A neutral-colored tri-silver coated glass and its preparation method
By replacing the nickel-chromium alloy layer with a copper-nickel alloy layer in triple-silver coated glass, the spectral differences are balanced, solving the problems of greenish and yellowish tints in the transmitted color, and achieving triple-silver coated glass with neutral color tone and high energy-saving performance.
Patent Information
- Application Number
- CN202611454098.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing triple-silver low-emissivity coated glass has problems with greenish or yellowish tint and cloudy color tone. Conventional color adjustment methods cannot completely solve these problems and may sacrifice energy-saving performance.
A copper-nickel alloy layer is used to replace the traditional nickel-chromium alloy layer as a protective tuning layer. By adjusting the thickness and ratio of the copper-nickel alloy, the spectral differences of the multiple silver layers are balanced to achieve a neutral tone.
The neutral-toned triple-silver coated glass maintains high light transmittance and low emissivity, improving the color consistency and stability of the product and avoiding secondary defects caused by traditional color matching.
Smart Images

Figure CN123106014A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of triple silver coated glass technology, specifically relating to a neutral-colored triple silver coated glass and its preparation method. Background Technology
[0002] Triple-silver low-emissivity coated glass has extremely low emissivity and ultra-high infrared blocking rate, and its energy-saving performance far exceeds that of single-silver and double-silver products. It is the core material for high-end ultra-energy-saving building curtain walls, skylights, and passive energy-saving buildings.
[0003] Currently, all mass-produced triple silver low-emissivity coated glass film systems in the industry uniformly use nickel-chromium alloy as the protective barrier layer for the three silver layers. Nickel-chromium alloy has excellent anti-oxidation, anti-corrosion, and tempering properties, which can effectively protect the multi-layer silver layers from oxidation and failure.
[0004] However, existing nickel-chromium-coated triple-silver structures have inherent technical defects that cannot be overcome: nickel-chromium alloys exhibit selective absorption deviations in the green and yellow wavelengths of visible light. Even a single layer of nickel-chromium can produce a slight color shift, and the spectral shift effect is amplified exponentially after three layers are stacked, resulting in a common problem of greenish or yellowish tints and a cloudy, opaque tone in triple-silver coated glass. Conventional color-correction methods in the industry can only passively compensate by fine-tuning the thickness of the dielectric layer, the silver layer, and the sputtering power. The adjustment margin is extremely small and cannot fundamentally offset the inherent color shift caused by the nickel-chromium material itself, making it difficult to achieve a high-purity, neutral, and transparent color tone. At the same time, forcibly adjusting the film parameters to correct the color shift can easily cause a decrease in light transmittance, an increase in emissivity, and an imbalance in film stress, leading to secondary defects such as reduced energy-saving performance, poor tempering, and film peeling. Summary of the Invention
[0005] The technical problem to be solved by this invention is: to address the inherent spectral color deviation of the all-nickel-chromium protective triple silver structure in the prior art, which results in the finished product having a greenish or yellowish tint and a cloudy color tone, which cannot be completely solved by conventional color adjustment and easily sacrifices energy-saving performance, and to provide a neutral-color triple silver coated glass and its preparation method.
[0006] To address the aforementioned technical problems, this invention provides neutral-colored triple-silver coated glass, wherein each silver layer in the neutral-colored triple-silver coated glass uses a copper-nickel alloy layer as a protective tuning layer on its surface. This invention abandons the all-nickel-chromium protective structure, replacing all three protective tuning layers with copper-nickel alloy layers. Utilizing the material characteristics of copper-nickel alloy—a flat visible light absorption curve with no significant band-selective shift—it replaces the color-shifting spectral characteristics of nickel-chromium, eliminating the yellow-green color shift problem caused by multi-layer superposition at its source. Simultaneously, copper-nickel alloy retains excellent oxidation and high-temperature resistance properties, without affecting the film stability and secondary processing performance, achieving the effect of unchanged protective function, undiminished energy-saving performance, and completely neutral color tone.
[0007] The neutral-color triple-silver coated glass includes a substrate, on one side of which are sequentially disposed from the inside out a bottom dielectric layer, a first silver layer, a first protective tuning layer, a first intermediate dielectric layer, a second silver layer, a second protective tuning layer, a second intermediate dielectric layer, a third silver layer, a third protective tuning layer, and a top dielectric layer; the first protective tuning layer, the second protective tuning layer, and the third protective tuning layer are all copper-nickel alloy layers.
