Aluminum-doped high-temperature thermistor material, its preparation method and application
By using aluminum-doped high-temperature thermistor materials, the problem of resistivity decrease in spinel structures at high temperatures has been solved, thereby improving the stability and electrical performance of thermistors at high temperatures. This method is suitable for medium- and high-temperature thermistors.
Patent Information
- Application Number
- CN202611252304.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing spinel-structured mid-temperature NTC thermistors are prone to metal oxide precipitation at high temperatures, leading to a decrease in resistivity and making them unsuitable for use in high-temperature thermistors.
A high-temperature thermistor material doped with aluminum, with the chemical formula Mg(AlxMn1-x)2O4, is used. The electrical properties of the thermistor ceramic material are regulated by Al3+ doping at the B site, which transforms its phase structure from MgMn2O4 to high-temperature resistant MgAl2O4, thereby improving the sintering density. The high-temperature thermistor material is prepared by a process including ball milling, drying, grinding, sieving, pressing, and sintering.
The stability and electrical performance of the thermistors at high temperatures have been improved. The material has a negative temperature resistivity in the range of 25~1000℃, and the B value and ρ value are adjustable, making it suitable for manufacturing medium and high temperature thermistors.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials technology, and more specifically, to an aluminum-doped high-temperature thermistor material, its preparation method, and its application. Background Technology
[0002] Negative temperature coefficient (NTC) thermistors can be classified into low-temperature (<-60℃), medium-temperature (-60℃~300℃), and high-temperature (>300℃) thermistors according to their operating temperature range. Currently, the medium-temperature NTC thermistors with spinel structures are mainly used in the market. The spinel structure is unstable and will precipitate metal oxides at high temperatures to promote conductivity, causing the room temperature resistivity of the thermistor to drop sharply. Therefore, traditional spinel materials are difficult to use in high-temperature thermistors. Summary of the Invention
[0003] The purpose of this invention is to overcome the shortcomings of the existing technology and provide an aluminum-doped high-temperature thermistor material, its preparation method and application.
[0004] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0005] The first aspect of this invention provides an aluminum-doped high-temperature thermistor material, said material being made from alumina, manganese dioxide, and magnesium carbonate, with the chemical formula Mg(Al) x Mn 1-x )2O4, where x satisfies: 0.2≤x≤0.8.
[0006] In some implementations, one or more of the following features are also included:
[0007] (a) The x satisfies: 0.4 ≤ x ≤ 0.6;
[0008] (b) The crystal structure of the aluminum-doped high-temperature thermistor material is a spinel structure;
[0009] (c) The aluminum-doped high-temperature thermistor material has a measurement temperature range of 25~1000℃, a thermistor constant B25 / 1000 of 6137~6477 K, and a resistivity of 2.3×10⁻⁶ K at 25℃. 7 ~6.2×10 7 Ω·cm.
[0010] A second aspect of the present invention provides a method for preparing an aluminum-doped high-temperature thermistor material, comprising the following steps:
[0011] (1) According to Mg(Al) x Mn 1-xAlumina, manganese dioxide, and magnesium carbonate were weighed out and mixed evenly in a molar ratio of 0.2 ≤ x ≤ 0.8 to obtain a mixture. The mixture was then ball-milled, dried, ground, and sieved to obtain powder A.
[0012] (2) Powder A is calcined, and then subjected to preliminary grinding, ball milling, drying, re-grinding and sieving to obtain powder B;
[0013] (3) Powder B is added to the binder and mixed evenly. After grinding, drying and sieving, powder C is obtained.
[0014] (4) The powder C is pressed into blocks and then subjected to cold isostatic pressing and sintering to obtain a negative temperature coefficient thermistor ceramic material;
[0015] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with platinum paste on both sides, and after drying and electrode sintering, aluminum-doped high-temperature thermistor material is obtained.
[0016] In some implementations, step (1) includes one or more of the following features:
[0017] (11) The ball milling specifically involves: horizontally ball milling the mixture with zirconia ball milling beads and anhydrous ethanol medium for 24 hours;
[0018] (12) The Dv50 particle size of the powder A is <1.0μm.
[0019] In some implementations, step (2) includes one or more of the following features:
[0020] (21) The Dv50 particle size of powder B is <1.2 μm;
[0021] (22) The calcination temperature of powder A is 750~850℃;
[0022] (23) The calcination time of powder A is 1~2 h.
[0023] In some implementations, step (3) includes one or more of the following features:
[0024] (31) The Dv50 particle size of the powder C is <1.2 μm;
[0025] (32) The adhesive is an aqueous solution of PVA or an aqueous solution of PVB.
