A surface-modified steel fiber with silane-silica composite, its preparation method and application
By using a composite modification technology combining silane coupling agent and nano-silica to form a dense composite interface layer on the surface of steel fiber, the problem of nanoparticle agglomeration was solved, and the interfacial bonding force and mechanical properties between the fiber and the cement matrix were significantly improved.
Patent Information
- Application Number
- CN202510599127.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing nano-silica modified steel fibers have insufficient bonding strength at the cement matrix interface, and the nanoparticles are prone to agglomeration, resulting in limited interface reinforcement effect.
By employing a composite modification technology combining silane coupling agent and nano-silica, a uniform spherical nano-silica layer is grown in situ on the surface of steel fiber through molecular-level modification and sol-gel method. Combined with chemical bonding and mechanical anchoring, a dense composite interface layer is formed.
It significantly improves the interfacial bonding between steel fibers and cement-based materials, increasing flexural strength by more than 26% and compressive strength by more than 20%.
Smart Images

Figure CN123106048A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building materials technology, specifically relating to a silane-silica composite modification technology for steel fiber surfaces and its application in cement-based composite materials, which is particularly suitable for high-performance concrete structure reinforcement, seismic strengthening engineering and marine environmental infrastructure construction. Background Technology
[0002] Steel fiber reinforced cementitious composites are widely used in building engineering, long-span bridges, and special structures due to their excellent tensile strength, toughness, and impact resistance. However, the interfacial bonding strength between the steel fibers and the cement matrix directly affects the mechanical properties of the composite material, becoming a key factor restricting its development.
[0003] Currently, methods to improve bonding strength mainly fall into two categories: one is to achieve mechanical anchoring by changing the shape of the steel fibers, such as corrugated fibers, hooked fibers, semi-hooked fibers, new types of steel stranded fibers, and new types of curved fibers; the other is to enhance interfacial bonding by modifying the surface of the steel fibers, with modification methods including physical modification and chemical modification. Physical modification mainly involves increasing the surface roughness of the steel fibers through methods such as grinding; chemical modification includes phosphating, CTAB modification, pickling, coupling agent modification, and nano-silica modification.
[0004] Among the methods described above, nano-silica modification has attracted much attention due to its unique interface enhancement mechanism. On the one hand, nano-silica particles can increase the surface roughness of steel fibers, providing more mechanical anchoring points; on the other hand, its active surface energy can undergo secondary reactions with cement hydration products (such as Ca(OH)2) to generate dense CSH gel, filling the micropores in the interfacial transition zone, thereby significantly improving the chemical bonding force between the fiber and the matrix. However, traditional nano-silica modification still has obvious defects: first, particle agglomeration, as nano-silica has a large specific surface area and high surface energy, making it prone to agglomeration, resulting in uneven distribution on the steel fiber surface; second, uneven growth, as directly deposited silica is difficult to form a continuous and dense covering layer, affecting the interface enhancement effect.
[0005] To address the aforementioned issues, researchers have explored composite modification strategies using silane coupling agents in conjunction with nano-silica. For example, Tian et al. ("Parameter Optimization and Mechanical Properties of Silane-Nano SiO2 Composite Surface Modified Steel Fiber Ultra-High Performance Concrete") proposed directly incorporating nano-silica particles into a silane coupling agent KH-550 solution to improve interfacial bonding through the bridging effect of the coupling agent. While this method improves the fiber-cement matrix interfacial properties to some extent, the physically mixed nano-silica particles are prone to agglomeration, making it difficult to distribute uniformly on the steel fiber surface. Furthermore, the improvement in concrete compressive strength is slight, indicating that interfacial optimization remains insufficient.
