A method for preparing barium titanate nanopowder and a chip-type multilayer ceramic capacitor

By combining microwave heating and ultraviolet irradiation, barium titanate nanoparticles were prepared by low-temperature crystallization, which solved the problems of powder agglomeration and uneven performance in the existing technology. This method achieved the preparation of high-purity, ultrafine, and narrow-distribution barium titanate powder, thereby improving the dielectric properties of MLCCs.

CN123105705APending Publication Date: 2026-11-17SHENZHEN THREE-CIRCLE ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611083622.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare high-purity, ultrafine, and narrowly distributed barium titanate powder, and high-temperature calcination leads to severe powder agglomeration, affecting its performance.

Method used

By employing the combined effects of microwave heating and ultraviolet irradiation, titanium source, barium source, and template agent are mixed to form a supercritical state, and low-temperature crystallization is used to prepare nano-barium titanate powder, avoiding high-temperature calcination.

Benefits of technology

Barium titanate nanoparticles with narrow particle size distribution, high crystallinity, and good dispersibility were prepared to meet the dielectric performance requirements of high-performance MLCCs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention belongs to the technical field of multilayer ceramic chip capacitors, specifically disclosing a method for preparing nano-barium titanate powder and a multilayer ceramic chip capacitor. The method for preparing nano-barium titanate powder includes the following steps: mixing raw materials including a titanium source, a barium source, and a template agent to obtain a mixed liquid; using microwave heating and ultraviolet light irradiation to bring the mixed liquid to a supercritical state, obtaining pre-crystallized barium titanate particles; and crystallizing the pre-crystallized barium titanate particles to obtain the nano-barium titanate powder. The preparation method of this invention uses a titanium source, a barium source, and a template agent as reactants, obtaining pre-crystallized barium titanate particles through photothermal synergy, followed by low-temperature calcination, effectively avoiding the powder agglomeration problem caused by traditional high-temperature calcination. The resulting nano-barium titanate powder has a narrow particle size distribution, high crystallinity, high dielectric constant, and low dielectric loss, meeting the requirements of high-performance MLCC products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chip multilayer ceramic capacitor technology, and particularly to a method for preparing nano-barium titanate powder and a chip multilayer ceramic capacitor. Background Technology

[0002] Perovskite-type barium titanate is a core powder raw material for the preparation of functional ceramics, and is widely used in piezoelectric elements, optoelectronic devices, semiconductor ceramics, sensors, and multilayer ceramic capacitors (MLCCs). In recent years, MLCCs have been developing towards higher capacitance, requiring increased layer count and improved dielectric constant. Therefore, barium titanate raw materials are required to possess characteristics such as high purity, ultrafine particle size, high crystallinity, narrow distribution, and uniform Ba / Ti ratio.

[0003] Currently, barium titanate powder is mainly prepared by solid-state synthesis and oxalic acid precipitation synthesis. The solid-state synthesis method uses TiO2 and BaCO3 powders as raw materials, which are dispersed through mixing, stirring, and milling, followed by high-temperature calcination to obtain barium titanate. This method yields a product with high crystallinity, but the powder particle size is limited by the raw material particle size, making it difficult to stably prepare ultrafine powders, and the Ba / Ti ratio distribution is uneven. While the oxalic acid precipitation synthesis method can improve the powder morphology, the synthesis process is complex, and batch-to-batch consistency and insufficient crystallinity are easily caused by concentration fluctuations and incomplete reactions. Furthermore, both methods require high-temperature calcination, resulting in severe internal agglomeration of the obtained powder, significantly affecting its performance. Summary of the Invention

[0004] In order to overcome at least one of the technical problems existing in the prior art, one of the objectives of the present invention is to provide a method for preparing nano barium titanate powder.

[0005] The second objective of this invention is to provide a chip-type multilayer ceramic capacitor.