[0008] The copper-nickel alloy layer has a copper to nickel mass ratio of 3:7 to 5:5. This ratio range can smoothly absorb visible light clutter and accurately offset the yellow-green color shift caused by the superposition of the three silver film system.
[0009] The thickness of the first protective tuning layer is 1.5~5nm, the thickness of the second protective tuning layer is 1.8~5nm, and the thickness of the third protective tuning layer is 2.0~5.0nm. This gradient thickness ratio adapts to the spectral differences of the three silver layers, achieving global tone balance.
[0010] The thickness of the first silver layer is 8.0~10.0 nm, the thickness of the second silver layer (6) is 9.0~11.0 nm, and the thickness of the third silver layer is 10.0~12.0 nm. Combined with a copper-nickel alloy protective layer, this achieves a three-in-one performance of high transmittance, low radiation, and neutral color tone.
[0011] The bottom dielectric layer is one of a metal layer or metal alloy layer, a metal oxide layer, a metal nitride layer, a non-metal oxide layer, or a non-metal nitride layer; the thickness of the bottom dielectric layer (2) is 80~120nm. The refractive index of the bottom dielectric layer matches the spectral characteristics of the copper-nickel alloy layer, which helps to improve the color uniformity and film density.
[0012] The first intermediate dielectric layer and the second intermediate dielectric layer are one of a metal layer or a metal alloy layer, a metal oxide layer, and a non-metal oxide layer; the thicknesses of the first intermediate dielectric layer and the second intermediate dielectric layer are 50-80 nm and 50-80 nm, respectively. The top dielectric layer is one of a metal layer or a metal alloy layer, a metal nitride layer, a non-metal nitride layer, and a non-metal oxide nitride layer; the thickness of the top dielectric layer is 30-70 nm. This invention also provides a method for preparing the neutral-color three-silver coated glass, the method comprising the following steps:
[0013] S1. Pretreatment: The substrate is cleaned, dried and vacuum activated.
[0014] S2. Vacuum Setup: The substrate is placed into the magnetron sputtering vacuum chamber and evacuated to a vacuum level of 2.5 × 10⁻⁶. -3 ~4.5×10 -3 Pa, argon gas is introduced;
[0015] S3. Deposition: From the inside out, the following layers are deposited sequentially on the surface: bottom dielectric layer, first silver layer, first protective tuning layer, first intermediate dielectric layer, second silver layer, second protective tuning layer, second intermediate dielectric layer, third silver layer, third protective tuning layer, and top dielectric layer; wherein, the first protective tuning layer, the second protective tuning layer, and the third protective tuning layer are all deposited to form a copper-nickel alloy layer.
[0016] In step S3, the copper-nickel alloy layer is deposited using a DC magnetron sputtering process with a sputtering power of 2.0~3.2kW and an argon gas pressure of 0.3~0.5Pa.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. In terms of the material system, this invention uses a copper-nickel alloy layer to replace the traditional nickel-chromium alloy layer as the protective tuning layer for each silver layer. Since the visible light spectrum absorption curve of the copper-nickel alloy is flat and has no obvious band selective shift, it avoids the spectral shift caused by the superposition of multiple nickel-chromium layers from the material source, and solves the problem of greenish and yellowish color transmission in triple silver coated glass, so that the finished product presents a neutral and transparent visual effect.
[0019] 2. In terms of protective performance, the copper-nickel alloy possesses excellent oxidation resistance, corrosion resistance, and high-temperature resistance, effectively protecting the silver layer from oxidation and peeling during processing and use, ensuring the adhesion and temperability of the film. After tempering and hollow composite bonding, there is no discoloration or film peeling, and the product exhibits good mass production stability.
[0020] 3. In terms of energy-saving performance, this invention only replaces the protective layer material without changing the core structure of the silver layer and the main structure of the dielectric layer. It retains the original high light transmittance and ultra-low radiation energy-saving performance of triple silver coated glass, avoiding the problems of decreased light transmittance or increased emissivity caused by adjusting the film parameters during the traditional color matching process.
[0021] 4. Regarding product consistency, by designing the thickness and ratio of the three copper-nickel alloy layers in a gradient manner, the optical parameters of each silver layer are matched layer by layer, balancing the interference colors of the film system, effectively reducing color difference in mass production, and improving the consistency of product color tone.