[0006] The patent "A method for preparing surface hyperbranched modified steel fibers and ultra-high performance concrete based on the modified steel fibers" (patent number: ZL202210414663.2) invented by Sun Hao et al. proposes a steel fiber surface modification technology. Its core process involves first immersing hydroxylated steel fibers in a silane coupling agent hydrolysate, followed by drying to form a silane coupling agent coating; then placing the coupling agent-coated steel fibers in a mixed solution composed of tetraethyl orthosilicate, anhydrous ethanol, and deionized water for stirring and reaction, and finally obtaining surface hyperbranched modified steel fibers through a drying process. However, this process has obvious technical limitations: First, the nano-silica generated during the reaction has a three-dimensional dendritic structure, which is prone to agglomeration, resulting in uneven distribution on the surface of the steel fiber; second, this unevenly distributed silica is difficult to form a uniform and effective interface reaction with the surrounding cement-based materials, ultimately forming a weak area at the steel fiber-cement matrix interface. It is precisely because of the existence of these interface defects that the modification method has a limited effect on improving the flexural strength of concrete composite materials, and its practical engineering application value is significantly restricted.
[0007] Therefore, how to achieve uniform growth and stable dispersion of nano-silica on the surface of steel fibers, and further strengthen the fiber-matrix interface bonding, remains a technical bottleneck that needs to be overcome in current research. Summary of the Invention
[0008] To address the key issues of uneven dispersion of nano-silica and insufficient interfacial bonding in existing steel fiber surface modification technologies, this invention proposes an innovative technical solution based on silane coupling agent-nano-silica composite modification. This technology achieves precise functional modification of the steel fiber surface through molecular-level interfacial design and nanoscale structural control, and grows a uniformly sized spherical nano-silica layer in situ on the steel fiber surface. First, the steel fiber surface is molecularly modified using a silane coupling agent. The silanol groups generated by its hydrolysis form stable chemical bonds with the hydroxyl groups on the steel fiber surface, while the terminal amino groups provide active sites for subsequent nanostructure growth. Then, nano-silica is grown in situ on the activated surface using a sol-gel method. A gradient deposition process is employed to precisely control the particle size and distribution density, constructing a uniform and dense composite interfacial layer with spherical nanostructures. This multi-scale modification strategy not only solves the problem of nanoparticle agglomeration but also significantly improves the interfacial bonding between steel fibers and cement-based materials through the synergistic effect of chemical bonding and mechanical anchoring. Experimental results show that, compared with the unmodified system, the modified steel fiber cementitious material prepared based on this technology has increased flexural strength by more than 26% and compressive strength by more than 20%, providing a breakthrough solution for the development of high-performance fiber-reinforced cementitious materials.
[0009] To achieve the above objectives, the technical solution of the present invention is as follows:
[0010] This invention provides a surface-modified steel fiber with silane-silica composite and its preparation method, specifically including:
[0011] (1) Steel fiber pretreatment: The steel fibers were immersed in a NaOH solution to remove surface grease and impurities and to introduce hydroxyl functional groups onto the surface of the steel fibers. Subsequently, they were cleaned with anhydrous ethanol and deionized water in sequence and dried to prepare for subsequent silane coupling agent modification.
[0012] (2) Preparation of silane coupling agent hydrolysate: Stir the silane coupling agent, anhydrous ethanol and deionized water evenly in a water bath and heat to ensure that the silane coupling agent is fully hydrolyzed.
[0013] (3) Silane coupling agent modified steel fiber: The pretreated steel fiber in step (2) is immersed in the silane coupling agent hydrolysate prepared in step (3) to ensure that the coupling agent adheres to the surface of the steel fiber. After the reaction is completed, the steel fiber is dried in an oven to obtain silane coupling agent modified steel fiber.
[0014] (4) Surface-modified steel fibers with silane-silica composite: Tetraethyl orthosilicate, CTAB, anhydrous ethanol and deionized water were mixed and dispersed in an ultrasonic cleaner to ensure thorough mixing of the solution and reagents. During this process, ammonia was added to adjust the pH of the solution to alkaline to ensure uniform precipitation of silica particles. The silane coupling agent-modified steel fibers obtained in step (3) were placed in the above mixed solution and heated. After the reaction was completed, the steel fibers were removed, aged at room temperature, then cleaned with deionized water and dried in an oven to obtain silane-silica composite modified steel fibers.