[0026] In some implementations, step (3) further includes one or more of the following features:
[0027] (321) The mass of the binder is 10-20% of the mass of powder B;
[0028] (322) The mass fraction of the adhesive is 1~3.5%;
[0029] (323) The molecular weight of the PVA or PVB is 80,000 to 100,000.
[0030] In some implementations, step (4) includes one or more of the following features:
[0031] (41) In the briquetting process, powder C is pre-pressed into round discs at a pressure of 150~250 MPa and the holding time is 3~5 min;
[0032] (42) The pressure of the cold isostatic pressing is 200~300 MPa, and the holding time is 3~5 min;
[0033] (43) The sintering temperature is 1350~1470℃;
[0034] (44) The sintering time is 3~6 h.
[0035] In some implementations, step (5) includes one or more of the following features:
[0036] (51) The drying temperature is 100~150℃;
[0037] (52) The sintering temperature of the electrode is 1100~1300℃;
[0038] (53) The heating rate for electrode sintering is 8~12℃ / min;
[0039] (54) The holding time for electrode sintering is 15~25 min;
[0040] (55) The sintering temperature of the platinum paste is 1150~1200℃.
[0041] A third aspect of the present invention provides an aluminum-doped high-temperature thermistor material as described above, and / or an aluminum-doped high-temperature thermistor material prepared by the preparation method described above, for use in high-temperature thermistors.
[0042] The beneficial effects of this invention are as follows:
[0043] This invention utilizes B-position Al 3+ Doping modulates the electrical properties of thermosensitive ceramic materials, with Al at the B site. 3+Doping transforms the ceramic phase structure from MgMn2O4 to the high-temperature resistant MgAl2O4, increasing sintering density and thus improving the consistency of the B value over a wide temperature range and the long-term stability of the thermistor. Furthermore, the thermistor material described in this invention exhibits a significant negative temperature resistivity characteristic in the temperature range of 25℃ to 1000℃. The material system demonstrates stable electrical properties, exhibits good linearity in the lnρ-1 / T curve of its resistance-temperature characteristics, and has adjustable B and ρ values, making it suitable for manufacturing thermistors used in medium- and high-temperature applications. Attached Figure Description
[0044] The embodiments of this invention are not limited to the drawings described below, which are only some embodiments of this invention. Those skilled in the art can obtain drawings of other embodiments based on the content of this invention.
[0045] Figure 1 Mg(Al) in Example 1 of this invention 0.2 Mn 0.8 Temperature resistance characteristic curve of LnR-1000 / T for 2O4.
[0046] Figure 2 Mg(Al) in Example 2 of this invention 0.4 Mn 0.6 Temperature resistance characteristic curve of LnR-1000 / T for 2O4.
[0047] Figure 3 Mg(Al) in Example 3 of this invention 0.6 Mn 0.4 Temperature resistance characteristic curve of LnR-1000 / T for 2O4.
[0048] Figure 4 Mg(Al) in Example 3 of this invention 0.6 Mn 0.4 XRD patterns of 2O4 before and after aging.
[0049] Figure 5 Mg(Al) in Example 4 of this invention 0.8 Mn 0.2 Temperature resistance characteristic curve of LnR-1000 / T for 2O4.
[0050] Figure 6 The image shows the XRD patterns of MgMn2O4 before and after aging in Comparative Example 1 of this invention.
[0051] Figure 7 The LnR-1000 / T resistance temperature characteristic curve of MgMn2O4 in Comparative Example 1 of this invention is shown.
[0052] Figure 8 Mg(Al) in Example 3 of this invention 0.6Mn 0.4 Comparison of aging performance between MgMn2O4 and MgMn2O4 in Comparative Example 1. Detailed Implementation
[0053] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0054] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.
[0055] In this invention, numerical ranges are involved. Unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe features or characteristics, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included.
[0056] This invention provides an aluminum-doped high-temperature thermistor material, which uses alumina, manganese dioxide, and magnesium carbonate as raw materials and has the chemical formula Mg(Al) x Mn 1-x )2O4, where x satisfies: 0.2≤x≤0.8.
[0057] This invention utilizes B-position Al 3+ Doping modulates the electrical properties of thermosensitive ceramic materials, with Al at the B site. 3+ Doping transforms the ceramic phase structure from MgMn2O4 to the high-temperature resistant MgAl2O4, increasing sintering density and thus improving the consistency of the B value over a wide temperature range and the long-term stability of the thermistor. Furthermore, the thermistor material described in this invention exhibits a significant negative temperature resistivity characteristic in the temperature range of 25℃ to 1000℃. The material system demonstrates stable electrical properties, exhibits good linearity in the lnρ-1 / T curve of its resistance-temperature characteristics, and has adjustable B and ρ values, making it suitable for manufacturing thermistors used in medium- and high-temperature applications.
