A non-contact solar interfacial evaporator for saline-alkali land remediation, its preparation method and application
By employing a conical aluminum substrate with separately arranged capillary salt-collecting fiber paper and photothermal layer in a solar interface evaporator, the problem of salt scale accumulation is solved, achieving efficient evaporation and salt resource recovery, which is suitable for saline-alkali land remediation and freshwater resource regeneration.
Patent Information
- Application Number
- CN202611204846.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solar interface evaporators suffer from scale buildup in seawater desalination and high-salinity brine treatment, leading to decreased photothermal conversion efficiency and insufficient equipment stability, making it difficult to achieve efficient evaporation and salt resource recovery.
The system employs a separate capillary salt-collecting fiber paper and a conical aluminum substrate coated with a black photothermal layer to form a physically isolated double-layer structure. Salt crystallizes and precipitates directionally within the fiber paper, avoiding contact with the photothermal layer. The fiber paper can be replaced multiple times, enabling salt resource recovery.
It achieves high photothermal conversion efficiency, long-lasting anti-scaling and stable water production, extends equipment life, is suitable for remote areas without power grids, and supports saline-alkali land restoration and freshwater resource regeneration.
Smart Images

Figure CN123105772A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional materials technology, and relates to functional materials for the restoration of water resources in saline-alkali land by photothermal means and their preparation methods. Specifically, it relates to a non-contact solar interface evaporator for the restoration of saline-alkali land, its preparation method and application. Background Technology
[0002] In the large-scale application of seawater desalination and high-salinity brine resource utilization, the disposal of high-salinity concentrated wastewater is a severe challenge facing the industry. Current data shows that global seawater desalination produces a total of 142 million cubic meters of concentrated brine daily, an increase of approximately 50% compared to previous statistics. The disposal of high-salinity concentrated wastewater is costly, and direct discharge into the ocean can disrupt nearshore salinity balance, harm marine communities, and cause irreversible ecological negative impacts. Solar-driven interfacial evaporation technology, relying on a localized photothermal regulation mechanism, selectively heats only the water-air interface, eliminating the need for overall water heating and significantly reducing energy loss. Combined with evaporation devices made from nanomaterials and biomimetic water-conveying structures, steam conversion efficiency can exceed 90%, providing a green and low-cost new approach for seawater desalination and high-salinity brine resource utilization, and possessing promising prospects for large-scale engineering applications.
[0003] However, the current application of solar interfacial evaporation technology faces a core technical bottleneck: salt scaling. During evaporation, the diffusion of salt ions at the water-air interface is limited, leading to a continuous surge in local salt concentration and the continuous precipitation and deposition of salt crystals on the device surface. Salt scale, on the one hand, covers the photothermal absorption layer, weakening the ability to capture sunlight and reducing photothermal conversion efficiency; on the other hand, it blocks capillary water transport channels, cutting off the continuous water supply and causing rapid degradation of evaporation performance under long-term operation.
[0004] Existing anti-scaling technologies have significant drawbacks, failing to simultaneously ensure long-term stable operation and salt resource recovery. The first type involves brine recirculation and dilution, along with antifouling coating protection. This approach dilutes the bulk solution through recirculated concentrated brine or relies on a coating to delay salt accumulation. However, this only provides short-term relief and cannot recover salt, continuously generating high-salt wastewater and increasing the burden on end-of-pipe wastewater treatment and ecological pollution risks. The second type involves directional salt accumulation structures. By controlling the internal temperature, pressure, and salt concentration gradient of the evaporator, salt is guided to crystallize and precipitate in a predetermined area, achieving salt resource recovery. However, in this type of solution, the integrated design of the photothermal layer and water delivery channel means that over time, salt crystals gradually migrate and accumulate towards the photothermal absorption interface, ultimately contaminating the photothermal functional layer, leading to a continuous decline in evaporation efficiency and insufficient long-term operational stability of the equipment.
[0005] In summary, existing solar interface evaporators cannot simultaneously achieve high photothermal conversion efficiency, long-term salt scale isolation, stable water production, and simultaneous salt resource recovery, which restricts their large-scale promotion in the fields of seawater desalination concentrated brine treatment and high-salt brine remediation. The industry urgently needs to develop a non-contact solar interface evaporation device that can achieve physical isolation between the photothermal layer and the salt accumulation area, long-term salt scale resistance, and stable evaporation performance. Summary of the Invention
[0006] To address the shortcomings of the existing technologies, the present invention aims to provide a non-contact solar interface evaporator for saline-alkali land remediation, its preparation method, and its application. This invention achieves salt crystal confinement in the outer fiber paper, completely isolating the photothermal aluminum substrate from salt scale corrosion, resulting in excellent evaporation rate and salt collection efficiency. The fiber salt collection layer can be replaced multiple times, and the main performance of the device remains unchanged. Furthermore, the preparation process is simple and the raw material cost is low.
