A method for preparing silicon fertilizer using magnetic separation-mechanical activation synergistic hydrothermal reaction technology of iron tailings

By employing a synergistic technology of magnetic separation for iron removal, mechanical activation, and hydrothermal reaction, the problem of inert silicon conversion in iron tailings has been solved, enabling efficient and low-cost silicon fertilizer preparation, reducing energy consumption and pollution, and yielding significant social, environmental, and economic benefits.

CN123106262APending Publication Date: 2026-11-17ANHUI MAGANG MINING RESOURCES GRP MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611266627.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient to efficiently and cost-effectively convert inert silicon in iron tailings into usable silicon that can be absorbed by plants. Furthermore, high-temperature melting and chemical extraction methods are characterized by high energy consumption, large equipment investment, and the risk of secondary pollution.

Method used

A three-step synergistic technology of magnetic separation for iron removal, mechanical activation and hydrothermal reaction is adopted. Magnetic separation removes iron impurities, mechanical activation improves the reactivity of materials, and combined with alkaline and high-calcium solid waste-based activators, silicon is efficiently converted under hydrothermal conditions.

Benefits of technology

The efficient conversion of silicon in iron tailings was achieved under mild conditions, reducing energy consumption, pollution, and increasing the effective silicon content of silicon fertilizer products, resulting in significant social, environmental, and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106262A_ABST
    Figure CN123106262A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing silicon fertilizer from iron tailings using a magnetic separation-mechanical activation synergistic hydrothermal reaction technology, belonging to the field of high-value-added utilization of solid waste. Iron tailings undergo magnetic separation to remove weakly magnetic iron-containing minerals to increase SiO2 content, and then the silicon-containing minerals are activated through ultrafine grinding. The magnetically separated and mechanically activated iron tailings are mixed with a high-calcium solid waste-based activator and an alkaline activator for a hydrothermal reaction. Finally, after drying and grinding, silicon fertilizer with an effective silicon content of 20%-37% is obtained. This invention solves the problems of low silicon activation efficiency, high energy consumption, and poor product solubility in existing iron tailings silicon fertilizer preparation technologies. This method achieves large-scale, high-value-added utilization of iron tailings, with a simple process flow, low cost, and significant economic and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-value-added utilization of solid waste, specifically, it relates to a method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings. Background Technology

[0002] Iron tailings are the main solid waste generated after iron ore beneficiation. Their storage not only occupies large amounts of land but also poses environmental risks such as dust pollution, heavy metal pollution of soil, and water acidification. my country has a huge stockpile of iron tailings, and its comprehensive utilization rate is low, making it a pressing problem to be solved in achieving the goal of "zero-waste mines." The main chemical components of iron tailings are SiO2, Fe2O3, Al2O3, CaO, and MgO, with SiO2 content typically reaching 35%-65%, representing a potential silicon resource.

[0003] Silicon is a beneficial element for plant growth and development, enhancing crops' resistance to lodging, pests, and diseases, as well as their overall resilience. Silicon fertilizer primarily originates from silicate minerals, but the key lies in ensuring that the silicon element is "available silicon" (i.e., citric acid-soluble silicon that can be absorbed by plants). Silicon in natural minerals or untreated tailings often exists in the form of crystalline silicates (such as quartz and feldspar), which are chemically stable and difficult for plants to directly absorb. Therefore, developing efficient and economical technologies to activate the inert silicon in tailings and convert it into available silicon is crucial for realizing the agricultural resource utilization of iron tailings.

[0004] Currently, the main methods for preparing silicon fertilizer from silicon-containing solid waste include high-temperature melting, high-temperature calcination, and chemical extraction. High-temperature melting / calcination typically occurs at temperatures above 1000℃, as illustrated in CN119080565A, "Method for Preparing Copper Tailings Silicon Fertilizer Using High-Energy Ball Milling Combined with Low-Temperature Calcination Technology." While effective, this method is extremely energy-intensive, requires significant equipment investment, and is prone to secondary pollution, resulting in poor economic efficiency. To address these issues, the hydrothermal method, a technique utilizing a medium-temperature (typically 100-250℃), high-pressure water medium in a closed system, offers a new approach for activating silicates under mild conditions. The hydrothermal environment accelerates mass transfer and reaction processes, potentially enabling efficient silicon dissolution and recombination in a shorter time. However, direct hydrothermal reaction of untreated iron tailings still faces challenges such as low reactivity, the need for high alkali concentrations and temperatures, and unsatisfactory silicon conversion rates. The root cause lies in the complex composition of iron tailings (containing a large amount of iron-phase impurities) and the high crystallinity and strong inertness of silicon minerals. For example, CN117383990A, "Method for Preparing Silicon Fertilizer from High-Silicon Iron Tailings", uses hydrothermal reaction to make the effective silicon content in the silicon fertilizer prepared from iron tailings reach 20-31%, but it has certain limitations because the iron tailings themselves have a high silicon content.