[0058] It should be noted that the high-temperature resistant spinel structure is MgAl2O4, while the aluminum-doped high-temperature thermistor material described in this invention has a structure of Mg(Mn,Al)2O4, where Mg is at the A site and a mixture of Mn and Al is at the B site. Al is dissolved into the B site of MgMn2O4, forming a single MgAl2O4 structure. Furthermore, because Mn is at the B site, the weakening of aging properties caused by the easier ion rearrangement (AB site mixing) that occurs when Mn is at the A site is avoided.
[0059] This invention uses Al for doping without adding other variable-valence ions such as Fe, thus avoiding performance fluctuations caused by multiple variable-valence ions (Mn and Fe), which is beneficial for large-scale production in practical applications. Furthermore, by not using the variable-valence ion Fe and controlling the position of Mn, this invention helps improve the aging stability of the material.
[0060] In some implementations, x satisfies: 0.2 ≤ x ≤ 0.8, and x can be, for example, a range of 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or any combination thereof.
[0061] In some implementations, x satisfies: 0.4 ≤ x ≤ 0.6.
[0062] In some embodiments, the crystal structure of the aluminum-doped high-temperature thermistor material is a spinel structure.
[0063] In some embodiments, the aluminum-doped high-temperature thermistor material has a measurement temperature range of 25~1000℃ and a thermistor constant B. 25 / 1000 The K value is 6137~6477 K, and the resistivity at 25℃ is 2.3×10⁻⁶. 7 ~6.2×10 7 Ω·cm.
[0064] This invention provides a method for preparing an aluminum-doped high-temperature thermistor material, comprising the following steps:
[0065] (1) According to Mg(Al) x Mn 1-x Alumina, manganese dioxide, and magnesium carbonate were weighed out and mixed evenly in a molar ratio of 0.2 ≤ x ≤ 0.8 to obtain a mixture. The mixture was then ball-milled, dried, ground, and sieved to obtain powder A.
[0066] (2) Powder A is calcined, and then subjected to preliminary grinding, ball milling, drying, re-grinding and sieving to obtain powder B;
[0067] (3) Powder B is added to the binder and mixed evenly. After grinding, drying and sieving, powder C is obtained.
[0068] (4) The powder C is pressed into blocks and then subjected to cold isostatic pressing and sintering to obtain a negative temperature coefficient thermistor ceramic material;
[0069] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides, and after drying and electrode sintering, aluminum-doped high temperature thermistor material is obtained.
[0070] In some embodiments, in step (1), the ball milling specifically involves: horizontally ball milling the mixture with zirconia ball milling beads and anhydrous ethanol medium for 24 hours.
[0071] In some embodiments, in step (1), the Dv50 particle size of powder A is <1.0 μm.
[0072] In some embodiments, in step (2), the Dv50 particle size of the powder B is <1.2 μm.
[0073] In some embodiments, in step (2), the calcination temperature of powder A is 750~850℃, for example, it can be a range of 750℃, 760℃, 780℃, 800℃, 820℃, 850℃ or any combination thereof.
[0074] In some embodiments, in step (2), the calcination time of powder A is 1 to 2 hours, for example, it can be a range of 1 hour, 1.2 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.8 hours, 2 hours or any combination thereof.
[0075] In some embodiments, in step (3), the Dv50 particle size of the powder C is <1.2 μm.
[0076] In some embodiments, in step (3), the adhesive is an aqueous PVA solution or an aqueous PVB solution.
[0077] In some embodiments, the mass of the binder is 10-20% of the mass of powder B, for example, it can be a range of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any combination thereof. If the binder content is too low, cracking is likely during tableting; if the binder content is too high, granulation will cause agglomeration, leading to tablet cracking. Therefore, by controlling the quality of the binder, this invention helps to reduce the risk of preform cracking during tableting, improve the molding yield, and ensure the structural integrity and performance stability of the final thermistor.
[0078] In some embodiments, the adhesive has a mass fraction of 1 to 3.5%, for example, it may be a range of 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, or any combination thereof.
[0079] In some embodiments, the molecular weight of the PVA or PVB is 80,000 to 100,000, for example, it can be a range of 80,000, 85,000, 90,000, 95,000, 100,000 or any combination thereof.
[0080] In some embodiments, in step (4), the powder C is pre-pressed into a disc at a pressure of 150~250 MPa during the briquetting process, and the holding time is 3~5 min.
[0081] In some embodiments, the pressure during the molding of the briquette is 150~250 MPa, for example, it can be a range of 150MPa, 160MPa, 180MPa, 200MPa, 220MPa, 240MPa, 250MPa or any combination thereof.
[0082] In some embodiments, the pressure holding time is 3 to 5 minutes, for example, it can be a range of 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes or any combination thereof.
[0083] In some embodiments, the diameter Φ of the disc is 10~15 mm and the thickness is 0.5~1.5 mm.
