A stable luminescent neodymium-doped quartz glass with low temperature coefficient and its preparation method

By introducing β-lithium nepheline, B2O3, LaF3/MgO nanocomposite coating and nano ZrO2/Y2O3 components into neodymium-doped quartz glass, the refractive index temperature coefficient and luminescence stability are synergistically controlled, solving the problem of low temperature coefficient and stable luminescence in existing technologies, and achieving efficient refractive index stabilization and improved luminescence performance.

CN123105964APending Publication Date: 2026-11-17SHANDONG INTELLIGENT OPTICAL COMM DEV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611491341.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve both low temperature coefficients and stable luminescence performance in neodymium-doped quartz glass while maintaining high concentration and uniform doping.

Method used

By introducing β-lithium nepheline and B2O3 components to form a glass network structure with low expansion micro-regions and negative thermo-optic coefficients, and combining it with a LaF3/MgO nanocomposite coating layer to stabilize the Nd3+ ion environment, and adding nano ZrO2 and Y2O3 buffer components, the refractive index temperature coefficient and luminescence stability are synergistically regulated.

Benefits of technology

The refractive index temperature coefficient of neodymium-doped quartz glass was significantly reduced, improving luminescence stability and fluorescence lifetime, while maintaining the transparency and optical quality of the glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105964A_ABST
    Figure CN123105964A_ABST
Patent Text Reader

Abstract

This invention discloses a stable, low-temperature-coefficient, neodymium-doped quartz glass with light emission and its preparation method, relating to the field of special glass technology and belonging to patent classification number C03C3 / 06. The method includes preparing Nd2O3 by mixing silica sol with aluminum and neodymium salts. 3+ / Al 3+ A basic sol was co-doped; boric acid and β-lithium nepheline were introduced to obtain a low temperature coefficient modified powder; the surface of LaF3 nanoparticles was modified with a silane coupling agent and then composited with MgO. The modified powder was then coated and heat-treated to obtain modified Nd:Nd:Nd:quartz powder; this powder was then mixed with nano-ZrO2 and nano-Y2O3, ball-milled, shaped, purified at high temperature, hot isostatic pressing sintered, and annealed to obtain the finished product. This invention utilizes thermal expansion compensation and polarizability inverse regulation to synergistically reduce the temperature coefficient, construct a low phonon microregion and stabilize the coordination environment to improve luminescence stability, while eliminating intercomponent interference, achieving a combination of low temperature coefficient, high luminescence stability, and excellent optical quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of special glass technology, belonging to patent classification number C03C3 / 06, specifically to a low-temperature coefficient stable luminescent neodymium-doped quartz glass and its preparation method. Background Technology

[0002] Neodymium doping (Nd) 3+ Quartz glass, as an important laser gain medium material, combines the extremely low coefficient of thermal expansion of quartz glass with the high Nd: 3+ The excellent laser properties of Nd:ion have broad application prospects in fields such as high-repetition-rate laser shock strengthening, precision machining, and national defense security. Compared with traditional phosphate and silicate laser Nd:ion glass, Nd:ion quartz glass has a coefficient of thermal expansion that is more than an order of magnitude lower, which theoretically can greatly improve the thermal shock resistance of lasers during high-repetition-rate operation. Chinese patent CN106396378B discloses a Nd:ion ion silicide... 3+ A method for preparing uniformly doped quartz glass, which employs a sol-gel method combined with high-temperature sintering technology, using Al... 3+ Ti 4+ Co-doping to improve Nd 3+ By adjusting the doping concentration and uniformity within the quartz matrix, an emission cross section of 1.8 pm was obtained. 2 High-performance Nd:Nd2+ doped silica glass. This technology effectively solves the Nd:Nd2+ doped silica glass problem. 3+ The challenge of achieving high-concentration uniform doping in quartz glass remains. However, with the rapid development of high-power laser technology, practical applications place higher demands on Nd:dI quartz glass. On the one hand, lasers generate a large amount of heat during high-repetition-rate operation, causing changes in the glass's refractive index (i.e., the thermo-optic effect), leading to beam wavefront distortion and mode instability, severely limiting the output power and beam quality of the laser system. Therefore, it is urgent to reduce the refractive index temperature coefficient of Nd:dI quartz glass. On the other hand, under long-term continuous operation or high pump power conditions, Nd:dI quartz glass... 3+ The fluorescence intensity of Nd+ ions gradually decreases with prolonged operation, exhibiting luminescence instability. This is mainly due to the fact that Nd+ ions... 3+ Factors such as localized structural relaxation, enhanced nonradiative transitions, and defect state trapping of ions under high-temperature conditions severely affect the long-term stability of laser output. Current technologies mainly focus on improving the performance of Nd... 3+ While the doping concentration and uniformity of neodymium-doped quartz glass are important, research on how to simultaneously reduce the temperature coefficient and improve its luminescence stability is still insufficient. Currently, there is no systematic modification method that can achieve both low temperature coefficient and stable luminescence performance in neodymium-doped quartz glass while maintaining high concentration and uniform doping. Summary of the Invention

[0003] The purpose of this invention is to provide a stable luminescent neodymium-doped quartz glass with a low temperature coefficient and a method for preparing the same, so as to solve the technical problems mentioned in the background art.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0006] 1) Nd2 is obtained by mixing silica sol, aluminum nitrate, and neodymium nitrate, followed by hydrolysis, polycondensation, and aging. 3+ / Al 3+ Co-doping with basic sol;

[0007] 2) Reconstitute the boric acid aqueous solution with the Nd 3+ / Al 3+ The basic sol was stirred and mixed to obtain a boron-doped sol; β-lithium nepheline dispersion was added to the boron-doped sol and stirred to form a composite; after drying, pre-calcination, grinding and sieving, a low temperature coefficient modified powder was obtained.

[0008] 3) Graft γ-aminopropyltriethoxysilane onto the surface of LaF3 nanoparticles to obtain a surface-modified LaF3 dispersion, and then mix it with MgO nanoparticles to form a composite modified suspension; add the low temperature coefficient modified powder to the composite modified suspension, and after stirring, coating, solvent removal and inert atmosphere heat treatment, obtain modified Nd:N quartz powder;

[0009] 4) Modified neodymium-doped quartz powder, nano ZrO2 and nano Y2O3 were mixed and then ball-milled to obtain a uniformly mixed powder;

[0010] 5) The uniformly mixed powder is formed into a blank, and then subjected to high-temperature purification treatment, high-temperature hot isostatic pressing sintering and annealing treatment in sequence to obtain the final product.

