An organic glassy luminescent material based on 2,4,5-triphenylimidazole derivatives, its preparation method and application

By regulating the molecular structure of 2,4,5-triphenylimidazole derivatives and introducing Cu4I4L2 cluster compounds, a highly transparent and thermally stable organic glass material was prepared. This solved the balance problem between melting and decomposition in organic-inorganic hybrid glass materials, achieving efficient circularly polarized luminescence and reducing preparation costs.

CN123106534APending Publication Date: 2026-11-17FUJIAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611262301.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing organic-inorganic hybrid glass materials are difficult to balance between stable melting and decomposition, and the preparation methods are costly. Furthermore, traditional chiral luminescent materials cannot simultaneously achieve high luminous efficiency and a large asymmetry factor.

Method used

Organic glass-like luminescent materials were prepared by melt doping by controlling the molecular structure of 2,4,5-triphenylimidazole derivatives and introducing Cu4I4L2 cluster compounds. The intermolecular stacking mode was adjusted and host-guest doping was achieved, resulting in high transparency and circularly polarized luminescence.

Benefits of technology

A transparent organic glass material with good thermal stability was prepared, which enabled efficient circularly polarized light emission, reduced the difficulty of preparation, improved glass forming ability and optical transparency, and significantly reduced the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106534A_ABST
    Figure CN123106534A_ABST
Patent Text Reader

Abstract

This invention discloses an organic glass-state luminescent material based on 2,4,5-triphenylimidazole derivatives and its applications, belonging to the field of luminescent material technology. It proposes a series of strategies for constructing functional hybrid glasses based on 2,4,5-triphenylimidazole (TPI) derivatives. By controlling the substituent at the 3-N position (alkyl, aryl, or chiral chain), the intermolecular stacking mode can be adjusted, resulting in transparent and thermally stable bulk glasses. Furthermore, by incorporating the metal halide Cu4I4L2 (L=diphenyl-2-pyridylphosphine) into the glass substrate through melt doping, a uniform glassy state is formed. This effectively solves the problems of existing organic-inorganic hybrid materials, such as difficulty in forming a stable glassy state independently, poor processability, and lack of integrated functions like circularly polarized luminescence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of luminescent materials technology, specifically relating to an organic glass luminescent material based on 2,4,5-triphenylimidazole derivatives, its preparation method, and its application. Background Technology

[0002] Glass, as a typical amorphous solid, plays a vital role in modern photonics and optoelectronics. Traditional glass materials are mainly divided into inorganic glasses and organic glasses. The building blocks of these glass systems are connected by strong chemical bonds such as covalent and ionic bonds. For example, the tetrahedral or triangular building blocks in oxide glasses form a network structure through mixed covalent-ionic bridging; chalcogenide glasses are connected by covalent bonds in multi-coordinate building blocks. Furthermore, organic glasses are typically composed of abundant intramolecular covalent bonds and non-covalently cross-linked molecular chains between molecular chains.

[0003] Inorganic glasses typically require a synthesis temperature of around 1000℃ due to their high lattice formation energy, leading to high energy consumption and safety risks during manufacturing. Although the synthesis temperature of plexiglass is lower than that of inorganic glasses, its lower hardness makes it more susceptible to surface damage. Organic-inorganic hybrid (OIMHS) glasses combine the characteristics of both, providing a broad space for compositional design to control the physicochemical properties of the material. However, two major challenges remain to be overcome. First, organic-inorganic hybrid crystals encompass a wide family of materials, including metal-organic frameworks (MOFs), coordination polymers (CPs), organic-inorganic hybrid perovskites (OIHPs), and metal cluster-based compounds. However, only a few crystal systems in organic-inorganic hybrid systems can undergo a glass transition and form stable glasses [Nature Communications 12 (2021): 5703], and most hybrid crystals cannot achieve the necessary balance between stable melting and decomposition. Second, the preparation method—how to prepare hybrids into a glassy state in a more convenient and cost-effective manner remains a key and ongoing challenge. Summary of the Invention

[0004] To address the problems existing in the prior art, this invention proposes a series of strategies for constructing functional hybrid glasses based on 2,4,5-triphenylimidazole (TPI) derivatives. By controlling the substituents (alkyl, aryl, or chiral chains) at the 3-N position, the intermolecular stacking mode can be adjusted to prepare transparent bulk glasses with good thermal stability. Furthermore, by incorporating the metal halide Cu4I4L2 (L=diphenyl-2-pyridylphosphine) into the glass substrate through melt doping, a uniform glassy state is formed.

