A glass microsphere with high retroreflectivity for highway markings and its preparation method
High retroreflectivity glass microspheres prepared by specific components and processes have solved the problems of low retroreflectivity and high crystallization rate in existing technologies, achieving high efficiency reflection and long lifespan for markings.
Patent Information
- Application Number
- CN202611134288.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
The retroreflection coefficient of existing glass microspheres used for highway markings is low and the crystallization rate is high, which affects the quality and safety of the markings.
Glass microspheres with high retroreflectivity are prepared using specific components and processes, including combinations of titanium dioxide, silicon dioxide, barium oxide, zirconium oxide, calcium oxide, niobium oxide, bismuth oxide, boron anhydride, and tellurium dioxide. These microspheres are then processed through melting, centrifugal spinning, annealing, and flame exposure.
The retroreflection coefficient of the glass microspheres was increased, the crystallization rate was reduced, and the visibility and service life of the markings were improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of highway marking technology, specifically relating to a glass microsphere for highway marking with a high retroreflectivity and its preparation method. Background Technology
[0002] Glass microspheres are used as the core material for achieving retroreflective function at night in road markings. Their performance is directly related to driving safety. According to statistics, the correlation between the retroreflective performance of road markings and traffic accidents is as high as 70%.
[0003] Currently, the two core technological challenges facing this field—low retroreflection coefficient and excessively high crystallization rate of glass microspheres—have become key bottlenecks restricting the improvement of road marking quality. From the perspective of retroreflection mechanism, the refractive index of glass microspheres is the primary factor determining the retroreflection coefficient. Theoretical studies show that the retroreflection performance of microspheres is optimal when the refractive index reaches 1.93. In practical applications, using high-refractive-index (1.9 and above) microspheres can significantly improve the visibility and service life of road markings. However, many existing road markings still use ordinary glass microspheres with a refractive index of only 1.5, and their retroreflection performance is far from ideal. Simultaneously, the particle size distribution, sphericity, and spreading process of the microspheres also significantly affect the reflective effect. Microspheres with uniform particle size distribution and high sphericity can achieve better directional reflection. Regarding crystallization rate, the production of high-refractive-index glass microspheres faces greater challenges. To achieve a high refractive index, a large amount of high-refractive-index oxides such as TiO2 and BaO must be introduced into the glass composition. However, this significantly increases the tendency of the glass to crystallize, leading to microsphere devitrification, reduced light transmittance, and consequently weakened reflective efficiency. Traditional production processes, such as water bath bead forming, often result in severe crystallization on the surface of microspheres and large quality fluctuations due to improper cooling methods and unstable temperature control.
[0004] To address the aforementioned shortcomings, recent technological improvements have primarily focused on optimizing glass formulations to balance refractive index and anti-crystallization performance. For example, adjusting the TiO2 / BaO molar ratio reduces the risk of devitrification. Simultaneously, improvements to the bead-forming process, such as employing a two-stage bead-forming method combined with air cooling and spray cooling, can effectively reduce devitrification and improve retroreflectivity. Furthermore, given the environmental hazards of lead-containing glass, the development of lead-free high-refractive-index glass systems has become an important direction. Lead-free formulations based on the BaO-TiO2-SiO2 system can meet refractive index requirements while avoiding lead contamination. Overall, resolving the contradiction between low retroreflectivity and high crystallization requires comprehensive efforts across multiple dimensions, including glass composition design, melting process optimization, and post-bead processing, to drive the development of road marking glass microspheres towards high refractive index, low devitrification, and uniform particle size. Summary of the Invention
[0005] The purpose of this invention is to provide a glass microsphere for highway markings with a high retroreflectivity and its preparation method.
[0006] A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 25-45 parts titanium dioxide, 20-30 parts silicon dioxide, 45-65 parts barium oxide, 5-15 parts zirconium oxide, 3-5 parts calcium oxide, 3-5 parts niobium oxide, 3-5 parts bismuth oxide, 1-3 parts boron anhydride, and 1-3 parts tellurium dioxide.
[0007] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 25-45 parts of titanium dioxide, 20-30 parts of silicon dioxide, 45-65 parts of barium oxide, 5-15 parts of zirconium oxide, 3-5 parts of calcium oxide, 3-5 parts of niobium oxide, 3-5 parts of bismuth oxide, 1-3 parts of boron anhydride, and 1-3 parts of tellurium dioxide according to the weight ratio, mix them evenly, and pass them through a 150-250 mesh sieve to obtain a mixture; (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microbead prototypes, and the glass microbead prototypes are annealed. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflection coefficient.