[0084] In some embodiments, in step (4), the pressure of the cold isostatic pressing is 200~300 MPa, for example, it can be a range of 200MPa, 220MPa, 240MPa, 250MPa, 260MPa, 280MPa, 300MPa or any combination thereof.
[0085] In some implementations, in step (4), the pressure holding time is 3-5 min, for example, it can be a range of 3 min, 3.5 min, 4 min, 4.5 min, 5 min or any two of them.
[0086] In this invention, if the pressure of cold isostatic pressing is too high, the green body is prone to cracking; if the pressure is too low, the green body will lack density; if the holding time is too long, it will waste time; if the holding time is too short, the central part of the ceramic will be difficult to densify. Therefore, this invention controls the pressure and holding time of cold isostatic pressing, which is beneficial to obtaining a ceramic green body with a uniform and dense structure, thereby improving the high-temperature stability of the material.
[0087] In some embodiments, the sintering temperature in step (4) is 1350~1470°C, for example, it can be a range of 1350°C, 1360°C, 1380°C, 1400°C, 1420°C, 1440°C, 1450°C, 1470°C or any combination thereof.
[0088] In some implementations, the sintering time in step (4) is 3 to 6 hours, for example, it can be a range of 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours or any combination thereof.
[0089] In this invention, if the sintering temperature is too low or the sintering time is too short, the sintering will not be dense enough, resulting in voids and affecting performance. If the sintering temperature is too high or the sintering time is too long, abnormal grain growth will occur, further affecting material properties. Therefore, this invention, by controlling the sintering temperature and time, facilitates the production of a thermistor ceramic preform with uniform grain growth and a dense structure. This ensures the purity of the spinel phase structure and avoids the negative impact of pores and abnormally grown grains on the electrical properties of the material, ultimately improving the performance stability and service life of the thermistor.
[0090] In some embodiments, the drying temperature in step (5) is 100~150°C, for example, it can be a range of 100°C, 11°C, 120°C, 130°C, 140°C, 150°C or any combination thereof.
[0091] In some embodiments, in step (5), the electrode sintering temperature is 1100~1300℃, for example, it can be a range of 1100℃, 1150℃, 1200℃, 1250℃, 1300℃ or any combination thereof.
[0092] In some embodiments, in step (5), the heating rate of the electrode sintering is 8~12℃ / min, for example, it can be a range of 8℃ / min, 9℃ / min, 10℃ / min, 11℃ / min, 12℃ / min or any combination thereof.
[0093] In some embodiments, in step (5), the holding time for electrode sintering is 15 to 25 min, for example, it can be a range of 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min or any combination thereof.
[0094] In some embodiments, in step (5), the sintering temperature of the high-temperature platinum paste is 1150~1200℃, and it can be used for a long time at 800~900℃.
[0095] This invention provides an aluminum-doped high-temperature thermistor material as described above, and / or the application of the aluminum-doped high-temperature thermistor material prepared by the above-described preparation method in high-temperature thermistors.
[0096] In the following embodiments, unless otherwise specified, all the raw materials of the present invention are commercially available or prepared according to conventional methods in the art.
[0097] Example 1
[0098] This embodiment discloses a method for preparing an aluminum-doped high-temperature thermistor material, including the following steps:
[0099] (1) Weigh 55.32g of magnesium carbonate (MgCO3), 13.38g of aluminum oxide (Al2O3), and 91.30g of manganese dioxide (MnO2), respectively, and mix them evenly to obtain a mixture. Then, put the mixture and grinding beads into a 2000ML polyethylene ball mill jar, and add 96g of anhydrous ethanol as a medium for horizontal ball milling for 24 hours. The grinding beads include 190g of zirconia grinding beads with a diameter of 6mm and 220g of zirconia grinding beads with a diameter of 3mm. After drying, grind and sieve the powder in an agate mortar to obtain powder A, with a Dv50 particle size of powder A <1.0μm.
[0100] (2) Powder A was calcined at 800℃ for 2 hours, then pre-ground in an agate mortar and horizontally ball-milled for 24 hours. After drying, it was ground again in an agate mortar and sieved to obtain powder B. The Dv50 particle size of powder B is <1.2μm.
[0101] (3) Powder B is added to PVA aqueous solution and mixed evenly. The mass of PVA aqueous solution is 15% of the mass of powder B, and the mass fraction of PVA aqueous solution is 3%. Then, it is ground in an agate mortar and dried. After grinding again, it is sieved to obtain powder C. The Dv50 particle size of powder C is <1.2μm.
[0102] (4) Powder C is pre-pressed into a circular piece with a diameter of Φ12 mm and a thickness of 1 mm at a pressure of 200 MPa for 5 min. The formed block material is then subjected to cold isostatic pressing at a pressure of 300 MPa for 3 min and then sintered at 1350℃ for 5 h to obtain a negative temperature coefficient thermistor ceramic material.