[0011] The temperature coefficient of refractive index of neodymium-doped quartz glass essentially depends on the competition between two factors: the change in polarizability and the volume expansion of the glass network structure with temperature. In this invention, this temperature response behavior is synergistically regulated from two levels: (1) β-nepheline is a lithium aluminum silicate crystal material with negative thermal expansion characteristics. Although it undergoes inconsistent melting (decomposition melting) under high temperature conditions, in the high-temperature sintering stage of this invention, after the decomposition melting of β-nepheline, its components are uniformly integrated into the surrounding quartz glass network, forming a local micro-region structure rich in Li-Al-Si-O. Although the thermal expansion coefficient of this lithium aluminum silicate glass micro-region formed in situ by the decomposition products of β-nepheline is higher than that of crystalline β-nepheline, the thermal expansion coefficient of Li2O-Al2O3-SiO2 glass is still significantly lower than that of the doped quartz matrix. These relatively low-expansion micro-regions are uniformly dispersed in the matrix, which can reduce the overall thermal expansion response of the material to a certain extent and indirectly reduce the temperature drift of the refractive index. (2) After the B2O3 component introduced by boric acid during the sol-gel process enters the glass network, it forms a planar triangular [BO3] structural unit. The temperature dependence of the polarizability of this structural unit is opposite to that of the [SiO4] tetrahedron, that is, the B2O3 component itself has a negative thermo-optic coefficient contribution. When it is embedded in the silicon-oxygen network in an appropriate proportion, it can compensate for the positive refractive index shift of the quartz matrix caused by the increase in temperature from the electronic polarization level. It should be noted that although B2O3 has a certain volatilization loss at high temperature, the sintering process of the present invention is carried out under a high-pressure N2 atmosphere. The high-pressure atmosphere effectively suppresses the volatilization of B2O3, so that most of the boron component is retained in the glass network. The low expansion micro-area compensation at the above-mentioned structural level and the reverse adjustment of polarizability at the electronic level significantly reduce the temperature coefficient of refractive index of Nd:YAG quartz glass.

[0012] Nd 3+ The luminescence stability of Nd ions in a quartz glass matrix is ​​mainly constrained by two factors: one is Nd 3+ The phonon energy environment surrounding the ion, with high phonon energies, accelerates the multiphonon relaxation process, increases the probability of nonradiative transitions, and causes the fluorescence intensity to gradually decrease with increasing operating temperature or operating time; secondly, Nd 3+ The symmetry and stability of the local coordination field of ions; unfavorable coordination environments can lead to Nd... 3+ Ions undergo localized structural relaxation under thermal excitation, causing their energy level splitting states to drift and resulting in fluctuations in luminescence performance. This invention addresses these two problems by constructing a LaF3 / MgO nanocomposite coating layer on the surface of powder particles. During the low-temperature heat treatment stage, LaF3 nanoparticles are coated onto the surface of the powder particles and Nd... 3+A specific spatial distribution pattern of fluorine-containing compounds was established in the ion neighborhood region. During the subsequent high-temperature sintering stage, although LaF3 lost its original crystal structure due to exceeding its melting point, the La... 3+ Integrating into the glass network to form a La-O bonded structure, while some F - Then replace Nd 3+ Neighboring bridging oxygen atoms form non-bridging fluoride sites. Because the electronegativity and mass of fluoride ions differ from those of oxygen ions, the local vibrational frequencies of fluoride-containing Si-F and La-F bonds are lower than those in a pure silicon-oxygen network. Therefore, in Nd... 3+ The surrounding area forms modified microregions with localized phonon energies lower than those of the pure quartz matrix. This fluorine-containing low-phonon microregion structure, formed by pre-positioning of the LaF3 precursor followed by high-temperature network reconstruction, effectively reduces the probability of nonradiative transitions caused by multiphonon relaxation, thereby maintaining long-term stability of fluorescence intensity. Simultaneously, MgO nanoparticles, as alkaline earth metal oxides, enter the glass structure as network modifiers during high-temperature sintering, and their Mg... 2+ Ions possess a high field strength, which can effectively stabilize Nd. 3+ The coordinated oxygen environment surrounding the ions inhibits Nd. 3+ The local structural relaxation of ions under thermal excitation conditions enables Nd 3+ The energy level structure of the ions remains stable. The construction of fluorine-containing low-phonon microregions in the LaF3 precursor and the stabilization of the coordination environment of MgO work synergistically from two dimensions: reducing local phonon energy and stabilizing the coordination environment, respectively, to achieve the luminescence stability of the quartz glass.

[0013] Preferably, the silica sol in step 1) is obtained by hydrolysis and polycondensation of tetraethyl orthosilicate, anhydrous ethanol and water under the catalysis of dilute nitric acid.

[0014] Preferably, the mass ratio of aluminum nitrate to neodymium nitrate in step 1) is 7:(0.5-0.8).

[0015] Preferably, the β-nepheline particle size in the β-nepheline dispersion in step 2) is 1–3 μm.

[0016] Preferably, the amount of γ-aminopropyltriethoxysilane used in step 3) is 3 to 10 wt% of the mass of LaF3 nanoparticles.

[0017] Preferably, the mass ratio of LaF3 nanoparticles to MgO nanoparticles in step 3) is 3:(1-2).

[0018] Preferably, the mass ratio of LaF3 nanoparticles to low temperature coefficient modified powders in step 3) is 3:(7-9).

[0019] As a preference, the amount of nano ZrO2 used in step 4) is 1.0 to 3.0 wt% of the mass of the modified neodymium-doped quartz powder.

[0020] As a preference, the amount of nano-Y2O3 used in step 4) is 0.5 to 2.0 wt% of the mass of the modified neodymium-doped quartz powder.