[0005] Therefore, developing a synergistic technology that can specifically remove impurities, efficiently destroy mineral crystal structures, and couple efficient reaction processes is the inevitable direction for achieving low-temperature, rapid, and efficient preparation of high-quality silicon fertilizer from iron tailings. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology based on magnetic separation and mechanical activation of iron tailings. This method achieves efficient and targeted conversion of inert silicon in iron tailings into highly active citrate-soluble silicon through a three-step synergistic process of magnetic separation for iron removal, mechanical activation, and hydrothermal reaction.

[0007] The objective of this invention can be achieved through the following technical solutions: A method for preparing silicon fertilizer using a magnetic separation-mechanical activation synergistic hydrothermal reaction technology for iron tailings includes the following steps: (1) Magnetic separation to remove iron: The iron tailings raw material is subjected to wet magnetic separation to separate the magnetic part (mainly containing magnetite, hematite, etc.) and the non-magnetic part. The non-magnetic part is collected as silicon extraction raw material. This step aims to remove iron oxides that are not beneficial to silicon fertilizer products and may interfere with subsequent reactions in advance, enrich silicon and aluminum components, improve the "grade" of raw materials, and reduce the reagent consumption of subsequent processes. (2) Mechanical activation: The silicon-extracting raw material obtained in step (1) is mechanically ground for 30-180 minutes to make its specific surface area reach 400-800 m². 2 / kg, thereby obtaining activated material; this step significantly increases the specific surface area of ​​the material through the action of high-intensity mechanical force, and generates a large number of lattice defects, amorphization and even nano-sized particles inside the particles, which greatly improves the surface energy and chemical reactivity of the material, creating a kinetic advantage for subsequent hydrothermal reactions under mild conditions. (3) Hydrothermal reaction: The activated material obtained in step (2), alkaline activator, high calcium solid waste-based activator and water are mixed in proportion and hydrothermal reaction is carried out in a closed reactor. After the reaction is completed, solid-liquid separation is carried out to obtain solid product; (4) Post-processing: The solid product obtained in step (3) is dried and ground at 80-120℃ to obtain silicon fertilizer product.

[0008] In a more optimized manner, in step (1), the content of SiO2 in the silicon extraction raw material is 65-75 wt.% and the content of Fe2O3 is 5-15 wt.%.

[0009] In a more optimized manner, in step (3), the alkaline activator is one or more of sodium hydroxide, potassium hydroxide, and calcium oxide; the molar ratio of the alkaline activator to silicon in the activated material is (0.8-1.5):1.

[0010] In a more optimized manner, in step (3), the high-calcium solid waste-based activator is carbide slag or steel slag; the amount of the high-calcium solid waste-based activator added is 5-20 wt. of the activated material.

[0011] In a more optimized manner, in step (3), the temperature of the hydrothermal reaction is 150-220℃ and the reaction time is 2-12h.

[0012] In a more optimized manner, in step (3), the liquid-solid mass ratio of the hydrothermal reaction system is (2-6):1.

[0013] Ideally, the effective silicon content in the silicon fertilizer product is 20-37%.

[0014] Ideally, the content of heavy metals chromium, arsenic, cadmium, mercury, lead and thallium in the iron tailings meets the requirements of the "Limits of Toxic and Hazardous Substances in Fertilizers" (GB 38400-2019).

[0015] The beneficial effects of this invention are: This invention achieves efficient conversion and resource utilization of silicon in iron tailings by creatively integrating three key steps: magnetic separation for iron removal, mechanical activation, and hydrothermal reaction. Magnetic separation, as a pretreatment step, can remove major iron impurities at low cost and effectively purify the silicon source; mechanical activation significantly improves the reactivity of the material, providing a highly active precursor for the hydrothermal process; and the hydrothermal reaction achieves selective dissolution and recombination of silicon under mild conditions. The three processes work synergistically and are indispensable, producing a significant synergistic enhancement effect, thereby achieving a high silicon conversion rate at relatively low temperatures and in a short time.