[0103] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides and dried at 150℃. Then, the electrode is sintered at 1200℃ for 20 min at a heating rate of 10℃ / min to obtain aluminum-doped high temperature thermistor material.
[0104] In this embodiment, the chemical formula of the aluminum-doped high-temperature thermistor material is Mg(Al) 0.2 Mn 0.8 )2O4, the measurement temperature range is 25~1000 ℃, and the thermistor constant is B. 25 / 1000 =6277 K, resistivity at 25 ℃ is 2.32×10 7Ω·cm. After Al doping at the B site, the aluminum-doped high-temperature thermistor material exhibits stable structure and does not precipitate oxide particles after high-temperature aging; this demonstrates that the prepared aluminum-doped high-temperature thermistor material possesses excellent high-temperature stability.
[0105] Example 2
[0106] This embodiment discloses a method for preparing an aluminum-doped high-temperature thermistor material, including the following steps:
[0107] (1) Weigh 58.80 g of magnesium carbonate, 28.44 g of aluminum oxide, and 72.76 g of manganese dioxide, respectively, and mix them evenly to obtain a mixture. Then, put the mixture and grinding beads into a 2000 mL polyethylene ball mill jar, and add 96 g of anhydrous ethanol as a medium for horizontal ball milling for 24 hours. The grinding beads include 190 g of 6 mm diameter zirconia grinding beads and 220 g of 3 mm diameter zirconia grinding beads. After drying, grind and sieve the powder in an agate mortar to obtain powder A, with a Dv50 particle size of <1.0 μm.
[0108] (2) Powder A was calcined at 800℃ for 2 hours, then pre-ground in an agate mortar and horizontally ball-milled for 24 hours. After drying, it was ground again in an agate mortar and sieved to obtain powder B. The Dv50 particle size of powder B is <1.2μm.
[0109] (3) Powder B is added to PVA aqueous solution and mixed evenly. The mass of PVA aqueous solution is 15% of the mass of powder B, and the mass fraction of PVA aqueous solution is 3%. Then, it is ground in an agate mortar and dried. After grinding again, it is sieved to obtain powder C. The Dv50 particle size of powder C is <1.2μm.
[0110] (4) Powder C is pre-pressed into a circular sheet with a diameter of Φ12 mm and a thickness of 1 mm at a pressure of 200 MPa for 5 min. The formed block material is then subjected to cold isostatic pressing at a pressure of 200 MPa for 5 min and then sintered at 1360℃ for 5 h to obtain a negative temperature coefficient thermistor ceramic material.
[0111] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides and dried at 150℃. Then, the electrode is sintered at 1200℃ for 20 min at a heating rate of 10℃ / min to obtain aluminum-doped high temperature thermistor material.
[0112] In this embodiment, the chemical formula of the aluminum-doped high-temperature thermistor material is Mg(Al) 0.4 Mn 0.6 )2O4, the measurement temperature range is 25~1000 ℃, and the thermistor constant is B. 25 / 1000=6337 K, resistivity at 25 ℃ is 2.80×10 7 Ω·cm. After Al doping at the B site, the aluminum-doped high-temperature thermistor material exhibits stable structure and does not precipitate oxide particles after high-temperature aging; this demonstrates that the prepared aluminum-doped high-temperature thermistor material possesses excellent high-temperature stability.
[0113] Example 3
[0114] This embodiment discloses a method for preparing an aluminum-doped high-temperature thermistor material, including the following steps:
[0115] (1) Weigh 62.73 g of magnesium carbonate, 45.52 g of aluminum oxide, and 51.75 g of manganese dioxide, respectively, and mix them evenly to obtain a mixture. Then, put the mixture and grinding beads into a 2000 mL polyethylene ball mill jar, and add 96 g of anhydrous ethanol as a medium for horizontal ball milling for 24 hours. The grinding beads include 190 g of zirconia grinding beads with a diameter of 6 mm and 220 g of zirconia grinding beads with a diameter of 3 mm. After drying, grind and sieve the powder in an agate mortar to obtain powder A, with a Dv50 particle size of <1.0 μm.
[0116] (2) Powder A was calcined at 800℃ for 2 hours, then pre-ground in an agate mortar and horizontally ball-milled for 24 hours. After drying, it was ground again in an agate mortar and sieved to obtain powder B. The Dv50 particle size of powder B is <1.2μm.
[0117] (3) Powder B is added to PVA aqueous solution and mixed evenly. The mass of PVA aqueous solution is 15% of the mass of powder B, and the mass fraction of PVA aqueous solution is 3%. Then, it is ground in an agate mortar and dried. After grinding again, it is sieved to obtain powder C. The Dv50 particle size of powder C is <1.2μm.
