A corrosion-resistant outdoor cement pole material and its preparation method

By employing a split-type stress-bearing design and a multi-layer protection system in the cement pole, the problem of repairing cement poles after corrosion and localized damage in outdoor environments has been solved, achieving high strength, long service life, corrosion resistance, and self-repair capability.

CN123106068APending Publication Date: 2026-11-17TIBET HENGZE ELECTRIC POWER TECHNOLOGY DEVELOPMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611471129.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing cement pole materials are prone to corrosion in outdoor environments. After local damage, the bonding strength of the repair interface is weak, making it difficult to carry out segmented repairs. Furthermore, the protection system is singular and cannot effectively resist long-term deterioration problems such as frost heave, alkali-aggregate reaction, and steel rust heave.

Method used

The structure employs a split-load design with three continuous main ribs and a layered triangular spatial truss structure. Combined with biomimetic lotus root fiber bundles, stress-triggered self-healing microbeads, and a multi-layered protection system, it achieves modular repair and self-repair through a segmented gradient arrangement of the skeleton and inner and outer coatings to form multiple layers of protection.

Benefits of technology

It improves the structural strength and service life of cement poles, enables precise repair after local damage, resists outdoor environmental corrosion, extends the service life of cement poles, and enhances protective durability and self-healing ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106068A_ABST
    Figure CN123106068A_ABST
Patent Text Reader

Abstract

This invention relates to the field of cement pole technology, specifically to a corrosion-resistant outdoor cement pole material and its preparation method, comprising base materials, skeleton materials, additive materials, and auxiliary materials. The base materials include cement pole base materials and reinforcing steel materials. The base materials are used to prepare a highly fluid concrete matrix suitable for centrifugal molding and constitute the main load-bearing and spatial truss bearing system of the pole. The cement pole of this invention employs a split-type load-bearing design with main reinforcing bars supporting the load and a positioning skeleton guiding the load. Three continuous main reinforcing bars, in conjunction with a layered triangular spatial truss, bear the main bending and shear loads. The metal and waste plastic modified positioning skeleton is arranged in a segmented gradient according to the bending moment envelope, serving only as a positioning, force transmission, and interlocking limiter. This design ensures the overall mechanical strength of the pole while constructing a segmented modular repair benchmark, solving the problems of traditional continuous reinforcing steel cages being unable to replace sections locally and insufficient interface bonding strength after repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cement pole technology, specifically to a corrosion-resistant outdoor cement pole material and its preparation method. Background Technology

[0002] Cement poles for power transmission are the core supporting components of overhead power transmission lines. They are widely used in urban and rural power transmission and distribution networks. They mainly bear conductor loads, wind loads, and icing loads, and withstand the corrosive effects of the outdoor environment, ensuring the safe and stable operation of the transmission lines. Their structure is mainly composed of a concrete matrix, an internal steel reinforcement skeleton, and a protective layer. The material properties and manufacturing process directly determine the mechanical strength, weather resistance, durability, and service life of the pole.

[0003] Currently, some cement pole materials and preparation technologies have emerged in the field of cement poles for power transmission. For example, application number CN202511790288.1, published on February 24, 2026, describes a method for preparing eco-friendly cement power poles using industrial solid waste. This method involves co-grinding steel slag and granulated blast furnace slag to obtain activated mixed micro-powder, which is then compounded with fly ash, carbide slag, and desulfurized gypsum in a specific ratio to form an eco-friendly synergistic cementitious material. This material is then mixed with aggregates, polycarboxylate superplasticizer, and modified polypropylene fibers to form eco-friendly concrete. After installation of a reinforcing steel frame and centrifugal molding, the concrete is cured using a composite curing system that includes stepped heating, constant temperature activation, and low-temperature compensation stages. Finally, the product is demolded. By combining the synergistic activation of multiple solid wastes with a specialized curing process, high-volume resource utilization of industrial solid waste is achieved. The prepared power poles exhibit high early strength and good volume stability, and are fully compatible with existing centrifugal molding and steam curing production lines. However, the above cases only use traditional full-length steel reinforcement cages, without involving segmented positioning cages, gradient material layouts and modular repair designs, which cannot achieve segmented repair after local damage; at the same time, without introducing stress-triggered self-healing and multi-scale toughening systems, the ability to actively repair concrete micro-cracks and expansion cracks is insufficient, making it difficult to cope with long-term deterioration problems such as outdoor frost heave, alkali-aggregate reaction and steel reinforcement rust expansion.

[0004] For example, a waterproof and anti-corrosion cement pole with application number CN201010256862.2 and authorization announcement date of 20130102 is mainly used in poles and towers. It includes a pole body made of concrete, characterized in that at least a portion of the outer surface of the pole body has a resin protective layer. This waterproof and anti-corrosion cement pole is mainly used in poles, communication poles, and public utility poles. The outer surface of the pole body has at least one or more resin protective layers, resulting in high mechanical strength, simple manufacturing method, low cost, and waterproof and anti-corrosion properties. It can be widely used, especially in saline-alkali areas. However, the above case relies solely on the outer surface resin coating for protection, resulting in a single protective system. The difference in thermal expansion coefficients between the resin layer and the concrete matrix is ​​large, making it prone to delamination and cracking under repeated temperature changes, wind vibration, and bending conditions outdoors, leading to insufficient protective durability. Furthermore, it does not address the internal toughening and self-healing design of the concrete matrix, nor does it optimize the internal skeleton structure. Its shear resistance and crack control capabilities are limited, making it difficult to meet the long-term service requirements of areas with high corrosion and strong wind loads.

[0005] However, the existing technologies and current cement poles have a single skeleton form, mostly continuous long steel cages. After local damage to the cement pole, although traditional cement poles can be repaired with cement, the interface bonding of the repaired cement pole is weak, which will affect the strength of the cement pole and make it difficult to guarantee the structural strength of the cement pole. Therefore, it is urgent to design a corrosion-resistant outdoor cement pole special material and its preparation method to solve the above problems. Summary of the Invention

[0006] The purpose of this invention is to provide a corrosion-resistant outdoor cement pole material and its preparation method to overcome the above-mentioned shortcomings in the prior art.