[0007] This invention is achieved through the following technical solution: A method for preparing a non-contact solar interface evaporator for saline-alkali land remediation includes the following steps: Step 1: Take 20-25% carbon black, 30-35% wetting and dispersing agent, 0.5-1% anti-settling agent, 3-5% humectant, and the remainder is deionized water by mass fraction. After stirring evenly, grind and filter to obtain a nano black pigment with a particle size D50 of 40 nm. Step 2: Select a cone-shaped aluminum substrate and polish the surface of the substrate with 800-grit sandpaper to achieve a surface roughness Ra value of 0.8 μm to 1.6 μm. Spray the black pigment obtained in Step 1 evenly onto the outer surface of the cone and cure it to form a high solar energy absorption radiation layer with a thickness of 50 to 70 μm, thus obtaining an aluminum substrate with a black photothermal layer. Step 3: Pulp the wood fibers, controlling the freeness to 20°SR~35°SR. Add 5%~15% of resin / emulsion by weight of oven-dry wood fibers to the resulting pulp, stir and mix at room temperature for 1~1.5 h, and finally add water and stir evenly to obtain a pulp suspension with a solid content of 5.0%~5.5%. Step 4: Spread the pulp suspension on a circular mold to form a wet paper sheet. After drying and cutting, the paper is bonded together with double-sided adhesive to form a cone-shaped fiber paper with a thickness of 0.08 ~ 0.20 mm. Step 5: Secure the conical fiber paper sleeve around the aluminum substrate coated with black photothermal layer to obtain a non-contact solar interface evaporator.
[0008] The present invention also has the following technical features: Preferably, the grinding process in step one is performed using a vibratory mill, and the grinding media is TZP zirconium beads with a density of 6.0 g / cm³. 3The zirconium beads have a diameter of 0.8~1.2 mm, the mass ratio of grinding media to the mixture is 3:1, and the grinding time is 2~3 h.
[0009] Preferably, the moisturizer mentioned in step one includes any one of propylene glycol, glycerol, and polypropylene glycol 2000.
[0010] Preferably, the semi-apex angle of the conical aluminum substrate in step two is 30°, 45° or 60°, and the unfolded radii corresponding to the semi-apex angles from small to large are 3.5 cm, 2.94 cm and 2.66 cm respectively.
[0011] Preferably, the drying in step four is performed in an oven at 50-60°C for 8-12 hours.
[0012] This invention also protects a non-contact solar interface evaporator for saline-alkali land remediation prepared according to the above method, and its application in seawater desalination, high-salinity brine resource utilization, and saline-alkali land remediation.
[0013] Compared with the prior art, the present invention has the following beneficial effects: This invention employs a separate capillary salt-collecting fiber paper and a conical aluminum substrate coated with a black photothermal layer. Nano-black pigment is sprayed onto the polished surface of the conical aluminum substrate to form a broad-spectrum light-absorbing photothermal layer. The aluminum material combined with the conical structure can collect solar energy, achieving localized heating at the evaporation interface and reducing ineffective energy consumption of water. Wood fibers are adjusted to a suitable degree of beating, compounded into fibers, and resin-impregnated to strengthen the hydrophilic structure. After pulping, the fibers are laid, dried, cut, and bonded into a conical sleeve that matches the aluminum cone. Finally, the fiber paper... It is directly fitted onto the outside of the aluminum photothermal cone, forming a physically isolated double-layered structure. The cone can be configured with three semi-apex angles: 30°, 45°, and 60°, to regulate the balance between water delivery and heat generation. High-salt brine is transported upwards through capillary channels inside the outer fiber layer. The water on the fiber surface rapidly vaporizes and evaporates upon contact with light and heat, while the dissolved salt is dispersed with the water and crystallizes directionally within the fiber paper, preventing it from contacting the inner aluminum-based photothermal layer. This completely eliminates the problem of salt crystals blocking the light-absorbing surface and clogging the heat transfer channels. Once the fiber paper becomes saturated with salt, it can be directly disassembled and replaced. After multiple cycles of use, the equipment's evaporation and salt collection capabilities show no significant decline, greatly extending the equipment's service life. Meanwhile, the cone's apex angle exhibits a balance mechanism between heat and water transport: a smaller apex angle results in strong light-gathering and heat generation, but insufficient fiber water transport flux, limiting brine supply; a larger apex angle leads to faster water transport, but a large volume of water continuously carries away interfacial heat, failing to meet stable salt precipitation temperatures; a medium apex angle coordinates water