[0015] (5) The NaOH solution in step (1) has a mass concentration of 10%-30% and a soaking time of 10-30 min.
[0016] (6) The steel fiber mentioned in step (1) has a length of 8-12 mm and a diameter of 0.12-1 mm.
[0017] (7) In step (2), the mixture is heated for 6-8 hours in a water bath at <50℃, and the pH of the mixture is adjusted to 10-11 using ammonia. The mixture is stirred and mixed evenly to obtain the silane coupling agent hydrolysate.
[0018] (8) The pH value of the alkaline solution in step (4) is about 8-10. Use concentrated ammonia to adjust the pH value.
[0019] (9) Based on the pretreated steel fibers described in step (1), the hydrolysate in step (2) is a mixture of silane coupling agent, deionized water, and anhydrous ethanol. The mass of the silane coupling agent accounts for 8%-12% of the total mass of the solution, the alcohol-to-water ratio is 1:7-9, and the steel fibers account for 10%-20% of the mass of the silane coupling agent. In step (4), the volume ratio of deionized water to anhydrous ethanol is 1:1-3, and then 8%-10% of the solvent mass of tetraethyl orthosilicate, 0.8%-1% of CTAB, and ammonia water are added sequentially according to the pH value.
[0020] (10) The present invention also provides a fiber cement-based material based on the above-mentioned composite modification, the raw material components of which include ordinary silicate cement (P.O42.5), fly ash, quartz sand, water, water-reducing agent and composite modified steel fiber.
[0021] (11) Cement 990-1150g, fly ash 175-200g, quartz sand 625-810g, water 300-400g, water-reducing agent 3-4g, steel fiber 30-180g.
[0022] (12) The silane-silica composite modified steel fiber accounts for 0.5%-3% of the volume content of the cement-based material.
[0023] (13) The mass ratio of the mixing water to the cementitious materials (ordinary silicate cement, fly ash, and quartz sand) is 0.25-0.35.
[0024] The present invention also provides a method for preparing the steel fiber cement-based material, comprising the following steps:
[0025] Mix ordinary silicate cement, fly ash, and quartz sand evenly, add a small amount of water to the mixing pot, and stir at low speed for 60-90 seconds. Then add the remaining water-reducing agent and water, and stir at high speed for 200-240 seconds. Finally, add the modified steel fiber and stir at low speed for 200-240 seconds.
[0026] (14) Place the mixed steel fiber cement-based material in a mold and cure it according to the standard specifications.
[0027] (15) The beneficial effects of the present invention are as follows:
[0028] The method for preparing silane-silica composite modified steel fibers involves first attaching a silane coupling agent coating to the surface of the steel fibers. This increases the surface roughness of the steel fibers, thereby increasing their surface area and promoting the adsorption of silica on the fiber surface. This results in silica particles being uniformly and densely adsorbed onto the uneven surface of the coupling agent, forming the silane-silica composite modified coating. The addition of ammonia catalyzes tetraethyl orthosilicate (TEO), which more readily decomposes silica particles in an alkaline environment. CTAB can further modify the surface of silica particles precipitated in the solution, ensuring uniform particle size. Compared to single silica modification, this composite modified coating not only improves the surface roughness of the steel fibers but also enables more uniform and dense adsorption of silica particles on the fiber surface. This further improves the interfacial transition zone between the steel fiber and cementitious materials, increasing the hydration degree of the cementitious material near the fibers. It also enhances interfacial friction, physical adsorption, and chemical bonding strength. This method exhibits excellent performance, overcomes the shortcomings of single modification, and has broad application and development prospects.
[0029] (16) When the silane-silica composite modified steel fiber obtained by the method of the present invention is incorporated into cement-based materials, its compressive strength, flexural strength and other mechanical properties are improved. Attached Figure Description
[0030] Figure 1 This is a SME diagram of a surface-modified steel fiber with silane-silica composite structure according to the present invention.