[0005] The mechanism of molecular structure regulation and host-guest doping in the preparation of organic composite glass materials in this technical solution is as follows: Firstly, this invention discloses an organic glass-like luminescent material constructed based on 2,4,5-triphenylimidazole derivatives. Regarding the 2,4,5-triphenylimidazole (TPI) derivative, the difference in its glass-forming ability and flexibility is caused by the substituents on the nitrogen atom: as the carbon chain further elongates (C1-C2), the rigidity of the formed glass gradually weakens, eventually transforming into a viscous glass (C4). This difference is due to the difference in molecular configuration: on the one hand, according to classical nucleation theory, the nucleation rate and growth rate of crystals are inversely proportional to the melt viscosity; high viscosity allows for… Effective inhibition of molecular migration is beneficial to glass formation; therefore, structures with stronger intermolecular forces have higher viscosity when molten. On the other hand, molecular motion slows down when cooled below the freezing point. If cooling is fast enough, crystallization can be avoided, and the final molecular rearrangement becomes very slow, making it impossible to fully sample the configuration within the cooling time. Under a certain cooling rate, the more possible configurations of molecules there are, the more difficult it is to form a regular arrangement and crystallize. Therefore, based on the above theoretical basis, this invention studies how to gradually increase the possible configurations of molecules by extending the carbon chain, thereby reducing their crystal formation ability and improving the glass formation ability.

[0006] Secondly, there is the host-guest doping strategy. The Cu4I4L2 cluster compound used in this invention was selected through theoretical calculations. The calculations revealed that the Cu4I4L2 HOMO-LUMO energy levels are located between the energy levels of the organic substrate. This energy level arrangement makes intermolecular charge transfer easier, thus providing a basis for the fusion of the luminescence properties of the two. Therefore, incorporating OIMHs materials into the organic glass matrix can effectively bring in their luminescence properties. At the same time, when a chiral substrate is used, the substrate generates a chiral transfer effect, which makes the originally chiral material have strong circularly polarized luminescence.

[0007] To achieve the purpose of the invention, the following technical solution is provided: This invention discloses an organic glass-like luminescent material based on a 2,4,5-triphenylimidazole derivative, wherein the 2,4,5-triphenylimidazole derivative is selected from one of the following compounds:

[0008] The substituent R is: benzyl, β-phenylethyl, R-α-phenylethyl, or S-α-phenylethyl.

[0009] Furthermore, the preparation method of the 2,4,5-triphenylimidazole derivative is as follows: S1. Weigh benzoyl, benzaldehyde, organic amine (R-NH2), acetic acid, and L-proline. Add the weighed benzoyl, benzaldehyde, organic amine, acetic acid, and L-proline sequentially to a methanol solution to prepare a mixed solution. S2. Heat and stir the mixed solution prepared in S1 to 65°C and keep it at a constant temperature for at least 12 hours. After the reaction is complete, let it cool naturally to room temperature. S3. After cooling, the solvent in the mixed solution is evaporated to obtain the solidified compound, which is then transferred to a liquid chromatography column for purification and separation to obtain a 2,4,5-triphenylimidazole derivative.

[0010] Furthermore, the molar ratio of benzoyl, benzaldehyde, organic amine (R-NH2), acetic acid, and L-proline in S1 is 1:1:(1.2~2):(2~3):(0.3~0.5).

[0011] Furthermore, the mobile phase separated by the liquid chromatography column in S3 is petroleum ether: dichloromethane = 2:1.

[0012] The present invention also discloses a method for preparing an organic glass-like material based on a 2,4,5-triphenylimidazole derivative. The preparation method is as follows: the above-mentioned 2,4,5-triphenylimidazole derivative is placed in a mold and heated to completely melt the material. After melting, it is taken out and allowed to cool naturally at room temperature to obtain the organic glass-like luminescent material.

[0013] This invention also discloses an application of organic glass composite materials prepared from organic glass luminescent materials based on 2,4,5-triphenylimidazole derivatives.

[0014] Furthermore, using the aforementioned organic glass luminescent material based on 2,4,5-triphenylimidazole derivatives as the host and Cu4I4L2 (L=diphenyl-2-pyridinium phosphine) cluster compound as the guest molecule, organic glass composite materials were prepared through host-guest doping.