[0007] To achieve the above objectives, the present invention provides the following technical solution: A corrosion-resistant material for outdoor cement poles includes base materials, frame materials, additive materials, and auxiliary materials, as detailed below: The special material for cement poles is used in centrifugally molded power cement poles; The basic materials include cement pole foundation materials and steel reinforcement materials, wherein: The base material is used to prepare a highly fluid concrete matrix adapted to centrifugal molding process and to form the main load-bearing system of the pole and the space truss bearing system. The steel reinforcement material includes three main bars arranged in an equilateral triangle along the entire length of the bar, and short metal connecting rods arranged in layers at each frame position; The cement pole base material is a high-flowability modified concrete suitable for centrifugal molding, composed of cementitious materials, continuously graded coarse aggregate, fine aggregate, mineral admixtures, water, and polycarboxylate superplasticizer. The coarse aggregate has a maximum particle size ≤20mm, a water-cement ratio of 0.28-0.35, and a paste spread ≥180mm. The cementitious materials include ordinary Portland cement and / or sulfoaluminate cement, and the mineral admixtures include one or more of Grade I fly ash, slag powder, and silica fume. It should be noted that: Cementitious materials are the core powder materials in concrete that generate bond strength through hydration reactions, binding aggregates into a whole. They are the source of concrete's mechanical properties. Cementitious materials are mainly cement-based and can be used alone or in combination. The following options can be selected based on the requirements for cement pole placement: Ordinary Portland cement (P·O 42.5 / 52.5 grade): the mainstream matrix cementing material, with high hydration strength, good volume stability, and mature technology, is the standard cementing material for power cement poles; prestressed cement poles generally use grade 52.5 to ensure early tension strength; Sulfoaluminate cement (SAC): A corrosion-resistant cementitious material with early strength and rapid hardening, resistance to sulfate attack, and excellent frost resistance. It is used for cement poles in highly corrosive environments such as saline-alkali land and coastal areas, which meets the functional requirements of corrosion resistance and salt and alkali resistance in the solution. In continuously graded coarse aggregate, coarse aggregate consists of rock particles with a diameter greater than 4.75 mm (commonly known as crushed stone), which are the rigid skeleton phase of concrete and mainly bear compressive stress. Continuous gradation refers to the continuous distribution of aggregate particle size from the smallest to the largest, rather than a single particle size range, and the particle gradation conforms to the continuous gradation curve. Fine aggregate consists of sand and gravel particles with a particle size of less than 4.75 mm (commonly known as sand), which fill the voids between coarse aggregates to optimize the workability, encapsulation, and density of concrete paste. Mineral admixtures are mineral powders or industrial by-products with active aluminosilicates as the main component. They are added to concrete to replace part of the cement and improve the workability and durability of concrete through the pozzolanic effect and micro-aggregate effect, while reducing the heat of hydration and cost. Grade I fly ash, granulated blast furnace slag powder (S95 grade), and silica fume can be selected. The four types of materials, when combined, together form a concrete matrix material system that is suitable for centrifugal molding, can pass smoothly through the holes of multi-layer skeletons, and takes into account both structural strength and outdoor durability. The main reinforcing bars are selected from prestressed steel wire, cold-drawn steel wire, or ordinary ribbed steel bars, and short metal connecting rods are installed at each layer of the skeleton to connect the three main reinforcing bars to form a multi-layer independent triangular spatial truss structure, wherein: Ordinary ribbed steel bars are welded to short metal connecting rods; Prestressed steel wire, cold-drawn steel wire and metal short connecting rod are connected by mechanical sleeve buckle; The skeleton materials are divided into two categories: metal positioning skeletons and waste plastic modified positioning skeletons, and a segmented gradient arrangement mode is adopted. Both the metal positioning frame and the waste plastic modified positioning frame are circular ring structures composed of a triangular outer ring and a circular inner ring, arranged along the rod length axis, with a frame thickness of 30-45mm. The skeleton body has three large flow holes and six small interlocking holes that are axially connected. The large flow holes of each skeleton are coaxially aligned and form a continuous straight material flow channel. The upper and lower end faces of the skeleton are also provided with annular interlocking grooves. Neither the metal positioning frame nor the waste plastic modified positioning frame replaces the three main reinforcing bars to bear the main force; they are only used for positioning the main reinforcing bars, axial force transmission through the concrete, mechanical interlocking and limiting, and segmented repair benchmarks. in: The large flow hole has a diameter of not less than 60mm and not less than 3 times the maximum particle size of the coarse aggregate. It is an axial flared guide hole set along the concrete placement direction, with the hole diameter gradually decreasing from 65mm to 60mm and the hole opening having a rounded transition throughout. The large flow holes are biased towards the compression side of the rod to ensure unobstructed path of the principal compressive stress in the concrete; the small interlocking holes are concentrated on the tension side of the rod to enhance the mechanical bonding effect between the concrete and the skeleton in the tension zone. Each large flow hole has a micro exhaust groove at the top opening, which is used to expel air from the hole during centrifugal fabric distribution, thus preventing the formation of air pockets or voids inside the hole. The skeleton facing the concrete placement surface is provided with a guide slope of R8-10mm; the small interlocking hole has a diameter of 20-22mm and is a dovetail-shaped hole that is narrow inside and wide outside, forming a reverse mechanical lock after the concrete is embedded. The annular interlocking groove has a trapezoidal groove with a narrow outer edge and a wide inner edge. The inner wall of the groove is provided with annular serrated anti-slip teeth. A water-swellable sealing strip is pre-placed at the bottom of the groove. The groove is 8mm wide and 5mm deep, and is used to achieve mechanical interlocking between concrete and skeleton, segmented positioning, and mechanical locking when repairing new and old concrete. Three radial reinforcing ribs are provided between the triangular outer ring and the circular inner ring. The radial reinforcing ribs are arranged at the midpoints of the three sides of the triangular outer ring and are staggered with the large flow hole. The outer edge of the skeleton is uniformly provided with 6 radial shear protrusions along the circumference. The protrusions are 10-15mm high and are embedded in the surrounding concrete to enhance the transverse shear capacity of the section. The skeleton is arranged in a segmented gradient pattern along the length of the rod according to the bending moment envelope, as shown below: The maximum bending moment zone from 0 to 1 / 4 of the pole height at the pole root is entirely equipped with a metal positioning frame, and the spacing between the frames is reduced to 200-250mm. The transition bending moment zone between 1 / 4 and 1 / 2 of the pole height uses alternating arrangements of metal positioning frames and modified waste plastic positioning frames; In the low-load area above 1 / 2 pole height, all positions are made of modified waste plastic with a spacing of 300-350mm. The frame has pre-reserved positioning slots for three main reinforcing bars and buckle slots for transverse connecting rods. The three main reinforcing bars and the short metal connecting rods are all mechanically fastened to the frame to form an integrated positioning-truss force-bearing unit. Each of the skeletons has a coaxial boss and a coaxial groove on the upper and lower end faces of the inner circular ring. When the upper and lower adjacent skeletons are installed, they are automatically aligned by inserting the boss and the groove, ensuring that the three large flow holes are coaxially aligned throughout the process. The outer edge of the frame is provided with three equidistant limiting legs, the length of which is equal to the design thickness of the concrete protective layer, and they abut against the inner wall of the mold during installation. The frame is pre-embedded with a colorimetric tracer strip. When the concrete of the pole cracks or the deformation of the frame exceeds the set value, the tracer strip breaks and releases the colorimetric substance, which leaks from the surface of the pole, and is used to identify internal damage during operation and maintenance inspection. The side end face of the frame is provided with an annular repair stop. When partially removing the damaged section of concrete, the end face of the frame is used as the repair reference surface. The new and old concrete form a mechanical interlock through the annular interlocking groove and small interlocking holes. The additive material is used to improve the waterproofness, toughness, corrosion resistance, and salt and alkali resistance of cement poles. It is divided into waterproof and seepage-proof components, toughening and crack-resistant components, stress-triggered self-healing components, and corrosion-resistant and salt and alkali-resistant components. The toughening and crack-resistant component includes biomimetic lotus root-like bundles of PVA fibers, and may also incorporate one or more of steel fibers, PE fibers, basalt fibers, rubber powder, carbon nanotubes, and graphene, wherein: The carbon nanotube content is 0.5-0.8% of the cement mass; The biomimetic lotus root-like bundle-shaped PVA fiber has a single filament diameter of 18-22μm, an effective bundle length of 12mm, and a volumetric admixture of 0.18%-0.22% of the total concrete volume. The stress-triggered self-healing component includes stress-triggered brittle glass microspheres and / or microcapsule-Bacillus composite self-healing materials; The stress-triggered brittle glass microspheres have a particle size of 1.2-1.8 mm, a dosage of 1.2%-1.5% of the total mass of concrete, a fracture threshold of 1.8-2.2 MPa, and are internally encapsulated with a cement-based penetrating crystallization repair slurry containing ultrafine silicate cement powder, active silica sol and micro-expansion crystals. The microcapsule-Bacillus composite self-healing material includes phenolic-epoxy resin microcapsules and Bacillus immobilized on expanded perlite, and is internally encapsulated with Bacillus spores and calcium source nutrient substrate. The self-healing component is used to repair micro-cracks in concrete and delay structural deterioration, but does not replace the main reinforcement to bear the main load-bearing function. The waterproof and seepage-resistant component adopts an inner and outer double-layer structure, wherein: The inner wall of the rod is made of a cement-based penetrating crystalline material to form a rigid inner waterproof layer; The outer surface of the pole is coated with a weather-resistant and anti-corrosion coating to form an external waterproof layer. The weather-resistant and anti-corrosion coating includes one or more of acrylic elastic coating, polyurea, montmorillonite-modified polyurea, and rubber-modified asphalt coating. The outer layer of the rod is provided with an outer protective cement matrix made of recycled aggregate from waste building materials and cement base material, which, together with the inner wall penetrating crystalline waterproof layer and the outer surface weather-resistant and anti-corrosion layer, forms a protective system that combines internal waterproofing, external weather resistance and matrix impermeability. The corrosion-resistant and salt-alkali-resistant components include one or more of the following: rust inhibitor, montmorillonite, fly ash, silica fume, mineral powder, sulfoaluminate cement, and MICP mineralized Bacillus. The additive material also includes process regulating components, which include one or more of polycarboxylate superplasticizers, expanding agents, setting regulators, and defoamers. The auxiliary materials are waste building materials, waste plastics, waste glass, and plant ash pH adjusting materials, which can be classified and graded for resource utilization and applied to different structural parts of the pole; The auxiliary materials are utilized in a differentiated and resource-based manner as follows: The waste building materials, after being crushed and screened, replace natural fine aggregates at a ratio of 10%-30% and are used to prepare the outer protective cement matrix of the pole or repair mortar. The waste plastic is modified and blended to form the upper and middle sections of the waste plastic modified positioning skeleton, or it is ground into micro powder and added to the concrete matrix at a dosage of 5%-10%. The waste glass, after being modified and processed, can be used as the shell material for self-healing microspheres, or ground to below 200 mesh and used to replace part of the mineral admixtures at a ratio of 3%-8%. The amount of plant ash added is 2%-5% of the mass of the cementitious material, and it is used to adjust the alkalinity of concrete, inhibit alkali-aggregate reaction, and supplement active silica-alumina components. The modified positioning frame of waste plastic, waste glass, waste building materials, and plant ash respectively realize the resource utilization of four types of solid waste.

[0008] A method for preparing a corrosion-resistant outdoor cement pole includes the following steps: Step 1. Data Collection and Model Building Training: Collect environmental degradation parameters of the target service area, pole design mechanical indicators, centrifugal forming process parameters, skeleton parameters, concrete mix proportions and service damage data, construct a "material-structure-process-performance" database, and establish a multi-parameter mapping model for materials-structure-process, structural stress, concrete flow-centrifugal coupling and self-healing trigger prediction model, and use some methods to complete model training; in: The “materials-structure-process-performance” database is constructed based on historical production data and type test data, with an effective sample size of no less than 200 groups; The model includes a material-structure-process multi-parameter mapping model, a pole structure stress finite element model, a concrete flow-centrifugal forming coupled simulation model, and a self-healing trigger prediction model. The model is trained and iterated using machine learning, neural networks, digital twins, or response surface methodology. The model takes material ratio, skeleton arrangement, and centrifugation process parameters as inputs, and outputs mechanical properties, durability, crack repair rate, and molding defect risk. It calibrates the stress triggering threshold of self-healing microbeads (1.8-2.2 MPa), skeleton segment arrangement rules, and centrifugation timing parameters for prediction and optimization of subsequent processes. The model input variables also include skeleton modification parameters, self-healing microsphere parameters, and fiber parameters, and the output variables also include 7d / 28d compressive strength, flexural strength, impermeability, freeze-thaw resistance, salt corrosion resistance, crack repair rate, and molding defect risk. When the prediction error of flexural bearing capacity exceeds 10% or the prediction error of crack repair rate exceeds 15%, the model is retrained.

[0009] Step 2. Material Selection and Pretreatment: Based on the scheme given in the previous step, select cementitious materials, aggregates, mineral admixtures, reinforcing bars, skeleton raw materials, functional additives and solid waste auxiliary materials, and process each type of raw material separately using the processing technology given in the scheme. After pretreatment, store and process each type of raw material according to its category and application process. in: The specific preprocessing is as follows: Preparation of high-flowability concrete substrate: using ordinary Portland cement and / or sulfoaluminate cement as cementing material, combined with continuous graded coarse aggregate, fine aggregate and one or more mineral admixtures from Class I fly ash, slag powder and silica fume, and adding polycarboxylate superplasticizer, controlling the maximum particle size of coarse aggregate ≤20mm, water-cement ratio 0.28-0.35, and paste spread ≥180mm; Pre-treatment of reinforcing bars and connectors: Select three continuous main reinforcing bars and short metal connecting rods. The main reinforcing bars are selected from prestressed steel wire, cold-drawn steel wire or ordinary ribbed steel bars. Welding positions are reserved for ordinary ribbed steel bars. Mechanical connection sleeves are prefabricated at the ends of prestressed / cold-drawn steel wires. After pre-treatment, they are stored according to category. The functional additives include toughening and crack-resistant components, stress-triggered self-healing components, waterproof and corrosion-resistant components, and process adjustment components. The solid waste auxiliary materials include waste building materials, waste plastics, waste glass and wood ash; each type of material is processed according to its corresponding process and then stored according to its category and usage procedure.

[0010] Step 3. Material strengthening and mixing treatment: Select a portion of the cementitious materials, aggregates and mineral admixtures pretreated in the previous step, and then disperse and strengthen the biomimetic lotus root bundle PVA fibers, stress-triggered self-healing microspheres and carbon nanotube functional components. After strengthening, add the selected materials to the mixing equipment in the proportion and mix them to obtain a high-flowability self-healing concrete mixture. in: The specific details of functional component dispersion enhancement are as follows: The biomimetic lotus root-like bundle-shaped PVA fibers are pre-dispersed and split to control the single filament diameter to 18-22μm and the bundle length to 12mm. Carbon nanotubes and an aqueous surfactant solution were mixed at a mass ratio of 4:1 and then ultrasonically dispersed to form a uniform suspension. The stress-triggered self-healing microspheres were subjected to density sieving to control the particle size at 1.2-1.8 mm and the fracture threshold at 1.8-2.2 MPa. The specific steps of stirring and mixing are as follows: First, dry mix the cementitious materials, coarse aggregate, fine aggregate and mineral admixture for 60-120 seconds; Add water and mix with polycarboxylate superplasticizer for 120-180 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time. Finally, add the carbon nanotube suspension and self-healing microbeads, and continue stirring for 60-90 seconds until homogeneous. The concrete temperature is controlled between 5-35℃ throughout the mixing process; after mixing, the spread, slump, air content, fiber dispersion uniformity, and microsphere integrity rate are tested.