[0006] The third objective of this invention is to provide the application of the nano-barium titanate powder prepared by the above method in functional ceramic products.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of this invention provides a method for preparing barium titanate nanoparticles, comprising the following steps: The raw materials, including titanium source, barium source and template agent, are mixed to obtain a mixture; The mixture was heated by microwave and irradiated with ultraviolet light to bring it to a supercritical state, thereby obtaining pre-crystallized barium titanate particles. The initially crystallized barium titanate particles are crystallized to obtain the nano-barium titanate powder. The power of the microwave heating is 40-100kW; The wavelength of the ultraviolet light irradiation is 200-400nm; The crystallization temperature is 500~800℃.

[0008] The method for preparing nano-barium titanate powder of the present invention involves mixing a precursor titanium source, a barium source, and a template agent, and then obtaining pre-crystallized barium titanate particles through the synergistic effect of microwave heating and ultraviolet light irradiation. High-purity, narrow-particle-size nano-barium titanate powder is then directly obtained through low-temperature crystallization. In this invention, the supercritical state refers to the state where the temperature and pressure in the reaction system reach critical conditions, at which point the boundary between the liquid and gaseous states disappears, transforming the system into a supercritical fluid, thereby significantly increasing the reaction rate.

[0009] Taking titanium tetrachloride as an example, the inventive principle of this invention is as follows: (1) Hydrolysis of titanium source: TiCl4 + H2O → TiOCl2 + 2HCl; (2) Titanium source, barium source, and template agent are mixed together and co-precipitated by photothermal synergistic treatment (i.e., microwave heating and ultraviolet irradiation) to obtain pre-crystallized barium titanate particles: TiOCl2 + BaCl2 + H2O → BaTiO3 + HCl The preparation method of the present invention mixes titanium source, barium source and template agent together, and obtains initially crystalline barium titanate particles through photothermal synergistic treatment. By mixing all raw materials together, the initial concentration of the reaction system can be increased, the collision probability between reactants can be increased, and rapid nucleation can be promoted, thereby refining the particle size of the initially crystalline barium titanate particles.

[0010] The fundamental difference between the photothermal synergistic effect and the traditional oxalic acid precipitation method lies in the heating and reaction methods. The traditional oxalic acid precipitation method uses external heating, which easily leads to uneven local temperatures in the reaction system, resulting in uneven synthesis reactions between the barium and titanium sources, and differences in the composition and particle size of the final product. Furthermore, this method typically uses a dropwise addition method, leading to different growth and crystallization times for the products at the beginning, middle, and end of the reaction, resulting in inconsistent crystallinity of the final barium titanate nanoparticles, thus affecting the dielectric properties of MLCCs. The advantages of the photothermal synergistic effect are reflected in two aspects: heating method and reaction control. In terms of heating, microwaves directly act on each water molecule, causing internal vibration and heating, achieving uniform heating from the inside out, thus ensuring a highly consistent thermal field throughout the reaction system. In terms of reaction control, mixing all reactants together before heating allows for synchronized growth and crystallization times at each stage, ensuring the stability of the crystallinity of the final barium titanate nanoparticles. In addition, ultraviolet irradiation can induce the photocatalytic reaction of the precursor TiO2, effectively reducing the generation of oxygen vacancies during the reaction, thereby obtaining well-crystallized and fine-sized primary barium titanate particles.

[0011] This invention can crystallize barium titanate at a low temperature of 500~800℃, which is much lower than the high temperature of 1200℃ or above required by traditional processes. The preparation method of this invention does not require high-temperature calcination, and can effectively suppress hard agglomeration between particles and significantly improve the dispersibility of powder.

[0012] In some embodiments of the present invention, the mixture further contains water as a solvent.

[0013] In some embodiments of the present invention, the power of the microwave heating is any value or a range formed by any combination of 40kW, 50kW, 60kW, 70kW, 80kW, 90kW, and 100kW. In some preferred embodiments of the present invention, the power of the microwave heating is 60-80kW.