[0022] 5. In terms of process implementation, this solution can be directly implemented on the existing magnetron sputtering production line by changing the target material, without the need for new equipment. It has strong process adaptability and is conducive to large-scale production applications. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the layered structure of the neutral-color three-silver coated glass multilayer composite film system of the present invention;
[0024] Wherein, 1-substrate, 2-bottom dielectric layer, 3-first silver layer, 4-first protective tuning layer, 5-first intermediate dielectric layer, 6-second silver layer, 7-second protective tuning layer, 8-second intermediate dielectric layer, 9-third silver layer, 10-third protective tuning layer, 11-top dielectric layer. Detailed Implementation
[0025] like Figure 1 As shown, this embodiment provides a neutral-color triple silver coated glass, including a substrate 1 and a multilayer composite film system deposited on one side of the substrate 1; the multilayer composite film system is provided from the inside out with a bottom dielectric layer 2, a first silver layer 3, a first protective tuning layer 4, a first intermediate dielectric layer 5, a second silver layer 6, a second protective tuning layer 7, a second intermediate dielectric layer 8, a third silver layer 9, a third protective tuning layer 10 and a top dielectric layer 11; wherein, the first protective tuning layer 4, the second protective tuning layer 7 and the third protective tuning layer 10 are all copper-nickel alloy layers.
[0026] The mass ratio of copper to nickel in the copper-nickel alloy layer is 3:7 to 5:5.
[0027] The thickness of the first protective tuning layer is 1.5~5nm, the thickness of the second protective tuning layer is 1.8~5nm, and the thickness of the third protective tuning layer is 2.0~5.0nm.
[0028] The thickness of the first silver layer is 8.0~10.0 nm, the thickness of the second silver layer is 9.0~11.0 nm, and the thickness of the third silver layer is 10.0~12.0 nm.
[0029] The underlying dielectric layer is one of the following: a metal layer or metal alloy layer, a metal oxide layer, a metal nitride layer, a non-metal oxide layer, or a non-metal nitride layer, preferably ZnSn, ZnAl, ZnO, or ZnSnO. x AZO, SiO2, Si3N4, SiAlN x SiZrN x SiN x O y Any one of the following. The thickness of the underlying dielectric layer is 80~120nm.
[0030] The first intermediate dielectric layer and the second intermediate dielectric layer are one of the following: a metal layer or a metal alloy layer, a metal oxide layer, and a non-metal oxide layer, preferably ZnSn, ZnAl, Si3N4, ZnO, or ZnSnO. x The first intermediate dielectric layer and the second intermediate dielectric layer are each selected from the following: AZO, GZO, BZO, SnO2, TiO2, Nb2O5, Ta2O5, ZrO2, and ITO. The thickness of each intermediate dielectric layer is 50~80 nm.
[0031] The top dielectric layer is one of a metal layer or metal alloy layer, a metal nitride layer, a non-metal nitride layer, or a non-metal oxide nitride layer, preferably Si3N4 or SiAlN. x SiZrN x SiN x O y It is any one of TiN and ZrN. The thickness of the top dielectric layer is 30~70nm.
[0032] The preparation method of the tri-silver coated glass in this embodiment includes the following steps:
[0033] S1. Pretreatment: The substrate 1 is subjected to multi-stage pure water spray cleaning, brush cleaning, hot air drying and vacuum activation treatment to thoroughly remove surface dust, oil and impurities.
[0034] S2. Vacuum Establishment: Substrate 1 is placed into the magnetron sputtering vacuum chamber and evacuated to a vacuum level of 2.5 × 10⁻⁶. -3 ~4.5×10 -3 Pa, introduce high-purity argon gas to stabilize the working pressure;
[0035] S3. Deposition: A magnetron sputtering process is used to deposit the following layers sequentially from the inside out on the surface of substrate 1: bottom dielectric layer 2, first silver layer 3, first protective tuning layer 4, first intermediate dielectric layer 5, second silver layer 6, second protective tuning layer 7, second intermediate dielectric layer 8, third silver layer 9, third protective tuning layer 10, and top dielectric layer 11. The first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 are all deposited to form copper-nickel alloy layers. The copper-nickel alloy layers are deposited using a DC magnetron sputtering process with a sputtering power of 2.0~3.2kW and an argon gas pressure of 0.3~0.5Pa.
[0036] The present invention will now be described in detail with reference to the embodiments.