[0016] The entire process is based on physical and wet chemical processes, eliminating the need for high-temperature melting and significantly reducing energy consumption. The main raw materials used are all solid waste, achieving "waste treatment of waste, turning waste into treasure." Process wastewater can be recycled after simple treatment, and there are no toxic or harmful gas emissions, meeting the requirements of green chemistry and the circular economy. This invention transforms large quantities of stockpiled iron tailings into high-value-added agricultural silicon fertilizer, which not only helps alleviate environmental pressure but also creates economic benefits, possessing significant social, environmental, and industrial application prospects. Attached Figure Description

[0017] The invention will now be further described with reference to the accompanying drawings.

[0018] Figure 1 The XRD pattern of the iron tailings used in Example 1; Figure 2 The XRD pattern of the activated material obtained in step (2) of Example 1 is shown. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] It should be noted that there are no special restrictions on the suppliers of the raw materials used in this invention; the high-silicon iron tailings used are from an iron ore plant in Anhui Province, and the main mineral composition is quartz, montmorillonite, anorthite, and hematite, with a SiO2 content of 60.6 wt.% and an Fe2O3 content of 18.19 wt.%. The iron tailings with a particle size greater than 200 mesh account for 20.29% of the mass, those between 200 and 600 mesh account for 23.34%, and those less than 600 mesh account for 53.57%.

[0021] The contents of heavy metals chromium, arsenic, cadmium, mercury, lead, and thallium in the iron tailings were determined according to the method in "Determination of Arsenic, Cadmium, Chromium, Lead, and Mercury Content in Fertilizers" (GB / T 23349-2020), and were all lower than the limits in "Limits of Toxic and Hazardous Substances in Fertilizers" (GB38400-2019). The test results are shown in Table 1. This confirms that the iron tailings can be used for silicon fertilizer preparation and applied to the soil in the mining area.

[0022] Table 1. Heavy metal content in iron tailings (mg / kg)

[0023] ND: Below the limit of detection (0.0001 mg / L) The steel slag used in this embodiment of the invention was taken from a steel plant in Hebei Province, with a CaO content as high as 50%; the calcium carbide slag was taken from a power plant in Hebei Province, with a CaO content as high as 80%.

[0024] The effective silicon content of the prepared silicon fertilizer was determined according to the effective silicon determination method in the silicon fertilizer industry standard NY / T 797-2004.

[0025] Example 1

[0026] (1) Magnetic separation to remove iron: Take 1 kg of iron tailings (XRD pattern can be found in the image). Figure 1 Wet drum magnetic separator (magnetic field strength 0.3T) was used for weak magnetic separation to separate magnetic iron powder. The tailings after weak magnetic separation were added to a strong magnetic separator, and the magnetic field strength was adjusted to 1T (current 7.1A) for strong magnetic separation to collect the non-magnetic part. After drying, about 720g of silicon extraction raw material was obtained, with its Fe2O3 content reduced to 10.8wt.% and SiO2 content enriched to 71.44wt.%. (2) Mechanical activation: The above silicon-extracting raw materials were placed in a planetary ball mill (ball-to-material mass ratio 6:1, zirconia balls) and dry-milled at 400 rpm for 50 min to obtain a specific surface area of ​​650 m². 2 / kg activated material; XRD pattern (see Figure 2 The data showed that the sharp quartz peaks in the raw materials were significantly broadened and weakened, indicating a decrease in crystallinity and mechanical activation. Furthermore, the peaks of montmorillonite and hematite were significantly weakened, indicating that some iron-containing minerals were removed, resulting in the enrichment of silicon. (3) Hydrothermal reaction: Accurately weigh 5g of activated material, calculate the SiO2 content to be 3.572g, weigh 4.286g of analytical grade sodium hydroxide according to the alkali-silicon molar ratio (NaOH / SiO2) of 1.2:1, and weigh 1g of carbide slag as 20% of the mass of activated iron tailings. Mix the activated iron tailings, NaOH, carbide slag and deionized water (liquid-solid mass ratio 3:1) in a polytetrafluoroethylene beaker for 1min to form a uniform slurry; transfer the slurry to a 50mL stainless steel high-pressure reactor with a polytetrafluoroethylene liner, seal it, place it in an oven, heat it to 180℃, and react at this temperature for 6h. After the reaction is completed, cool it naturally to room temperature, open the reactor, filter the reaction product, wash the solid product with deionized water until the filtrate is neutral (pH≈7). Dry the filter cake in an oven at 105℃ for 12h to obtain the solid product; (4) Post-processing: The dried solid product is gently ground with an agate mortar and passed through a 100-mesh sieve to obtain the silicon fertilizer product.

