Edge painting process for colored crystal glass in home appliances
By using the edge-oiling process for colored crystal glass in home appliances, the color and pattern of the glass side and front are integrated and densely protected, solving the problems of inconsistent appearance and insufficient protective performance of traditional colored crystal glass side, and enhancing the high-end design value and mass production stability of the product.
Patent Information
- Application Number
- CN202611282211.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
The existing side processing technology for colored crystal glass in home appliances has problems such as poor appearance consistency, severe visual discontinuity, and weak protective performance. It cannot meet the minimalist integrated design requirements of high-end home appliances, and it is difficult to improve the yield rate of mass production.
Using the color crystal glass edge coating process for home appliances, through substrate pretreatment, ink formulation and automated coating and curing processes, the color and pattern of the front and side of the glass are presented in an integrated manner, and a dense protective coating is formed on the side. The coating is highly matched with the front decorative layer, and has high adhesion and weather resistance.
This achieves a unified color and pattern design between the glass side and the front, enhancing the product's aesthetic appearance and structural protection, as well as its high-end design value and mass production stability.
Smart Images

Figure CN123106007A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of glass processing technology, specifically to a process for applying an edge coating to colored crystal glass for home appliances. Background Technology
[0002] Currently, the side processing technology of colored crystal glass for home appliances (refrigerators, air conditioners, kitchen and bathroom decorative glass) in the industry generally adopts mechanical rough grinding or fine turning processing. Only the glass side is ground, chamfered, deburred, and smoothed. The glass side is a transparent substrate exposed without any coloring or protective coating treatment, and is directly used for the assembly of the whole machine.
[0003] Existing technologies suffer from two major flaws that hinder the high-end upgrade of colored crystal glass products: First, poor appearance consistency and severe visual disjointedness: Traditional colored crystal glass only prints colored patterns and decorative coatings on the front, limiting the color decoration effect to the front view. The sides retain the original color of transparent glass, resulting in a disconnect between the front and side views. This leads to insufficient overall integration and a monotonous appearance, failing to meet the minimalist integrated design requirements of high-end home appliances, and resulting in low added value for product design. Second, weak side protection, limiting yield: Exposed glass sides lack protective layers, leading to stress concentration at the edges. During production, transportation, assembly, and daily use, these edges are prone to chipping, minor scratches, dust accumulation, moisture erosion, and oxidation. This not only affects the product's appearance quality but also shortens its lifespan, reduces weather resistance and structural stability, making it difficult to further improve mass production yield.
[0004] Currently, there is no integrated coloring process in the industry that matches the pattern and color of the front side of colored crystal glass. In response to the shortcomings of existing traditional colored crystal glass side processing technology and the industry's technological gap, this invention aims to provide an integrated coloring and protection process for the sides of colored crystal glass used in home appliances. This process breaks through the limitations of traditional single-sided decoration, achieving an integrated presentation of color and pattern on the front and sides of the glass. At the same time, a special ink coating is used to form a dense protection on the glass sides, taking into account both the aesthetic upgrade of the product's appearance and the improvement of its structural protection performance. This fills the technological gap in the industry for homogeneous coloring of the sides of colored crystal glass, and enhances the high-end design value and mass production stability of the product. Summary of the Invention
[0005] In view of the technical problems existing in the background art, this application provides a process for edge painting of colored crystal glass for home appliances. This process can break through the limitations of traditional single-sided decoration, realize the integrated presentation of color and pattern on the front and side of the glass, and at the same time form a dense protection on the side of the glass through a special ink coating, taking into account both the aesthetic upgrade of the product appearance and the improvement of structural protection performance, filling the technical gap of homogeneous coloring of the side of colored crystal glass in the industry, and improving the high-end design value and mass production stability of the product.