[0021] In experiments, this invention revealed that while β-lithium nepheline micropowder and B2O3 components can effectively reduce the temperature coefficient, during the subsequent high-temperature sintering stage, β-lithium nepheline, due to its inconsistent melting temperature, completely decomposes and melts during the sintering heating process. This destroys its crystal structure and releases a large amount of Li. + Ions enter the surrounding glass matrix. This sudden Li... + Unlike slow, gradual diffusion, a large influx will occur in Nd 3+ Localized areas of ion enrichment cause severe fluctuations in the concentration of alkali metal ions. Li + As alkali metal ions, Nd2 exhibits a strong tendency for network modification and a high diffusion rate, leading to a large influx of Nd2. 3+ The MgO ion will form a MgO bond with the nearest neighbor region of the ion. 2+ Coordination-stabilized structures generate competitive interference: Li + Tends to replace Mg 2+ Occupying non-bridging oxygen sites disrupts the Nd binding of MgO. 3+ The stabilizing effect of the coordination environment leads to the partial reduction of Nd in certain regions. 3+ The decreased local symmetry of ions and increased fluctuations in the coordination field create an unstable coordination environment for Nd... 3+ Ions are more prone to thermally driven localized structural relaxation under prolonged continuous pumping conditions, leading to a significant deterioration in luminescence stability (manifested as decreased fluorescence lifetime and increased fluorescence decay rate under continuous pumping). Meanwhile, Li... + Excessive enrichment in certain areas can also cause micro-regions of non-uniform refractive index in the glass network, resulting in reduced transparency. To address this technical problem, this invention introduces two synergistic buffering components, nano-ZrO2 and nano-Y2O3, during the ball milling mixing stage. Nano-ZrO2 possesses excellent high-temperature chemical stability and is distributed as highly stable particles between powders during sintering, acting as physical isolation and diffusion inhibition. The ZrO2 particles are located at the original β-lithium nepheline particle decomposition sites and Nd... 3+ Between enriched regions, the extension of Li+ ion to Nd... 3+ The nearest-neighbor diffusion path slows down the influx rate of Li+, allowing Li... + This allows for dispersion and dilution over a larger spatial area rather than concentration in a localized area. Furthermore, due to the extremely small amount of ZrO2 added, its impact on the overall thermal expansion coefficient of the glass is negligible, and it does not weaken the temperature coefficient reduction effect; the Y in nano-Y2O3...3 + Ions and Nd 3+ The ions have similar ionic radii and coordination chemistry characteristics, enabling them to preferentially occupy Nd at high temperatures. 3+ The surrounding area of ​​ions due to Li + The coordination defect sites caused by interference play a role in coordination repair, restoring and further stabilizing Nd. 3+ The local coordination environment of ions. The diffusion hindrance function of nano-ZrO2 and the coordination repair function of nano-Y2O3 work together to slow down the diffusion of Li. + The two aspects of influx and repair of coordination defects work together to eliminate the negative interference of step (2) on the improvement of luminescence stability in step (3), so that the final glass maintains good optical transparency and fluorescence lifetime while having both low temperature coefficient and high luminescence stability.

[0022] A stable luminescent neodymium-doped quartz glass with a low temperature coefficient is prepared by the method described above.

[0023] Compared with the prior art, the beneficial effects of the present invention are:

[0024] 1. By utilizing the synergistic effect of physical compensation of low-expansion micro-regions formed by the decomposition of β-lithium nepheline and chemical compensation of the negative thermo-optic coefficient of B2O3[BO3] units, the refractive index temperature drift is suppressed from two aspects: structural expansion and electronic polarization, and the refractive index temperature coefficient is significantly reduced.

[0025] 2. Constructing fluorine-containing low-phonon microregions using LaF3 precursors to suppress multiphonon relaxation and stabilize Nd with MgO. 3+ The coordination environment effectively reduces the probability of nonradiative transitions, suppresses fluorescence decay under continuous pumping, and significantly improves luminescence stability.

[0026] 3. Introducing nano-ZrO2 for physical barrier and retardation of Li + The concentrated influx of nano-Y2O3, combined with the repair of coordination defects, achieves a low temperature coefficient and high luminescence stability while maintaining the glass's complete transparency and excellent fluorescence lifetime. Attached Figure Description

[0027] Figure 1 This is a low-magnification SEM image of the surface of the neodymium-doped quartz glass prepared in Example 4 of the present invention.

[0028] Figure 2 This is a medium-magnification SEM image of the surface of the neodymium-doped quartz glass prepared in Example 4 of the present invention.

[0029] Figure 3 This is a high-magnification SEM image of the surface of the neodymium-doped quartz glass prepared in Example 4 of the present invention.

[0030] Figure 4 The XRD pattern of the neodymium-doped quartz glass prepared in Example 4 of this invention is shown. Detailed Implementation

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0032] Example 1

[0033] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0034] Step 1) Mix 50 mL of tetraethyl orthosilicate (TEOS) and 200 mL of anhydrous ethanol in a round-bottom flask until homogeneous. Add 30 mL of deionized water and stir magnetically at 300 rpm for 30 min at room temperature. Then, add 0.2 mol / L dilute nitric acid dropwise to adjust the pH to 3 and continue stirring for 2 h to allow TEOS to fully hydrolyze and condense to form a transparent silica sol. Dissolve 7.0 g of aluminum nitrate nonahydrate in 30 mL of deionized water to obtain an aluminum salt solution. Dissolve 0.7 g of neodymium nitrate hexahydrate in 10 mL of deionized water to obtain a neodymium salt solution. Under stirring conditions, first add the aluminum salt solution dropwise to the silica sol at a rate of 1 mL / min and stir for 1 h. Then, add the neodymium salt solution dropwise at a rate of 0.5 mL / min and stir for 2 h. After sealing, age in a constant temperature oven at 30 °C for 5 days to obtain a transparent and uniform Nd2O3 solution. 3+ / Al 3+ Co-doping with basic sol.

[0035] Step 2) Dissolve 0.44 g of boric acid in 15 mL of deionized water and add it dropwise to the basic sol obtained in Step 1) at a rate of 2 mL / min. Stir for 1.5 h to obtain a boron-doped sol. Separately, mix 100 mL of anhydrous ethanol and 10 mL of glacial acetic acid as a modifying solvent, add 0.40 g of β-lithium nepheline micropowder (1-3 μm), and ultrasonically disperse in a 70 °C water bath for 45 min to obtain a β-lithium nepheline dispersion. Slowly add the β-lithium nepheline dispersion to the boron-doped sol while stirring at 500 rpm, heat to 60 °C and stir continuously for 4 h, then cool to room temperature to obtain a low temperature coefficient modified sol. Rotate the modified sol at 60 °C and 0.09 MPa vacuum to obtain a wet gel, transfer it to a drying oven and heat from 60 °C to 120 °C at a rate of 2 °C / min for 3 h to obtain a dry gel. The dry gel was placed in a muffle furnace under air atmosphere and heated to 400℃ at 3℃ / min for 1.5h to pre-burn off organic matter. Then it was heated to 680℃ at 4℃ / min for 3h to deeply decarbonize and dehydroxylate. After cooling, it was ground through a 150-mesh sieve to obtain a low temperature coefficient modified powder.

