water is 5-10mmol:60-70mL.
[0042] 3) Then, solution A and solution B are mixed in a constant temperature water bath, and stirred for 1 hour until uniformly mixed to obtain a mixed solution, and the mixed solution is crystallized at 30-40°C for 24-36 hours, and the obtained product is collected by centrifugation, washed and dried with water and anhydrous ethanol for multiple times to obtain a spherical agglomerated Prussian blue analog precursor, and the obtained sample is recorded as Fe-CoPBAs. Among them, PBAs are Prussian blue analogs, which have the characteristics of simple preparation, uniform size, and variable composition, morphology and structure, and can be used as a precursor for synthesizing a rich active site.
[0043] 4) After purifying the quartz tube with inert gas, place the Fe-Co PBAs in the quartz tube and heat it in the inert gas at 2-10℃·min -1 The temperature was raised to 500-700°C at a heating rate of 1.5°C and calcined at 500-700°C for 2-3h to obtain a catalyst, which was recorded as Fe-Co@FeCoO x . Wherein, the inert gas is Ar or N2.
[0044] The catalyst prepared by the above method is composed of a metal and a surface oxide, wherein the metal includes Fe1Co3, Fe or Co; the surface oxide includes FeCoO x ,FeO x or CoO x ;
[0045] When used, the prepared shaped granular catalyst is filled into a quartz tube, and the quartz tube is placed in the induction coil area of the magnetic induction heating equipment. The reaction pressure is normal pressure, and the reaction temperature is 220°C generated by the ferromagnetic material itself. By adjusting the input voltage, the magnetic field strength can be varied between 14-58mT, and the N2:H2 feed ratio is 3:1.
[0046] Prussian blue is pyrolyzed in an inert gas to form a Fe1Co3 core with FeCoO on the surface. x Fe-Co@FeCoO x Ferromagnetic catalyst. The catalyst was placed in an alternating magnetic field and its activity in catalytic synthesis of ammonia was tested. In an alternating magnetic field, the unpaired electrons in the catalyst are arranged in a specific direction. When the magnetic field is reversed, the arranged magnetic moment is deflected, and the magnetization curve shows "hysteresis behavior". The electromagnetic energy is converted into heat energy through hysteresis loss, which can realize self-heating and self-catalysis of the catalyst, so that it can achieve excellent performance at a lower temperature. At the same time, magnetic induction heating can avoid the problems of high energy consumption, low energy utilization and uneven heating of traditional catalytic reactions. In a very local, fast and energy-saving way, it saves the need to heat the entire reaction system environment, making the reaction temperature milder and the energy consumption lower.
[0047] The obtained ferromagnetic material was mixed with an equal mass of white carbon black and pelletized to obtain particles with a diameter of 0.4 to 0.9 mm for activity evaluation.
[0048] The following are specific embodiments.
[0049] Example 1
[0050] 1) First, 5 mmol of an iron source and 5 g of a surfactant are dissolved in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and magnetically stirred for 1 h until the solid is completely dissolved to form a solution A, wherein the iron source is preferably K3[Fe(CN)6], and the surfactant is preferably polyvinylpyrrolidone (PVP).
[0051] 2) Dissolve 5 mmol of cobalt salt in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and stir magnetically for 1 hour until the solid is completely dissolved to form solution B, wherein the cobalt salt is preferably Co(NO3)2.
[0052] 3) Then, solution A and solution B were mixed in a constant temperature water bath, and stirred continuously for 1 hour until uniformly mixed, and the mixed solution was crystallized at 35° C. for 24 hours.
[0053] 4) Finally, the product in the mixed solution is collected by centrifugation, washed with water and anhydrous ethanol for multiple times and dried, and the obtained Prussian blue sample is recorded as Fe-Co PBAs.
[0054] 5) Fe-Co PBAs were heated in Ar atmosphere at 10 °C min -1 The temperature was raised to 600 °C at a heating rate of 1.50 °C and calcined at 600 °C for 2 h to obtain a catalyst, which was recorded as Fe-Co@FeCoO x .