[0006] To achieve the above objectives, in a first aspect, embodiments of this application provide a process for edge painting of colored crystal glass for home appliances, including: Substrate pretreatment: The substrate of colored crystal glass for home appliances is processed according to standard. The sides of the glass are treated by rough grinding and rounding or fine turning and fine edge processing, and then deep cleaning is performed to obtain the pretreated substrate. Ink Formulation: Add curing agent and diluent to the base ink to formulate a special color-patterned edge paint ink for colored crystal glass; wherein, the base ink includes oil-based epoxy resin, pigments, fillers and additives; the mass percentage of oil-based epoxy resin in the special color-patterned edge paint ink for colored crystal glass is 35%-50%, and the total solid content of the base ink is 70%-85%; Automated edge coating process: Using automated glass edge coating equipment, the four sides of the pretreated substrate are coated at a uniform speed and in a quantitative manner to obtain the coated substrate. Integrated curing and molding process: The coated substrate is cured to obtain a substrate with integrated coloring and molding on all sides.
[0007] Furthermore, the thickness of the substrate is 2mm-12mm.
[0008] Furthermore, in the special homologous color pattern edge ink for colored crystal glass, the mass percentage of curing agent is 9%-11%.
[0009] Furthermore, in the special homologous color pattern edge ink for colored crystal glass, the mass percentage of diluent is 1%-5%.
[0010] Furthermore, automated glass edge painting equipment includes edge painting machines.
[0011] Furthermore, in the automated edge coating process, the thickness of the paint film is 35μm-120μm.
[0012] Furthermore, the curing process includes tempering or baking.
[0013] Furthermore, the baking temperature is 70℃-185℃.
[0014] Furthermore, the baking time is 6-20 minutes.
[0015] Secondly, this application also provides a colored crystal glass for home appliances, which is obtained by the edge-oiling process of colored crystal glass for home appliances described in any of the above claims.
[0016] The beneficial technical effects of this application are as follows: In the technical solution of this application, the substrate pretreatment ensures that the sides are free of burrs, gaps, wavy edges, and obvious grinding scratches, and that the corner curvature is uniform and regular. Subsequently, the glass sides are deeply cleaned to remove surface dust, oil, water stains, and impurities, ensuring the substrate surface is dry and clean, providing a suitable base for the tight adhesion of the ink. The ink formulation is specifically tailored to the thermal expansion coefficient and tempering / baking process characteristics of colored crystal glass, and is highly compatible with the material, color system, and curing parameters of the colored crystal printing coating on the front of the glass, possessing high adhesion and high weather resistance. With its low-sagging and pinhole-free characteristics, it perfectly replicates the color and texture of the front surface. Automated coating, through precise control of equipment coating speed, pressure, and ink output, ensures a continuous, uniform, and smooth side ink coating with rounded and natural corner transitions, making the side coloring patterns and colors completely consistent with the crystal effect on the front of the glass. Curing and molding create a dense and stable protective coloring layer on the side ink coating, with a strong bond between the coating and the glass side and front decorative layer, eliminating delamination, fading, and discoloration issues, ultimately achieving integrated coloring and molding of the entire side of the glass. This process, through deep cleaning of the side pretreatment, automated and precise coating of specialized homogeneous ink, and simultaneous curing, results in crystal glass products with no transparent exposed edges and edges covered by a homogeneous decorative protective layer. It combines the dual functions of integrated appearance upgrade and structural protection, filling the gap in homogeneous coloring technology for crystal glass sides and enhancing the high-end design value of the product.
[0017] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0019] Figure 1 This is a side view of the glass without the edge painting process. Figure 2 This is a side view of the glass after the edge painting process. Detailed Implementation
[0020] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.
[0022] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0023] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0024] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0025] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0026] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0027] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0028] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0029] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0030] Currently, the side processing technology of colored crystal glass for home appliances (refrigerators, air conditioners, kitchen and bathroom decorative glass) in the industry generally adopts mechanical rough grinding or fine turning processing. Only the glass side is ground, chamfered, deburred, and smoothed. The glass side is a transparent substrate exposed without any coloring or protective coating treatment, and is directly used for the assembly of the whole machine.
[0031] Existing technologies suffer from two major flaws that hinder the high-end upgrade of colored crystal glass products: First, poor appearance consistency and severe visual disjointedness: Traditional colored crystal glass only prints colored patterns and decorative coatings on the front, limiting the color decoration effect to the front view. The sides retain the original color of transparent glass, resulting in a disconnect between the front and side views. This leads to insufficient overall integration and a monotonous appearance, failing to meet the minimalist integrated design requirements of high-end home appliances, and resulting in low added value for product design. Second, weak side protection, limiting yield: Exposed glass sides lack protective layers, leading to stress concentration at the edges. During production, transportation, assembly, and daily use, these edges are prone to chipping, minor scratches, dust accumulation, moisture erosion, and oxidation. This not only affects the product's appearance quality but also shortens its lifespan, reduces weather resistance and structural stability, making it difficult to further improve mass production yield.