[0014] Microwave heating power has a significant impact on the synthesis of barium titanate. When the microwave heating power is below 40kW, the heating driving force is insufficient, the reaction is incomplete, leading to an imbalance in the Ba / Ti stoichiometric ratio in the initially crystallized barium titanate particles, and the final product performance is unqualified. When the microwave heating power is within the range specified in this invention, i.e., 40-100kW, the heating power is sufficient, the reaction is complete, the Ba / Ti ratio of the precursor is appropriate, and the crystallinity of both the initially crystallized barium titanate particles and the final powder meets the requirements. When the microwave heating power is above 100kW, the heating rate is too fast, the reaction temperature is too high, causing the titanium phase of the precursor to precipitate during the reaction, generating a second phase, ultimately leading to abnormal particle growth of the barium titanate powder.

[0015] In some embodiments of the present invention, the wavelength of the ultraviolet light irradiation is any value or a range formed by any two of 200nm, 220nm, 250nm, 280nm, 300nm, 320nm, 350nm, 380nm, and 400nm. In some preferred embodiments of the present invention, the wavelength of the ultraviolet light irradiation is 280-320nm.

[0016] Ultraviolet (UV) irradiation is a key factor in inducing the primary crystallization of barium titanate, and its wavelength has a decisive influence on the reaction effect. When the irradiation wavelength is below 200 nm, the excitation energy is too high, causing the precursor TiO2 to generate a large number of electron-hole pairs, reducing the barium source, resulting in a severe imbalance in the Ba / Ti molar ratio of the final product, leading to product defects. When the irradiation wavelength is within the range of this invention, the excitation energy is moderate, which can effectively activate the catalytic effect of TiO2, promote the co-precipitation of titanium and barium, and accelerate the reaction. When the irradiation wavelength is above 400 nm, the excitation energy is insufficient, failing to initiate the catalytic effect of TiO2, resulting in a slow co-precipitation reaction, and ultimately incomplete reaction between the barium and titanium sources, leading to insufficient crystallinity of the product and affecting the performance of the final product.

[0017] In some embodiments of the present invention, the crystallization temperature is any value or a range formed by any combination of 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, and 800°C. In some preferred embodiments of the present invention, the crystallization temperature is 600-700°C. The crystallization temperature has a significant impact on the grain size and crystallinity of barium titanate. When the temperature is below 500°C, the reaction of Ba and Ti in the system is incomplete, resulting in small grain size and insufficient crystallinity in the primary crystal particles and the final powder. When the crystallization temperature is within the range of the present invention, the Ba and Ti in the system can react completely, and the grain size and crystallinity of the primary crystal particles and the final powder both meet the requirements. When the temperature is above 800°C, the primary crystal particles and the final powder undergo excessive growth. Although the crystallinity of the final product is qualified, the grain size is too large, causing the obtained powder to not meet the requirements for use.

[0018] In some embodiments of the present invention, the preparation method further includes the steps of cleaning and drying the obtained barium titanate nanoparticles.

[0019] In some embodiments of the present invention, the cleaning is performed by solvent cleaning of the barium titanate nanoparticles to reduce the chloride ion content in the barium titanate nanoparticles to <70ppm (obtained by potentiometric titration).

[0020] In some embodiments of the present invention, the drying temperature is 100~150°C.

[0021] In some embodiments of the present invention, the drying time is 5 to 10 hours.

[0022] In some embodiments of the present invention, the concentration of titanium ions in the titanium source in the mixture is 2-5 mol / L, for example, it can be any value or a range formed by any two of 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, and 5 mol / L. In some preferred embodiments of the present invention, the concentration of titanium ions in the titanium source in the mixture is 3-4 mol / L. When the titanium ion concentration is 2-5 mol / L, i.e., within the range of the present invention, as the titanium ion concentration increases, the precursor solid content increases, and the system viscosity continuously increases (10,000-30,000 cps within the acceptable range, viscosity at room temperature tested using a rheometer). According to the nucleation theory, the nucleation process dominates at this time, and the particle size of the initially crystallized barium titanate particles shows a trend of first decreasing and then increasing, but always within the acceptable range (i.e., <1 μm). Under the same post-processing, the size of the final product barium titanate powder is also within the acceptable range. Too high or too low a concentration of titanium ions can easily lead to the agglomeration or abnormal growth of the initially crystallized barium titanate particles, resulting in barium titanate powder that does not meet the requirements for use.