[0037] Example 1
[0038] A neutral-colored triple-silver coated glass includes a substrate 1. On one side of the substrate 1, from the inside out, are sequentially disposed a bottom dielectric layer 2, a first silver layer 3, a first protective tuning layer 4, a first intermediate dielectric layer 5, a second silver layer 6, a second protective tuning layer 7, a second intermediate dielectric layer 8, a third silver layer 9, a third protective tuning layer 10, and a top dielectric layer 11. The substrate 1 is a transparent glass substrate; the bottom dielectric layer 2 is a Si3N4 layer with a thickness of 100 nm; the first silver layer 3 has a thickness of 9.0 nm; and the first protective tuning layer 4 is a copper-nickel alloy layer with a thickness of 2.0 nm, with a copper-nickel mass ratio... The ratio of Cu to Ni is 4:6; the first intermediate dielectric layer 5 is a ZnSn layer with a thickness of 65nm; the second silver layer 6 has a thickness of 10.0nm; the second protective tuning layer 7 is a copper-nickel alloy layer with a thickness of 2.3nm, and the mass ratio of copper to nickel is Cu:Ni=4:6; the second intermediate dielectric layer 8 is a ZnAl layer with a thickness of 70nm; the third silver layer 9 has a thickness of 11.0nm; the third protective tuning layer 10 is a copper-nickel alloy layer with a thickness of 2.6nm, and the mass ratio of copper to nickel is Cu:Ni=4:6; the top dielectric layer 11 is a Si3N4 layer with a thickness of 45nm.
[0039] The preparation method of the neutral-colored triple-silver coated glass includes the following steps:
[0040] S1. Pretreatment: The substrate 1 is subjected to multi-stage pure water spray cleaning, brush cleaning, hot air drying and vacuum activation treatment to thoroughly remove surface dust, oil and impurities.
[0041] S2. Vacuum Establishment: Substrate 1 is placed into the magnetron sputtering vacuum chamber and evacuated to a vacuum level of 2.5 × 10⁻⁶. -3 ~4.5×10 -3 Pa, introduce high-purity argon gas to stabilize the working pressure;
[0042] S3. Deposition: A magnetron sputtering process is used to deposit the following layers sequentially from the inside out on the surface of substrate 1: bottom dielectric layer 2, first silver layer 3, first protective tuning layer 4, first intermediate dielectric layer 5, second silver layer 6, second protective tuning layer 7, second intermediate dielectric layer 8, third silver layer 9, third protective tuning layer 10, and top dielectric layer 11. The first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 are all deposited to form copper-nickel alloy layers. The copper-nickel alloy layers are deposited using a DC magnetron sputtering process with a sputtering power of 2.8 kW and an argon gas pressure of 0.4 Pa.
[0043] S4. Post-treatment: After coating is completed, the glass is slowly cooled at a constant temperature to release the stress of the film and solidify the structure. After tempering and homogenization, the finished neutral-colored three-silver coated glass is obtained.
[0044] The neutral-colored triple-silver coated glass in this embodiment has a visible light transmittance of 68.5%, an emissivity of 0.02, and excellent energy-saving performance. The transmittance parameters L=86.2, a=-1.5, b=-2.0 are completely within the high-purity neutral range, with no visible green or yellow tint. After tempering, the color difference ΔE=0.5, the coating layer does not peel off, oxidize, or discolor, and the surface is clear and clean.
[0045] Example 2
[0046] A neutral-colored triple-silver coated glass includes a substrate. On one side of the substrate, from the inside out, are sequentially disposed a bottom dielectric layer 2, a first silver layer 3, a first protective tuning layer 4, a first intermediate dielectric layer 5, a second silver layer 6, a second protective tuning layer 7, a second intermediate dielectric layer 8, a third silver layer 9, a third protective tuning layer 10, and a top dielectric layer 11. The bottom dielectric layer 2 is a Si3N4 layer with a thickness of 80 nm; the first silver layer 3 has a thickness of 8 nm; and the first protective tuning layer 4 is a copper-nickel alloy layer with a thickness of 1.5 nm, where the mass ratio of copper to nickel is Cu:Ni. =3:7; the first intermediate dielectric layer 5 is a ZnSn layer with a thickness of 50nm; the second silver layer 6 has a thickness of 9.0nm; the second protective tuning layer 7 is a copper-nickel alloy layer with a thickness of 1.8nm, and the mass ratio of copper to nickel is Cu:Ni=3:7; the second intermediate dielectric layer 8 is a ZnAl layer with a thickness of 50nm; the third silver layer 9 has a thickness of 10nm; the third protective tuning layer 10 is a copper-nickel alloy layer with a thickness of 2.0nm, and the mass ratio of copper to nickel is Cu:Ni=3:7; the top dielectric layer 11 is a Si3N4 layer with a thickness of 30nm.