[0008] The melting temperature in step (2) is 1450-1550℃, and the clarification and homogenization temperature is 1600-1700℃.
[0009] The centrifugal bead feeding speed in step (3) is 2-6 kg / min, and the centrifugal speed is 4000-10000 rpm.
[0010] The annealing process in step (3) is as follows: the glass microsphere prototype is heated to 600-700℃ and held for 20-40 minutes, and then cooled in the furnace.
[0011] The flame exposure in step (4) is performed using a flame gun, and the volume ratio of natural gas to oxygen in the flame gun is 1: (1.3-1.6).
[0012] The exposure time of the flame exposure in step (4) is 0.1-0.3s.
[0013] The method of using the glass microspheres involves dividing the prepared glass microspheres into those with a particle size of 50-70μm and 100-120μm, mixing them evenly in a weight ratio of (0.5-2):1, and using them as raw materials for preparing road marking paint.
[0014] A paint for road markings, comprising the prepared high retroreflective glass microspheres.
[0015] The beneficial effects of this invention are as follows: The glass microspheres prepared by this invention possess a high retroreflection coefficient and excellent reflective effect, making them suitable for road marking. In the raw material components for preparing the glass microspheres, the combined use of niobium oxide and bismuth oxide improves the retroreflection coefficient, while the combined use of boron anhydride and tellurium dioxide reduces the crystallization rate. Different combinations of particle sizes in the prepared glass microspheres achieve the highest retroreflection coefficient. Detailed Implementation
[0016] To facilitate understanding of the present invention, a more comprehensive description will be provided below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention. Example 1
[0017] A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 35 parts titanium dioxide, 25 parts silicon dioxide, 55 parts barium oxide, 10 parts zirconium oxide, 4 parts calcium oxide, 4 parts niobium oxide, 4 parts bismuth oxide, 2 parts boron anhydride, and 2 parts tellurium dioxide.
[0018] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 35 parts of titanium dioxide, 25 parts of silicon dioxide, 55 parts of barium oxide, 10 parts of zirconium oxide, 4 parts of calcium oxide, 4 parts of niobium oxide, 4 parts of bismuth oxide, 2 parts of boron anhydride, and 2 parts of tellurium dioxide according to the weight ratio, mix them evenly, and pass them through a 200-mesh sieve to obtain a mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1500℃ and the clarification and homogenization temperature is 1650℃. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed rate is 4 kg / min and the centrifugal speed is 8000 rpm; the annealing process is: the glass microsphere prototypes are heated to 650℃ and held for 30 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.4; the exposure time of the flame exposure is 0.2s. Example 2
[0019] A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 25 parts titanium dioxide, 22 parts silicon dioxide, 45 parts barium oxide, 5 parts zirconium oxide, 3 parts calcium oxide, 3 parts niobium oxide, 3 parts bismuth oxide, 1 part boron anhydride, and 1 part tellurium dioxide.
[0020] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 25 parts of titanium dioxide, 22 parts of silicon dioxide, 45 parts of barium oxide, 5 parts of zirconium oxide, 3 parts of calcium oxide, 3 parts of niobium oxide, 3 parts of bismuth oxide, 1 part of boron anhydride, and 1 part of tellurium dioxide according to the weight proportions, mix them evenly, and pass them through a 150-mesh sieve to obtain a mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1450°C and the clarification and homogenization temperature is 1600°C. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead-spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead-spinning feeding speed is 3 kg / min and the centrifugal speed is 6000 rpm; the annealing process is: the glass microsphere prototypes are heated to 600℃ and held for 40 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.3; the exposure time of the flame exposure is 0.15s. Example 3
[0021] A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 45 parts titanium dioxide, 30 parts silicon dioxide, 65 parts barium oxide, 15 parts zirconium oxide, 5 parts calcium oxide, 5 parts niobium oxide, 5 parts bismuth oxide, 3 parts boron anhydride, and 3 parts tellurium dioxide.