[0031] Figure 2 This is a SEM image of the unmodified fiber. Detailed Implementation
[0032] The invention will be further illustrated below with reference to examples. The following description is merely exemplary and does not limit its scope.
[0033] Example 1
[0034] (1) Pretreatment of steel fibers: steel fibers with a length of 10 mm and a diameter of 0.2 mm were immersed in a 10% NaOH solution for 10 min and then washed with deionized water to obtain pretreated steel fibers, so that active hydroxyl groups were obtained on the surface of the steel fibers.
[0035] (2) Preparation of silane coupling agent hydrolysate: The silane coupling agent, anhydrous ethanol and deionized water were stirred and mixed evenly, and stirred in a water bath at 30°C for 4 hours to prepare the silane coupling agent hydrolysate. The pH value of the hydrolysate was 9. The silane coupling agent KH-550 accounted for 8% of the mass of the mixture, the steel fiber accounted for 15% of the mass of the KH-550 hydrolysate, and the weight ratio of anhydrous ethanol to deionized water was 1:7.
[0036] (3) Coupling agent modified steel fiber: The pretreated steel fiber obtained in step (1) is placed in the silane coupling agent hydrolysate prepared in step (2) and reacted for 10 min. After the reaction is completed, it is placed in an oven at 110℃ and dried for 1 h to obtain silane coupling agent modified steel fiber.
[0037] (4) Preparation of silane-silica composite modified steel fibers: First, 125 ml of anhydrous ethanol and 375 ml of deionized water were used as solvents. Then, 36 g of tetraethyl orthosilicate and 3.6 g of CTAB were added to the mixture, and the mixture was ultrasonically cleaned for 30 min to ensure that the solution and reagents were fully mixed. During this process, ammonia water was added to adjust the pH value to 8 to ensure that the silica particles were uniformly precipitated. The silane coupling agent modified steel fibers obtained in step (3) were added to the mixed solution and reacted in a water bath at 45℃ for 6 h. After the reaction was completed, the steel fibers were taken out and aged at room temperature for 24 h. The steel fibers were thoroughly cleaned with deionized water to remove surface residues. Finally, the steel fibers were dried in an oven at 110℃ for 1 h to obtain the silane-silica composite modified steel fibers.
[0038] (5) Add 996g of silicate cement, 175g of fly ash, 804g of quartz sand, 325g of water and 3g of water-reducing agent into a mixer and stir at low speed for 90s. Then add the remaining water-reducing agent and water and stir at high speed for 240s. Finally, add 30.15g of the prepared silane-silica composite modified steel fiber and stir at low speed for 240s to ensure thorough mixing and obtain fresh steel fiber cementitious material. The mass ratio of mixing water to cementitious material is 0.28. The material stirring speed is 65r / min at low speed and 125r / min at high speed.
[0039] (6) Place the freshly mixed cementitious material prepared in step (1) into a mold and cure it to the specified age to obtain the silane-silica composite modified steel fiber cementitious material.
[0040] Example 2
[0041] (1) Pretreatment of steel fibers: steel fibers with a length of 12 mm and a diameter of 0.22 mm were immersed in a 15% NaOH solution for 20 min and then washed with deionized water to obtain pretreated steel fibers, so that active hydroxyl groups were obtained on the surface of the steel fibers.
[0042] (2) Preparation of silane coupling agent hydrolysate: The silane coupling agent, anhydrous ethanol and deionized water were stirred and mixed evenly, and stirred in a water bath at 35°C for 5 hours to prepare the silane coupling agent hydrolysate. The pH value of the hydrolysate was 10. The silane coupling agent KH-550 accounted for 10% of the mass of the mixture, and the steel fiber accounted for 45% of the mass of the KH-550 hydrolysate. The weight ratio of anhydrous ethanol and deionized water was 1:8.