[0023] In some embodiments of the present invention, the molar ratio of barium ions in the barium source to titanium ions in the titanium source in the mixture is (1-1.05):1. For example, it can be any value or a range formed by any two of 1:1, 1.01:1, 1.02:1, 1.03:1, 1.04:1, 1.05:1. The formation mechanism of barium titanate is essentially a process of continuous diffusion and reaction of Ba to Ti. When the molar ratio of Ba ions to Ti ions is within the range defined by the present invention, the Ba and Ti in the system are uniformly distributed, and the diffusion of Ba to Ti is also uniform. At this time, the particle size and viscosity of the precursor are also within a suitable range. Under the same post-processing conditions, the particle size and Ba / Ti molar ratio of the resulting finished powder are both qualified. However, when the molar ratio of Ba ions to Ti ions deviates from the range of the present invention, whether too high or too low, it is easy to cause the initially crystallized barium titanate particles to agglomerate and grow abnormally large, thereby causing the particle size, crystallinity, and Ba / Ti molar ratio of the final barium titanate product to exceed the qualified indicators.

[0024] In some embodiments of the present invention, the titanium source includes at least one of titanium tetrachloride, titanium sulfate, and tetrabutyl titanate.

[0025] In some embodiments of the present invention, the barium source includes at least one of barium chloride, barium hydroxide, and barium sulfate.

[0026] In some embodiments of the present invention, the template agent includes at least one of polyvinylpyrrolidone, dodecyltrimethylammonium bromide, and sodium dodecylbenzenesulfonate.

[0027] In some embodiments of the present invention, the added mass of the template agent is 1-5 wt% of the theoretical yield of barium titanate, for example, it can be any value among 1 wt%, 2 wt%, 3 wt%, 4 wt%, and 5 wt%, or a range formed by any two of these. In some preferred embodiments of the present invention, the added mass of the template agent is 2.5-3.5 wt% of the theoretical yield of barium titanate. When the amount of template agent added is within the range defined by the present invention, the guiding effect of the template agent is good, which can effectively guide the barium titanate particles to grow in the designed orientation, resulting in small primary crystal particles and final powder particles with a narrow particle size distribution, and the grain size meets the requirements. If the amount of template agent added is too large, the guiding effect is too strong, which easily generates two-dimensional plate-like by-products, and too much template agent will hinder degassing during the post-processing, ultimately leading to abnormal growth of barium titanate powder grains, exceeding the size standard and becoming unqualified.

[0028] In some embodiments of the present invention, the stirring rate during mixing is 50-100 rpm; in some embodiments of the present invention, the stirring rate during mixing is any value of 50 rpm, 60 rpm, 70 rpm, 80 rpm, 90 rpm, 100 rpm, or a range formed by any two of these values.

[0029] In some embodiments of the present invention, the mixing time is 100-200 min; in some embodiments of the present invention, the mixing time is any value of 100 min, 120 min, 140 min, 150 min, 160 min, 180 min, 200 min, or a range formed by any two of these values.

[0030] In some embodiments of the present invention, the mixing temperature is 60-100°C; in some embodiments of the present invention, the mixing temperature is any value of 60°C, 70°C, 80°C, 90°C, 100°C, or a range formed by any two of them.

[0031] In some embodiments of the present invention, the crystallization time is 1-5 hours, which can be any value of 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, or a range formed by any two of them.

[0032] In some embodiments of the present invention, the particle size of the nano-barium titanate powder is 100~120nm.

[0033] In some embodiments of the present invention, the molar ratio of barium to titanium in the nano barium titanate powder is (0.98~1.02):1, for example, it can be any value among 0.98:1, 0.99:1, 1.0:1, 1.01:1, 1.02:1 or any range formed by both.