[0027] Example 2

[0028] (1) Same as step (1) in Example 1, to obtain the same silicon extraction raw material; (2) The mechanical activation conditions were changed to: wet ball milling (adding water of equal mass to the raw material), grinding time 50 min, to obtain a specific surface area of ​​520 m². 2 / kg of activated material, and the remaining steps are the same as step (2) in Example 1. (3) Adjustment of hydrothermal reaction conditions: The alkali-silicon molar ratio was changed to 1.0:1, the liquid-solid mass ratio was changed to 4:1, the reaction temperature was changed to 160℃, the reaction time was changed to 8h, and the remaining steps were the same as step (3) in Example 1, to obtain solid products; (4) The dried solid product is gently ground with an agate mortar and passed through a 100-mesh sieve to obtain the silicon fertilizer product.

[0029] Example 3

[0030] (1) Same as step (1) in Example 1, to obtain the same silicon extraction raw material; (2) Following the same procedure as in Example 1 (2), a specific surface area of ​​650 m² was obtained. 2 / kg activated material; (3) Adjustment of hydrothermal reaction conditions: The solid waste-based activator was changed to steel slag, the reaction temperature was changed to 200℃, the reaction time was changed to 4h, and the remaining steps were the same as step (3) in Example 1, to obtain solid products; (4) The dried solid product is gently ground with an agate mortar and passed through a 100-mesh sieve to obtain the silicon fertilizer product.

[0031] Example 4

[0032] (1) Same as step (1) in Example 1, to obtain the same silicon extraction raw material; (2) Following the same procedure as in Example 1 (2), a specific surface area of ​​650 m² was obtained. 2 / kg activated material; (3) The specific steps are the same as step (3) in Example 1, except that the hydrothermal conditions have an alkali-silicon molar ratio of 0.9:1, the amount of solid waste-based activator is 10%, the temperature is 170℃, and the time is 7h to obtain a solid product; (4) The dried solid product is gently ground with an agate mortar and passed through a 100-mesh sieve to obtain the silicon fertilizer product.

[0033] Comparative Example 1 (No magnetic separation + no mechanical activation) Take 1 kg of iron ore tailings used in Example 1 and crush it directly to 200 mesh (specific surface area 120 m²). 2 / kg), without magnetic separation to remove iron and mechanical activation treatment, directly use the hydrothermal reaction conditions of step (3) of Example 1, and then process according to step (4) of Example 1 to obtain silicon fertilizer product.

[0034] Comparative Example 2 (without mechanical activation) Complete the magnetic separation to remove iron according to step (1) of Example 1 to obtain silicon-extracting raw material. Omit the mechanical activation step and directly use the silicon-extracting raw material to carry out the hydrothermal reaction in step (3) of Example 1 and the post-processing in step (4) to obtain silicon fertilizer product.

[0035] Comparative Example 3 (without magnetic separation) Take the original iron ore tailings used in Example 1, omit the magnetic separation iron removal step, complete the mechanical activation according to step (2) of Example 1, and then carry out the hydrothermal reaction of step (3) and post-processing of step (4) of Example 1 to obtain silicon fertilizer product.

[0036] Comparative Example 4 (without high-calcium solid waste-based activator) Complete the magnetic separation and mechanical activation according to steps (1) and (2) of Example 1. Omit the carbide slag (high calcium solid waste base activator) during the hydrothermal reaction. Keep the other conditions unchanged. Then, complete the post-processing according to step (4) of Example 1 to obtain the silicon fertilizer product.

[0037] Comparative Example 5 Referring to the invention patent CN117383990A "Method for preparing silicon fertilizer using high silicon iron tailings", high silicon iron tailings, calcium hydroxide and calcium carbonate are mixed in a mass ratio of 1:1.5:0.54, and then subjected to ultrasonic treatment. The hydrothermal reaction temperature is 150℃ and the reaction time is 7h. After drying, the silicon fertilizer product is obtained.

[0038] Comparative Example 6 Referring to the invention patent CN119080565A "Method for preparing copper tailings silicon fertilizer using high-energy ball milling and low-temperature calcination technology", fine-grained copper tailings, calcium-containing activator and alkaline flux are mixed in a ratio of 1:0.45:0.25 and then ball-milled. After that, they are calcined at 700℃ for 30 minutes and then ground to obtain silicon fertilizer product.