[0047] The neutral-colored triple-silver coated glass in this embodiment has a visible light transmittance of 70.5% and an emissivity of 0.028, exhibiting excellent energy-saving performance. The transmittance parameters L=87.24, a=-1.0, and b=-1.3 are entirely within the high-purity neutral range, with no visible green or yellow tint. After tempering, the color difference ΔE=1.0, with no film peeling, oxidation, or discoloration, resulting in a clear and clean surface.
[0048] Example 3
[0049] A neutral-colored triple-silver coated glass includes a substrate. On one side of the substrate, from the inside out, are sequentially disposed a bottom dielectric layer 2, a first silver layer 3, a first protective tuning layer 4, a first intermediate dielectric layer 5, a second silver layer 6, a second protective tuning layer 7, a second intermediate dielectric layer 8, a third silver layer 9, a third protective tuning layer 10, and a top dielectric layer 11. The bottom dielectric layer 2 is a Si3N4 layer with a thickness of 110 nm; the first silver layer 3 has a thickness of 10 nm; and the first protective tuning layer 4 is a copper-nickel alloy layer with a thickness of 5.0 nm, where the mass ratio of copper to nickel is Cu: Ni=5:5; the first intermediate dielectric layer 5 is a ZnSn layer with a thickness of 80nm; the second silver layer 6 has a thickness of 11nm; the second protective tuning layer 7 is a copper-nickel alloy layer with a thickness of 4.5nm, and the mass ratio of copper to nickel is Cu:Ni=5:5; the second intermediate dielectric layer 8 is a ZnAl layer with a thickness of 80nm; the third silver layer 9 has a thickness of 12nm; the third protective tuning layer 10 is a copper-nickel alloy layer with a thickness of 4.5nm, and the mass ratio of copper to nickel is Cu:Ni=5:5; the top dielectric layer 11 is a Si3N4 layer with a thickness of 70nm.
[0050] The neutral-colored triple-silver coated glass in this embodiment has a visible light transmittance of 67.3% and an emissivity of 0.02, exhibiting excellent energy-saving performance. The transmittance parameters L=85.66, a=-2.0, and b=-2.2 are entirely within the high-purity neutral range, with no visible green or yellow tint. After tempering, the color difference ΔE=0.8, with no film peeling, oxidation, or discoloration, resulting in a clear and clean surface.
[0051] Comparative Example 1
[0052] The rest is the same as in Embodiment 1, except that the first protective tuning layer 4 is a NiCr layer.
[0053] Comparative Example 2
[0054] The rest is the same as in Embodiment 1, except that the second protective tuning layer 7 is a Ti layer.
[0055] Comparative Example 3
[0056] The rest is the same as in Embodiment 1, except that the third protective tuning layer 10 is an AZO layer.
[0057] Comparative Example 4
[0058] The rest is the same as in Embodiment 1, except that the first protective tuning layer 4 and the second protective tuning layer 7 are both Ti layers.
[0059] Comparative Example 5
[0060] The rest is the same as in Embodiment 1, except that the first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 are all NiCr layers.
[0061] Comparative Example 6
[0062] The rest is the same as in Embodiment 1, except that the first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 are omitted.
[0063] The performance of the triple silver coated glass in the above embodiments and comparative examples is shown in Table 1.
[0064] Table 1
[0065]
[0066] In Table 1, Y represents reflectance, a and b represent color values, and T represents transmittance.
[0067] As can be seen from the above, the triple-silver coated glass produced according to the embodiment of the present invention is entirely within the high-purity neutral range. Furthermore, it exhibits no visible green or yellow tint; after tempering, there is no color difference, the coating shows no peeling, oxidation, or discoloration, and the surface is clear and clean.
[0068] In Comparative Example 1, only the first protective tuning layer 4 is a NiCr layer, and the transmitted color appears greenish and yellowish compared to the embodiment.
[0069] In Comparative Example 2, the second protective tuning layer 7 is a Ti layer, which has a lower transmittance compared to the embodiment, and the transmitted color does not reach the hue of the embodiment.