[0036] Step 3) Add 0.30g of LaF3 nanoparticles to a mixture of 80mL anhydrous ethanol and 10mL DMF. Stir magnetically for 30min, then ultrasonically disperse for 30min. Add 0.025g of KH-550 and stir for 1.5h to graft the silane coupling agent onto the LaF3 surface, obtaining a surface-modified LaF3 dispersion. Add 0.18g of MgO nanoparticles to the dispersion and stir at 70℃ for 3h to form a LaF3 / MgO composite modified suspension. Add all of the low temperature coefficient modified powder obtained in Step 2) to the suspension and stir at 600rpm for 3h to uniformly coat the nanoparticles onto the powder surface. Remove the solvent by rotary evaporation at 50℃ and 0.09 MPa to obtain wet powder. The wet powder was placed in a tube furnace and heated to 250°C at 3°C / min under an argon atmosphere (30 L / h) for 1.5 h to remove organic groups. The temperature was then maintained at 4°C / min to 600°C for 3 h to solidify and bond the coating layer. After cooling, the modified neodymium-doped quartz powder was obtained.

[0037] Step 4) The modified Nd:YAG quartz powder obtained in step 3) is ball-milled in a planetary ball mill at 200 rpm until the median particle size is about 15 μm. After weighing, 2.5 wt% of the modified Nd:YAG quartz powder is weighed into nano ZrO2 (particle size 30 nm) and 1.5 wt% of the modified Nd:YAG quartz powder is weighed into nano Y2O3 (particle size 50 nm). The three are premixed in a V-type mixer at 30 rpm for 45 min and then transferred to a planetary ball mill at 300 rpm for 2 h (with a 10 min cooling stop every 30 min) to obtain a uniformly mixed powder.

[0038] Step 5) The uniformly mixed powder is cold isostatically pressed into a green blank at 150 MPa. The green blank is placed in a tube furnace and first purged with Cl2 (8 L / h) at 800℃ for 2 h to remove hydroxyl groups and impurities. Then, O2 (30 L / h) is switched on and held at 1.5 h to remove residual chlorine and carbon. The purified green blank is then placed in a gas pressure sintering furnace and sintered at 100 MPa. -2 Under vacuum, the temperature is increased to 1720℃ at 5℃ / min, and then high-purity N2 is introduced to 2MPa for densification. The temperature is then slowly decreased to 1100℃ at 3℃ / min and held for 3 hours for annealing to eliminate thermal stress. After cooling to room temperature in the furnace, the glass is removed, cut, ground, and polished to optical grade surface quality, thus obtaining stable luminescent neodymium-doped quartz glass with a low temperature coefficient.

[0039] Example 2

[0040] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0041] Step 1) Mix 50 mL of tetraethyl orthosilicate (TEOS) and 200 mL of anhydrous ethanol in a round-bottom flask until homogeneous. Add 30 mL of deionized water and stir magnetically at 300 rpm for 30 min at room temperature. Then, add 0.2 mol / L dilute nitric acid dropwise to adjust the pH to 3 and continue stirring for 2 h to allow TEOS to fully hydrolyze and condense to form a transparent silica sol. Dissolve 7.0 g of aluminum nitrate nonahydrate in 30 mL of deionized water to obtain an aluminum salt solution. Dissolve 0.6 g of neodymium nitrate hexahydrate in 10 mL of deionized water to obtain a neodymium salt solution. Under stirring conditions, first add the aluminum salt solution dropwise to the silica sol at a rate of 1 mL / min and stir for 1 h. Then, add the neodymium salt solution dropwise at a rate of 0.5 mL / min and stir for 2 h. After sealing, age in a constant temperature oven at 30 °C for 5 days to obtain a transparent and uniform Nd2O3 solution. 3+ / Al 3+ Co-doping with basic sol.

[0042] Step 2) Dissolve 0.44 g of boric acid in 15 mL of deionized water and add it dropwise to the basic sol obtained in Step 1) at a rate of 2 mL / min. Stir for 1.5 h to obtain a boron-doped sol. Separately, mix 100 mL of anhydrous ethanol and 10 mL of glacial acetic acid as a modifying solvent, add 0.40 g of β-lithium nepheline micropowder (1-3 μm), and ultrasonically disperse in a 70 °C water bath for 45 min to obtain a β-lithium nepheline dispersion. Slowly add the β-lithium nepheline dispersion to the boron-doped sol while stirring at 500 rpm, heat to 60 °C and stir continuously for 4 h, then cool to room temperature to obtain a low temperature coefficient modified sol. Rotate the modified sol at 60 °C and 0.09 MPa vacuum to obtain a wet gel, transfer it to a drying oven and heat from 60 °C to 120 °C at a rate of 2 °C / min for 3 h to obtain a dry gel. The dry gel was placed in a muffle furnace under air atmosphere and heated to 400℃ at 3℃ / min for 1.5h to pre-burn off organic matter. Then it was heated to 680℃ at 4℃ / min for 3h to deeply decarbonize and dehydroxylate. After cooling, it was ground through a 150-mesh sieve to obtain a low temperature coefficient modified powder.

[0043] Step 3) Add 0.30g of LaF3 nanoparticles to a mixture of 80mL anhydrous ethanol and 10mL DMF. Stir magnetically for 30min, then ultrasonically disperse for 30min. Add 0.015g of KH-550 and stir for 1.5h to graft the silane coupling agent onto the LaF3 surface, obtaining a surface-modified LaF3 dispersion. Add 0.12g of MgO nanoparticles to the dispersion and stir at 70℃ for 3h to form a LaF3 / MgO composite modified suspension. Add all of the low temperature coefficient modified powder obtained in Step 2) to the suspension and stir at 600rpm for 3h to uniformly coat the nanoparticles onto the powder surface. Remove the solvent by rotary evaporation at 50℃ and 0.09 MPa to obtain wet powder. The wet powder was placed in a tube furnace and heated to 250°C at 3°C / min under an argon atmosphere (30 L / h) for 1.5 h to remove organic groups. The temperature was then maintained at 4°C / min to 600°C for 3 h to solidify and bond the coating layer. After cooling, the modified neodymium-doped quartz powder was obtained.

[0044] Step 4) The modified Nd:YAG quartz powder obtained in step 3) is ball-milled in a planetary ball mill at 200 rpm until the median particle size is about 15 μm. After weighing, 1.5 wt% of the mass of the modified Nd:YAG quartz powder is weighed into nano ZrO2 (particle size 30 nm) and 0.8 wt% of the mass of the modified Nd:YAG quartz powder is weighed into nano Y2O3 (particle size 50 nm). The three are premixed in a V-type mixer at 30 rpm for 45 min and then transferred to a planetary ball mill at 300 rpm for 2 h (stopping for 10 min every 30 min to cool down) to obtain a uniformly mixed powder.