[0043] (3) Coupling agent modified steel fiber: The pretreated steel fiber obtained in step (1) is placed in the silane coupling agent hydrolysate prepared in step (2) and reacted for 15 min. After the reaction is completed, it is placed in an oven at 110℃ and dried for 3 h to obtain silane coupling agent modified steel fiber.
[0044] (4) Preparation of silane-silica composite modified steel fibers: First, 166 ml of anhydrous ethanol and 332 ml of deionized water were used as solvents. Then, 40.5 g of tetraethyl orthosilicate and 4.05 g of CTAB were added to the mixture and ultrasonicated for 45 min in an ultrasonic cleaner to ensure that the solution and reagents were fully mixed. During this process, ammonia water was added to adjust the pH value to 8 to ensure that the silica particles were uniformly precipitated. The silane coupling agent modified steel fibers obtained in step (3) were added to the mixed solution and reacted in a 50°C water bath for 8 h. After the reaction was completed, the steel fibers were taken out and aged at room temperature for 3 days. The steel fibers were thoroughly washed with deionized water to remove residues. Finally, the steel fibers were dried in an oven at 105°C for 3 h to obtain silane-silica composite modified steel fibers.
[0045] (5) Add 1139g of ordinary silicate cement, 200g of fly ash, 636g of quartz sand, 350g of water and 4g of water-reducing agent into a mixer and mix at low speed for 70s. Then add the remaining water-reducing agent and water and mix at high speed for 220s. Finally, add 90g of the prepared silane-silica composite modified steel fiber and mix at low speed for 220s to ensure thorough mixing and obtain fresh steel fiber cementitious material. The mixing speed of the material is 65r / min at low speed and 125r / min at high speed. The mass ratio of mixing water to cementitious material is 0.26.
[0046] (6) Place the freshly mixed cementitious material in a mold and cure it to the specified age to obtain the silane-silica composite modified steel fiber cementitious material;
[0047] Example 3
[0048] (1) Pretreatment of steel fibers: steel fibers with a length of 8 mm and a diameter of 0.12 mm were immersed in a 20% NaOH solution for 30 min and then washed with deionized water to obtain pretreated steel fibers, so that active hydroxyl groups were obtained on the surface of the steel fibers.
[0049] (2) Preparation of silane coupling agent hydrolysate: The silane coupling agent, anhydrous ethanol and deionized water were stirred and mixed evenly, and stirred in a water bath at 40°C for 6 hours to prepare the silane coupling agent hydrolysate. The pH value of the hydrolysate was 11, the content of silane coupling agent KH-550 was 12%, the steel fiber accounted for 30% of the mass of KH-550 hydrolysate, and the weight ratio of anhydrous ethanol to deionized water was 1:9.
[0050] (3) Coupling agent modified steel fiber: The pretreated steel fiber obtained in step (1) is placed in the silane coupling agent hydrolysate prepared in step (2) and reacted for 20 min. After the reaction is completed, it is placed in an oven at 110℃ and dried for 2 h to obtain silane coupling agent modified steel fiber.
[0051] (4) Preparation of silane-silica composite modified steel fiber: First, 250 ml of anhydrous ethanol and 250 ml of deionized water were used as solvents. Then, 43.2 g of tetraethyl orthosilicate and 4.3 g of CTAB were added to the mixture. The mixture was ultrasonically treated in an ultrasonic cleaner for 50 min to ensure that the solution and reagents were fully mixed. During this process, ammonia water was added to adjust the pH value to 9 to ensure uniform precipitation of silica. The silane coupling agent modified steel fiber obtained in step (3) was added to the mixed solution and reacted at 60 °C for 10 h. After the reaction was completed, the steel fiber was taken out and aged at room temperature for 2 days. The steel fiber was thoroughly cleaned with deionized water to remove surface residues. Finally, the steel fiber was dried in an oven at 110 °C for 2 h to obtain silane coupling agent-silica composite modified steel fiber, the surface morphology of which is as follows. Figure 1 As shown:
[0053] (5) Add 1062g of ordinary silicate cement, 188g of fly ash, 625g of quartz sand, 375g of water and 3.3g of water-reducing agent into a mixer and mix at low speed for 60s. Then add the remaining water-reducing agent and water and mix at high speed for 200s. Finally, add 60g of the prepared silane-silica composite modified steel fiber and mix at low speed for 200s to ensure thorough mixing and obtain fresh steel fiber cementitious material. The mixing speed of the material is 65r / min at low speed and 125r / min at high speed. The mass ratio of mixing water to cementitious material is 0.3.