[0034] In some embodiments of the present invention, the agglomeration index of the nano-barium titanate powder is less than 1; in some embodiments of the present invention, the agglomeration index of the nano-barium titanate powder is 0.45-0.7, for example, it can be any value among 0.45, 0.5, 0.55, 0.6, 0.65, 0.7 or a range formed by any two of them.

[0035] In some embodiments of the present invention, the dielectric constant of the nano-barium titanate powder is >2500; in some embodiments of the present invention, the dielectric constant of the nano-barium titanate powder is 2505-2700, for example, it can be any value or a range formed by any two of 2505, 2510, 2520, 2530, 2540, 2550, 2560, 2570, 2580, 2590, 2610, 2620, 2630, 2640, 2650, 2660, 2670, 2680, 2690, 2700.

[0036] In some embodiments of the present invention, the dielectric loss of the nano-barium titanate powder is <0.02; in some embodiments of the present invention, the dielectric loss of the nano-barium titanate powder is 0.01-0.019, for example, it can be any value or a range formed by any two of 0.01, 0.011, 0.012, 0.013, 0.014, 0.015, 0.016, 0.017, 0.018, and 0.019.

[0037] A second aspect of the present invention provides a chip-type multilayer ceramic capacitor, comprising a ceramic dielectric layer, wherein the raw material for preparing the ceramic dielectric layer comprises barium titanate nanoparticles, and the barium titanate nanoparticles are prepared by the preparation method described in the first aspect of the present invention.

[0038] The third aspect of the present invention provides the application of the barium titanate nanoparticles prepared by the preparation method described in the first aspect of the present invention in functional ceramic products.

[0039] In some embodiments of the present invention, the functional ceramic products include multilayer ceramic chip capacitors, multilayer ceramic chip inductors, and resistance temperature detectors (RTDs).

[0040] Compared with existing technologies, the beneficial effects of this invention are as follows: The preparation method of this invention uses titanium source, barium source, and template agent as reaction raw materials, and obtains pre-crystallized barium titanate particles through photothermal synergy. After low-temperature calcination, the powder agglomeration problem caused by traditional high-temperature calcination is effectively avoided. The resulting nano-barium titanate powder has a narrow particle size distribution, high crystallinity, high dielectric constant, and low dielectric loss, meeting the requirements of high-performance MLCC products. This preparation method is simple, with mild reaction conditions, low energy consumption, and produces nano-barium titanate powder with uniform particle size, good dispersibility, and excellent crystallinity. Detailed Implementation

[0041] The following examples provide a more detailed description of the specific implementation of the present invention, but the implementation and protection of the present invention are not limited thereto. It should be noted that any processes not specifically described below are methods that can be implemented or understood by those skilled in the art by referring to existing technology. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0042] Example 1 This example provides a method for preparing nano-barium titanate powder, the specific steps of which are as follows: S1: Mix titanium tetrachloride, barium chloride, template agent polyvinylpyrrolidone, and water together to obtain a mixture; In the mixture, the concentration of Ti ions in titanium tetrachloride is 3.5 mol / L, and the molar ratio of Ba ions to Ti ions in the mixture is 1:1; the added mass of the template agent is 3 wt% of the theoretical synthesis mass of the nano-barium titanate powder. The mixing was carried out by stirring at a speed of 80 rpm for 150 min at a temperature of 80℃. S2: The obtained mixture was heated to a supercritical state by microwave heating with a power of 70kW, and simultaneously irradiated with ultraviolet light with a wavelength of 300nm. The reaction time was 80min. After the reaction, the mixture was washed with water to obtain pre-crystallized barium titanate particles. S3: The obtained pre-crystallized barium titanate particles are directly crystallized at low temperature to obtain barium titanate nanopowder; wherein, the low-temperature crystallization temperature is 650℃ and the time is 3h; S4: The barium titanate nanoparticles obtained in S3 are cleaned and dried to obtain barium titanate nanoparticles with high purity and narrow particle size distribution. The cleaning process requires that the chloride ion content in the barium titanate nanoparticles after cleaning be controlled to be <70ppm (obtained by potentiometric titration). The drying temperature is 120℃ and the drying time is 7h.