[0055] Example 2
[0056] 1) First, 10 mmol of an iron source and 8 g of a surfactant were dissolved in a mixed solution of 70 mL of deionized water and 70 mL of anhydrous ethanol, and magnetic stirring was performed for 1 h until the solid was completely dissolved to form a solution A, wherein the iron source was FeCl3 and the surfactant was terephthalic acid.
[0057] 2) Then, 5 mmol of the cobalt salt was dissolved in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and magnetic stirring was performed for 1 h until the solid was completely dissolved to form solution B, in which the cobalt salt was CoCl2.
[0058] 3) Then, solution A and solution B were mixed in a constant temperature water bath, and stirred continuously for 1 hour until they were uniformly mixed. The mixed solution was crystallized at 30° C. for 36 hours.
[0059] 4) Finally, the product in the mixed solution is collected by centrifugation, washed with water and anhydrous ethanol for multiple times and dried, and the obtained Prussian blue sample is recorded as Fe-Co PBAs.
[0060] 5) Fe-Co PBAs were heated in N2 atmosphere at 10℃·min -1 The temperature was raised to 600°C at a heating rate of and calcined at 600°C for 2h to obtain a catalyst.
[0061] Example 3
[0062] 1) First, 7 mmol of iron source and 10 g of surfactant were dissolved in a mixed solution of 65 mL of deionized water and 65 mL of anhydrous ethanol, and magnetic stirring was performed for 1 h until the solid was completely dissolved to form solution A, wherein the iron source was FeC6H5O7 and the surfactant was trimesic acid.
[0063] 2) 8 mmol of the cobalt salt was dissolved in a mixed solution of 65 mL of deionized water and 65 mL of anhydrous ethanol, and magnetic stirring was performed for 1 h until the solid was completely dissolved to form a solution B, in which the cobalt salt was (CH3COO)2Co.
[0064] 3) Then, solution A and solution B were mixed in a constant temperature water bath, and stirred continuously for 1 hour until they were uniformly mixed. The mixed solution was crystallized at 40° C. for 24 hours.
[0065] 4) Finally, the product in the mixed solution is collected by centrifugation, washed with water and anhydrous ethanol for multiple times and dried, and the obtained Prussian blue sample is recorded as Fe-Co PBAs.
[0066] 5) Fe-Co PBAs were heated in Ar atmosphere at 5 °C min -1 The temperature was raised to 700°C at a heating rate of and calcined at 700°C for 2 h to obtain a catalyst.
[0067] Example 4
[0068] 1) First, 5 mmol of iron source and 5 g of surfactant were dissolved in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and magnetically stirred for 1 h until the solid was completely dissolved to form solution A, wherein the iron source was Fe(NO3)3 and the surfactant was urea.
[0069] 2) 10 mmol of the cobalt salt was dissolved in a mixed solution of 70 mL of deionized water and 70 mL of anhydrous ethanol, and magnetic stirring was performed for 1 hour until the solid was completely dissolved to form a solution B, in which the cobalt salt was cobalt citrate dihydrate.
[0070] 3) Then, solution A and solution B were mixed in a constant temperature water bath, and stirred continuously for 1 hour until they were uniformly mixed. The mixed solution was crystallized at 35° C. for 30 hours.
[0071] 4) Finally, the product in the mixed solution is collected by centrifugation, washed with water and anhydrous ethanol for multiple times and dried, and the obtained Prussian blue sample is recorded as Fe-Co PBAs.
[0072] 5) Fe-Co PBAs were heated in Ar atmosphere at 2℃·min -1 The temperature was raised to 500°C at a heating rate of and calcined at 500°C for 3 h to obtain a catalyst.
[0073] Comparative Example 1
[0074] Preparation of Fe@FeO x ;
[0075] The same as Example 1, except that step 2) is: dissolving 5 mmol of iron salt in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and stirring magnetically for 1 hour until the solid is completely dissolved to form solution B, wherein the iron salt is preferably Fe(NO3)3. The other conditions remain the same.
[0076] Comparative Example 2
[0077] Preparation of Co@CoO x ;
[0078] The same as Example 1, except that step 1) is: 5 mmol of cobalt source and 5 g of surfactant are dissolved in a mixed solution of 60 mL of deionized water and 60 mL of anhydrous ethanol, and magnetic stirring is performed for 1 hour until the solid is completely dissolved to form solution A, wherein the iron source is preferably K3[Co(CN)6]. Other conditions remain the same.