[0011] Step 4. Skeleton Preparation and Quality Inspection: Select pretreated metal raw materials and modified waste plastic raw materials, and send them into the corresponding molding molds. Then, the skeleton in the mold is formed by stamping, injection molding or casting process to obtain the triangular ring composite positioning skeleton. Subsequently, the dimensional accuracy, structural performance and surface quality of the formed skeleton are inspected to determine whether the product is qualified. If it is not qualified, the above steps and plans are adjusted until the product is qualified. Otherwise, if it is qualified, proceed to the next step to continue production. in: The skeleton forming process is as follows: metal raw materials are formed by stamping or casting, and modified waste plastic raw materials are formed by injection molding or compression molding, both of which are made into a circular ring structure composed of a triangular outer ring and a circular inner ring, and the skeleton thickness is controlled to be 25-30mm. The specific processing of the skeleton hole guiding structure is as follows: Three axially penetrating large flow holes and six small interlocking holes are machined in the skeleton body; The large flow hole is a flared guide hole with a diameter that gradually decreases from 65mm to 60mm along the fabric direction. The hole diameter is ≥60mm and not less than 3 times the maximum particle size of the coarse aggregate. The hole opening has a rounded corner transition throughout, and the skeleton facing the fabric is machined with an R8-10mm guide slope. The small engagement holes are 20-22mm in diameter and are dovetail-shaped with a narrow inner diameter and a wide outer diameter; the large flow holes are arranged on the compression side of the rod, while the small engagement holes are concentrated on the tension side of the rod. The specific processing of the skeleton interlocking water-stopping structure is as follows: Annular interlocking grooves are machined on the upper and lower end faces of the skeleton. The groove cross-section is a trapezoid with a narrow outer edge and a wide inner edge, with a groove width of 8mm and a depth of 5mm. The inner wall of the tank is machined with annular serrated anti-slip teeth, and the bottom of the tank is pre-installed with water-swellable sealing strips. The specific processing of the skeleton-reinforced shear-resistant structure is as follows: Three radial reinforcing ribs are machined between the triangular outer ring and the circular inner ring, and are arranged corresponding to the midpoint of the triangular side and intersected with the large flow hole; Six radial shear protrusions, each 10-15 mm high, are machined along the circumferential direction on the outer edge of the skeleton. The modified skeleton of waste plastic uses waste plastic as the matrix and incorporates short glass fibers and talc filler accounting for 15%-20% of the total mass of the matrix for blending and modification. After modification, the elastic modulus is increased by more than 60% and the coefficient of thermal expansion is reduced by 40% compared with pure waste plastic. The surface of the waste plastic modified skeleton is subjected to micro-rough sandblasting treatment after molding and coated with a cement-based coupling coating. The surface of the metal skeleton is sequentially treated with knurling, hot-dip galvanizing, and silane coupling agent.

[0012] The machining skeleton positioning and connection structure is as follows: The main reinforcement positioning slot and the transverse connecting rod buckle slot are reserved on the frame; A coaxial boss and a coaxial groove are machined on the upper and lower end faces of the circular inner ring, respectively. Three equidistant limiting legs are machined on the outer edge of the frame, and the length of the legs is equal to the design thickness of the protective layer. The functional structure of the processing skeleton is as follows: A miniature venting groove is machined at the top opening of each large flow hole; Pre-embed colorimetric tracer strips inside the skeleton; A ring-shaped repair stop is machined on the side end face of the skeleton; The quality inspection includes dimensional accuracy, coaxiality, hole penetration, groove integrity, bending and torsion resistance, surface quality, and embedded part position detection. If the quality is not up to standard, the material ratio, mold, or process parameters are adjusted until the quality is up to standard.

[0013] Step 5. Secondary mixing and integral casting: Select the steel bars and matching connectors not selected in the above steps, and then perform end pretreatment on the steel bars and connectors. After the pretreatment, assemble the integral truss frame according to the bending moment envelope gradient and the positioning skeleton. After the assembly is completed, hoist it into the centrifugal forming mold. Then, pour the concrete mixture prepared in step 4 into the mold containing the skeleton, and use the segmented variable speed centrifugal process for integral casting. After gradient curing and construction of inner and outer protective layers, the composite cement pole is obtained. in: The overall truss assembly is as follows: the skeleton is arranged according to the bending moment envelope gradient. Metal positioning skeletons are used throughout the maximum bending moment zone from 0-1 / 4 of the member height, with a spacing of 200-250mm. In the transition zone from 1 / 4 to 1 / 2 of the member height, metal and recycled plastic modified positioning skeletons are arranged alternately. In the low-load zone above 1 / 2 of the member height, recycled plastic modified positioning skeletons are used throughout, with a spacing of 300-350mm. The upper and lower skeletons are automatically aligned via coaxial bosses and grooves, ensuring coaxial alignment of the large flow holes throughout. The main reinforcement bars are snapped into the skeleton slots, and short metal connecting rods connect to form a multi-layered triangular spatial truss. The thickness of the main reinforcement protective layer is controlled to be 25-35mm by limiting supports. After assembly, the entire assembly is hoisted into a centrifugal mold. The segmented variable-speed centrifugation process is as follows: in the low-speed material spreading stage, the rotation speed is 120-180 r / min, and the duration is extended by 2-4 min compared to the conventional process, supplemented by 20-40 Hz vibration to help the concrete pass through the multi-layer skeleton holes; in the medium-speed compaction stage, the rotation speed is 290-410 r / min, maintained for 4-5 min; in the high-speed slurry throwing stage, the rotation speed is 420-650 r / min, maintained for 6-10 min; the total centrifugation time is extended by 2-4 min compared to the conventional process. The gradient curing process is as follows: after centrifugation, the mixture is first allowed to stand still for 1-2 hours at 20-30℃ and relative humidity ≥90%; then, it is heated to 60-80℃ at 15-20℃ / h and steamed at normal pressure for 4-8 hours; then, it is cooled to room temperature at 10-15℃ / h; after demolding, it is allowed to cure naturally for no less than 7 days. The construction of the inner and outer protective layers is as follows: After cleaning the floating slurry and dust from the inner wall of the pole, spray the cement-based penetrating crystallizing material in two coats, each coat being 0.5 mm thick, for a total thickness of 1.0 mm. After spraying, keep the material moist for at least 72 hours. Apply a weather-resistant and anti-corrosion coating to the outer surface of the pole, or use recycled aggregate from waste construction to prepare protective mortar for the outer protective cement base.

[0014] Step Six. Finished Product Verification: Conduct comprehensive verification tests on the mechanical properties, durability, self-healing properties, and waterproof properties of the cement poles obtained in Step Six. Simultaneously verify the bonding strength of the modular repair interface. Determine whether the product parameters are qualified based on the tests. If qualified, place the product in the warehouse for shipment. If unqualified, conduct failure analysis on the cement pole products. in: The finished product verification includes: Mechanical performance testing includes tests for flexural bearing capacity, shear strength, compressive strength, and deflection. Durability testing includes tests for impermeability, freeze-thaw cycles, sulfate resistance, salt spray aging, and UV aging. The self-healing performance test adopts a dry-wet cycle method after pre-compression cracking, which causes 100-400μm cracks in the concrete. One cycle is performed every 24 hours, and the crack width and area repair rate at different ages are tested. Simultaneously verify the interface strength, impermeability, and freeze-thaw resistance of the new and old concrete in the modular repair.

[0015] Step 7. Full-process detection and model verification: Simultaneously conduct online detection throughout the entire production process, including material mixing, skeleton preparation, centrifugal casting, and curing. Detect the workability of concrete and the uniformity of functional material dispersion, the dimensional accuracy of the skeleton and the coaxiality of the assembly, the uniformity of centrifugal material distribution and the density of the skeleton's pores, and the internal defects and material distribution of the formed rods. Input the real-time collected process parameters and detection data into the material selection calculation model from Step 1, compare the predicted values ​​with the measured values ​​to verify the model's accuracy, and correct the material ratio, skeleton structural parameters, and preparation process parameters in a closed loop. in: The entire process of online monitoring covers all steps, including material mixing, skeleton preparation, centrifugal casting, and curing. The entire process of online detection employs one or more of the following methods: ultrasonic detection, X-ray computed tomography, shock echo, infrared imaging, and sensor monitoring. The detection process involves pre-embedding pressure or fiber optic sensors at the outlet of the large flow holes in the skeleton to monitor the concrete flow resistance and filling status in real time. When insufficient filling of a certain layer of holes is detected, the corresponding low-speed material placement time is automatically extended or the vibration frequency is increased to compensate.

[0016] The detection process inputs the real-time collected process parameters and detection data into the model in step one, compares the predicted values ​​with the measured values, and corrects the material ratio, skeleton pore structure, centrifugal cloth speed, centrifugation time and vibration frequency in a closed loop. The finished product inspection data and repair data are synchronously fed back to the database and model, and used as new training samples to update parameters, forming a complete closed-loop iterative optimization system. Furthermore, the three main reinforcing bars bear the main tensile and bending loads, while the two types of positioning skeletons only serve as positioning, force transmission, interlocking, and repair references, without replacing the main reinforcing bars in bearing the load; the self-healing components are used to repair micro-cracks, restrain fragment detachment, and delay structural deterioration; waste plastics, waste glass, waste building materials, and plant ash are used to achieve the resource utilization of four types of solid waste.

[0017] In the above technical solution, the present invention provides a corrosion-resistant outdoor cement pole material and its preparation method, which has the following beneficial effects: (1) The cement pole of the present invention adopts a split force design of "main reinforcement bearing + positioning skeleton guidance". Three continuous main reinforcements are used in conjunction with layered triangular space trusses to bear the main bending and shear loads. The metal and waste plastic modified positioning skeleton is arranged in segments according to the bending moment envelope, so that it only plays the role of positioning, force transmission and interlocking limit. It can build a segmented modular repair benchmark while ensuring the overall mechanical strength of the pole. It solves the problems that traditional continuous steel cages cannot be replaced in sections and the interface bonding strength is insufficient after repair. When the cement pole is partially damaged, it can be accurately chiseled and repaired by relying on the skeleton stop. After repair, the new and old concrete form a mechanical lock through the groove and the interlocking hole, which greatly improves the structural strength retention rate after repair.

[0018] (2) After the cement pole of the present invention is damaged, the biomimetic lotus root bundle-shaped PVA fiber in the cement pole can achieve cracking without disintegration. In addition, the carbon nanotubes can not only bridge microcracks at the microscale, but also work with stress-triggered self-healing microspheres to accurately release repair components when expanding and cracking, thereby actively hydrating and bonding the cracks. This overcomes the shortcomings of traditional concrete, which can only passively resist cracking and cannot repair expansion damage on its own. It effectively resists long-term deterioration problems such as freeze-thaw cycles, alkali-aggregate reaction, and steel rust expansion of outdoor cement poles, and greatly improves the service life of cement poles.

[0019] (3) The cement pole of the present invention adopts a double-layer waterproof and seepage-proof design with rigid inner wall penetration and weather-resistant coating on outer wall. This design can make the cement-based penetrating crystalline material on the inner wall of the cement pole homogeneously bonded with the matrix without delamination. At the same time, the weather-resistant and anti-corrosion coating on the outer wall of the cement pole can adapt to the changing outdoor temperature and wind vibration conditions. In addition, with the addition of corrosion-resistant and salt-alkali-resistant components and wood ash alkalinity adjustment, the cement pole can form multiple protective barriers from the inside to the outside, which solves the problems of thermal expansion mismatch, easy delamination and cracking, and insufficient protective durability of traditional single outer coating. It greatly improves the long-term service life and corrosion resistance of cement poles in salt-alkali, high humidity and heavy pollution environments.