[0045] Step 5) The uniformly mixed powder is cold isostatically pressed into a green blank at 150 MPa. The green blank is placed in a tube furnace and first purged with Cl2 (8 L / h) at 800℃ for 2 h to remove hydroxyl groups and impurities. Then, O2 (30 L / h) is switched on and held at 1.5 h to remove residual chlorine and carbon. The purified green blank is then placed in a gas pressure sintering furnace and sintered at 100 MPa. -2 Under vacuum, the temperature is increased to 1720℃ at 5℃ / min, and then high-purity N2 is introduced to 2MPa for densification. The temperature is then slowly decreased to 1100℃ at 3℃ / min and held for 3 hours for annealing to eliminate thermal stress. After cooling to room temperature in the furnace, the glass is removed, cut, ground, and polished to optical grade surface quality, thus obtaining stable luminescent neodymium-doped quartz glass with a low temperature coefficient.

[0046] Example 3

[0047] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0048] Step 1) Mix 50 mL of tetraethyl orthosilicate (TEOS) and 200 mL of anhydrous ethanol in a round-bottom flask until homogeneous. Add 30 mL of deionized water and stir magnetically at 300 rpm for 30 min at room temperature. Then, add 0.2 mol / L dilute nitric acid dropwise to adjust the pH to 3 and continue stirring for 2 h to allow TEOS to fully hydrolyze and condense to form a transparent silica sol. Dissolve 7.0 g of aluminum nitrate nonahydrate in 30 mL of deionized water to obtain an aluminum salt solution. Dissolve 0.65 g of neodymium nitrate hexahydrate in 10 mL of deionized water to obtain a neodymium salt solution. Under stirring conditions, first add the aluminum salt solution dropwise to the silica sol at a rate of 1 mL / min and stir for 1 h. Then, add the neodymium salt solution dropwise at a rate of 0.5 mL / min and stir for 2 h. After sealing, age in a constant temperature oven at 30 °C for 5 days to obtain a transparent and uniform Nd2O3 solution. 3+ / Al 3+ Co-doping with basic sol.

[0049] Step 2) Dissolve 0.44 g of boric acid in 15 mL of deionized water and add it dropwise to the basic sol obtained in Step 1) at a rate of 2 mL / min. Stir for 1.5 h to obtain a boron-doped sol. Separately, mix 100 mL of anhydrous ethanol and 10 mL of glacial acetic acid as a modifying solvent, add 0.40 g of β-lithium nepheline micropowder (1-3 μm), and ultrasonically disperse in a 70 °C water bath for 45 min to obtain a β-lithium nepheline dispersion. Slowly add the β-lithium nepheline dispersion to the boron-doped sol while stirring at 500 rpm, heat to 60 °C and stir continuously for 4 h, then cool to room temperature to obtain a low temperature coefficient modified sol. Rotate the modified sol at 60 °C and 0.09 MPa vacuum to obtain a wet gel, transfer it to a drying oven and heat from 60 °C to 120 °C at a rate of 2 °C / min for 3 h to obtain a dry gel. The dry gel was placed in a muffle furnace under air atmosphere and heated to 400℃ at 3℃ / min for 1.5h to pre-burn off organic matter. Then it was heated to 680℃ at 4℃ / min for 3h to deeply decarbonize and dehydroxylate. After cooling, it was ground through a 150-mesh sieve to obtain a low temperature coefficient modified powder.

[0050] Step 3) Add 0.30g of LaF3 nanoparticles to a mixture of 80mL anhydrous ethanol and 10mL DMF. Stir magnetically for 30min, then ultrasonically disperse for 30min. Add 0.02g of KH-550 and stir for 1.5h to graft the silane coupling agent onto the LaF3 surface, obtaining a surface-modified LaF3 dispersion. Add 0.15g of MgO nanoparticles to the dispersion and stir at 70℃ for 3h to form a LaF3 / MgO composite modified suspension. Add all of the low temperature coefficient modified powder obtained in Step 2) to the suspension and stir at 600rpm for 3h to uniformly coat the nanoparticles onto the powder surface. Remove the solvent by rotary evaporation at 50℃ and 0.09 MPa to obtain wet powder. The wet powder was placed in a tube furnace and heated to 250°C at 3°C / min under an argon atmosphere (30 L / h) for 1.5 h to remove organic groups. The temperature was then maintained at 4°C / min to 600°C for 3 h to solidify and bond the coating layer. After cooling, the modified neodymium-doped quartz powder was obtained.

[0051] Step 4) The modified NdO2-doped quartz powder obtained in Step 3) is ball-milled in a planetary ball mill at 200 rpm until the median particle size is about 15 μm. After weighing, 2 wt% of the modified NdO2-doped quartz powder mass of nano ZrO2 (particle size 30 nm) and 1 wt% of the modified NdO2-doped quartz powder mass of nano Y2O3 (particle size 50 nm) are weighed. The three are premixed in a V-type mixer at 30 rpm for 45 min, and then transferred to a planetary ball mill and ball-milled at 300 rpm for 2 h (stopping for 10 min every 30 min to cool down) to obtain a uniformly mixed powder.

[0052] Step 5) The uniformly mixed powder is cold isostatically pressed into a green blank at 150 MPa. The green blank is placed in a tube furnace and first purged with Cl2 (8 L / h) at 800℃ for 2 h to remove hydroxyl groups and impurities. Then, O2 (30 L / h) is switched on and held at 1.5 h to remove residual chlorine and carbon. The purified green blank is then placed in a gas pressure sintering furnace and sintered at 100 MPa. -2 Under vacuum, the temperature is increased to 1720℃ at 5℃ / min, and then high-purity N2 is introduced to 2MPa for densification. The temperature is then slowly decreased to 1100℃ at 3℃ / min and held for 3 hours for annealing to eliminate thermal stress. After cooling to room temperature in the furnace, the glass is removed, cut, ground, and polished to optical grade surface quality, thus obtaining stable luminescent neodymium-doped quartz glass with a low temperature coefficient.

[0053] Example 4

[0054] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0055] Step 1) Mix 50 mL of tetraethyl orthosilicate (TEOS) and 200 mL of anhydrous ethanol in a round-bottom flask until homogeneous. Add 30 mL of deionized water and stir magnetically at 300 rpm for 30 min at room temperature. Then, add 0.2 mol / L dilute nitric acid dropwise to adjust the pH to 3 and continue stirring for 2 h to allow TEOS to fully hydrolyze and condense to form a transparent silica sol. Dissolve 7.0 g of aluminum nitrate nonahydrate in 30 mL of deionized water to obtain an aluminum salt solution. Dissolve 0.8 g of neodymium nitrate hexahydrate in 10 mL of deionized water to obtain a neodymium salt solution. Under stirring conditions, first add the aluminum salt solution dropwise to the silica sol at a rate of 1 mL / min and stir for 1 h. Then, add the neodymium salt solution dropwise at a rate of 0.5 mL / min and stir for 2 h. After sealing, age in a constant temperature oven at 30 °C for 5 days to obtain a transparent and uniform Nd2O3 solution. 3+ / Al 3+ Co-doping with basic sol.