[0054] (6) Place the freshly mixed cementitious material in a mold and cure it to the specified age to obtain the silane-silica composite modified steel fiber cementitious material.
[0055] Comparison Examples
[0056] The surface morphology of the unmodified steel fiber is as follows: Figure 2 As shown:
[0058] (1) Add 1062g of ordinary Portland cement, 188g of fly ash, 625g of quartz sand, 375g of water and 3.3g of water-reducing agent into a mixer and mix at low speed for 60s. Then add the remaining mass fraction of water-reducing agent and water and mix at high speed for 240s. Finally, add 60g of steel fiber and mix at low speed for 240s to ensure thorough mixing and obtain fresh steel fiber cement-based material. The material mixing speed is 65r / min at low speed and 125r / min at high speed.
[0059] (2) Place the freshly mixed cementitious material in a mold and cure it to the specified age to obtain steel fiber cementitious material;
[0060] Table 1. Strength values of steel fiber cement-based materials prepared in each embodiment and comparative example.
[0061]
[0062]
[0063] As shown in Table 1, the silane-silica composite modified steel fiber cementitious material has better performance, with a 20% increase in 3d compressive strength and an approximately 26% increase in 3d flexural strength compared to the comparative example.
Claims
1. A surface-modified steel fiber with silane-silica composite, its preparation method and application, characterized in that, Includes the following steps: (1) Hydroxylation of steel fiber surface: Soak the steel fiber in a 10%-20% NaOH solution for 20-30 minutes, and then wash it with deionized water to remove the grease and impurities on the surface of the steel fiber, so as to hydroxylate the surface of the steel fiber. (2) Preparation of silane coupling agent hydrolysate: Mix silane coupling agent, anhydrous ethanol and deionized water, stir evenly in a water bath, and heat at 30℃-40℃ for 4-6h to obtain silane coupling agent hydrolysate; (3) Silane coupling agent modified steel fiber: The steel fiber with surface hydroxylation in step (1) is immersed in the silane coupling agent hydrolysate prepared in step (2) for 10-20 minutes. After immersion, it is taken out and dried in an oven at 100℃-110℃ for 1-3 hours to obtain silane coupling agent modified steel fiber. (4) Surface-modified steel fibers with silane-silica composite: First, a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1-3 was used as the solvent. Then, 8%-10% tetraethyl orthosilicate and 0.8%-1% hexadecyltrimethylammonium bromide (CTAB) by mass of the solvent were added to the mixture. The mixture was placed in an ultrasonic cleaner and dispersed for 30-60 minutes to ensure that the solution and reagents were fully mixed. During this process, ammonia was added to adjust the pH value to 8-10 to ensure that the silica particles were uniformly precipitated. The silane coupling agent modified steel fibers obtained in step (3) were placed in the above mixed solution and heated in a water bath at 45℃-60℃ for 6-12 hours. After the reaction was completed, the steel fibers were taken out, aged at room temperature for 1-3 days, cleaned with deionized water, and dried in an oven at 100℃-110℃ for 1-3 hours to obtain silane-silica composite modified steel fibers.