[0079] Comparative Example 3
[0080] Preparation of FeCoO x ;
[0081] The same as Example 1, except that step 5) is: the obtained Prussian blue Fe-Co PBAs is heated in air at 10°C·min -1 The temperature was raised to 600°C at a heating rate of 1.5°C and calcined at 600°C for 2 h. Other conditions remained the same.
[0082] In order to compare the reaction rates of synthesizing ammonia under magnetic induction catalysis with different catalysts, the FeCoO prepared in Example 1 and Comparative Examples 1-3 were x 、Fe@FeO x 、Co@CoO x and Fe-Co@FeCoO x The catalytic activity of the catalyst for ammonia synthesis reaction was evaluated at room temperature and pressure. The evaluation results are shown in Table 1. Compared with other catalysts, Fe-Co@FeCoO x Ferromagnetic catalysts have the highest activity in synthesizing ammonia.
[0083] Table 1Fe-Co@FeCoO x 、Fe@FeO x 、Co@CoO x and FeCoO x Synthetic ammonia properties
[0084]
[0085] Catalytic performance evaluation:
[0086] The activity of N2-H2 electromagnetic induction ammonia synthesis was evaluated on a MIH fixed bed reactor by means of a magnetic induction heating device, see Figure 3 The magnetic induction heating device includes a nitrogen bottle 1 and a hydrogen bottle 2. The outlet of the nitrogen bottle 1 is connected to the MIH fixed bed reactor through a first mass flow controller 3, and the outlet of the hydrogen bottle 2 is connected to the MIH fixed bed reactor 5 through a second mass flow controller 4. An infrared camera 6 is arranged in the MIH fixed bed reactor 5. The inner diameter of the MIH fixed bed reactor 5 is 4 mm and the outer diameter is 10 mm. The outlet of the MIH fixed bed reactor 4 is connected to a container 7, and the container 7 is used to receive water generated by the reaction.
[0087] N2 and H2 are mixed into the reaction system in a volume ratio of 1:3, and the flow rate is controlled by a mass flowmeter. A fixed bed quartz tube reactor with an inner diameter of 4 mm and an outer diameter of 10 mm is used. The catalyst powder obtained in Example 1 is loaded into the quartz tube. The catalyst is supported by quartz wool above and below, and the catalyst bed temperature is monitored at all times by an infrared camera. MIH can generate an alternating magnetic field with a frequency of 78-103kHz. By adjusting the input voltage, the electromagnetic field strength can be varied between 14mt and 58mt. The reaction product NH3 is absorbed by H2O, and the NH4 in the product is determined by colorimetry. + concentration.
[0088] In order to compare the difference between magnetic catalysis and thermal catalysis, the Fe-Co@FeCoO prepared in Example 1 was x The catalytic activity of the catalyst for the ammonia synthesis reaction was evaluated on a conventional thermal catalytic fixed bed and a magnetic induction catalytic device. The evaluation results are shown in Table 2. Compared with thermal catalysis, at about 220°C under normal pressure, the reaction rate of ammonia synthesis by magnetic induction catalysis is nearly ten times higher than that of conventional thermal catalysis.
[0089] Table 2Fe-Co@FeCoO x Catalytic performance of ammonia synthesis under conventional thermal catalysis and magnetic catalysis
[0090]
[0091] The catalyst hysteresis loop (VSM) was obtained by testing on a Lake Shore 7404 vibrating sample magnetometer (USA). Figure 1 The VSM curve shows the hysteresis phenomenon of Prussian blue derivatives. At room temperature 300K, Fe-Co@FeCoO x It has obvious ferromagnetic ring behavior, indicating that it is a ferromagnetic material.