[0020] (4) By constructing a material-structure-process-performance database and a multi-model coupled simulation system, this invention can directly output the optimal solution for material ratio, skeleton arrangement and centrifugation process by means of machine learning calibration during production. This can greatly reduce the amount of experimentation and improve the matching accuracy. In addition, the preparation process also collects data in real time for comparison and correction, and uses finished product data to update the model. This solves the problem of difficult identification of defects in multi-process coupling and difficulty in tracing the source of quality problems in the original production process. It can improve the quality stability and intelligent management level of cement pole production. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this invention. For those skilled in the art, other drawings can be obtained based on these drawings.

[0022] Figure 1 This is a schematic diagram of the material table structure provided in an embodiment of the present invention, which describes a corrosion-resistant outdoor cement pole material and its preparation method.

[0023] Figure 2 This is a flowchart illustrating an embodiment of the present invention: a corrosion-resistant outdoor cement pole material and its preparation method. Detailed Implementation

[0024] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0025] like Figure 1 As shown in the figure, the corrosion-resistant outdoor cement pole material provided by this invention includes base material, frame material, additive material and auxiliary material, as detailed below: Specialized materials for cement poles are used in centrifugally molded cement poles for electric power plants; The basic materials include cement pole foundation materials and steel reinforcement materials, among which: The base material is used to prepare a highly fluid concrete matrix adapted to the centrifugal molding process and to form the main load-bearing system of the pole and the space truss load-bearing system. The steel reinforcement material includes three main bars arranged in an equilateral triangle along the entire length of the pole, as well as short metal connecting rods arranged in layers at each frame position; The cement pole foundation material is a high-flowability modified concrete suitable for centrifugal molding, composed of cementitious materials, continuously graded coarse aggregate, fine aggregate, mineral admixtures, water, and polycarboxylate superplasticizer. Specifically, the maximum particle size of the coarse aggregate is ≤20mm, the water-cement ratio is 0.28-0.35, and the slurry spread is ≥180mm. The cementitious materials include ordinary Portland cement and / or sulfoaluminate cement, and the mineral admixtures include one or more of Grade I fly ash, slag powder, and silica fume. It should be noted that: Cementitious materials are the core powder materials in concrete that generate bond strength through hydration reactions, binding aggregates into a whole. They are the source of concrete's mechanical properties. Cementitious materials are mainly cement-based and can be used alone or in combination. The following options can be selected based on the requirements for cement pole placement: Ordinary Portland cement (P·O 42.5 / 52.5 grade): the mainstream matrix cementing material, with high hydration strength, good volume stability, and mature technology, is the standard cementing material for power cement poles; prestressed cement poles generally use grade 52.5 to ensure early tension strength; Sulfoaluminate cement (SAC): A corrosion-resistant cementitious material with early strength and rapid hardening, resistance to sulfate attack, and excellent frost resistance. It is used for cement poles in highly corrosive environments such as saline-alkali land and coastal areas, which meets the functional requirements of corrosion resistance and salt and alkali resistance in the solution. In continuously graded coarse aggregate, coarse aggregate consists of rock particles with a diameter greater than 4.75 mm (commonly known as crushed stone), which are the rigid skeleton phase of concrete and mainly bear compressive stress. Continuous gradation refers to the continuous distribution of aggregate particle size from the smallest to the largest, rather than a single particle size range, and the particle gradation conforms to the continuous gradation curve. Fine aggregate consists of sand and gravel particles with a particle size of less than 4.75 mm (commonly known as sand), which fill the voids between coarse aggregates to optimize the workability, encapsulation, and density of concrete paste. Mineral admixtures are mineral powders or industrial by-products with active aluminosilicates as the main component. They are added to concrete to replace part of the cement and improve the workability and durability of concrete through the pozzolanic effect and micro-aggregate effect, while reducing the heat of hydration and cost. Grade I fly ash, granulated blast furnace slag powder (S95 grade), and silica fume can be selected. The four types of materials, when combined, together form a concrete matrix material system that is suitable for centrifugal molding, can pass smoothly through the holes of multi-layer skeletons, and takes into account both structural strength and outdoor durability. The main reinforcement bars are selected from prestressed steel wire, cold-drawn steel wire, or ordinary ribbed steel bars, and short metal connecting rods are installed at each layer of the skeleton to connect the three main reinforcement bars to form a multi-layer independent triangular spatial truss structure, wherein: Ordinary ribbed steel bars are welded to short metal connecting rods; Prestressed steel wire, cold-drawn steel wire and metal short connecting rod are connected by mechanical sleeve buckle; The skeleton materials are divided into two categories: metal positioning skeletons and waste plastic modified positioning skeletons, and a segmented gradient arrangement mode is adopted. Both the metal positioning frame and the waste plastic modified positioning frame are circular ring structures composed of a triangular outer ring and a circular inner ring, arranged along the rod length axis, with a frame thickness of 30-45mm. The skeleton body has three large flow holes and six small interlocking holes that are axially connected. The large flow holes of each skeleton are coaxially aligned and form a continuous straight material flow channel. The upper and lower end faces of the skeleton are also provided with annular interlocking grooves. Neither the metal positioning frame nor the waste plastic modified positioning frame replaces the three main reinforcing bars to bear the main force. They are only used for positioning the main reinforcing bars, axial force transmission through the concrete, mechanical interlocking and limiting, and segmented repair benchmarks. in: The diameter of the large flow hole is not less than 60mm and not less than 3 times the maximum particle size of the coarse aggregate. It is an axial flared guide hole set along the concrete placement direction, with the hole diameter gradually decreasing from 65mm to 60mm and the hole opening having a rounded transition throughout. Large flow holes are arranged biased towards the compression side of the bar to ensure unobstructed path of principal compressive stress in the concrete; small interlocking holes are concentrated on the tension side of the bar to enhance the mechanical bond between the concrete and the skeleton in the tension zone. Each large flow hole has a micro exhaust groove at the top opening, which is used to expel air from the hole during centrifugal fabric distribution, thus preventing the formation of air pockets or voids inside the hole. The concrete surface facing the skeleton is provided with a guide slope of R8-10mm; the small interlocking hole has a diameter of 20-22mm and is a dovetail-shaped hole that is narrow inside and wide outside. After the concrete is embedded, it forms a reverse mechanical lock. The annular interlocking groove has a trapezoidal groove with a narrow outer edge and a wide inner edge. The inner wall of the groove is equipped with annular serrated anti-slip teeth. A water-swellable sealing strip is pre-installed at the bottom of the groove. The groove is 8mm wide and 5mm deep. It is used to achieve mechanical interlocking between concrete and skeleton, segmented positioning, and mechanical locking when repairing new and old concrete. Three radial reinforcing ribs are provided between the triangular outer ring and the circular inner ring. The radial reinforcing ribs are arranged at the midpoints of the three sides of the triangular outer ring and are staggered with the large flow hole. Six radial shear protrusions are evenly arranged along the circumference of the outer edge of the skeleton. The protrusions are 10-15mm high and are embedded in the surrounding concrete to enhance the transverse shear capacity of the section. The skeleton is arranged in a segmented gradient pattern along the length of the rod, following the bending moment envelope, as shown below: The maximum bending moment zone from 0 to 1 / 4 of the pole height at the pole root is entirely equipped with a metal positioning frame, and the spacing between the frames is reduced to 200-250mm. The transition bending moment zone between 1 / 4 and 1 / 2 of the pole height uses alternating arrangements of metal positioning frames and modified waste plastic positioning frames; In the low-load area above 1 / 2 pole height, all positions are made of modified waste plastic with a spacing of 300-350mm. The frame has pre-drilled positioning slots for three main reinforcing bars and snap-fit ​​slots for transverse connecting rods. The three main reinforcing bars and the short metal connecting rods are all mechanically snapped to the frame to form an integrated positioning-truss load-bearing unit. Each frame has a coaxial boss and a coaxial groove on the upper and lower end faces of the inner circle. When adjacent frames are installed, they are automatically aligned by inserting the boss and groove, ensuring that the three large flow holes are coaxially aligned throughout the process. The outer edge of the frame is equipped with three equidistant limiting legs, the length of which is equal to the design thickness of the concrete protective layer, and they rest against the inner wall of the mold during installation. The frame is pre-embedded with color-developing tracer strips. When the concrete of the pole cracks or the deformation of the frame exceeds the set value, the tracer strips break and release color-developing substances, which leak from the surface of the pole, for operation and maintenance inspection to identify internal damage. The side end face of the frame is provided with an annular repair stop. When partially removing the damaged section of concrete, the end face of the frame is used as the repair reference surface. The new and old concrete form a mechanical interlock through the annular interlocking groove and small interlocking holes. Additive materials are used to improve the waterproofness, toughness, corrosion resistance, and salt and alkali resistance of cement poles. They are divided into waterproof and seepage-proof components, toughening and crack-resistant components, stress-triggered self-healing components, and corrosion-resistant and salt and alkali-resistant components. The toughening and crack-resistant components include biomimetic lotus root-like bundles of PVA fibers, and may also incorporate one or more of steel fibers, PE fibers, basalt fibers, rubber powder, carbon nanotubes, and graphene, wherein: The carbon nanotube content is 0.5-0.8% of the cement mass; The biomimetic lotus root-like bundle of PVA fiber has a single filament diameter of 18-22μm and an effective bundle length of 12mm, with a volumetric admixture of 0.18%-0.22% of the total concrete volume. The stress-triggered self-healing components include stress-triggered brittle glass microspheres and / or microcapsule-Bacillus composite self-healing materials; The stress-triggered brittle glass microspheres have a particle size of 1.2-1.8 mm, a dosage of 1.2%-1.5% of the total mass of concrete, a fracture threshold of 1.8-2.2 MPa, and are internally encapsulated with a cement-based penetrating crystallization repair slurry containing ultrafine silicate cement powder, active silica sol and micro-expansion crystals. The microcapsule-Bacillus composite self-healing material includes phenolic-epoxy resin microcapsules and Bacillus immobilized on expanded perlite, and is internally encapsulated with Bacillus spores and calcium-source nutrient substrates. The self-healing component is used to repair micro-cracks in concrete and delay structural deterioration, but does not replace the main reinforcement to bear the main load-bearing function. The waterproof and seepage-proof component adopts a double-layer structure, including: The inner wall of the rod is made of a cement-based penetrating crystalline material to form a rigid inner waterproof layer; The outer surface of the pole is coated with a weather-resistant and corrosion-resistant coating to form an external waterproof layer. The weather-resistant and corrosion-resistant coating includes one or more of the following: acrylic elastic coating, polyurea, montmorillonite-modified polyurea, and rubber-modified asphalt coating. The outer layer of the pole is made of recycled aggregate from waste building materials and cement substrate. Combined with the inner wall penetrating crystalline waterproof layer and the outer surface weather-resistant and anti-corrosion layer, it forms a protective system that combines internal waterproofing, external weather resistance and substrate impermeability. The corrosion-resistant and salt-alkali-resistant components include one or more of the following: rust inhibitor, montmorillonite, fly ash, silica fume, mineral powder, sulfoaluminate cement, and MICP mineralized Bacillus. Additive materials also include process control components, which include one or more of polycarboxylate superplasticizers, expanding agents, setting regulators, and defoamers; The auxiliary materials are waste building materials, waste plastics, waste glass, and plant ash pH adjusting materials, which can be classified and graded for resource utilization and applied to different structural parts of the pole; Auxiliary materials are classified and utilized for resource recovery in the following ways: After being crushed and screened, waste building materials are used to replace natural fine aggregates at a ratio of 10%-30% for the preparation of outer protective cement matrix or repair mortar for poles. Waste plastics are modified and blended to form the upper and middle sections of the modified positioning skeleton, or ground into micro powder and added to the concrete matrix at a dosage of 5%-10%. Waste glass, after being modified and processed, can be used as the shell material for self-healing microspheres, or ground to a finer mesh than 200 mesh and used to replace part of the mineral admixtures at a ratio of 3%-8%. The amount of wood ash added is 2%-5% of the mass of cementitious materials. It is used to adjust the alkalinity of concrete, inhibit alkali-aggregate reaction, and supplement active silica-alumina components. Waste plastic modified positioning frames, waste glass, waste building materials, and plant ash are respectively used to achieve the resource utilization of four types of solid waste.