[0015] Furthermore, the preparation method of the plexiglass composite material is as follows: S1. Add Cu4I4L2 to dichloromethane and stir vigorously until completely dissolved. Then add organic glass luminescent material based on 2,4,5-triphenylimidazole derivative and continue stirring until completely dissolved. S2. Place the solution prepared in S1 at room temperature to allow it to slowly evaporate and precipitate solids, i.e., mixed materials; S3. Place the obtained solid into a mold, place it on a heating table, heat it up to completely melt the material, and after melting, remove it from the heating table and let it cool naturally in the air to obtain the plexiglass composite material.

[0016] Furthermore, the mass ratio of Cu4I4L2 to the organic glass luminescent material based on 2,4,5-triphenylimidazole derivatives is (0.1~0.5):1.

[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention discloses a series of 2,4,5-triphenylimidazole (TPI) derivatives. By systematically adjusting the carbon chain length (from C0 to C4), a structure-activity relationship between molecular structure and glass-forming ability was established, which suppressed recrystallization tendency, improved glass-forming ability (GFA), and screened out a glassy matrix with suitable flexibility. Compared with existing OIMHs crystals that rely on melt extraction and are easily decomposed, the glassy luminescent materials prepared by this invention have isotropy, no grain boundaries, and high optical transparency (visible light transmittance > 90%).

[0018] 2. The molecular structure regulation and host-guest doping strategy provided by this invention prepares a multifunctional organic glass composite material. By adjusting the carbon chain length, introducing chiral groups and physical doping, it effectively solves the problems of existing organic-inorganic hybrid materials, such as difficulty in forming a stable glassy state, poor processability, and lack of integrated functions such as circular polarization luminescence.

[0019] 3. In this invention, by introducing a chiral matrix into the molecular framework, highly efficient circularly polarized luminescence is achieved in the OIMHs-doped glass system, which is significantly higher than the asymmetry factor (g) of existing chiral luminescent materials. lum Small (usually <10) -3 Compared to the present invention, the chiral hybrid glass prepared by the present invention has a higher g content. lum Value can reach 10 -2 With a maximum luminous efficiency of 0.02 and excellent chiral stability, it solves the technical problem that traditional CPL materials cannot achieve both high luminous efficiency and large asymmetry factor.

[0020] 4. In this invention, a physical doping strategy is used to incorporate OIMHs such as Cu4I4L2 clusters into the organic glass matrix. The preparation method is simple. Compared with the reported hybrid glass systems such as ZIF-62 glass, which require high-temperature melting above 1500 °C, this method can obtain large-area bulk glass through melting processing at normal pressure and 180 °C, which significantly reduces the difficulty of material preparation. Attached Figure Description

[0021] Figure 1 The preparation steps of the organic glass composite material prepared according to the present invention are as follows; Figure 2 A schematic diagram illustrating the performance differences of organic compound substrates with different carbon chain lengths prepared in embodiments of the present invention; Figure 3The above are characterization test images of the organic compounds prepared in the embodiments of the present invention; where a is the DSC curve of crystal 1 and the glassy state before and after doping; b is the transmittance of crystal 2 before and after doping; c is the XRD pattern of crystal 2 before and after preparation of the glassy state; d is the emission spectrum before and after doping. Figure 4 The doped circularly polarized emission spectrum and g prepared for embodiments of the present invention lum ; Figure 5 A comparison of the organic ligand with the HOMO-LUMO of Cu4I4L2; Figure 6 The CD spectrum after doping was prepared for an embodiment of the present invention. Detailed Implementation

[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] Unless otherwise specified, all raw materials used in the following examples were purchased commercially.

[0024] Unless otherwise specified, the methods used in the following embodiments are conventional operating methods in the art.

[0025] Example 1 This embodiment provides a synthetic method based on 2,4,5-triphenylimidazole (TPI) derivatives. The synthetic route is as follows:

[0026] Wherein, the substituent R is: 1. benzyl, 2. β-phenylethyl, 3. R-α-phenylethyl, 4. S-α-phenylethyl; The specific synthesis steps are as follows: S1. Weigh benzoyl, benzaldehyde, organic amine (R-NH2), acetic acid and L-proline according to a molar ratio of 1:1:1.5:2:0.3, and add the weighed benzoyl, benzaldehyde, organic amine, acetic acid and L-proline to methanol solution in sequence to prepare a mixed solution. S2. Heat and stir the above mixed solution to 65°C, and keep it at 65°C for 12 hours. After the reaction is complete, let it cool naturally to room temperature. S3. The solvent in the mixed solution after the reaction in S2 is evaporated by rotary evaporator. The product is then transferred to a silica gel column for separation and purification to prepare 2,4,5-triphenylimidazolium derivatives. The mobile phase is petroleum ether: dichloromethane = 2:1.