[0092] The powder X-ray diffraction (XRD) results of the catalyst were obtained by testing on a Rigaku Smart Lab diffractometer (Japan). Figure 2 .Fe-Co@FeCoO x The diffraction peaks at 2θ = 45.1° and 65.7° are characteristic peaks of Fe1Co3, corresponding to the (110) and (200) crystal planes (JCPDS No. 48-1818), respectively. It is worth noting that a new characteristic peak appears at 2θ = 30.6°, which is attributed to the FeCoO on the surface of Fe1Co3. x 、Fe@FeO x 、Co@CoO x and Fe-Co@FeCoO xThe results are similar, showing a mixed phase of metal and a small amount of oxide (JCPDS No.06-0696, JCPDS No.05-0727), FeCoO x It is a CoFe2O4 oxide with a spinel structure (JCPDS No.03-0864).
[0093] The present invention uses a coprecipitation method to prepare Fe-Co / PBAs derived Fe-Co@FeCoO x Ferromagnetic catalysts, in conjunction with alternating magnetic fields, achieve low-temperature and normal-pressure ammonia synthesis. The Fe-Co@FeCoOx catalyst exhibits excellent catalytic ability. In response to the current great demand for low-temperature and low-pressure green ammonia synthesis, the alternating magnetic field and catalyst have high energy utilization, uniform temperature distribution, simple equipment, and safe and controllable operation process, which greatly reduces the energy consumption of the reaction. Compared with traditional thermal catalysis under the same conditions, the alternating magnetic field can improve the performance of ammonia synthesis by nearly ten times. The reasons for this difference were preliminarily explored, and through kinetic analysis, it was found that the alternating magnetic field reduced the apparent activation energy of the ammonia synthesis reaction. The Fe-Co@FeCoO x Apparent activation energy of the catalyst. The apparent activation energy (E a =4.558 kJ mol -1 ) and traditional thermal catalysis (E a =7.604 kJ mol -1 ) is much smaller than that of the conventional thermal catalysis. These results indicate that the alternating magnetic field significantly reduces the apparent activation energy of the reaction for synthesizing ammonia, thereby increasing the reaction rate for synthesizing ammonia at room temperature and pressure. Therefore, the alternating magnetic field is expected to provide new possibilities for promoting other traditional thermal reactions. This system can avoid the problems of high energy consumption, low energy utilization and uneven heating in traditional thermal catalysis.
[0094] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0095] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a catalyst for ammonia synthesis reaction, characterized in that: The following steps are involved: The solution containing an iron source, a surfactant, water and ethanol is uniformly mixed with the solution containing a cobalt salt, water and ethanol, and then crystallized at 30-40° C. for 24-36 hours to obtain a Prussian blue analog precursor; The Prussian blue analog precursor is calcined at 500-700° C. for 2-3 hours to obtain a catalyst for ammonia synthesis reaction.
2. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: The iron source is one or more of Fe(NO3)3, FeCl3, FeC6H5O7 and K3[Fe(CN)6].
3. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: The surfactant is one or more of terephthalic acid, trimesic acid, urea and polyvinyl pyrrolidone.
4. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: The usage ratio of the iron source and the surfactant is 5-10mmol:5-10g.
5. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: In the solution containing an iron source, a surfactant, water and ethanol, the volume ratio of water to anhydrous ethanol is 1:
1.
6. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: The usage ratio of iron source to deionized water is 5-10mmol:60-70mL.
7. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: The cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt acetate and cobalt citrate dihydrate.
8. The method for preparing a catalyst for ammonia synthesis reaction according to claim 1, characterized in that: In the solution containing cobalt salt, water and ethanol, the ratio of cobalt salt to water is 5-10mmol:60-70mL, and the volume of water to ethanol is 1:1; The inert gas is Ar or N2; 2-10℃·min -1 The heating rate is increased to 500-700°C.
9. A catalyst prepared according to the method according to any one of claims 1 to 8, characterized in that: It includes metal and surface oxide, wherein the metal includes Fe1Co3, Fe or Co; the surface oxide includes FeCoO x ,FeO x or CoO x .
10. Use of a catalyst prepared according to the method according to any one of claims 1 to 8 in ammonia synthesis reaction, characterized in that: The catalyst is subjected to a synthetic ammonia reaction under an alternating magnetic field, the pressure is normal pressure, and the magnetic field strength is 14-58 mT.
Citation Information
Cited By
Method for synthesizing ammonia by using iron-based catalyst