transport rate and interfacial temperature, simultaneously achieving efficient water production and continuous salt accumulation; it combines the triple characteristics of high photothermal conversion, long-lasting anti-scaling, and simultaneous water production and salt collection, allowing for complete stripping and recovery of salt crystals, eliminating salt resource waste; This invention is entirely powered by solar energy, requiring no external power source, and is suitable for remote saline-alkali areas without power grids. The raw materials prepared by this invention are readily available in the market, the processing conditions are mild, and it supports batch modular assembly and deployment. The operation process does not discharge high-salt concentrated waste liquid, the fresh water obtained by evaporation can be directly used for irrigation of saline-alkali land, and the precipitated solid salt can be used as a chemical raw material for resource utilization. It simultaneously completes the desalination and improvement of saline-alkali soil, fresh water resource regeneration, salt resource recovery, seawater desalination, high-salt brine resource treatment and saline-alkali land ecological restoration, and has significant promotional value. Attached Figure Description
[0014] Figure 1 Photographs showing the hydrophilicity of the evaporators prepared in Examples 1-3 of this invention; Figure 2 These are photographs showing the temperature changes of the evaporators prepared in Examples 1-3 of this invention under one sun. Figure 3 The evaporation rates of the evaporators prepared in Examples 1-3 of this invention in a 20 wt% NaCl solution; Figure 4 The salt collection rate of the evaporators prepared in Examples 1-3 of this invention in a 20 wt% NaCl solution; Figure 5 Photograph showing the salt collection capacity of the evaporator prepared in Example 2 of this invention in a 20 wt% NaCl solution. Detailed Implementation
[0015] The present invention will be further described in detail below with reference to specific embodiments. These descriptions are for explanation purposes only and are not intended to limit the scope of the invention.
[0016] The conductive carbon black used in this invention is EC600JD conductive carbon black produced by Lion Corporation of Japan; the wetting and dispersing agent used is 760W water-based special wetting and dispersing agent produced by TEGO GmbH of Germany. Its chemical type is modified polyacrylate type polymeric anionic dispersant, which is a special dispersion and stabilizing agent for carbon black powder in the system of this invention. The anti-settling agent used in this invention is AG-507, a water-based associative polyurethane rheology anti-settling agent produced by Zhongtai Lianhua New Materials Co., Ltd. It is a non-ionic rheology modifier used to optimize the rheological properties and storage stability of the water-based conductive coating of this invention.
[0017] The film-forming matrix resin used in this invention is Steba UW F5068 water-based functional emulsion produced by China Bangtai New Materials Co., Ltd. It is the core film-forming carrier of the conductive coating of this invention, and plays a core role in filling material support, film curing, coating adhesion and performance assurance.
[0018] Example 1 Step 1: By mass fraction, take 20% Lion King EC600JD carbon black, 35% Digo 760W wetting and dispersing agent, 1% AG-507 anti-settling agent, 3% propylene glycol, and 41% water. After stirring evenly, grind using a vibratory mill. The grinding media is TZP zirconium beads with a density of 6.0 g / cm³. 3 The zirconium beads had a diameter of 0.8~1.2 mm, the mass ratio of grinding media to mixture was 3:1, the grinding time was 2 h, and the mixture was filtered to obtain a nano black pigment with a particle size D50 of 40 nm. Step 2: Select a cone-shaped aluminum substrate with a semi-apex angle of 30° and an unfolding radius of 3.5 cm. Polish the surface of the substrate with 800-grit sandpaper to achieve a surface roughness Ra value of 0.8 μm. Spray the black pigment obtained in Step 1 evenly onto the outer surface of the cone and cure it to form a high solar energy absorption radiation layer with a thickness of 50 μm, thus obtaining an aluminum substrate with a black photothermal layer. Step 3: Pulp the wood fibers, control the freeness to 20°SR, add 5% Steba UW F5068 resin / emulsion by weight of oven-dry wood fibers to the obtained pulp, stir and mix at room temperature for 1 hour, and finally add water and stir evenly to obtain a pulp suspension with a solid content of 5.0%. Step 4: Spread the pulp suspension on a circular mold to form a wet paper sheet, dry it in a 50℃ oven for 12 hours, cut it, and then bond it with double-sided adhesive to form a cone-shaped fiber paper with a paper thickness of 0.08 mm and an angle and size that match the cone-shaped aluminum substrate. Step 5: Secure the conical fiber paper sleeve around the aluminum substrate coated with black photothermal layer to obtain a non-contact solar interface evaporator.