[0032] Currently, there is no integrated coloring process in the industry that matches the pattern and color of the front side of colored crystal glass. In response to the shortcomings of existing traditional colored crystal glass side processing technology and the industry's technological gap, this invention aims to provide an integrated coloring and protection process for the sides of colored crystal glass used in home appliances. This process breaks through the limitations of traditional single-sided decoration, achieving an integrated presentation of color and pattern on the front and sides of the glass. At the same time, a special ink coating is used to form a dense protection on the glass sides, taking into account both the aesthetic upgrade of the product's appearance and the improvement of its structural protection performance. This fills the technological gap in the industry for homogeneous coloring of the sides of colored crystal glass, and enhances the high-end design value and mass production stability of the product.
[0033] To address the aforementioned technical problems, in a first aspect, embodiments of this application provide a process for edge painting of colored crystal glass for home appliances, including: Substrate pretreatment: The substrate of colored crystal glass for home appliances is processed according to standard. The sides of the glass are treated by rough grinding and rounding or fine turning and fine edge processing, and then deep cleaning is performed to obtain the pretreated substrate. Ink Formulation: Add curing agent and diluent to the base ink to formulate a special color-patterned edge paint ink for colored crystal glass; wherein, the base ink includes oil-based epoxy resin, pigments, fillers and additives; the mass percentage of oil-based epoxy resin in the special color-patterned edge paint ink for colored crystal glass is 35%-50%, and the total solid content of the base ink is 70%-85%; Automated edge coating process: Using automated glass edge coating equipment, the four sides of the pretreated substrate are coated at a uniform speed and in a quantitative manner to obtain the coated substrate. Integrated curing and molding process: The coated substrate is cured to obtain a substrate with integrated coloring and molding on all sides.
[0034] In the technical solution of this application, the substrate pretreatment ensures that the sides are free of burrs, gaps, wavy edges, and obvious grinding scratches, and that the corner curvature is uniform and regular. Subsequently, the glass sides are deeply cleaned to remove surface dust, oil, water stains, and impurities, ensuring the substrate surface is dry and clean, providing a suitable base for the tight adhesion of the ink. The ink formulation is specifically tailored to the thermal expansion coefficient and tempering / baking process characteristics of colored crystal glass, and is highly compatible with the material, color system, and curing parameters of the colored crystal printing coating on the front of the glass, possessing high adhesion and high weather resistance. With its low-sagging and pinhole-free characteristics, it perfectly replicates the color and texture of the front surface. Automated coating, through precise control of equipment coating speed, pressure, and ink output, ensures a continuous, uniform, and smooth side ink coating with rounded and natural corner transitions, making the side coloring patterns and colors completely consistent with the crystal effect on the front of the glass. Curing and molding create a dense and stable protective coloring layer on the side ink coating, with a strong bond between the coating and the glass side and front decorative layer, eliminating delamination, fading, and discoloration issues, ultimately achieving integrated coloring and molding of the entire side of the glass. This process, through deep cleaning of the side pretreatment, automated and precise coating of specialized homogeneous ink, and simultaneous curing, results in crystal glass products with no transparent exposed edges and edges covered by a homogeneous decorative protective layer. It combines the dual functions of integrated appearance upgrade and structural protection, filling the gap in homogeneous coloring technology for crystal glass sides and enhancing the high-end design value of the product.
[0035] In some embodiments, the thickness of the substrate is 2mm-12mm.
[0036] In this embodiment, the thickness of the substrate is set to 2mm-12mm, covering the commonly used thickness range of colored crystal glass for home appliances. This ensures that the uniformity, adhesion, and curing consistency of the side ink coating are maintained under both thin and thick conditions, ensuring stable integrated coloring effect on the front and sides and edge protection performance. This meets the diverse requirements of different home appliance products for glass thickness and structural strength, and improves the batch adaptability and mass production stability of the process.