[0043] The preparation parameters involved in the preparation method in this example are shown in Table 1 below.

[0044] Examples 2-5 The only difference between the preparation methods of the nano barium titanate powder in Examples 2-5 and Example 1 is that the microwave heating power is different in step S2, as shown in Table 1 below.

[0045] Examples 6-9 The only difference between the preparation method of the nano barium titanate powder in Examples 6-9 and Example 1 is that the wavelength of the ultraviolet light used for ultraviolet irradiation in step S2 is different, as shown in Table 1 below.

[0046] Examples 10-13 The preparation methods of the nano barium titanate powder in Examples 10-13 differ from those in Example 1 only in that the low-temperature crystallization temperature is different in step S3, as shown in Table 1 below.

[0047] Comparative Examples 1-2 The only difference between the preparation method of the nano barium titanate powder in Comparative Examples 1-2 and Example 1 is that the microwave heating power is different in step S2, as shown in Table 1 below.

[0048] Comparative Examples 3-4 The only difference between the preparation method of the nano barium titanate powder in Comparative Examples 3-4 and Example 1 is that the wavelength of the ultraviolet light used for ultraviolet irradiation in step S2 is different, as shown in Table 1 below.

[0049] Comparative Examples 5-6 The only difference between the preparation method of the nano barium titanate powder in Comparative Examples 5-6 and Example 1 is that the low-temperature crystallization temperature in step S3 is different, as shown in Table 1 below.

[0050] Table 1. Partial preparation parameters of Examples 1-13 and Comparative Examples 1-6

[0051] Comparative Example 7 The only difference between the preparation method of the nano barium titanate powder in this example and that in Example 1 is that the conventional water bath heating method is used in step S2, and the heating temperature is 60°C. The rest is the same as in Example 1.

[0052] Comparative Example 8 The preparation method of the nano barium titanate powder in this example differs from that in Example 1 only in that microwave heating is performed in step S2, without ultraviolet irradiation; the rest is the same as in Example 1.

[0053] Performance testing: The properties of the barium titanate nanoparticles prepared in Examples 1-13 and Comparative Examples 1-8 were tested according to the following test methods: a) The particle size of the nano-barium titanate powder should meet the standard of 100~120nm; Test method: By preparing barium titanate nanoparticles on conductive adhesive, the morphology of the powder was photographed using FE-SEM. The particle size of the final barium titanate nanoparticles was obtained by statistically analyzing the average diameter of more than 600 particles in 3 images.

[0054] b) The Ba / Ti molar ratio should be between 0.98 and 1.02. Test method: Weigh 0.3g of nano barium titanate powder, then add 50wt% lithium tetraborate and 50wt% lithium metaborate of nano barium titanate powder. After mixing, melt the mixture at 1000℃ to form a glass slide sample to be tested. The Ba / Ti molar ratio of the nano barium titanate powder is tested by X-ray fluorescence spectrometry (XRF).

[0055] c) The crystallinity of the nano-barium titanate powder meets the standard of c / a > 1.0080; Test method: Weigh 0.5g of barium titanate nanoparticles, flatten the sample with a glass slide, and test the crystallinity of the barium titanate nanoparticles by X-ray diffraction (XRD).

[0056] d) Reunion Index T = (D 90 -D 10 ) / D 50 The standard for compliance is T < 1; Test method: The SEM test method described in a) above was used to obtain D. 10 D 50 D 90 The data is then used to calculate the reunion index according to the formula described above.

[0057] e) Dielectric constant and dielectric loss, the standard is: dielectric constant > 2500, dielectric loss < 0.02; Test method: 1) Sample preparation 1. Powder drying: Dry at 110℃ for 3 hours to remove moisture.

[0058] 2. Granulation: Mix the nano barium titanate powder with a PVA aqueous solution of 7wt% (the mass of PVA is 6% of the mass of the nano barium titanate powder) and pass through a 100-mesh sieve.