[0118] (4) Powder C is pre-pressed into a circular piece with a diameter of Φ12 mm and a thickness of 1 mm at a pressure of 200 MPa for 5 min. The formed block material is then subjected to cold isostatic pressing at a pressure of 300 MPa for 3 min and then sintered at 1370℃ for 5 h to obtain a negative temperature coefficient thermistor ceramic material.
[0119] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides and dried at 150℃. Then, the electrode is sintered at 1200℃ for 20 min at a heating rate of 10℃ / min to obtain aluminum-doped high temperature thermistor material.
[0120] In this embodiment, the chemical formula of the aluminum-doped high-temperature thermistor material is Mg(Al) 0.6 Mn 0.4)2O4, the measurement temperature range is 25~1000 ℃, and the thermistor constant is B. 25 / 1000 =6359 K, resistivity at 25 ℃ is 4.67×10 7 Ω·cm. After Al doping at the B site, the aluminum-doped high-temperature thermistor material exhibits stable structure and does not precipitate oxide particles after high-temperature aging; this demonstrates that the prepared aluminum-doped high-temperature thermistor material possesses excellent high-temperature stability.
[0121] Example 4
[0122] This embodiment discloses a method for preparing an aluminum-doped high-temperature thermistor material, including the following steps:
[0123] (1) Weigh 67.22g of magnesium carbonate, 65.04g of aluminum oxide, and 27.74g of manganese dioxide, respectively, and mix them evenly to obtain a mixture. Then, put the mixture and grinding beads into a 2000ml polyethylene ball mill jar, and add 96g of anhydrous ethanol as a medium for horizontal ball milling for 24 hours. The grinding beads include 190g of 6mm diameter zirconia grinding beads and 220g of 3mm diameter zirconia grinding beads. After drying, grind and sieve the powder in an agate mortar to obtain powder A, with a Dv50 particle size of <1.0μm.
[0124] (2) Powder A was calcined at 800℃ for 2 hours, then pre-ground in an agate mortar and horizontally ball-milled for 24 hours. After drying, it was ground again in an agate mortar and sieved to obtain powder B. The Dv50 particle size of powder B is <1.2μm.
[0125] (3) Powder B is added to PVA aqueous solution and mixed evenly. The mass of PVA aqueous solution is 15% of the mass of powder B, and the mass fraction of PVA aqueous solution is 3%. Then, it is ground in an agate mortar and dried. After grinding again, it is sieved to obtain powder C. The Dv50 particle size of powder C is <1.2μm.
[0126] (4) Powder C is pre-pressed into a circular sheet with a diameter of Φ12 mm and a thickness of 1 mm at a pressure of 200 MPa for 5 min. The formed block material is then subjected to cold isostatic pressing at a pressure of 300 MPa for 3 min and then sintered at 1380℃ for 5 h to obtain a negative temperature coefficient thermistor ceramic material.
[0127] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides and dried at 150℃. Then, the electrode is sintered at 1200℃ for 20 min at a heating rate of 10℃ / min to obtain aluminum-doped high temperature thermistor material.
[0128] In this embodiment, the chemical formula of the aluminum-doped high-temperature thermistor material is Mg(Al) 0.8Mn 0.2 )2O4, the measurement temperature range is 25~1000 ℃, and the thermistor constant is B. 25 / 1000 =6415 K, resistivity at 25 ℃ is 6.29 × 10⁻⁶ 7 Ω·cm. After Al doping at the B site, the aluminum-doped high-temperature thermistor material exhibits stable structure and does not precipitate oxide particles after high-temperature aging; this demonstrates that the prepared aluminum-doped high-temperature thermistor material possesses excellent high-temperature stability.
[0129] Comparative Example 1
[0130] This comparative example discloses a method for preparing a high-temperature thermistor material, including the following steps:
[0131] (1) Weigh 52.24 g of magnesium carbonate and 107.76 g of manganese dioxide, mix them evenly to obtain a mixture; then put the mixture and grinding beads into a 2000 mL polyethylene ball mill jar, and add 96 g of anhydrous ethanol as a medium for horizontal ball milling for 24 hours. The grinding beads include 190 g of 6 mm diameter zirconia grinding beads and 220 g of 3 mm diameter zirconia grinding beads. After drying, grind and sieve in an agate mortar to obtain powder A, with a Dv50 particle size of <1.0 μm.
[0132] (2) Powder A was calcined at 800℃ for 2 hours, then pre-ground in an agate mortar and horizontally ball-milled for 24 hours. After drying, it was ground again in an agate mortar and sieved to obtain powder B. The Dv50 particle size of powder B is <1.2μm.