[0037] In some embodiments, the curing agent in the special homologous color pattern edge ink for colored crystal glass is 9%-11% by mass.
[0038] In this embodiment, the curing agent in the special homologous color pattern edge ink for colored crystal glass is set to 9%-11% by mass, so that the oil-based epoxy resin can be fully cross-linked and cured after being coated on the side, forming a dense, tough ink protective layer with high adhesion to the glass substrate, ensuring the coating hardness, weather resistance and edge structure protection performance.
[0039] In some embodiments, the mass percentage of the diluent in the special homologous color pattern edge ink for colored crystal glass is 1%-5%.
[0040] In this embodiment, the mass percentage of the diluent in the special homologous color pattern edge ink for colored crystal glass is set to 1%-5%. The ink is adjusted to a viscosity and leveling property suitable for automated and precise coating, so that the side coating is uniform and flat, with no ink piling at corners and no missed coating, reducing sagging and uneven thickness. It also ensures that the ink is cured synchronously with the front colored crystal coating under high temperature tempering or low temperature baking conditions, realizing homologous integrated coloring of the front and sides and mass production stability.
[0041] In some embodiments, automated glass edge painting equipment includes an edge painting machine.
[0042] In this embodiment, mechanized and parameterized precise coating replaces traditional manual edge coating, enabling the special homologous colored crystal edge coating ink to be uniformly, continuously, and quantitatively coated along the four sides of the glass, ensuring that the side coating is flat and consistent, with no ink piling at corners and no missed coating, thereby improving edge coating efficiency and batch consistency.
[0043] In some embodiments, the thickness of the paint film in the automated edge coating process is 35μm-120μm.
[0044] In this embodiment, automated edge coating forms a continuous, uniform, and sufficiently opaque homologous ink layer on the glass side, creating a dense and effective edge protection layer. This balances decorative effect, edge protection, and synchronous curing stability under high-temperature tempering or low-temperature baking, thereby improving mass production consistency and yield.
[0045] In some embodiments, the curing process includes tempering or baking.
[0046] In this embodiment, the special homologous colored crystal edge ink coated on the side of the glass is fully cross-linked and cured by high-temperature tempering or low-temperature baking, forming a protective decorative layer with strong adhesion, dense and uniform texture, and consistent with the color and texture of the front colored crystal coating at the glass edge. Tempering can complete the ink curing while strengthening the glass substrate, while baking can be adapted to substrates of different thicknesses and ink systems. Both can ensure the coating hardness, weather resistance, and edge structure protection performance, thereby improving the integrated appearance effect of the front and side of the colored crystal glass for home appliances and the stability of mass production.
[0047] In some embodiments, the baking temperature is 70°C-185°C.
[0048] In this embodiment, the baking temperature is set to 70℃-185℃, and the ratio of special oil-based epoxy resin and its curing agent and diluent is matched. Under the condition of 70℃-185℃, the ink can be fully cross-linked and cured, forming a dense, uniform, and strongly adhesive homologous protective decorative layer on the glass side. This takes into account the hardness, weather resistance, edge protection performance and the consistency of the front and side integrated appearance of the side coating, thereby improving the stability and yield of mass production.
[0049] In some embodiments, the baking time is 6 min to 20 min.
[0050] In this embodiment, the baking time is set to 6-20 minutes, matched with a baking temperature of 70℃-185℃ and a special oil-based epoxy resin system, so that the side ink coating can be fully cross-linked and cured within 6-20 minutes, forming a dense, uniform, and strongly adhesive protective decorative layer that is consistent with the color and texture of the front colored crystal coating. This balances the hardness of the side coating, edge protection, consistent appearance of the front and side, as well as mass production efficiency and yield.
[0051] Secondly, this application also provides a colored crystal glass for home appliances, which is obtained by the edge-oiling process of colored crystal glass for home appliances described in any of the above claims.