[0022] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 45 parts of titanium dioxide, 30 parts of silicon dioxide, 65 parts of barium oxide, 15 parts of zirconium oxide, 5 parts of calcium oxide, 5 parts of niobium oxide, 5 parts of bismuth oxide, 3 parts of boron anhydride, and 3 parts of tellurium dioxide according to the weight proportions, mix them evenly, and pass them through a 250-mesh sieve to obtain a mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1550°C and the clarification and homogenization temperature is 1700°C. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed speed is 5 kg / min and the centrifugal speed is 10000 rpm; the annealing process is: the glass microsphere prototypes are heated to 700℃ and kept at that temperature for 20 min, and then cooled in the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.5; the exposure time of the flame exposure is 0.25s.
[0023] Comparative Example 1 A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 35 parts titanium dioxide, 25 parts silicon dioxide, 55 parts barium oxide, 10 parts zirconium oxide, 4 parts calcium oxide, 8 parts niobium oxide, 2 parts boron anhydride, and 2 parts tellurium dioxide.
[0024] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 35 parts of titanium dioxide, 25 parts of silicon dioxide, 55 parts of barium oxide, 10 parts of zirconium oxide, 4 parts of calcium oxide, 8 parts of niobium oxide, 2 parts of boron anhydride, and 2 parts of tellurium dioxide according to the weight ratio, mix them evenly, and pass them through a 200-mesh sieve to obtain the mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1500℃ and the clarification and homogenization temperature is 1650℃. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed rate is 4 kg / min and the centrifugal speed is 8000 rpm; the annealing process is: the glass microsphere prototypes are heated to 650℃ and held for 30 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.4; the exposure time of the flame exposure is 0.2s.
[0025] Comparative Example 2 A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 35 parts titanium dioxide, 25 parts silicon dioxide, 55 parts barium oxide, 10 parts zirconium oxide, 4 parts calcium oxide, 8 parts bismuth oxide, 2 parts boron anhydride, and 2 parts tellurium dioxide.
[0026] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 35 parts of titanium dioxide, 25 parts of silicon dioxide, 55 parts of barium oxide, 10 parts of zirconium oxide, 4 parts of calcium oxide, 8 parts of bismuth oxide, 2 parts of boron anhydride, and 2 parts of tellurium dioxide according to the weight ratio, mix them evenly, and pass them through a 200-mesh sieve to obtain the mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1500℃ and the clarification and homogenization temperature is 1650℃. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed rate is 4 kg / min and the centrifugal speed is 8000 rpm; the annealing process is: the glass microsphere prototypes are heated to 650℃ and held for 30 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.4; the exposure time of the flame exposure is 0.2s.
[0027] Comparative Example 3 A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 35 parts titanium dioxide, 25 parts silicon dioxide, 55 parts barium oxide, 10 parts zirconium oxide, 4 parts calcium oxide, 4 parts niobium oxide, 4 parts bismuth oxide, and 4 parts boron anhydride.
[0028] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 35 parts of titanium dioxide, 25 parts of silicon dioxide, 55 parts of barium oxide, 10 parts of zirconium oxide, 4 parts of calcium oxide, 4 parts of niobium oxide, 4 parts of bismuth oxide, and 4 parts of boric anhydride according to the weight ratio, mix them evenly, and pass them through a 200-mesh sieve to obtain a mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1500℃ and the clarification and homogenization temperature is 1650℃. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed rate is 4 kg / min and the centrifugal speed is 8000 rpm; the annealing process is: the glass microsphere prototypes are heated to 650℃ and held for 30 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.4; the exposure time of the flame exposure is 0.2s.
[0029] Comparative Example 4 A type of glass microsphere for highway marking with high retroreflectivity is made of the following components in parts by weight: 35 parts titanium dioxide, 25 parts silicon dioxide, 55 parts barium oxide, 10 parts zirconium oxide, 4 parts calcium oxide, 4 parts niobium oxide, 4 parts bismuth oxide, and 4 parts tellurium dioxide.
[0030] The preparation method of the high retroreflectivity highway marking glass microspheres is carried out according to the following steps; (1) Take 35 parts of titanium dioxide, 25 parts of silicon dioxide, 55 parts of barium oxide, 10 parts of zirconium oxide, 4 parts of calcium oxide, 4 parts of niobium oxide, 4 parts of bismuth oxide, and 4 parts of tellurium dioxide according to the weight proportions, mix them evenly, and pass them through a 200-mesh sieve to obtain a mixture. (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; the melting temperature is 1500℃ and the clarification and homogenization temperature is 1650℃. (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microsphere prototypes, and the glass microsphere prototypes are annealed; the centrifugal bead spinning feed rate is 4 kg / min and the centrifugal speed is 8000 rpm; the annealing process is: the glass microsphere prototypes are heated to 650℃ and held for 30 min, and then cooled with the furnace. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflectivity; the flame exposure is performed using a flame torch, and the volume ratio of natural gas to oxygen in the flame torch is 1:1.4; the exposure time of the flame exposure is 0.2s.