2. The surface-modified steel fiber with silane-silica composite as described in claim 1, its preparation method and application, characterized in that: Based on the pretreated steel fibers in step (1), the silane coupling agent content in step (2) is 8%-12% of the hydrolysate mass, the alcohol-to-water ratio is 1:7-9, and the steel fiber mass accounts for 10%-20% of the silane coupling agent hydrolysate mass. In step (4), the volume ratio of deionized water to anhydrous ethanol is 1:1-3, tetraethyl orthosilicate and CTAB account for 8%-10% and 0.8%-1% of the solvent mass, respectively, and ammonia water is added according to the pH value.
3. The surface-modified steel fiber with silane-silica composite as described in claim 1 and its preparation method, characterized in that: The steel fibers mentioned in step (1) are 8-12 mm in length and 0.12-1 mm in diameter; The pH value of the silane coupling agent hydrolysate in step (2) is 9-11; The solution in step (4) has a pH of 8-10. The addition of ammonia water has a catalytic effect on tetraethyl orthosilicate. Tetraethyl orthosilicate is more likely to decompose into silica particles in an alkaline environment. The CTAB described in step (4) can modify the surface of silica decomposed from tetraethyl orthosilicate, so that the silica in the solution and on the fiber surface are of uniform size.
4. The surface-modified steel fiber with silane-silica composite as described in claim 1 and its preparation method, characterized in that: The NaOH solution in step (1) has a mass concentration of 10%-20% and a soaking time of 20-30 minutes.
5. The surface-modified steel fiber with silane-silica composite as described in claim 1 and its preparation method, characterized in that: In step (2), the pH value of the silane coupling agent hydrolysate is around 9-11.
6. The surface-modified steel fiber with silane-silica composite as described in claim 1 and its preparation method, characterized in that: The pH of the mixed solution prepared in step (4) is adjusted to 8-10 with ammonia water to hydrolyze the silica particles in an alkaline environment. The steel fibers modified with silane coupling agent are placed in the mixed solution prepared in step (4), first ultrasonically dispersed in an ultrasonic cleaner for 30-60 minutes, then heated in a water bath for 6-12 hours, and left to stand at room temperature for 1-3 days. The steel fibers are then taken out, washed with deionized water, and then placed in an oven to dry at 100℃-110℃ for 1-3 hours.
7. A surface-modified steel fiber based on any one of claims 1 to 6, its preparation method, and its application, characterized in that: A composite modified steel fiber cementitious material is obtained by incorporating the composite modified steel fiber into cement-based materials. Its raw material components include ordinary Portland cement, fly ash, quartz sand, polycarboxylate superplasticizer, surface-modified silane-silica composite steel fiber, and water. The mass of each component is as follows: cement 990-1150g, fly ash 175-200g, quartz sand 625-810g, water 300-400g, superplasticizer 3-4g, and steel fiber 30-180g. The steel fiber content accounts for 0.5%-3% of the volume of cement-based materials, and the mass ratio of mixing water to cementitious materials is 0.25-0.
35.
8. The surface silane-silica composite modified steel fiber according to claim 7, a preparation method and application thereof, characterized in that, Includes the following steps: (1) Mix ordinary silicate cement, fly ash, and quartz sand evenly. Add 50% by weight of water and water-reducing agent to the mixing pot and mix at a low speed of 65-70 r / min for 60-90 s. Then add the remaining water-reducing agent and water and mix at a high speed of 120-125 r / min for 200-240 s. Finally, add the modified steel fibers and mix at a low speed of 65-70 r / min for 200-240 s to obtain fresh steel fiber cementitious material. (2) Place the fresh steel fiber cementitious material prepared in step (1) into a mold and cure it to the specified age to obtain the composite modified steel fiber cementitious material.
9. The method for preparing the composite modified steel fiber cementitious material according to claim 8, characterized in that: In step (1), the stirring speed of each material is 65-70 r / min at low speed and 120-125 r / min at high speed.
Citation Information
Patent Citations
A method for preparing surface hyperbranched modified steel fibers and ultra-high performance concrete based on the modified steel fibers.
CN114656181B