[0019] The prepared evaporator can transfer water to the top edge after 170 s, and the surface temperature of the evaporator rises to 40.8 °C after 40 min. The water supply rate is slow, but the surface temperature rises rapidly. The brine transfer cannot be supplied quickly.
[0020] Example 2 Step 1: By mass fraction, take 22% Lion King EC600JD carbon black, 30% Tigo 760W wetting and dispersing agent, 0.5% AG-507 anti-settling agent, 5% polypropylene glycol 2000, and 42.5% deionized water. After stirring evenly, grind using a vibratory mill. The grinding media is TZP zirconium beads with a density of 6.0 g / cm³. 3 The zirconium beads were 1.2 mm in diameter, the mass ratio of grinding media to the mixture was 3:1, the grinding time was 3 h, and the mixture was filtered to obtain a nano black pigment with a particle size D50 of 40 nm. Step 2: Select a cone-shaped aluminum substrate with a semi-apex angle of 45° and an unfolding radius of 2.94 cm. Polish the surface of the substrate with 800-grit sandpaper to achieve a surface roughness Ra value of 1.6 μm. Spray the black pigment obtained in Step 1 evenly onto the outer surface of the cone and cure it to form a high solar energy absorption radiation layer with a thickness of 70 μm, thus obtaining an aluminum substrate with a sprayed black photothermal layer. Step 3: Pulp the wood fibers, control the freeness to 35°SR, add Steba UW F5068 resin / emulsion (15% of the oven-dry wood fiber mass) to the obtained pulp, stir and mix at room temperature for 1.5 h, and finally add water and stir evenly to obtain a pulp suspension with a solid content of 5.5%. Step 4: Spread the pulp suspension on a circular mold to form a wet paper sheet, dry it in a 60 ℃ oven for 8 hours, cut it, and then bond it with double-sided adhesive to form a cone-shaped fiber paper with a paper thickness of 0.08 mm and an angle and size that match the cone-shaped aluminum substrate. Step 5: The conical fiber paper is fitted and fixed around the aluminum substrate coated with a black photothermal layer to obtain a non-contact solar interface evaporator. The prepared evaporator can transfer water to the top edge after 129 seconds, and the surface temperature of the evaporator rises to 36.8 °C after 40 minutes, at which point the water supply rate and the surface temperature rise rate reach equilibrium.
[0021] Example 3 Step 1: By mass fraction, take 25% Lion King EC600JD carbon black, 32% Digo 760W wetting and dispersing agent, 0.8% AG-507 anti-settling agent, 4% glycerol, and 38.2% deionized water. After stirring evenly, grind using a vibratory mill. The grinding media is TZP zirconium beads with a density of 6.0 g / cm³. 3 The zirconium beads were 1.0 mm in diameter, the mass ratio of grinding media to the mixture was 3:1, the grinding time was 2.5 h, and the mixture was filtered to obtain a nano black pigment with a particle size D50 of 40 nm. Step 2: Select a cone-shaped aluminum substrate with a semi-apex angle of 60° and an unfolding radius of 2.66 cm. Polish the surface of the substrate with 800-grit sandpaper to achieve a surface roughness Ra value of 1.2 μm. Spray the black pigment obtained in Step 1 evenly onto the outer surface of the cone and cure it to form a high solar energy absorption radiation layer with a thickness of 60 μm, thus obtaining an aluminum substrate with a sprayed black photothermal layer. Step 3: Pulp the wood fibers, control the freeness to 30°SR, add Steba UW F5068 resin / emulsion (10% of the oven-dry wood fiber mass) to the obtained pulp, stir and mix at room temperature for 1.2 h, and finally add water and stir evenly to obtain a pulp suspension with a solid content of 5.2%. Step 4: Spread the pulp suspension on a circular mold to form a wet paper sheet, dry it in an oven at 55 ℃ for 10 h, cut it, and then bond it with double-sided adhesive to form a cone-shaped fiber paper with a paper thickness of 0.10 mm and an angle and size that match the cone-shaped aluminum substrate. Step 5: Secure the conical fiber paper sleeve around the aluminum substrate coated with black photothermal layer to obtain a non-contact solar interface evaporator.