[0031] Experimental example: The retroreflectance coefficients of the glass microspheres prepared in Examples 1-3 and Comparative Examples 1-2 were measured according to GB / T18833-2012. Each experiment was repeated three times, and the average value was taken. Statistical analysis was performed using SPSS 24.0 software. Quantitative data were expressed as x̅±s (mean ± standard deviation). The Kolmogorov-Smirnov test was used to test the normality of the data. For normally distributed data, the t-test was used to compare the differences in means between two groups, with P < 0.05 considered statistically significant.
[0032] The measurement results are shown in Table 1: Table 1
[0033] Note: * indicates P < 0.05 compared to Example 1 group. The crystallization rate of the glass microspheres prepared in Examples 1-3 and Comparative Examples 3-4 was measured according to JC / T2511-2019. The results are shown in Table 2. Table 2
[0034] Note: * indicates P < 0.05 compared to Example 1 group. The glass microspheres prepared in Example 1 were divided into two groups: one with a particle size of 50-70 μm (Group 1) and the other with a particle size of 100-120 μm (Group 2). The two groups were then mixed uniformly at a weight ratio of 1:1 (Group 3). The retroreflection coefficients of the glass microspheres in Groups 1-3 were measured. The results are shown in Table 3. Table 3
[0035] Note: * indicates P < 0.05 compared to group 3. The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A type of glass microsphere for highway markings with high retroreflectivity, characterized in that, It is made from the following components in parts by weight: 25-45 parts titanium dioxide, 20-30 parts silicon dioxide, 45-65 parts barium oxide, 5-15 parts zirconium oxide, 3-5 parts calcium oxide, 3-5 parts niobium oxide, 3-5 parts bismuth oxide, 1-3 parts boron anhydride, and 1-3 parts tellurium dioxide.
2. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 1, characterized in that, Follow these steps; (1) Take 25-45 parts of titanium dioxide, 20-30 parts of silicon dioxide, 45-65 parts of barium oxide, 5-15 parts of zirconium oxide, 3-5 parts of calcium oxide, 3-5 parts of niobium oxide, 3-5 parts of bismuth oxide, 1-3 parts of boron anhydride, and 1-3 parts of tellurium dioxide according to the weight ratio, mix them evenly, and pass them through a 150-250 mesh sieve to obtain a mixture; (2) The mixture obtained in step (1) is placed in an electric furnace for melting and clarification to form a homogenized glass melt; (3) The glass liquid obtained in step (2) is passed through a centrifugal bead spinning device to form glass microbead prototypes, and the glass microbead prototypes are annealed. (4) The glass microsphere prototype after annealing in step (3) is subjected to flame exposure treatment using a flame torch to obtain glass microspheres with high retroreflection coefficient.
3. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 2, characterized in that, The melting temperature in step (2) is 1450-1550℃, and the clarification and homogenization temperature is 1600-1700℃.
4. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 2, characterized in that, The centrifugal bead feeding speed in step (3) is 2-6 kg / min, and the centrifugal speed is 4000-10000 rpm.
5. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 2, characterized in that, The annealing process in step (3) is as follows: the glass microsphere prototype is heated to 600-700℃ and held for 20-40 minutes, and then cooled in the furnace.
6. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 2, characterized in that, The flame exposure in step (4) is performed using a flame gun, and the volume ratio of natural gas to oxygen in the flame gun is 1: (1.3-1.6).
7. The method for preparing high retroreflectivity highway marking glass microspheres according to claim 2, characterized in that, The exposure time of the flame exposure in step (4) is 0.1-0.3s.
8. The method of using the glass microspheres prepared according to claim 1, characterized in that, The prepared glass microspheres were divided into those with a particle size of 50-70 μm and those with a particle size of 100-120 μm. The two were mixed evenly in a weight ratio of (0.5-2):1 and used as raw materials for preparing road marking paint.
9. A paint for highway markings, characterized in that, Including the high retroreflectivity glass microspheres prepared according to claim 1.