[0056] Step 2) Dissolve 0.44 g of boric acid in 15 mL of deionized water and add it dropwise to the basic sol obtained in Step 1) at a rate of 2 mL / min. Stir for 1.5 h to obtain a boron-doped sol. Separately, mix 100 mL of anhydrous ethanol and 10 mL of glacial acetic acid as a modifying solvent, add 0.40 g of β-lithium nepheline micropowder (1-3 μm), and ultrasonically disperse in a 70 °C water bath for 45 min to obtain a β-lithium nepheline dispersion. Slowly add the β-lithium nepheline dispersion to the boron-doped sol while stirring at 500 rpm, heat to 60 °C and stir continuously for 4 h, then cool to room temperature to obtain a low temperature coefficient modified sol. Rotate the modified sol at 60 °C and 0.09 MPa vacuum to obtain a wet gel, transfer it to a drying oven and heat from 60 °C to 120 °C at a rate of 2 °C / min for 3 h to obtain a dry gel. The dry gel was placed in a muffle furnace under air atmosphere and heated to 400℃ at 3℃ / min for 1.5h to pre-burn off organic matter. Then it was heated to 680℃ at 4℃ / min for 3h to deeply decarbonize and dehydroxylate. After cooling, it was ground through a 150-mesh sieve to obtain a low temperature coefficient modified powder.

[0057] Step 3) Add 0.30g of LaF3 nanoparticles to a mixture of 80mL anhydrous ethanol and 10mL DMF. Stir magnetically for 30min, then ultrasonically disperse for 30min. Add 0.03g of KH-550 and stir for 1.5h to graft the silane coupling agent onto the LaF3 surface, obtaining a surface-modified LaF3 dispersion. Add 0.2g of MgO nanoparticles to the dispersion and stir at 70℃ for 3h to form a LaF3 / MgO composite modified suspension. Add all of the low temperature coefficient modified powder obtained in Step 2) to the suspension and stir at 600rpm for 3h to uniformly coat the nanoparticles onto the powder surface. Remove the solvent by rotary evaporation at 50℃ and 0.09 MPa to obtain wet powder. The wet powder was placed in a tube furnace and heated to 250°C at 3°C / min under an argon atmosphere (30 L / h) for 1.5 h to remove organic groups. The temperature was then maintained at 4°C / min to 600°C for 3 h to solidify and bond the coating layer. After cooling, the modified neodymium-doped quartz powder was obtained.

[0058] Step 4) The modified Nd:YAG quartz powder obtained in step 3) is ball-milled in a planetary ball mill at 200 rpm until the median particle size is about 15 μm. After weighing, 3 wt% of the modified Nd:YAG quartz powder mass of nano ZrO2 (particle size 30 nm) and 2 wt% of the modified Nd:YAG quartz powder mass of nano Y2O3 (particle size 50 nm) are weighed. The three are premixed in a V-type mixer at 30 rpm for 45 min, and then transferred to a planetary ball mill and ball-milled at 300 rpm for 2 h (stopping for 10 min every 30 min to cool down) to obtain a uniformly mixed powder.

[0059] Step 5) The uniformly mixed powder is cold isostatically pressed into a green blank at 150 MPa. The green blank is placed in a tube furnace and first purged with Cl2 (8 L / h) at 800℃ for 2 h to remove hydroxyl groups and impurities. Then, O2 (30 L / h) is switched on and held at 1.5 h to remove residual chlorine and carbon. The purified green blank is then placed in a gas pressure sintering furnace and sintered at 100 MPa. -2 Under vacuum, the temperature is increased to 1720℃ at 5℃ / min, and then high-purity N2 is introduced to 2MPa for densification. The temperature is then slowly decreased to 1100℃ at 3℃ / min and held for 3 hours for annealing to eliminate thermal stress. After cooling to room temperature in the furnace, the glass is removed, cut, ground, and polished to optical grade surface quality, thus obtaining stable luminescent neodymium-doped quartz glass with a low temperature coefficient.

[0060] Example 5

[0061] A method for preparing stable luminescent neodymium-doped quartz glass with a low temperature coefficient includes the following steps:

[0062] Step 1) Mix 50 mL of tetraethyl orthosilicate (TEOS) and 200 mL of anhydrous ethanol in a round-bottom flask until homogeneous. Add 30 mL of deionized water and stir magnetically at 300 rpm for 30 min at room temperature. Then, add 0.2 mol / L dilute nitric acid dropwise to adjust the pH to 3 and continue stirring for 2 h to allow TEOS to fully hydrolyze and condense to form a transparent silica sol. Dissolve 7.0 g of aluminum nitrate nonahydrate in 30 mL of deionized water to obtain an aluminum salt solution. Dissolve 0.5 g of neodymium nitrate hexahydrate in 10 mL of deionized water to obtain a neodymium salt solution. Under stirring conditions, first add the aluminum salt solution dropwise to the silica sol at a rate of 1 mL / min and stir for 1 h. Then, add the neodymium salt solution dropwise at a rate of 0.5 mL / min and stir for 2 h. After sealing, age in a constant temperature oven at 30 °C for 5 days to obtain a transparent and uniform Nd2O3 solution. 3+ / Al 3+ Co-doping with basic sol.

[0063] Step 2) Dissolve 0.44 g of boric acid in 15 mL of deionized water and add it dropwise to the basic sol obtained in Step 1) at a rate of 2 mL / min. Stir for 1.5 h to obtain a boron-doped sol. Separately, mix 100 mL of anhydrous ethanol and 10 mL of glacial acetic acid as a modifying solvent, add 0.40 g of β-lithium nepheline micropowder (1-3 μm), and ultrasonically disperse in a 70 °C water bath for 45 min to obtain a β-lithium nepheline dispersion. Slowly add the β-lithium nepheline dispersion to the boron-doped sol while stirring at 500 rpm, heat to 60 °C and stir continuously for 4 h, then cool to room temperature to obtain a low temperature coefficient modified sol. Rotate the modified sol at 60 °C and 0.09 MPa vacuum to obtain a wet gel, transfer it to a drying oven and heat from 60 °C to 120 °C at a rate of 2 °C / min for 3 h to obtain a dry gel. The dry gel was placed in a muffle furnace under air atmosphere and heated to 400℃ at 3℃ / min for 1.5h to pre-burn off organic matter. Then it was heated to 680℃ at 4℃ / min for 3h to deeply decarbonize and dehydroxylate. After cooling, it was ground through a 150-mesh sieve to obtain a low temperature coefficient modified powder.