[0027] The chemical structural formulas of compounds 1-4 synthesized in this embodiment are as follows:

[0028] The selection of carbon chain length on the substituents in the embodiments of the present invention is based on experimental research. In addition to compounds 1-4 prepared in Example 1, based on the above-described synthetic method, the present invention also synthesized 2,4,5-triphenylimidazolium derivatives 5 and 6 with phenyl and phenylbutyl substituents R.

[0029] The properties of the prepared 2,4,5-triphenylimidazole derivatives 1-6 are as follows: Figure 2 As shown in Figures 1-4, the properties of organic substrates prepared from compounds with different carbon chain lengths vary. As the substituent carbon chain changes from C0 to C1, the molecule changes from being difficult to form a glassy state to being easy to form a glassy state. As the carbon chain is further extended (C1-C2), the rigidity of the formed glassy state gradually weakens, and then it transforms into a viscous glassy state (C4).

[0030] Example 2 This embodiment provides a method for preparing an organic glass-like luminescent material based on a 2,4,5-triphenylimidazole (TPI) derivative, comprising the following steps: The 2,4,5-triphenylimidazole (TPI) derivative prepared in Example 1 was placed in a mold, transferred to a heating platform and heated to 180°C to completely melt the material. After melting, the mold was removed from the heating platform and allowed to cool naturally at room temperature to prepare a glassy luminescent material.

[0031] Example 3 This embodiment provides an organic glass composite material, which uses an organic glass luminescent material based on 2,4,5-triphenylimidazolium (TPI) derivatives as the main matrix and dops it with Cu4I4L2 (L=diphenyl-2-pyridinephosphine) clusters to prepare the organic glass composite material. The preparation method of the plexiglass composite material is as follows: S1. Weigh 0.4g of the prepared organic glass luminescent material based on 2,4,5-triphenylimidazole (TPI) derivative and 0.1g of Cu4I4L2 cluster compound (doping concentration 20%). Add 0.1g of Cu4I4L2 to 10mL of dichloromethane and stir vigorously until completely dissolved. Then add 0.4g of the organic glass luminescent material based on 2,4,5-triphenylimidazole (TPI) derivative and continue stirring until completely dissolved. S2. Let the solution prepared in S1 stand at room temperature, allowing the solvent to slowly evaporate and precipitate a solid, i.e., a mixture; S3. Place the solid prepared in S2 into a mold, transfer it to a heating table and heat it to 180°C to completely melt the material. After melting, remove the mold from the heating table and allow it to cool naturally to obtain the plexiglass composite material.

[0032] The preparation method of the doped glass with a glassy matrix composite Cu4I4L2 (L=diphenyl-2-pyridinium phosphine) cluster described in this embodiment is as follows: Figure 1 As shown.

[0033] Performance study: like Figure 3 As shown, the DSC curves of 2,4,5-triphenylimidazolium (TPI) derivative (compound 2) crystal, glassy luminescent material based on 2,4,5-triphenylimidazolium (TPI) derivative (compound 2), and organic glass composite material doped with Cu4I4L2 cluster compounds are displayed. Figure 3 a) Small glass transition peaks (Tg) appeared at 33.4 and 48.8 °C before and after doping, respectively, and the glass transition temperature of the doped sample was higher. This means that doping increases its rigidity, makes chain movement more difficult, and increases the ability to form glass. The multiple crystallization peaks (Tc) in the doping curve indicate that the material is impure. The melting temperatures of the three materials are similar, which means that there is no strong interaction between the dopant and the glass matrix. A comparison of the UV transmittance of crystals based on 2,4,5-triphenylimidazolium (TPI) derivative (compound 2) and crystals based on 2,4,5-triphenylimidazolium (TPI) derivative (compound 2) doped with 20% Cu4I4L2 cluster compounds. Figure 3 b) The doping with Cu4I4L2 cluster compounds reduced the transmittance of the crystal. The transmittance of the initial sample was more than 80% at 400-800 nm, but after doping, the absorption inflection point appeared at around 500 nm, and the colorless and transparent crystal changed to yellow. Images of crystals and glassy powders prepared from 2,4,5-triphenylimidazolium (TPI) derivatives (compound 2) doped with 20% Cu4I4L2 cluster compounds. Figure 3c) When crystallized, sharp peaks can be observed, but when prepared into a glassy state, smooth peaks are observed, indicating that the crystalline phase has completely disappeared and an amorphous glassy state has been formed; The glassy luminescent material based on 2,4,5-triphenylimidazole (TPI) derivative (compound 2) and the glassy luminescent spectrum of the 2,4,5-triphenylimidazole (TPI) derivative (compound 2) doped with 20% Cu4I4L2 cluster compound are shown. The excitation spectrum after doping is basically the same as the emission spectrum before doping. This indicates that there is a very strong energy transfer effect between the organic substrate and the dopant. The luminescence of the glassy matrix is ​​completely converted into the luminescence of the dopant.