[0070] In Comparative Example 3, only the third protective tuning layer 10 is an AZO layer, and the transmittance color shows a yellowish-green tint compared to the embodiment.
[0071] In Comparative Example 4, both the first protective tuning layer 4 and the second protective tuning layer 7 are Ti layers. Compared with the embodiment, the transmittance is yellowish-green and the transmittance is lower.
[0072] In Comparative Example 5, only the first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 are all NiCr layers, and the transmitted color is more yellowish-green compared to the embodiment.
[0073] In Comparative Example 6, only the first protective tuning layer 4, the second protective tuning layer 7, and the third protective tuning layer 10 were omitted, resulting in oxidation and a poor film quality.
[0074] The above detailed description of a neutral-color tri-silver coated glass and its preparation method, with reference to the embodiments, is illustrative rather than limiting. Several embodiments can be listed according to the defined scope. Therefore, variations and modifications without departing from the overall concept of the present invention should be within the protection scope of the present invention.
Claims
1. A neutral-colored triple-silver coated glass, characterized in that, Each silver layer in the neutral-colored three-silver coated glass uses a copper-nickel alloy layer as a protective tuning layer on its surface.
2. The neutral-colored tri-silver coated glass according to claim 1, characterized in that, The neutral-color three-silver coated glass includes a substrate (1), and the substrate (1) is provided with a bottom dielectric layer (2), a first silver layer (3), a first protective tuning layer (4), a first intermediate dielectric layer (5), a second silver layer (6), a second protective tuning layer (7), a second intermediate dielectric layer (8), a third silver layer (9), a third protective tuning layer (10), and a top dielectric layer (11) from the inside to the outside. The first protective tuning layer (4), the second protective tuning layer (7) and the third protective tuning layer (10) are all copper-nickel alloy layers.
3. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The mass ratio of copper to nickel in the copper-nickel alloy layer is 3:7 to 5:
5.
4. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The thickness of the first protective tuning layer (4) is 1.5~5nm, the thickness of the second protective tuning layer (7) is 1.8~5nm, and the thickness of the third protective tuning layer (10) is 2.0~5.0nm.
5. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The thickness of the first silver layer (3) is 8.0~10.0 nm, the thickness of the second silver layer (6) is 9.0~11.0 nm, and the thickness of the third silver layer (9) is 10.0~12.0 nm.
6. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The bottom dielectric layer (2) is one of a metal layer or metal alloy layer, metal oxide layer, metal nitride layer, non-metal oxide layer, or non-metal nitride layer; the thickness of the bottom dielectric layer (2) is 80~120nm.
7. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The first intermediate dielectric layer (5) and the second intermediate dielectric layer (8) are one of the following: metal layer or metal alloy layer, metal oxide layer, and non-metal oxide layer; the thickness of the first intermediate dielectric layer (5) and the second intermediate dielectric layer (8) is 50~80nm.
8. The neutral-colored tri-silver coated glass according to claim 1 or 2, characterized in that, The top dielectric layer (11) is one of a metal layer or metal alloy layer, a metal nitride layer, a non-metal nitride layer, or a non-metal oxide layer; the thickness of the top dielectric layer (11) is 30~70nm. A method for preparing neutral-color tri-silver coated glass as described in any one of claims 1-8, characterized in that the preparation method comprises the following steps: S1. Pretreatment: The substrate (1) is cleaned, dried and vacuum activated. S2, Vacuum Setup: The substrate (1) is placed into the magnetron sputtering vacuum chamber and evacuated to a vacuum level of 2.5 × 10⁻⁶. -3 ~4.5×10 -3 Pa, argon gas is introduced; S3, Deposition: On the surface of (1), from the inside out, the following layers are deposited in sequence: bottom dielectric layer (2), first silver layer (3), first protective tuning layer (4), first intermediate dielectric layer (5), second silver layer (6), second protective tuning layer (7), second intermediate dielectric layer (8), third silver layer (9), third protective tuning layer (10), and top dielectric layer (11); wherein, the first protective tuning layer (4), the second protective tuning layer (7), and the third protective tuning layer (10) are all deposited to form a copper-nickel alloy layer.
9. The neutral-colored tri-silver coated glass according to claim 1, characterized in that, In step S3, the copper-nickel alloy layer is deposited using a DC magnetron sputtering process with a sputtering power of 2.0~3.2kW and an argon gas pressure of 0.3~0.5Pa.