[0059] 3. Dry pressing: Then, place it into a mold with a diameter of 10 mm and a thickness of 1.5 mm, and hold it under pressure at 13 MPa for 2 minutes to obtain the green body; 4. Glue removal: Heat to 600℃ at a heating rate of 1.5℃ / min and hold for 2 hours; 5. Sintering: Hold at 1300℃ for 3 hours, then allow to cool naturally to obtain the sintered body.

[0060] 6. Grinding and polishing: Grinding to make the two sides of the sintered body parallel, smooth, and of uniform thickness.

[0061] 7. Electrode coating: Brush silver paste on both sides, then heat at 700℃ for 12 minutes; 2) Instruments: LCR meter / impedance analyzer (such as Keysight E4980A, E4991A), frequency: 1kHz, temperature: 25℃ (room temperature), if temperature spectrum required: -55℃~150℃, voltage: 0.5-1Vmms (small signal, to avoid ferroelectric nonlinearity); 3) Testing and Calculation 1. Measure capacitance C (F) and loss tanδ (direct reading); 2. Calculate the relative permittivity: Permittivity = C × d / (k × A), where d is the sample thickness (m) and A is the electrode area (m²). 2 k = 8.854 × 10 -12 F / m; The performance test results obtained according to the above test method are shown in Table 2 below.

[0062] Table 2 Performance Test Results

[0063] As shown in Table 1, the barium titanate nanoparticles prepared in Examples 1-13 have narrow particle size distribution, high crystallinity, low agglomeration index, high dielectric constant, and low dielectric loss. Specifically, the particle size of the barium titanate nanoparticles prepared in Examples 1-13 is 100~120nm, the Ba / Ti molar ratio is 0.98~1.02, the crystallinity c / a>1.0080, the agglomeration index T<1, the dielectric constant>2500, and the dielectric loss<0.02.

[0064] The embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof can be combined with each other unless otherwise specified.

Claims

1. A method for preparing nano-barium titanate powder, characterized in that, Includes the following steps: The raw materials, including titanium source, barium source and template agent, are mixed to obtain a mixture; The mixture was heated by microwave and irradiated with ultraviolet light to bring it to a supercritical state, thereby obtaining pre-crystallized barium titanate particles. The initially crystallized barium titanate particles are crystallized to obtain the nano-barium titanate powder. The power of the microwave heating is 40-100kW; The wavelength of the ultraviolet light irradiation is 200-400nm; The crystallization temperature is 500~800℃.

2. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, In the mixture, the concentration of titanium ions in the titanium source is 2-5 mol / L.

3. The method for preparing nano-barium titanate powder according to claim 2, characterized in that, The molar ratio of barium ions in the barium source to titanium ions in the titanium source in the mixture is (1-1.05):

1.

4. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, The titanium source includes at least one of titanium tetrachloride, titanium sulfate, and tetrabutyl titanate. And / or, the barium source includes at least one of barium chloride, barium hydroxide, and barium sulfate.

5. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, The template agent includes at least one of polyvinylpyrrolidone, dodecyltrimethylammonium bromide, and sodium dodecylbenzenesulfonate.

6. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, The amount of template agent added is 1-5 wt% of the theoretical yield of barium titanate.

7. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, The mixture has at least one of the following characteristics: (a1) The stirring rate during mixing is 50-100 rpm; (a2) The mixing time is 100-200 min; (a3) The mixing temperature is 60-100℃.

8. The method for preparing nano-barium titanate powder according to claim 1, characterized in that, The crystallization time is 1-5 hours.

9. A multilayer ceramic chip capacitor, comprising a ceramic dielectric layer, characterized in that, The raw materials for preparing the ceramic dielectric layer include barium titanate nanoparticles, which are prepared by the preparation method described in any one of claims 1-8.

10. The application of the nano-barium titanate powder prepared by the preparation method according to any one of claims 1-8 in functional ceramic products.