[0034] like Figure 4 As shown, the circularly polarized emission spectra and g of 2,4,5-triphenylimidazolium (TPI) derivatives (compounds 3 and 4) doped with 20% Cu4I4L2 cluster compounds are displayed. lum Among them, compounds 3 and 4 exhibit circularly polarized luminescence. Figure 4 a and Figure 4 c, g of compounds 3 and 4 lum After doping, both glass states exhibit good circularly polarized luminescence and relatively high g-values. lum value.

[0035] Figure 5 LUMO-HOMO values ​​for compounds 1-4 and Cu4I4L2, calculated theoretically.

[0036] Figure 6 The CD spectra of plexiglass-like compounds doped with 20% Cu4I4L2 based on 2,4,5-triphenylimidazole (TPI) derivatives (compounds 3 and 4) indicate that compounds 3 and 4 are a pair of standard chiral enantiomers with opposite configurations.

[0037] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. An organic glassy light-emitting material based on 2,4,5-triphenylimidazole derivatives, characterized in that: The 2,4,5-triphenylimidazole derivative is selected from one of the following compounds: The substituent R is: benzyl, β-phenylethyl, R-α-phenylethyl, or S-α-phenylethyl.

2. The organic glassy light emitting material based on 2,4,5-triphenylimidazole derivative according to claim 1, characterized by: The preparation method of the 2,4,5-triphenylimidazole derivative is as follows: S1. Weigh benzoyl, benzaldehyde, organic amine, acetic acid and L-proline, and add the weighed benzoyl, benzaldehyde, organic amine, acetic acid and L-proline to methanol solution in sequence to prepare a mixed solution; S2. Heat and stir the mixed solution to 65°C and keep it at a constant temperature for at least 12 hours. After the reaction is complete, allow it to cool naturally to room temperature. S3. After cooling, the solvent in the mixed solution is evaporated to obtain the solidified compound, which is then transferred to a liquid chromatography column for purification and separation to obtain a 2,4,5-triphenylimidazole derivative.

3. The organic glass-like luminescent material based on 2,4,5-triphenylimidazole derivatives as described in claim 1, characterized in that: In step S1, the molar ratio of benzoyl, benzaldehyde, organic amine, acetic acid and L-proline in the mixed solution is 1:1:(1.2~2):(2~3):(0.3~0.5).

4. The organic glass-like luminescent material based on a 2,4,5-triphenylimidazole derivative as described in claim 1, characterized in that: In step S3, the mobile phase separated by the liquid chromatography column is petroleum ether: dichloromethane = 2:

1.

5. A method for preparing an organic glass-like luminescent material based on a 2,4,5-triphenylimidazole derivative, characterized in that, The 2,4,5-triphenylimidazole derivative as described in claim 1 is placed in a mold and heated until the material is completely melted. After melting, it is taken out and allowed to cool naturally at room temperature to obtain an organic glass-like luminescent material.

6. Using the 2,4,5-triphenylimidazole derivative-based plexiglass luminescent material as described in claim 1 to prepare plexiglass composite materials.

7. The application as described in claim 6, characterized in that: Organic glass composite materials were prepared by host-guest doping using organic glass luminescent materials based on 2,4,5-triphenylimidazole derivatives as the host and Cu4I4L2 cluster compounds as guest molecules.

8. The application as described in claim 7, characterized in that, The preparation method of the plexiglass composite material is as follows: S1. Add the Cu4I4L2 cluster compound to dichloromethane and stir vigorously until it is completely dissolved. Then add the organic glass luminescent material based on 2,4,5-triphenylimidazole derivative and continue stirring until it is completely dissolved. S2. Place the solution prepared in S1 at room temperature to allow it to slowly evaporate and precipitate solids, i.e., mixed materials; S3. Place the obtained solid into a mold, heat it to completely melt the material, and after melting, remove it from the heating table and let it cool naturally in the air to obtain the plexiglass composite material.

9. The application as described in claim 8, characterized in that: The mass ratio of Cu4I4L2 cluster compound to organic glass luminescent material based on 2,4,5-triphenylimidazole derivative is (0.1~0.5):1.