[0026] like Figure 2 The method for preparing a corrosion-resistant outdoor cement pole, as shown, includes the following steps: Step 1. Data Collection and Model Building Training: Collect environmental degradation parameters of the target service area, pole design mechanical indicators, centrifugal forming process parameters, skeleton parameters, concrete mix proportions and service damage data, construct a "material-structure-process-performance" database, and establish a multi-parameter mapping model for materials-structure-process, structural stress, concrete flow-centrifugal coupling and self-healing trigger prediction model, and use some methods to complete model training; in: The “Materials-Structure-Process-Performance” database is built based on historical production data and type test data, with an effective sample size of no less than 200 groups. The models include a material-structure-process multi-parameter mapping model, a pole structure stress finite element model, a concrete flow-centrifugal forming coupled simulation model, and a self-healing trigger prediction model; Model training employs machine learning, neural networks, digital twins, or response surface methodology for training and iteration. The model takes material ratio, skeleton arrangement, and centrifugation process parameters as inputs, and mechanical properties, durability, crack repair rate, and molding defect risk as outputs. It calibrates the stress triggering threshold of self-healing microbeads (1.8-2.2 MPa), skeleton segment arrangement rules, and centrifugation timing parameters for prediction and optimization of subsequent processes. The model input variables also include skeleton modification parameters, self-healing microsphere parameters, and fiber parameters, while the output variables include 7d / 28d compressive strength, flexural strength, impermeability, freeze-thaw resistance, salt corrosion resistance, crack repair rate, and molding defect risk. When the prediction error of flexural bearing capacity exceeds 10% or the prediction error of crack repair rate exceeds 15%, the model is retrained.

[0027] Step 2. Material Selection and Pretreatment: Based on the scheme given in the previous step, select cementitious materials, aggregates, mineral admixtures, reinforcing bars, skeleton raw materials, functional additives and solid waste auxiliary materials, and process each type of raw material separately using the processing technology given in the scheme. After pretreatment, store and process each type of raw material according to its category and application process. in: The specific preprocessing is as follows: Preparation of high-flowability concrete substrate: using ordinary Portland cement and / or sulfoaluminate cement as cementing material, combined with continuous graded coarse aggregate, fine aggregate and one or more mineral admixtures from Class I fly ash, slag powder and silica fume, and adding polycarboxylate superplasticizer, controlling the maximum particle size of coarse aggregate ≤20mm, water-cement ratio 0.28-0.35, and paste spread ≥180mm; Pre-treatment of reinforcing bars and connectors: Select three continuous main reinforcing bars and short metal connecting rods. The main reinforcing bars are selected from prestressed steel wire, cold-drawn steel wire or ordinary ribbed steel bars. Welding positions are reserved for ordinary ribbed steel bars. Mechanical connection sleeves are prefabricated at the ends of prestressed / cold-drawn steel wires. After pre-treatment, they are stored according to category. Functional additives include toughening and crack-resistant components, stress-triggered self-healing components, waterproof and corrosion-resistant components, and process conditioning components; Solid waste auxiliary materials include waste building materials, waste plastics, waste glass and wood ash; after each type of material is processed according to its corresponding process, it is stored according to its category and usage process.

[0028] Step 3. Material strengthening and mixing treatment: Select a portion of the cementitious materials, aggregates and mineral admixtures pretreated in the previous step, and then disperse and strengthen the biomimetic lotus root bundle PVA fibers, stress-triggered self-healing microspheres and carbon nanotube functional components. After strengthening, add the selected materials to the mixing equipment in the proportion and mix them to obtain a high-flowability self-healing concrete mixture. in: The specific details of functional component dispersion enhancement are as follows: The biomimetic lotus root-like bundle-shaped PVA fibers are pre-dispersed and split to control the single filament diameter to 18-22μm and the bundle length to 12mm. Carbon nanotubes and an aqueous surfactant solution were mixed at a mass ratio of 4:1 and then ultrasonically dispersed to form a uniform suspension. The stress-triggered self-healing microspheres were subjected to density sieving to control the particle size at 1.2-1.8 mm and the fracture threshold at 1.8-2.2 MPa. The specific steps of stirring and mixing are as follows: First, dry mix the cementitious materials, coarse aggregate, fine aggregate and mineral admixture for 60-120 seconds; Add water and mix with polycarboxylate superplasticizer for 120-180 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time. Finally, add the carbon nanotube suspension and self-healing microbeads, and continue stirring for 60-90 seconds until homogeneous. The concrete temperature is controlled between 5-35℃ throughout the mixing process; after mixing, the spread, slump, air content, fiber dispersion uniformity, and microsphere integrity rate are tested.

[0029] Step 4. Skeleton Preparation and Quality Inspection: Select pretreated metal raw materials and modified waste plastic raw materials, and send them into the corresponding molding molds. Then, the skeleton in the mold is formed by stamping, injection molding or casting process to obtain the triangular ring composite positioning skeleton. Subsequently, the dimensional accuracy, structural performance and surface quality of the formed skeleton are inspected to determine whether the product is qualified. If it is not qualified, the above steps and plans are adjusted until the product is qualified. Otherwise, if it is qualified, proceed to the next step to continue production. in: The skeleton forming process is as follows: metal raw materials are formed by stamping or casting, and modified waste plastic raw materials are formed by injection molding or compression molding. Both are made into a circular ring structure composed of a triangular outer ring and a circular inner ring. The skeleton thickness is controlled to be 25-30mm. The specific processing of the skeleton hole guide structure is as follows: Three axially penetrating large flow holes and six small interlocking holes are machined in the skeleton body; The large flow hole is a flared guide hole with a diameter that gradually decreases from 65mm to 60mm along the fabric direction. The hole diameter is ≥60mm and not less than 3 times the maximum particle size of the coarse aggregate. The hole opening has a rounded corner transition throughout, and the skeleton facing the fabric is machined with an R8-10mm guide slope. The small engagement holes are 20-22mm in diameter and are dovetail-shaped with a narrow inner diameter and a wide outer diameter; the large flow holes are arranged on the compression side of the rod, while the small engagement holes are concentrated on the tension side of the rod. The specific processing of the skeleton interlocking water-stop structure is as follows: Annular interlocking grooves are machined on the upper and lower end faces of the skeleton. The groove cross-section is a trapezoid with a narrow outer edge and a wide inner edge, with a groove width of 8mm and a depth of 5mm. The inner wall of the tank is machined with annular serrated anti-slip teeth, and the bottom of the tank is pre-installed with water-swellable sealing strips. The specific processing of the skeleton-reinforced shear structure is as follows: Three radial reinforcing ribs are machined between the triangular outer ring and the circular inner ring, and are arranged corresponding to the midpoint of the triangular side and intersected with the large flow hole; Six radial shear protrusions, each 10-15 mm high, are machined along the circumferential direction on the outer edge of the skeleton. The modified skeleton of waste plastic uses waste plastic as the matrix and incorporates short glass fibers and talc filler accounting for 15%-20% of the total mass of the matrix for blending and modification. After modification, the elastic modulus is increased by more than 60% and the coefficient of thermal expansion is reduced by 40% compared with pure waste plastic. After the waste plastic modified skeleton is formed, the surface is treated with micro-rough sandblasting and coated with a cement-based coupling coating. The surface of the metal skeleton is sequentially treated with knurling, hot-dip galvanizing, and silane coupling agent.

[0030] The machining skeleton positioning and connection structure is as follows: The main reinforcement positioning slot and the transverse connecting rod buckle slot are reserved on the frame; A coaxial boss and a coaxial groove are machined on the upper and lower end faces of the circular inner ring, respectively. Three equidistant limiting legs are machined on the outer edge of the frame, and the length of the legs is equal to the design thickness of the protective layer. The functional structure of the processed skeleton is as follows: A miniature venting groove is machined at the top opening of each large flow hole; Pre-embed colorimetric tracer strips inside the skeleton; A ring-shaped repair stop is machined on the side end face of the skeleton; Quality inspection includes dimensional accuracy, coaxiality, hole penetration, groove integrity, bending and torsion resistance, surface quality, and embedded part position detection. If any part fails to meet the requirements, the material ratio, mold, or process parameters are adjusted until the part meets the requirements.

[0031] Step 5. Secondary mixing and integral casting: Select the steel bars and matching connectors not selected in the above steps, and then perform end pretreatment on the steel bars and connectors. After the pretreatment, assemble the integral truss frame according to the bending moment envelope gradient and the positioning skeleton. After the assembly is completed, hoist it into the centrifugal forming mold. Then, pour the concrete mixture prepared in step 4 into the mold containing the skeleton, and use the segmented variable speed centrifugal process for integral casting. After gradient curing and construction of inner and outer protective layers, the composite cement pole is obtained. in: The overall truss assembly is as follows: the skeleton is arranged according to the bending moment envelope gradient. Metal positioning skeletons are used throughout the maximum bending moment zone from 0-1 / 4 of the member height, with a spacing of 200-250mm. In the transition zone from 1 / 4 to 1 / 2 of the member height, metal and recycled plastic modified positioning skeletons are arranged alternately. In the low-load zone above 1 / 2 of the member height, recycled plastic modified positioning skeletons are used throughout, with a spacing of 300-350mm. The upper and lower skeletons are automatically aligned via coaxial bosses and grooves, ensuring coaxial alignment of the large flow holes throughout. The main reinforcement bars are snapped into the skeleton slots, and short metal connecting rods connect to form a multi-layered triangular spatial truss. The thickness of the main reinforcement protective layer is controlled to be 25-35mm by limiting supports. After assembly, the entire assembly is hoisted into a centrifugal mold. The segmented variable-speed centrifugation process is as follows: in the low-speed material spreading stage, the rotation speed is 120-180 r / min, and the duration is extended by 2-4 min compared to the conventional process, supplemented by 20-40 Hz vibration to help the concrete pass through the multi-layer skeleton holes; in the medium-speed compaction stage, the rotation speed is 290-410 r / min, maintained for 4-5 min; in the high-speed slurry throwing stage, the rotation speed is 420-650 r / min, maintained for 6-10 min; the total centrifugation time is extended by 2-4 min compared to the conventional process. The gradient curing process is as follows: after centrifugation, the mixture is first allowed to stand still for 1-2 hours at 20-30℃ and relative humidity ≥90%; then, it is heated to 60-80℃ at 15-20℃ / h and steamed at normal pressure for 4-8 hours; then, it is cooled to room temperature at 10-15℃ / h; after demolding, it is allowed to cure naturally for no less than 7 days. The construction of the inner and outer protective layers is as follows: After cleaning the floating slurry and dust from the inner wall of the pole, spray the cement-based penetrating crystallizing material in two coats, each coat being 0.5 mm thick, for a total thickness of 1.0 mm. After spraying, keep the material moist for at least 72 hours. Apply a weather-resistant and anti-corrosion coating to the outer surface of the pole, or use recycled aggregate from waste construction to prepare protective mortar for the outer protective cement base.