[0064] Step 3) Add 0.30g of LaF3 nanoparticles to a mixture of 80mL anhydrous ethanol and 10mL DMF. Stir magnetically for 30min, then ultrasonically disperse for 30min. Add 0.009g of KH-550 and stir for 1.5h to graft the silane coupling agent onto the LaF3 surface, obtaining a surface-modified LaF3 dispersion. Add 0.1g of MgO nanoparticles to the dispersion and stir at 70℃ for 3h to form a LaF3 / MgO composite modified suspension. Add all of the low temperature coefficient modified powder obtained in Step 2) to the suspension and stir at 600rpm for 3h to uniformly coat the nanoparticles onto the powder surface. Remove the solvent by rotary evaporation at 50℃ and 0.09 MPa to obtain wet powder. The wet powder was placed in a tube furnace and heated to 250°C at 3°C / min under an argon atmosphere (30 L / h) for 1.5 h to remove organic groups. The temperature was then maintained at 4°C / min to 600°C for 3 h to solidify and bond the coating layer. After cooling, the modified neodymium-doped quartz powder was obtained.

[0065] Step 4) The modified Nd:YAG quartz powder obtained in step 3) is ball-milled in a planetary ball mill at 200 rpm until the median particle size is about 15 μm. After weighing, 1 wt% of the modified Nd:YAG quartz powder is weighed into nano ZrO2 (particle size 30 nm) and 0.5 wt% of the modified Nd:YAG quartz powder is weighed into nano Y2O3 (particle size 50 nm). The three are premixed in a V-type mixer at 30 rpm for 45 min and then transferred to a planetary ball mill at 300 rpm for 2 h (with a 10 min cooling stop every 30 min) to obtain a uniformly mixed powder.

[0066] Step 5) The uniformly mixed powder is cold isostatically pressed into a green blank at 150 MPa. The green blank is placed in a tube furnace and first purged with Cl2 (8 L / h) at 800℃ for 2 h to remove hydroxyl groups and impurities. Then, O2 (30 L / h) is switched on and held at 1.5 h to remove residual chlorine and carbon. The purified green blank is then placed in a gas pressure sintering furnace and sintered at 100 MPa. -2 Under vacuum, the temperature is increased to 1720℃ at 5℃ / min, and then high-purity N2 is introduced to 2MPa for densification. The temperature is then slowly decreased to 1100℃ at 3℃ / min and held for 3 hours for annealing to eliminate thermal stress. After cooling to room temperature in the furnace, the glass is removed, cut, ground, and polished to optical grade surface quality, thus obtaining stable luminescent neodymium-doped quartz glass with a low temperature coefficient.

[0067] Comparative Example 1: Compared with Example 4, boric acid and β-lithium nepheline powder were not added in step 2), and the remaining steps and dosages were exactly the same as in Example 4.

[0068] Comparative Example 2: Compared with Example 4, LaF3 nanoparticles, KH-550 and MgO nanoparticles were not added in step 3), and the remaining steps and dosages were exactly the same as in Example 4.

[0069] Comparative Example 3: Compared with Example 4, β-lithium nepheline powder was not added in step 2), and only 0.44 g of boric acid was retained as dopant. The remaining steps and dosages were exactly the same as in Example 4.

[0070] Comparative Example 4: Compared with Example 4, boric acid was not added in step 2), only 0.40g of β-nepheline powder was added, and the remaining steps and dosages were exactly the same as in Example 4.

[0071] Comparative Example 5: Compared with Example 4, step 4) does not include nano ZrO2 and nano Y2O3 (i.e., the synergistic buffering treatment is omitted), and the remaining steps and amounts are exactly the same as in Example 4.

[0072] Comparative Example 6: Compared with Example 4, in step 4), only 3 wt% of modified neodymium-doped quartz powder nano-ZrO2 was added without adding nano-Y2O3, and the remaining steps and dosages were exactly the same as in Example 4.

[0073] Comparative Example 7: Compared with Example 4, in step 4), only 2 wt% of modified neodymium-doped quartz powder nano-Y2O3 was added without nano-ZrO2, and the remaining steps and dosages were exactly the same as in Example 4.

[0074] Comparative Example 8: Compared with Example 4, no MgO nanoparticles were added in step 3), only 0.30g of LaF3 nanoparticles and 0.03g of KH-550 were retained for surface modification treatment, and the remaining steps and amounts were exactly the same as in Example 4.

[0075] Comparative Example 9: Compared with Example 4, LaF3 nanoparticles and KH-550 were not added in step 3), only 0.2g of MgO nanoparticles were added, and the remaining steps and dosages were exactly the same as in Example 4.

[0076] Comparative Example 10: Compared with Example 4, in step 3), KH-550 was not used to modify the surface of LaF3 (i.e., 0.30g of unmodified LaF3 nanoparticles were directly mixed with 0.2g of MgO nanoparticles), and the remaining steps and amounts were exactly the same as in Example 4.

[0077] Performance testing:

[0078] 1. Determination of the temperature coefficient of refractive index: The refractive index of the sample at different temperatures was determined using the prism coupling method. A polished glass sample (10 mm in diameter, 2 mm in thickness) was placed on a prism coupling apparatus equipped with a heating stage. Using a 1064 nm laser as the light source, the refractive index was measured every 20 °C within the range of 20 °C to 200 °C. Each temperature point was held at the temperature for 10 min before measurement. Measurements were repeated three times at each temperature point, and the average value was taken. A linear fit was performed between the refractive index and temperature; the slope of this fit is the temperature coefficient of refractive index, dn / dT, in units of ×10⁻¹⁰. -6 / K.

[0079] 2. Determination of fluorescence lifetime (τ): Nd was determined by time-resolved fluorescence spectroscopy. 3+ ion 4 F 3 / 2 Fluorescence lifetime of energy levels. Using an 808nm pulsed laser diode as the excitation source (pulse width 10ns, repetition frequency 10Hz), Nd in the sample was excited. 3+ Ions to 4 F 5 / 2 After the energy level relaxes to non-radiative levels 4 F 3 / 2 The energy level was detected at 1064 nm using an InGaAs photodetector. 4 F 3 / 2 → 4 I 11 / 2 The fluorescence decay curve of the transition was recorded using a digital oscilloscope. The decay curve was fitted with a single exponential curve I(t)=I0exp(-t / τ), and the obtained τ value is the fluorescence lifetime in μs. Each sample was measured 5 times and the average value was taken.