[0133] (3) Powder B is added to PVA aqueous solution and mixed evenly. The mass of PVA aqueous solution is 15% of the mass of powder B, and the mass fraction of PVA aqueous solution is 3%. Then, it is ground in an agate mortar and dried. After grinding again, it is sieved to obtain powder C. The Dv50 particle size of powder C is <1.2μm.
[0134] (4) Powder C is pre-pressed into a circular sheet with a diameter of Φ12 mm and a thickness of 1 mm at a pressure of 200 MPa for 5 min. The formed block material is then subjected to cold isostatic pressing at a pressure of 300 MPa for 3 min and then sintered at 1380℃ for 5 h to obtain a negative temperature coefficient thermistor ceramic material.
[0135] (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with high temperature platinum paste on both sides and dried at 150℃. Then, the electrode is sintered at 1200℃ for 20 min at a heating rate of 10℃ / min to obtain the high temperature thermistor material.
[0136] In this comparative example, the chemical formula of the high-temperature thermistor material is MgMn2O4, the measurement temperature range is 25~1000 ℃, and the thermistor constant is B. 25 / 1000 =5864 K, resistivity at 25 ℃ is 1.13×10 7 Ω·cm.
[0137] Comparative Example 2
[0138] The difference from Example 1 is that in step (1), 53.74g of magnesium carbonate, 6.499g of aluminum oxide and 99.76g of manganese dioxide are weighed and mixed evenly to obtain a mixture.
[0139] The chemical formula of the aluminum-doped high-temperature thermistor material prepared in this comparative example is Mg(Al) 0.1 Mn 0.9 )2O4.
[0140] Comparative Example 3
[0141] The difference from Example 1 is that in step (1), 69.72g of magnesium carbonate, 75.89g of aluminum oxide and 14.38g of manganese dioxide are weighed and mixed evenly to obtain a mixture.
[0142] The chemical formula of the aluminum-doped high-temperature thermistor material prepared in this comparative example is Mg(Al) 0.9 Mn 0.1 )2O4.
[0143] Comparative Example 4
[0144] The difference from Example 1 is that in step (1), equimolar amounts of Fe are used to replace Al. 52.83g of magnesium carbonate, 20.01g of iron oxide and 87.16g of manganese dioxide are weighed and mixed evenly to obtain a mixture.
[0145] The performance parameters of the aluminum-doped high-temperature thermistor materials prepared in the above embodiments and comparative examples are shown in Table 1.
[0146] Table 1
[0147] Material ρ25 (Ω·cm) <![CDATA[B 25 / 1000 (K)]]> <![CDATA[R 2 ]]> Example 1 <![CDATA[2.32×10 7 ]]> 6277 0.9975 Example 2 <![CDATA[2.80×10 7 ]]> 6337 0.9981 Example 3 <![CDATA[4.67×10 7 ]]> 6359 0.9939 Example 4 <![CDATA[6.29×10 7 ]]> 6415 0.9980 Comparative Example 1 <![CDATA[1.13×10 7 ]]> 5864 0.9997 Comparative Example 2 <![CDATA[2.15×10 7 ]]> 6083 0.9671 Comparative Example 3 <![CDATA[6.84×10 7 ]]> 6772 0.9725 Comparative Example 4 <![CDATA[12.7×10 7 ]]> 4215 0.9549
[0148] Note: ρ25 (Ω·cm) represents the resistivity at room temperature; B 25 / 1000 The B value constant represents the relationship between room temperature and 1000℃; R 2 The linearity of the lnρ-1 / T relationship curve representing the temperature resistance characteristics of a material.
[0149] As shown in Table 1, the aluminum-doped high-temperature thermistor material prepared by this invention has a measurement temperature range of 25~1000℃ and a thermistor constant B. 25 / 1000The K value is 6137~6477 K, and the resistivity at 25℃ is 2.32×10⁻⁶. 7 ~6.29×10 7 Ω·cm.
[0150] By comparing Comparative Example 1 with Examples 1-4, it can be seen that R in Examples 1-4 2 It is basically similar to Comparative Example 1, but the thermistor constant B of Example 1 is different. 25 / 1000 Both the ρ value and the ρ value are higher than those of Comparative Example 1.
[0151] Comparing Comparative Example 2 with Example 1, it can be seen that if the Al doping amount is too low, R 2 The values of B and ρ will all be affected.
[0152] Comparing Comparative Example 3 with Example 1, it can be seen that if the Al doping amount is too high, although the B value and ρ value of the material increase, the R... 2 This deterioration affects the stability of the material.
[0153] Comparing Comparative Example 4 with Example 1, it can be seen that if other elements (such as Fe) are used to replace Al, although the ρ value of the material is higher than that of Example 1, R... 2 Both the B value and the value of the thermosensitive ceramic material are lower than those in Example 1. This indicates that the effects of this invention cannot be achieved by using arbitrary element doping to control the thermosensitive ceramic material.