[0032] Step Six. Finished Product Verification: Conduct comprehensive verification tests on the mechanical properties, durability, self-healing properties, and waterproof properties of the cement poles obtained in Step Six. Simultaneously verify the bonding strength of the modular repair interface. Determine whether the product parameters are qualified based on the tests. If qualified, place the product in the warehouse for shipment. If unqualified, conduct failure analysis on the cement pole products. in: Finished product validation includes: Mechanical performance testing includes tests for flexural bearing capacity, shear strength, compressive strength, and deflection. Durability testing includes tests for impermeability, freeze-thaw cycles, sulfate resistance, salt spray aging, and UV aging. The self-healing performance test adopts a dry-wet cycle method after pre-compression cracking, which causes 100-400μm cracks in the concrete. One cycle is performed every 24 hours, and the crack width and area repair rate at different ages are tested. Simultaneously verify the interface strength, impermeability, and freeze-thaw resistance of the new and old concrete in the modular repair.

[0033] Step 7. Full-process detection and model verification: Simultaneously conduct online detection throughout the entire production process, including material mixing, skeleton preparation, centrifugal casting, and curing. Detect the workability of concrete and the uniformity of functional material dispersion, the dimensional accuracy of the skeleton and the coaxiality of the assembly, the uniformity of centrifugal material distribution and the density of the skeleton's pores, and the internal defects and material distribution of the formed rods. Input the real-time collected process parameters and detection data into the material selection calculation model from Step 1, compare the predicted values ​​with the measured values ​​to verify the model's accuracy, and correct the material ratio, skeleton structural parameters, and preparation process parameters in a closed loop. in: The entire process of online monitoring covers all steps, including material mixing, skeleton preparation, centrifugal casting, and curing. The entire process of online detection employs one or more of the following methods: ultrasonic detection, X-ray computed tomography, shock echo, infrared imaging, and sensor monitoring. The detection process involves pre-embedding pressure or fiber optic sensors at the outlet of the large flow holes in the skeleton to monitor the concrete flow resistance and filling status in real time. When insufficient filling of a certain layer of holes is detected, the corresponding low-speed material placement time is automatically extended or the vibration frequency is increased to compensate.

[0034] The detection process inputs the real-time collected process parameters and detection data into the model in step one, compares the predicted values ​​with the measured values, and corrects the material ratio, skeleton pore structure, centrifugal cloth speed, centrifugation time and vibration frequency in a closed loop. The finished product inspection data and repair data are synchronously fed back to the database and model, and used as new training samples to update parameters, forming a complete closed-loop iterative optimization system. In another embodiment of the present invention, the three main reinforcing bars bear the main tensile and bending loads, and the two types of positioning skeletons only serve as positioning, force transmission, interlocking and repair references, without replacing the main reinforcing bars in bearing the load; the self-healing component is used to repair micro-cracks, restrain fragments from falling off, and delay structural deterioration; waste plastics, waste glass, waste building materials and plant ash realize the resource utilization of four types of solid waste.

[0035] Example 1 A corrosion-resistant outdoor cement pole material and its preparation method include the following steps: S1. Data Modeling and Batching Calculation: Environmental parameters such as wind load, salt spray corrosion, and freeze-thaw cycles in coastal saline-alkali areas are collected. Design parameters for a 12m tapered prestressed cement pole (190mm tip diameter, crack test bending moment 29.00kN·m) are set according to GB / T4623-2025. A "material-structure-process-performance" database is constructed, and a multi-parameter coupled model is trained to output optimal batching and process parameters. The concrete design strength is C50, the water-cement ratio is 0.30, and the grout spread is 190mm. The main reinforcement consists of 6 prestressed steel wires with a diameter of 12mm. The positioning skeleton is arranged in a segmented gradient according to the bending moment envelope, and the stress triggering threshold of the self-healing microbeads is 2.0 MPa.

[0036] S2. Material pretreatment and skeleton preparation: Weigh the raw materials according to the following proportions: 100 parts of P・O52.5 ordinary Portland cement, 185 parts of 5-20mm continuously graded crushed stone, 115 parts of natural sand with a fineness modulus of 2.6, 20 parts of Grade I fly ash, 12 parts of S95 granulated slag powder, 8 parts of silica fume, 1.2 parts of polycarboxylate superplasticizer, and 30 parts of mixing water. Functional components: 12mm bundled PVA fibers (volume content 0.20%), carbon nanotubes (cement mass 0.6‰), 1.5mm stress-triggered glass microspheres (cement mass 1.5%, internally encapsulated with cement-based penetrating crystallization repair slurry), and MICP Bacillus subtilis microcapsules (cement mass 0.3%). Corrosion-resistant components: 1.0 part of steel reinforcement rust inhibitor and 1.5 parts of montmorillonite.

[0037] Pretreatment of various materials: aggregate screening to remove impurities, PVA fiber pre-dispersion and fiber opening, carbon nanotubes are dispersed into a suspension by surfactant and ultrasonic dispersion, and self-healing microbeads are screened for density matching. Graded treatment of solid waste materials: 15% of fine aggregate is replaced by waste construction stone after screening for use in the outer protective layer; waste plastic is modified by adding 18% short glass fiber and used to prepare the positioning skeleton; waste glass is ground to below 200 mesh to replace 5% of mineral admixtures; and 3 parts of wood ash are used to adjust the alkalinity of concrete.

[0038] Two types of positioning frames were prepared: the metal positioning frame was made of Q235 steel plate by stamping, with a thickness of 35mm. It was machined with three large flow holes with a diameter of 65mm tapering to 60mm and six small dovetail-shaped interlocking holes with a diameter of 22mm. The upper and lower end faces were machined with trapezoidal interlocking grooves with a width of 8mm and a depth of 5mm and pre-installed with water-swellable sealing strips. Three radial reinforcing ribs were set in the inner and outer rings. The outer edge was equipped with six radial shear-resistant protrusions with a height of 12mm and three equidistant limiting feet. The surface was successively treated with knurling, hot-dip galvanizing and silane coupling agent. The waste plastic modified positioning skeleton is injection molded with a thickness of 35mm. Its structural parameters are the same as those of the metal skeleton. The surface is treated with micro-rough sandblasting and coated with a cement-based coupling coating. Both types of frames are prepared for use after passing quality inspections for dimensional accuracy, coaxiality, and bending strength.

[0039] S3. Concrete mixing and truss assembly: First, put cement, aggregates and mineral admixtures into a forced mixer and dry mix for 90 seconds, then add water and water-reducing agent and wet mix for 150 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time. Finally, add the carbon nanotube suspension, self-healing components, and corrosion-resistant components, and continue stirring for 75 seconds until homogeneous. Control the mixing temperature at 25°C, and test the slurry expansion at 192 mm, slump at 160 mm, and air content at ≤1.5%.

[0040] Synchronous assembly of the overall truss frame: The metal positioning frame is densely arranged in the maximum bending moment section from 0-3m (1 / 4 of the member length) at a spacing of 220mm; The 3-6m transition section uses an alternating arrangement of metal and waste plastic frames; In the 6-12m low-load section, all sections are equipped with modified waste plastic positioning frames, spaced at 320mm intervals. The upper and lower frames are automatically aligned by coaxial bosses and grooves, ensuring that the large flow hole is coaxially aligned throughout. Six prestressed main reinforcement bars are inserted into the positioning slots of the skeleton, and short metal connecting rods at each layer of the skeleton are connected by mechanical sleeve buckles to form a multi-layer triangular space truss; the thickness of the protective layer of the main reinforcement bars is controlled to be 20mm by limiting the support feet, and the whole assembly is hoisted into the centrifugal steel mold.

[0041] S4. Centrifugal molding and curing: A segmented variable speed centrifugal process is adopted: the low-speed material feeding stage has a rotation speed of 150r / min and a duration of 4min, supplemented by 30Hz vibration to help the concrete pass through the multi-layer skeleton holes. During the medium-speed compaction stage, the rotation speed is 350 r / min, and this is maintained for 4.5 min. The high-speed centrifugation stage was carried out at a speed of 550 r / min for 8 min; the total centrifugation time was 16.5 min, which is 3 min longer than the conventional process.

[0042] After molding, a gradient curing process is adopted: first, the mixture is left to stand still for 1.5 hours at 25℃ and 95% relative humidity; Then, increase the temperature to 70℃ at a rate of 18℃ / h and perform normal pressure steam curing for 6 hours; It was then cooled to room temperature at a rate of 12℃ / h; After demolding, allow to cure naturally for 10 days.

[0043] After curing, the inner and outer protective layers are constructed: After cleaning the laitance and dust from the inner wall, the cement-based penetrating crystallizing material is sprayed in two coats, each coat being 0.5 mm thick, for a total thickness of 1.0 mm. After spraying, the material is kept moist for 72 hours. The outer wall is leveled with protective mortar made from recycled aggregates from waste buildings, and coated with a montmorillonite-modified polyurea weather-resistant coating with a thickness of 0.8mm, ultimately resulting in a corrosion-resistant, self-healing modular cement pole.

[0044] Example 2 A corrosion-resistant outdoor cement pole material and its preparation method include the following steps: S1. Data Modeling and Batching Calculation: Collect environmental parameters such as wind load and freeze-thaw cycles in inland high-wind-load areas. Based on GB / T4623-2025, set the design parameters for a 12m conical prestressed cement pole (190mm tip diameter, crack test bending moment 29.00kN·m), construct a database, train the model, and output the optimal parameters. The concrete design strength is C50, the water-cement ratio is 0.30, and the grout spread is 190mm. The main reinforcement consists of 4 prestressed steel wires and 2 ordinary ribbed steel bars. The positioning skeleton is arranged in a segmented gradient, and the stress triggering threshold of the self-healing microbeads is 2.0 MPa.