[0080] 3. Measurement of continuous-pump fluorescence attenuation rate: The sample was placed in the pump optical path of an 808nm continuous-wave semiconductor laser, and the pump power density was fixed at 5W / cm². 2 The fluorescence emission intensity at 1064 nm was monitored in real time using a fiber optic spectrometer. The initial fluorescence intensity I0 at the start of pumping and the fluorescence intensity I after 8 hours of continuous pumping were recorded. 8h The fluorescence decay rate is calculated using the formula ΔI=(I0-I 8h The value is calculated as (I0) / I0×100%, with each sample tested twice and the average value taken. This indicator directly reflects the luminescence stability of the glass.

[0081] 4. Measurement of optical transmittance: Using an ultraviolet-visible-near-infrared spectrophotometer with air as a reference, the transmittance spectrum of the polished glass sample (2 mm thick) was scanned in the wavelength range of 200–2000 nm. The transmittance value at 1064 nm was used as the evaluation index, and the unit is 1064 nm.

[0082] 5. Appearance evaluation: Place the polished glass sample in a standard light source box (D65 light source) with a black background, visually observe the transparency and color uniformity of the sample, and record the presence or absence of defects such as haze, streaks, bubbles or crystallization. Evaluate the sample according to three levels: completely transparent, slightly hazy, and obviously hazy.

[0083] Table 1: Test results of the examples and comparative samples:

[0084]

[0085] From the table above, we can obtain:

[0086] (1) Comparative Example 1, without B2O3 and β-nepheline, has a dn / dT as high as 10.6 × 10 -6 / K, which is 2.2 times that of Example 4, demonstrates that β-lithium nepheline and B2O3 are indispensable for reducing the temperature coefficient. The dn / dT of Comparative Example 3 (B2O3 only) is 7.2 × 10⁻⁶. -6 / K, Comparative Example 4 (β-nepheline only) is 7.5 × 10 -6 / K, all significantly higher than 4.8 × 10 in Example 4. -6 / K indicates that the two alone have limited effects and must work together to achieve a reduction of more than 50% in dn / dT.

[0087] (2) Comparative Example 2, which lacks both LaF3 and MgO, has a fluorescence lifetime of only 278 μs and a fluorescence decay rate of 16.5% after 8 hours, which is in stark contrast to Example 4 (355 μs, 1.8%). The decay rate of Comparative Example 8 (LaF3 only, no MgO) is 5.2%, and the decay rate of Comparative Example 9 (MgO only, no LaF3) is 8.5%, both higher than that of Example 4, indicating that the construction of low-phonon microregions of LaF3 and the stable coordination of MgO are both indispensable.

[0088] (3) Comparative Example 5 omitted the ZrO2 and Y2O3 synergistic buffer components, and its fluorescence lifetime plummeted to 308 μs, its decay rate increased to 9.8%, its transmittance dropped to 89.0%, and a slight haze appeared in its appearance, confirming that Li + The influx of phosphors has a detrimental effect on luminescence stability and transparency. The attenuation rates of Comparative Example 6 (ZrO2 only) and Comparative Example 7 (Y2O3 only) were 6.8% and 5.5%, respectively. While these were better than Comparative Example 5, they were still far inferior to Example 4, indicating that the diffusion hindrance of ZrO2 and the coordination repair of Y2O3 must work synergistically to fully eliminate Li. + Interference.

[0089] (4) Comparative Example 10 did not use KH-550 to modify the surface of LaF3. Its decay rate increased to 5.8% and a slight haze appeared, indicating that the silane coupling agent is of great significance for achieving uniform dispersion and effective coating of LaF3 nanoparticles.

[0090] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient, characterized in that, Includes the following steps: 1) Nd2 is obtained by mixing silica sol, aluminum nitrate, and neodymium nitrate, followed by hydrolysis, polycondensation, and aging. 3+ / Al 3+ Co-doping with basic sol; 2) Reconstitute the boric acid aqueous solution with the Nd 3+ / Al 3+ The basic sol was stirred and mixed to obtain a boron-doped sol; β-lithium nepheline dispersion was added to the boron-doped sol and stirred to form a composite; after drying, pre-calcination, grinding and sieving, a low temperature coefficient modified powder was obtained. 3) Graft γ-aminopropyltriethoxysilane onto the surface of LaF3 nanoparticles to obtain a surface-modified LaF3 dispersion, and then mix it with MgO nanoparticles to form a composite modified suspension; The low temperature coefficient modified powder is added to the composite modified suspension, and after stirring and coating, solvent removal and inert atmosphere heat treatment, modified neodymium-doped quartz powder is obtained. 4) Modified neodymium-doped quartz powder, nano ZrO2 and nano Y2O3 were mixed and then ball-milled to obtain a uniformly mixed powder; 5) The uniformly mixed powder is formed into a blank, and then subjected to high-temperature purification treatment, high-temperature hot isostatic pressing sintering and annealing treatment in sequence to obtain the final product.

2. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The silica sol mentioned in step 1) is obtained by hydrolyzing and polycondensing tetraethyl orthosilicate, anhydrous ethanol and water under the catalysis of dilute nitric acid.

3. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The mass ratio of aluminum nitrate to neodymium nitrate in step 1) is 7:(0.5-0.8).

4. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The β-nepheline particle size in the β-nepheline dispersion described in step 2) is 1–3 μm.

5. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The amount of γ-aminopropyltriethoxysilane used in step 3) is 3 to 10 wt% of the mass of LaF3 nanopowder.

6. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The mass ratio of LaF3 nanoparticles to MgO nanoparticles in step 3) is 3:(1-2).

7. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The mass ratio of LaF3 nanoparticles to low temperature coefficient modified powders in step 3) is 3:(7-9).

8. The method for preparing a stable luminescent neodymium-doped quartz glass with a low temperature coefficient according to claim 1, characterized in that, The amount of nano ZrO2 used in step 4) is 1.0 to 3.0 wt% of the mass of the modified neodymium-doped quartz powder.

9. The method for preparing a low-temperature-coefficient stable luminescent neodymium-doped quartz glass according to claim 1, characterized in that, The amount of nano-Y2O3 used in step 4) is 0.5 to 2.0 wt% of the mass of the modified neodymium-doped quartz powder.

10. A stable luminescent neodymium-doped quartz glass with a low temperature coefficient, characterized in that, It is prepared by the method described in any one of claims 1-9 above.

Citation Information

Patent Citations

  • A method for preparing Nd3+ uniformly doped quartz glass

    CN106396378B