[0039] Testing experiment: The effective SiO2 content in the silicon fertilizer products obtained in the examples and comparative examples was determined according to the hydrochloric acid extraction method in the standard "NY / T 797-2004 Silicon Fertilizer". The data obtained are shown in Table 2. Table 2. Effective silicon content in silicon fertilizer products prepared under different conditions

[0040] Conclusion: Comparative Example 1 shows that if iron tailings are directly subjected to hydrothermal reaction without magnetic separation and mechanical activation, the silicon conversion rate will be extremely low due to interference from iron impurities and the inertness of the raw material reaction, making it impractical for practical application.

[0041] Comparative Example 2 confirms that although magnetic separation without mechanical activation can remove iron impurities, the hydrothermal reaction efficiency is still not ideal due to insufficient chemical activity of the raw materials, and the silicon conversion rate is less than 40%.

[0042] Comparative Example 3 illustrates that mechanical activation alone, without prior magnetic separation to remove iron, also hinders the efficient enrichment and dissolution of silicon due to the high content of iron-containing minerals.

[0043] Comparative Example 4 further reveals that introducing a solid waste-based activator on the basis of the three-step synergistic process can further improve the conversion efficiency of effective silicon and achieve the synergistic disposal of solid waste.

[0044] Comparative Examples 5 and 6 respectively indicate that existing technologies either rely on high amounts of calcium activators, leading to increased costs, or employ high-temperature calcination processes, resulting in significantly increased energy consumption.

[0045] In contrast, the three-step synergistic process of "magnetic separation for iron removal - mechanical activation - hydrothermal reaction" represented by Examples 1-4 of this invention can achieve a stable silicon conversion rate of over 50% within 4-8 hours under mild conditions of 160-200℃, with a maximum exceeding 60%. This result fully demonstrates the synergistic effect of the process combination of this invention: mechanical activation provides a highly active precursor and reaction driving force for the subsequent hydrothermal reaction, while the hydrothermal process efficiently utilizes this activation energy, achieving efficient directional conversion and recombination of silicon under relatively mild conditions. This results in a higher effective silicon content in silicon fertilizer products while reducing energy consumption and costs.

[0046] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0047] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

Claims

1. A method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings, characterized in that, Includes the following steps: (1) Magnetic separation to remove iron: The iron tailings are subjected to magnetic separation to separate the non-magnetic part as raw material for silicon extraction; (2) Mechanical activation: The silicon-extracting raw material obtained in step (1) is mechanically ground for 30-180 minutes to make its specific surface area reach 400-800 m². 2 / kg, thus obtaining activated material; (3) Hydrothermal reaction: The activated material obtained in step (2), alkaline activator, high calcium solid waste activator and water are mixed in proportion and hydrothermal reaction is carried out in a closed reactor. After the reaction is completed, solid-liquid separation is carried out to obtain solid product; (4) Post-processing: The solid product obtained in step (3) is dried and ground at 80-120℃ to obtain silicon fertilizer product.

2. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings according to claim 1, characterized in that, In step (1), the content of SiO2 in the silicon extraction raw material is 65-75 wt.% and the content of Fe2O3 is 5-15 wt.%.

3. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation and mechanical activation of iron tailings according to claim 1, characterized in that, In step (3), the alkaline activator is one or more of sodium hydroxide, potassium hydroxide, and calcium oxide; the molar ratio of the alkaline activator to silicon in the activated material is (0.8-1.5):

1.

4. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings according to claim 1, characterized in that, In step (3), the high-calcium solid waste-based activator is carbide slag or steel slag; the amount of high-calcium solid waste-based activator added is 5-20 wt. of the activated material.

5. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings according to claim 1, characterized in that, In step (3), the temperature of the hydrothermal reaction is 150-220℃ and the reaction time is 2-12h.

6. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation-mechanical activation of iron tailings according to claim 1, characterized in that, In step (3), the liquid-solid mass ratio of the hydrothermal reaction system is (2-6):

1.

7. The method for preparing silicon fertilizer using a synergistic hydrothermal reaction technology of magnetic separation and mechanical activation of iron tailings according to claim 1, characterized in that, The effective silicon content in the silicon fertilizer product is 20-37%.

Citation Information

Patent Citations

  • Method for preparing silicon fertilizer by using high-silicon iron tailings

    CN117383990A

  • Method for preparing copper tailing silicon fertilizer by utilizing high-energy ball milling and low-temperature calcining technology

    CN119080565A