[0022] The prepared evaporator can transfer water to the top edge after 81 seconds, and the surface temperature of the evaporator rises to 32.3 °C after 40 minutes. The water supply rate is fast, but the surface temperature rise rate is slow and cannot reach the salt crystallization point.
[0023] The water absorption capacity of the prepared evaporator was tested, and the test results are attached. Figure 1 As shown; via appendix Figure 2 Observe the surface temperature changes of evaporators with different semi-apex angles; (attached) Figure 3 To illustrate the evaporation rate variation in an evaporator within a 20 wt% NaCl solution, Examples 1-3 showed evaporation rates of 0.67 kg / m³ after 1 h. -2 h -1 1.24 kg m -2 h -1 0.54 kgm -2 h -1 The evaporation efficiency reached its optimal value at 4 h, which was 1.28 kg m³. -2 h -1 1.39 kg m -2 h -1 0.93 kg m -2 h -1 Among them, the rate of Example 2 was relatively stable and high within 5 hours; Appendix Figure 4 The amount of salt crystals detached from the fiber paper collected per hour was measured. Examples 1-3 all showed good salt collection rates at the 4th hour, with collection rates of 78.46 gm³. -2 h -1 226.05 gm -2 h -1 49.42 gm -2 h -1 Example 2 showed a better salt collection rate; Appendix Figure 5 The images show the salt collection capacity of Example 2 in a 20 wt% NaCl solution at 0 h, 2 h, 3 h and 4 h.
[0024] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of the claims.
Claims
1. A method for preparing a non-contact solar interface evaporator for saline-alkali land remediation, characterized in that, Includes the following steps: Step 1: Take 20-25% carbon black, 30-35% wetting and dispersing agent, 0.5-1% anti-settling agent, 3-5% humectant, and the remainder is deionized water by mass fraction. After stirring evenly, grind and filter to obtain a nano black pigment with a particle size D50 of 40 nm. Step 2: Select a cone-shaped aluminum substrate and polish the surface of the substrate with 800-grit sandpaper to achieve a surface roughness Ra value of 0.8 μm to 1.6 μm. Spray the black pigment obtained in Step 1 evenly onto the outer surface of the cone and cure it to form a high solar energy absorption radiation layer with a thickness of 50 to 70 μm, thus obtaining an aluminum substrate with a black photothermal layer. Step 3: Pulp the wood fibers, controlling the freeness to 20°SR~35°SR. Add 5%~15% of resin / emulsion by weight of oven-dry wood fibers to the resulting pulp, stir and mix at room temperature for 1~1.5 h, and finally add water and stir evenly to obtain a pulp suspension with a solid content of 5.0%~5.5%. Step 4: Spread the pulp suspension on a circular mold to form a wet paper sheet. After drying and cutting, the paper is bonded together with double-sided adhesive to form a cone-shaped fiber paper with a thickness of 0.08 ~ 0.20 mm. Step 5: Secure the conical fiber paper sleeve around the aluminum substrate coated with black photothermal layer to obtain a non-contact solar interface evaporator.
2. The method for preparing a non-contact solar interface evaporator for saline-alkali land remediation according to claim 1, characterized in that, The grinding process in step one uses a vibratory mill, and the grinding media is TZP zirconium beads with a density of 6.0 g / cm³. 3 The zirconium beads have a diameter of 0.8~1.2 mm, the mass ratio of grinding media to the mixture is 3:1, and the grinding time is 2~3 h.
3. The method for preparing a non-contact solar interface evaporator for saline-alkali land remediation according to claim 1, characterized in that, The moisturizer mentioned in step one includes any one of propylene glycol, glycerol, and polypropylene glycol 2000.
4. The method for preparing a non-contact solar interface evaporator for saline-alkali land remediation according to claim 1, characterized in that, The cone-shaped aluminum substrate mentioned in step two has a semi-apex angle of 30°, 45° or 60°, and the unfolded radii corresponding to the semi-apex angles from small to large are 3.5 cm, 2.94 cm and 2.66 cm respectively.
5. The method for preparing a non-contact solar interface evaporator for saline-alkali land remediation according to claim 1, characterized in that, The drying process described in step four involves drying in an oven at 50-60°C for 8-12 hours.
6. A non-contact solar interface evaporator for saline-alkali land remediation prepared by the method according to any one of claims 1 to 5.
7. The application of a non-contact solar interface evaporator for saline-alkali land remediation according to claim 6 in seawater desalination, high-salinity brine resource utilization, and saline-alkali land remediation.