[0045] S2. Material pretreatment and skeleton preparation: Weigh the raw materials according to the following proportions: 100 parts of P・O52.5 ordinary Portland cement, 185 parts of 5-20mm continuously graded crushed stone, 115 parts of natural sand with a fineness modulus of 2.6, 20 parts of Grade I fly ash, 12 parts of S95 granulated slag powder, 8 parts of silica fume, 1.2 parts of polycarboxylate superplasticizer, and 30 parts of mixing water. Functional components: 12mm bundled PVA fibers (volume content 0.20%), carbon nanotubes (cement mass 0.6‰), and 1.5mm diameter stress-triggered glass microspheres (cement mass 1.5%, internally encapsulated with cement-based penetrating crystallization repair slurry). Corrosion-resistant component: 1.0 part of steel reinforcement rust inhibitor.

[0046] Pretreatment of various materials: aggregate screening to remove impurities, PVA fiber pre-dispersion and fiber opening, carbon nanotube ultrasonic dispersion to form a suspension, and self-healing microbead screening for density matching. Waste building stone is screened and replaced with 15% fine aggregate for the outer protective layer; waste plastic is modified with 18% short glass fiber to prepare the positioning skeleton; and waste glass is ground to replace 5% mineral admixtures.

[0047] The two types of positioning skeletons were prepared in the same manner as in Example 1, and were put into use after passing the quality inspection of dimensional accuracy and structural performance.

[0048] S3. Concrete mixing and truss assembly: First, dry mix cement, aggregate, and mineral admixtures for 90 seconds, then add water and water-reducing agent and wet mix for 150 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time. Add carbon nanotube suspension and self-healing microbeads, continue stirring for 75 seconds until uniform, control the mixing temperature at 25℃, and test the slurry expansion at 190mm and slump at 158mm.

[0049] The truss assembly is the same as in Example 1. The main reinforcement consists of 4 prestressed steel wires and 2 ordinary ribbed steel bars, which are connected by mechanical sleeves and welding respectively. After assembly, the whole structure is hoisted into the centrifugal steel mold.

[0050] S4. Centrifugal molding and curing: The segmented variable speed centrifugation process is the same as in Example 1; the gradient curing system is the same as in Example 1; Protective layer construction: The inner wall is sprayed with cement-based penetrating crystalline material to form a rigid inner waterproof layer, and the outer wall is coated with acrylic elastic weather-resistant coating with a thickness of 0.8mm, finally obtaining a corrosion-resistant self-healing cement pole.

[0051] Example 3 A corrosion-resistant outdoor cement pole material and its preparation method include the following steps: S1. Data Modeling and Batching Calculation: Collect environmental parameters of ordinary rural power distribution areas, set design parameters for 12m tapered reinforced concrete poles (top diameter 190mm, crack test bending moment 21.75kN·m) according to GB / T4623-2025, construct a database and train the model, and output the optimal parameters: The concrete design strength is C45, the water-cement ratio is 0.32, and the grout spread is 185mm. The main reinforcement consists of 6 ordinary ribbed steel bars with a diameter of 12mm. The positioning skeleton is arranged in sections, and the stress triggering threshold of the self-healing microbeads is 1.9MPa.

[0052] S2. Material pretreatment and skeleton preparation: Weigh the raw materials according to the following proportions: 100 parts of P・O42.5 ordinary Portland cement, 190 parts of 5-20mm continuously graded crushed stone, 120 parts of natural sand with a fineness modulus of 2.6, 25 parts of Grade I fly ash, 15 parts of S95 granulated slag powder, 5 parts of silica fume, 1.0 part of polycarboxylate superplasticizer, and 32 parts of mixing water; Functional components: 12mm bundled PVA fibers (volume content 0.18%), carbon nanotubes (cement mass 0.5‰), 1.4mm stress-triggered glass microspheres (cement mass 1.2%, internally encapsulated with cement-based penetrating crystallization repair slurry), and MICP Bacillus subtilis microcapsules (cement mass 0.2%). Corrosion-resistant component: 0.8 parts of steel reinforcement rust inhibitor.

[0053] Pretreatment of various materials: aggregate screening and impurity removal, PVA fiber pre-dispersion, carbon nanotube ultrasonic dispersion, and self-healing microbead screening; Waste building stone, after screening, replaces 10% of fine aggregate for the outer protective layer; waste plastic is modified with 15% short glass fiber to prepare the positioning skeleton; waste glass is ground to replace 3% of mineral admixtures; and 2 parts of wood ash are used to adjust the alkalinity.

[0054] The two types of positioning skeleton structures are the same as in Example 1, with a thickness of 30mm, and are ready for use after passing quality inspection.

[0055] S3. Concrete mixing and truss assembly: First, dry mix cement, aggregate, and mineral admixtures for 90 seconds, then add water and water-reducing agent and wet mix for 150 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time; add carbon nanotubes, self-healing components and corrosion-resistant components, and stir for 75 seconds until uniform. Control the mixing temperature at 25°C, and test the slurry spread at 186 mm and the slump at 155 mm.

[0056] Truss assembly: Metal positioning frames are installed in the 0-2.4m (1 / 5 of the length) section of the pole root, with a spacing of 250mm; the entire 2.4-12m section is installed with modified waste plastic positioning frames, with a spacing of 350mm. The upper and lower skeletons are coaxially aligned, with 6 ordinary ribbed steel bars inserted into the slots. Short metal connecting rods are welded together at each layer of the skeleton to form a triangular spatial truss. The thickness of the protective layer of the main reinforcement is controlled at 18mm. After assembly, the truss is hoisted into a centrifugal steel mold.

[0057] S4. Centrifugal molding and curing: A segmented variable-speed centrifugal process is used. The low-speed fabric feeding stage has a rotation speed of 140 r / min and a duration of 3.5 min; During the medium-speed compaction stage, the rotation speed is 320 r / min, and the speed is maintained for 4.5 min. The high-speed centrifugation stage was carried out at a speed of 500 r / min for 7 min; the total centrifugation time was 15 min, which is 2.5 min longer than the conventional process.

[0058] Gradient curing: 25℃ static stop for 1 hour, then heat to 65℃ and steam at normal pressure for 5 hours, then cool to room temperature and cure naturally for 7 days.

[0059] Protective layer construction: The inner wall is sprayed with cement-based penetrating crystallizing material, and the outer wall is coated with rubber-modified asphalt coating with a thickness of 0.7mm, finally obtaining a low-cost corrosion-resistant self-healing cement pole.

[0060] The test results show that the core performance of the three embodiments meets the requirements of GB / T 4623-2025 standard. Among them, Embodiment 1 has the best overall performance in terms of mechanical strength, weather resistance, self-healing effect and modular repair strength, and is the best embodiment.

[0061] The foregoing has only described certain exemplary embodiments of the present invention by way of illustration. Undoubtedly, those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the foregoing drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A corrosion-resistant outdoor cement pole material, comprising base material, frame material, additive material, and auxiliary material, characterized in that: The basic materials include cement pole foundation materials and steel reinforcement materials, wherein: The base material is used to prepare a highly fluid concrete matrix adapted to centrifugal molding process and to form the main load-bearing system of the pole and the space truss bearing system. The steel reinforcement material includes three main bars arranged in an equilateral triangle along the entire length of the bar, and short metal connecting rods arranged in layers at each frame position; The skeleton materials are divided into two categories: metal positioning skeletons and waste plastic modified positioning skeletons, and a segmented gradient arrangement mode is adopted. The additive material is used to improve the waterproofness, toughness, corrosion resistance, and salt and alkali resistance of cement poles. It is divided into waterproof and seepage-proof components, toughening and crack-resistant components, stress-triggered self-healing components, and corrosion-resistant and salt and alkali-resistant components. The auxiliary materials are waste building materials, waste plastics, waste glass, and plant ash pH adjusting materials, which can be classified and graded for resource utilization and applied to different structural parts of the pole.

2. The corrosion-resistant outdoor cement pole material according to claim 1, characterized in that, The special material for cement poles is used in centrifugally molded power cement poles; The cement pole base material is a high-flowability modified concrete suitable for centrifugal molding, which is composed of cementitious materials, continuously graded coarse aggregate, fine aggregate, mineral admixtures, water and polycarboxylate superplasticizer. The main reinforcing bars are selected from prestressed steel wire, cold-drawn steel wire, or ordinary ribbed steel bars, and short metal connecting rods are installed at each layer of the skeleton to connect the three main reinforcing bars to form a multi-layer independent triangular spatial truss structure, wherein: Ordinary ribbed steel bars are welded to short metal connecting rods; Prestressed steel wire, cold-drawn steel wire and metal short connecting rod are connected by mechanical sleeve buckle.

3. The corrosion-resistant outdoor cement pole material according to claim 1, characterized in that, Both the metal positioning frame and the waste plastic modified positioning frame are circular ring structures composed of a triangular outer ring and a circular inner ring, arranged along the rod length axis, with a frame thickness of 30-45mm. The skeleton body has three large flow holes and six small interlocking holes that are axially connected. The large flow holes of each skeleton are coaxially aligned and form a continuous straight material flow channel. The upper and lower end faces of the skeleton are also provided with annular interlocking grooves. Neither the metal positioning frame nor the waste plastic modified positioning frame replaces the three main reinforcing bars to bear the main force; they are only used for positioning the main reinforcing bars, axial force transmission through the concrete, mechanical interlocking and limiting, and segmented repair benchmarks.

4. The corrosion-resistant outdoor cement pole material according to claim 1, characterized in that, The toughening and crack-resistant component includes biomimetic lotus root-like bundles of PVA fibers, and may also incorporate one or more of steel fibers, PE fibers, basalt fibers, rubber powder, carbon nanotubes, and graphene, wherein: The carbon nanotube content is 0.5-0.8% of the cement mass; The biomimetic lotus root-like bundle-shaped PVA fiber has a single filament diameter of 18-22μm, an effective bundle length of 12mm, and a volumetric admixture of 0.18%-0.22% of the total concrete volume. The stress-triggered self-healing component includes stress-triggered brittle glass microspheres and / or microcapsule-Bacillus composite self-healing materials; The stress-triggered brittle glass microspheres have a particle size of 1.2-1.8 mm, a dosage of 1.2%-1.5% of the total mass of concrete, a fracture threshold of 1.8-2.2 MPa, and are internally encapsulated with a cement-based penetrating crystallization repair slurry containing ultrafine silicate cement powder, active silica sol and micro-expansion crystals. The microcapsule-Bacillus composite self-healing material includes phenolic-epoxy resin microcapsules and Bacillus immobilized on expanded perlite, and is internally encapsulated with Bacillus spores and calcium source nutrient substrate. The waterproof and seepage-resistant component adopts an inner and outer double-layer structure, wherein: The inner wall of the rod is made of a cement-based penetrating crystalline material to form a rigid inner waterproof layer; The outer surface of the pole is coated with a weather-resistant and corrosion-resistant paint to form an external waterproof layer; The corrosion-resistant and salt-alkali-resistant components include one or more of the following: rust inhibitor, montmorillonite, fly ash, silica fume, mineral powder, sulfoaluminate cement, and MICP mineralized Bacillus. The additive material also includes process control components, which include one or more of polycarboxylate superplasticizers, expanding agents, setting regulators, and defoamers.