[0052] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0053] I. Preparation Method Example 1 Substrate pretreatment: The substrate of colored crystal glass for home appliances is processed according to standard. The sides of the glass are treated by rough grinding and rounding or fine turning and fine edge processing, and then deep cleaning is performed to obtain the pretreated substrate. Ink formulation: Based on 100 parts of the total mass of finished ink: 38 parts epoxy resin; 4.5 parts reactive diluent; 15 parts pigment; 10 parts filler; 8 parts curing agent; 1.2 parts dispersant; 0.5 parts leveling agent; 0.3 parts defoamer; 22.5 parts solvent. (The solid content of the ink is 77.5%).
[0054] Automated edge coating process: Using automated glass edge coating equipment, the edges of the pretreated substrate are coated at a uniform speed and in a quantitative manner to obtain the coated substrate; the coating speed is 6m / min, the thickness is controlled at 60um, and the coating time for a glass with a circumference of 1 meter is 10s.
[0055] Integrated curing and molding process: The coated substrate is cured at a temperature of 150 degrees Celsius for 6 minutes and 20 seconds. After cooling, it is placed on a shelf to obtain a substrate with integrated coloring and molding on all sides.
[0056] Example 2 The difference from Example 1 is that the epoxy resin is 37 parts, the solvent is 30 parts, and the total solid content is 70%. The remaining steps are the same as in Example 1 and will not be repeated here. The colored crystal glass of Example 2 is obtained.
[0057] Example 3 The difference from Example 1 is that 46 parts of epoxy resin, 15 parts of solvent, and the total solid content of ink are about 85%. The remaining steps are the same as in Example 1 and will not be repeated here. The colored crystal glass of Example 3 is obtained.
[0058] Comparative Examples 1-9 The difference from Example 1 is that the type and proportion of ink are different. The remaining steps are the same as in Example 1 and will not be repeated here. Comparative Examples 1-9 colored crystal glass are obtained.
[0059] Table 1 shows the test results for the type and solid content of the main resin. As can be seen from Table 1, oil-based epoxy resin (70%-85%) can meet all performance requirements. After the prepared ink is processed using the above process for edge ink dripping, the baking is relatively smooth and the performance is qualified.
[0060] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, are also included in the scope of this application without departing from the spirit of this application.
[0061] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A process for the production of an oil edge on a domestic appliance colored crystal glass, characterized in that, The method comprises the following steps: Substrate pretreatment: the substrate of the household appliance crystal glass is subjected to standard processing, the side edges of the glass are treated by rough grinding or fine machining, and the substrate is subjected to deep cleaning to obtain a pretreated substrate; Ink preparation: a curing agent and a diluent are added to a base ink to prepare a special homologous color pattern oil edge ink for the crystal glass; wherein the base ink comprises an oily epoxy resin, pigments, fillers and additives; the mass percentage of the oily epoxy resin in the special homologous color pattern oil edge ink for the crystal glass is 35%-50%, and the total solid content of the base ink is 70%-85%; Automatic oil edge coating process: a glass oil edge automatic equipment is used to uniformly and quantitatively coat the four side edges of the pretreated substrate to obtain a coated substrate; Integrated curing and forming process: the coated substrate is cured to obtain a substrate with full-side integrated coloring and forming.
2. The appliance opalescent glass oil edge process according to claim 1, wherein, The thickness of the substrate is 2mm-12mm.
3. The appliance opalescent glass oil edge process according to claim 1, wherein, In the special homologous color pattern oil edge ink for the crystal glass, the mass percentage of the curing agent is 9%-11%.
4. The appliance opalescent glass oil edge process of claim 3, wherein, In the special homologous color pattern oil edge ink for the crystal glass, the mass percentage of the diluent is 1%-5%.
5. The appliance opalescent glass oil edge process of claim 1, wherein, The glass oil edge automatic equipment comprises an oil edge machine.
6. The appliance opalescent glass oil edge process of claim 1, wherein, In the automatic oil edge coating process, the thickness of the paint film coating is 35μm-120μm.
7. The appliance opalescent glass oil edge process of claim 1, wherein, The curing process comprises tempering or baking.
8. The appliance opalescent glass oil edge process of claim 7, wherein, The baking temperature is 70℃-185℃.
9. The appliance opalescent glass oil edge process of claim 7, wherein, The baking time is 6min-20min.
10. A household appliance colored crystal glass, characterized by, The household appliance crystal glass oil edge process is obtained by the method.