[0154] from Figure 4 It can be seen that the XRD pattern in Example 3 showed no change before and after aging, indicating that the internal structure was stable.
[0155] from Figure 6 It can be seen that the XRD of Comparative Example 1 showed obvious changes before and after aging, indicating that the internal microstructure had changed and the resistance was unstable.
[0156] from Figure 8 It can be seen that, under the same aging conditions, the resistance of Example 3 is relatively stable with little change, while the resistance of Comparative Example 1 drops sharply.
[0157] In summary, this invention utilizes B-site Al 3+ Doping and regulating thermistor ceramic materials can help improve the stability of the thermistor constant B value in a wide temperature range of 25~1000℃ and its aging stability.
[0158] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. An aluminum-doped high-temperature thermistor material, characterized in that, The material uses alumina, manganese dioxide, and magnesium carbonate as raw materials, and has the chemical formula Mg(Al) x Mn 1-x )2O4, where x satisfies: 0.2≤x≤0.
8.
2. The aluminum-doped high-temperature thermistor material according to claim 1, characterized in that, It also includes one or more of the following features: (a) The x satisfies: 0.4 ≤ x ≤ 0.6; (b) The crystal structure of the aluminum-doped high-temperature thermistor material is a spinel structure; (c) The aluminum-doped high-temperature thermistor material has a measurement temperature range of 25~1000℃ and a thermistor constant B. 25 / 1000 The K value is 6137~6477 K, and the resistivity at 25℃ is 2.3×10⁻⁶. 7 ~6.2×10 7 Ω·cm.
3. The method for preparing aluminum-doped high-temperature thermistor material according to any one of claims 1 to 2, characterized in that, Includes the following steps: (1) According to Mg(Al) x Mn 1-x Alumina, manganese dioxide, and magnesium carbonate were weighed out and mixed evenly in a molar ratio of 0.2 ≤ x ≤ 0.8 to obtain a mixture. The mixture was then ball-milled, dried, ground, and sieved to obtain powder A. (2) Powder A is calcined, and then subjected to preliminary grinding, ball milling, drying, re-grinding and sieving to obtain powder B; (3) Powder B is added to the binder and mixed evenly. After grinding, drying and sieving, powder C is obtained. (4) The powder C is pressed into blocks and then subjected to cold isostatic pressing and sintering to obtain a negative temperature coefficient thermistor ceramic material; (5) The negative temperature coefficient thermistor ceramic material is uniformly coated with platinum paste on both sides, and after drying and electrode sintering, aluminum-doped high-temperature thermistor material is obtained.
4. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 3, characterized in that, Step (1) includes one or more of the following features: (11) The ball milling specifically involves: horizontally ball milling the mixture with zirconia ball milling beads and anhydrous ethanol medium for 24 hours; (12) The Dv50 particle size of the powder A is <1.0μm.
5. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 3, characterized in that, Step (2) includes one or more of the following features: (21) The Dv50 particle size of powder B is <1.2 μm; (22) The calcination temperature of powder A is 750~850℃; (23) The calcination time of powder A is 1~2 h.
6. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 3, characterized in that, Step (3) includes one or more of the following features: (31) The Dv50 particle size of the powder C is <1.2 μm; (32) The adhesive is an aqueous solution of PVA or an aqueous solution of PVB.
7. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 6, characterized in that, Step (3) also includes one or more of the following features: (321) The mass of the binder is 10-20% of the mass of powder B; (322) The mass fraction of the adhesive is 1~3.5%; (323) The molecular weight of the PVA or PVB is 80,000 to 100,000.
8. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 3, characterized in that, Step (4) includes one or more of the following features: (41) In the briquetting process, powder C is pre-pressed into round discs at a pressure of 150~250 MPa and the holding time is 3~5 min; (42) The pressure of the cold isostatic pressing is 200~300 MPa, and the holding time is 3~5 min; (43) The sintering temperature is 1350~1470℃; (44) The sintering time is 3~6 h.
9. The method for preparing the aluminum-doped high-temperature thermistor material according to claim 3, characterized in that, Step (5) includes one or more of the following features: (51) The drying temperature is 100~150℃; (52) The sintering temperature of the electrode is 1100~1300℃; (53) The heating rate for electrode sintering is 8~12℃ / min; (54) The holding time for electrode sintering is 15~25 min; (55) The sintering temperature of the platinum paste is 1150~1200℃.
10. The aluminum-doped high-temperature thermistor material according to any one of claims 1 to 2, and / or the application of the aluminum-doped high-temperature thermistor material prepared by the preparation method according to any one of claims 3 to 9 in high-temperature thermistors.