5. The corrosion-resistant outdoor cement pole material according to claim 1, characterized in that, The auxiliary materials are utilized in a differentiated and resource-based manner as follows: The waste building materials, after being crushed and screened, replace natural fine aggregates at a ratio of 10%-30% and are used to prepare the outer protective cement matrix of the pole or repair mortar. The waste plastic is modified and blended to form the upper and middle sections of the waste plastic modified positioning skeleton, or it is ground into micro powder and added to the concrete matrix at a dosage of 5%-10%. The waste glass, after being modified and processed, can be used as the shell material for self-healing microspheres, or ground to below 200 mesh and used to replace part of the mineral admixtures at a ratio of 3%-8%. The amount of plant ash added is 2%-5% of the mass of the cementitious material, and it is used to adjust the alkalinity of concrete, inhibit alkali-aggregate reaction, and supplement active silica-alumina components.

6. A method for preparing a corrosion-resistant outdoor cement pole, characterized in that, Includes the following steps: Step 1. Data Collection and Model Building Training: Collect environmental degradation parameters of the target service area, pole design mechanical indicators, centrifugal forming process parameters, skeleton parameters, concrete mix proportions and service damage data, construct a "material-structure-process-performance" database, and establish a multi-parameter mapping model for materials-structure-process, structural stress, concrete flow-centrifugal coupling and self-healing trigger prediction model, and use some methods to complete model training; Step 2. Material Selection and Pretreatment: Based on the scheme given in the previous step, select cementitious materials, aggregates, mineral admixtures, reinforcing bars, skeleton raw materials, functional additives and solid waste auxiliary materials, and process each type of raw material separately using the processing technology given in the scheme. After pretreatment, store and process each type of raw material according to its category and application process. Step 3. Material strengthening and mixing treatment: Select a portion of the cementitious materials, aggregates and mineral admixtures pretreated in the previous step, and then disperse and strengthen the biomimetic lotus root bundle PVA fibers, stress-triggered self-healing microspheres and carbon nanotube functional components. After strengthening, add the selected materials to the mixing equipment in the proportion and mix them to obtain a high-flowability self-healing concrete mixture. Step 4. Skeleton Preparation and Quality Inspection: Select pretreated metal raw materials and modified waste plastic raw materials, and send them into the corresponding molding molds. Then, the skeleton in the mold is formed by stamping, injection molding or casting process to obtain the triangular ring composite positioning skeleton. Subsequently, the dimensional accuracy, structural performance and surface quality of the formed skeleton are inspected to determine whether the product is qualified. If it is not qualified, the above steps and plans are adjusted until the product is qualified. Otherwise, if it is qualified, proceed to the next step to continue production. Step 5. Secondary mixing and integral casting: Select the steel bars and matching connectors not selected in the above steps, and then perform end pretreatment on the steel bars and connectors. After the pretreatment, assemble the integral truss frame according to the bending moment envelope gradient and the positioning skeleton. After the assembly is completed, hoist it into the centrifugal forming mold. Then, pour the concrete mixture prepared in step 4 into the mold containing the skeleton, and use the segmented variable speed centrifugal process for integral casting. After gradient curing and construction of inner and outer protective layers, the composite cement pole is obtained. Step Six. Finished Product Verification: Conduct comprehensive verification tests on the mechanical properties, durability, self-healing properties, and waterproof properties of the cement poles obtained in Step Six. Simultaneously verify the bonding strength of the modular repair interface. Determine whether the product parameters are qualified based on the tests. If qualified, place the product in the warehouse for shipment. If unqualified, conduct failure analysis on the cement pole products. Step 7. Full-process detection and model verification: Simultaneous online detection is carried out in each production process, including material mixing, skeleton preparation, centrifugal casting and curing. The detection includes concrete workability and uniformity of functional material dispersion, skeleton dimensional accuracy and assembly coaxiality, uniformity of centrifugal material distribution and density of skeleton pore filling, and internal defects and material distribution of the formed rod. The real-time collected process parameters and detection data are input into the material selection calculation model in Step 1. The model accuracy is verified by comparing the predicted values ​​with the measured values, and the material ratio, skeleton structural parameters and preparation process parameters are corrected in a closed loop.

7. The method for preparing a corrosion-resistant outdoor cement pole according to claim 1, characterized in that, In step one: The "materials-structure-process-performance" database is constructed based on historical production data and type test data, with an effective sample size of no less than 200 groups. The model includes a material-structure-process multi-parameter mapping model, a pole structure stress finite element model, a concrete flow-centrifugal forming coupled simulation model, and a self-healing trigger prediction model. The model is trained and iterated using machine learning, neural networks, digital twins, or response surface methodology. The model takes material ratio, skeleton arrangement, and centrifugation process parameters as inputs, and outputs mechanical properties, durability, crack repair rate, and molding defect risk. When the prediction error of flexural bearing capacity exceeds 10% or the prediction error of crack repair rate exceeds 15%, the model is retrained.

8. The method for preparing a corrosion-resistant outdoor cement pole according to claim 1, characterized in that, The specific preprocessing in step two is as follows: Preparation of high-flowability concrete substrate: using ordinary Portland cement and / or sulfoaluminate cement as cementing material, combined with continuous graded coarse aggregate, fine aggregate and one or more mineral admixtures from Class I fly ash, slag powder and silica fume, and adding polycarboxylate superplasticizer, controlling the maximum particle size of coarse aggregate ≤20mm, water-cement ratio 0.28-0.35, and paste spread ≥180mm; Pre-treatment of reinforcing bars and connectors: Select three continuous main reinforcing bars and short metal connecting rods. The main reinforcing bars are selected from prestressed steel wire, cold-drawn steel wire or ordinary ribbed steel bars. Welding positions are reserved for ordinary ribbed steel bars. Mechanical connection sleeves are prefabricated at the ends of prestressed / cold-drawn steel wires. After pre-treatment, they are stored according to category. The functional additives include toughening and crack-resistant components, stress-triggered self-healing components, waterproof and corrosion-resistant components, and process adjustment components. The solid waste auxiliary materials include waste building materials, waste plastics, waste glass and wood ash; each type of material is processed according to its corresponding process and then stored according to its category and usage process. In step three: The specific details of functional component dispersion enhancement are as follows: The biomimetic lotus root-like bundle-shaped PVA fibers are pre-dispersed and split to control the single filament diameter to 18-22μm and the bundle length to 12mm. Carbon nanotubes and an aqueous surfactant solution were mixed at a mass ratio of 4:1 and then ultrasonically dispersed to form a uniform suspension. The stress-triggered self-healing microspheres were subjected to density sieving to control the particle size at 1.2-1.8 mm and the fracture threshold at 1.8-2.2 MPa. The specific steps of stirring and mixing are as follows: First, dry mix the cementitious materials, coarse aggregate, fine aggregate and mineral admixture for 60-120 seconds; Add water and mix with polycarboxylate superplasticizer for 120-180 seconds. Add the pre-dispersed PVA fiber in two batches, stirring for 30 seconds each time. Finally, add the carbon nanotube suspension and self-healing microbeads, and continue stirring for 60-90 seconds until homogeneous. The concrete temperature is controlled between 5-35℃ throughout the mixing process; after mixing, the spread, slump, air content, fiber dispersion uniformity, and microsphere integrity rate are tested.

9. The method for preparing a corrosion-resistant outdoor cement pole according to claim 1, characterized in that, In step four: The skeleton forming process is as follows: metal raw materials are formed by stamping or casting, and modified waste plastic raw materials are formed by injection molding or compression molding, both of which are made into a circular ring structure composed of a triangular outer ring and a circular inner ring, and the skeleton thickness is controlled to be 25-30mm. The specific processing of the skeleton hole guiding structure is as follows: Three axially penetrating large flow holes and six small interlocking holes are machined in the skeleton body; The waste plastic modified skeleton uses waste plastic as the matrix and incorporates short glass fibers and talc filler accounting for 15%-20% of the total mass of the matrix for blending and modification. The surface of the waste plastic modified skeleton is subjected to micro-rough sandblasting treatment after molding and coated with a cement-based coupling coating. The surface of the metal skeleton is sequentially treated with knurling, hot-dip galvanizing, and silane coupling agent. The quality inspection includes dimensional accuracy, coaxiality, hole penetration, groove integrity, bending and torsion resistance, surface quality, and embedded part location detection.

10. The method for preparing a corrosion-resistant outdoor cement pole according to claim 1, characterized in that, In step five: The segmented variable speed centrifugation process is specifically as follows: During the low-speed material feeding stage, the rotation speed is 120-180 r / min, and the duration is 2-4 min longer than the conventional process. The concrete is assisted by 20-40 Hz vibration to help it pass through the multi-layer skeleton holes. During the medium-speed compaction stage, the rotation speed is 290-410 r / min, and the speed is maintained for 4-5 min; during the high-speed slurry throwing stage, the rotation speed is 420-650 r / min, and the speed is maintained for 6-10 min. The total centrifugation time is 2-4 minutes longer than that of conventional processes; The specific steps of gradient maintenance are: After centrifugation, allow the mixture to stand still for 1-2 hours at 20-30℃ and relative humidity ≥90%. Then, increase the temperature to 60-80℃ at a rate of 15-20℃ / h and perform normal pressure steam curing for 4-8 hours; Subsequently, cool to room temperature at a rate of 10-15℃ / h; allow to cure naturally for at least 7 days after demolding. The specific construction of the inner and outer protective layers is as follows: After cleaning the inner wall of the rod to remove laitance and dust, apply cement-based penetrating crystallizing material in two coats, each coat being 0.5 mm thick, for a total thickness of 1.0 mm. After spraying, keep the material moist for at least 72 hours. The outer surface of the pole is coated with a weather-resistant and anti-corrosion coating, or a protective mortar made from recycled waste building aggregates is used to construct the outer protective cement matrix; In step six: The finished product verification includes: Mechanical performance testing includes tests for flexural bearing capacity, shear strength, compressive strength, and deflection. Durability testing includes tests for impermeability, freeze-thaw cycles, sulfate resistance, salt spray aging, and UV aging. The self-healing performance test adopts a dry-wet cycle method after pre-compression cracking, which causes 100-400μm cracks in the concrete. One cycle is performed every 24 hours, and the crack width and area repair rate at different ages are tested. Simultaneously verify the interface strength, impermeability, and freeze-thaw resistance of the new and old concrete in the modular repair. In step seven: The entire process of online monitoring covers all steps, including material mixing, skeleton preparation, centrifugal casting, and curing. The entire process of online detection employs one or more of the following methods: ultrasonic detection, X-ray computed tomography, shock echo, infrared imaging, and sensor monitoring. The detection process involves pre-embedding pressure or fiber optic sensors at the outlet of the large flow hole in the skeleton to monitor the concrete flow resistance and filling status in real time. The detection process inputs the real-time collected process parameters and detection data into the model in step one, compares the predicted values ​​with the measured values, and corrects the material ratio, skeleton pore structure, centrifugal cloth speed, centrifugation time and vibration frequency in a closed loop. The finished product testing data and repair data are synchronously fed back to the database and model, serving as new training samples to update parameters, forming a complete closed-loop iterative optimization system.

Citation Information

Patent Citations

  • Waterproof and corrosion-proof cement pole

    CN102010227B

  • Method for manufacturing ecological cement telegraph pole by utilizing industrial solid waste