Aerated polypropylene compositions exhibiting specific emission characteristics

By using a counter-flow aeration container and treating the polypropylene composition under specific conditions, the problem of high VOC and FOG content in polypropylene materials was solved, resulting in a low-VOC and FOG polypropylene composition suitable for automotive interiors, exhibiting good mechanical and processing properties.

CN123106954APending Publication Date: 2026-11-17BOREALIS AG
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202611305606.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-10-31
Filing Date
2019-10-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively reduce the content of volatile organic compounds (VOCs) and semi-volatile organic condensables (FOGs) in polypropylene materials while maintaining their mechanical and processing properties. This is particularly true in automotive interior applications, where the increased low molecular weight of the material leads to higher VOC and FOG levels, impacting passenger health and causing windshield fogging.

Method used

By aerating polypropylene compositions using an aeration container with counter-current gas flow, combined with specific Reynolds number and temperature conditions, volatile substances in the polymer are removed. A lubricant is added before aeration to ensure its uniform distribution and avoid subsequent additions, resulting in a polypropylene composition with low VOC and FOG.

Benefits of technology

Significant reductions in VOCs and FOGs in polypropylene compositions were achieved, while maintaining the material's mechanical and processing properties. This ensured that the material was easily released from the mold after injection molding, reduced the risk of windshield fogging, and improved the material's scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106954A_ABST
    Figure CN123106954A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for providing a polypropylene composition, the method comprising: blending the components in the presence of an additive to obtain a blend as a raw material for a polypropylene composition; and aerating the raw material for the polypropylene composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application filed on October 22, 2019, with application number 201980071549.0 (international application number PCT / EP2019 / 078707) and entitled "Aerated polypropylene composition exhibiting specific emission characteristics". Technical Field

[0002] This invention relates to a polypropylene composition having low volatile organic compounds (VOC, VDA 278, October 2011, China Association of Automobile Manufacturers) and semi-volatile organic condensable compounds (FOG, VDA 278, October 2011). This composition can be used for injection molding to produce molded products for automotive applications. Background Technology

[0003] Polyolefin polymers obtained by solution polymerization typically contain trace amounts of the reaction medium used to carry out the polymerization reaction. Various options for removing volatile organic compounds (VOCs, VDA 278, October 2011) and semi-volatile organic condensables (FOGs, VDA 278, October 2011) from polyolefin polymers are known. These options include using solvents (e.g., water), using steam, and using high-temperature gas streams in a process known as aeration or purging. Examples of commonly used aeration methods can be found in GB 1272778, WO 02 / 088194, WO 2004 / 039848, and US 6,218,504. These documents specifically address the aeration or purging of polyethylene compositions.

[0004] Materials used in automotive interior applications must meet certain specifications, particularly regarding emissions and fogging; these are typically caused by VOCs (VOC, VDA 278, October 2011) and FOGs (FOG, VDA 278, October 2011). This is necessary, on the one hand, to protect passengers from unpleasant odors and sometimes even toxic volatile substances, and on the other hand, to prevent the condensation of medium-molecular-weight oligomers on the windshield. Typical interior formulations are based on a combination of multiphase copolymers, fillers, and additives (slip agents), which are added to obtain further advantageous mechanical properties (including scratch resistance and UV resistance) and to produce materials suitable for injection molding and easily removed from the mold after the injection molding process.

[0005] To obtain polypropylene compounds with specific emission profiles, post-polymerization treatment methods (such as aeration) are often necessary. Developing aeration processes is challenging due to the inherent viscosity of polyolefin polymers and their tendency to coalesce at relatively low temperatures. This results in a limited temperature window for aeration. Polyolefin polymers obtained through solution polymerization typically have high volatile content (VOC, VDA 278, October 2011). Longer aeration times are often required, as these molecules are less volatile and more difficult to remove by definition, and are also important to remove semi-volatile organic compounds (FOG, VDA 278, October 2011). However, to ensure that polyolefin compositions retain their desired properties (e.g., mechanical properties and scratch resistance), it is important to avoid removing or eliminating additives necessary for producing materials with these properties.

[0006] Polyolefin compositions, such as polypropylene compositions that show low emission levels in standard tests (e.g., VDA277 and VDA278), can be broadly classified into two categories:

[0007] The low emission levels are attributed to the polyolefins used in the polymerization process, primarily due to the nature of the catalyst, as well as the purity of the monomers used, and possibly the choice of additives.

[0008] - Polyolefins and polyolefin compositions that undergo a post-purification step during or after blending may involve the use of specific substances (such as carriers or absorbents).

[0009] As discussed in WO2017 / 079246 on automotive applications, industry tends to reduce vehicle weight by decreasing the mass of plastic vehicle components. This reduction in mass is typically achieved by decreasing the wall thickness of the plastic parts. For example, producing thin-walled plastic parts using injection molding requires a sufficiently low viscosity of the component polymer resin to allow the molten resin to flow easily and fill the mold cavity uniformly without excessive injection pressure. Reducing the melt viscosity of the polymer resin requires reducing the molecular weight of the component polymer molecules. However, producing polymer resins with low molecular weight molecules increases the content of volatile organic compounds (VOCs, VDA 278, October 2011) and semi-volatile organic condensables (FOGs, VDA 278, October 2011) in the resin.

[0010] EP2154190 states that polypropylene is a material of choice for many applications. For example, polypropylene is increasingly used in automotive interiors, particularly due to its good processability and customizability. Especially in HVAC (heating, ventilation, and air conditioning) applications, low odor and volatile organic compound (VOC) levels are required to prevent fogging on windshields. This document discusses the use of a 1,3,5-triazine derivative stabilizer in polypropylene compositions to reduce FOG and VOC levels. Such a stabilizer is certainly desirable for recycling purposes.

[0011] WO2017 / 079246 describes a polypropylene-based resin characterized by a VOC content of less than 125 ppm and a FOG content of no more than 500 ppm, which is obtained by obtaining a polypropylene polymer resin without post-polymerization treatment. The examples in this document did not show a significant reduction in FOG.

[0012] EP3260489 describes a polypropylene composition comprising: (A) 60 to 95 wt% of a multiphase polypropylene (HECO), wherein the multiphase polypropylene comprises 10 to 30 wt% of a dispersed phase, the dispersed phase having a comonomer content of 30 to 45 wt%, and the HECO having a melt flow rate of 12 to 200 g / 10 min. The fogging gravimetric of this polypropylene compound is very low. However, this document does not address compounds subjected to aeration treatment. Furthermore, the VOC values ​​obtained in the embodiments of the invention are all higher than 80 μg / g.

[0013] EP2262858 describes a polypropylene polymer characterized by low emissions, high toughness, and good scratch resistance. An exemplary volatile matter level is given as 45 µgC / g (measured according to VDA277), and the VOC (according to VDA278, October 2011) is below 100 µg / hexadecane equivalent. These low levels of volatile matter are achieved through the detailed polymerization process described in this document. However, this document does not specifically focus on compositions obtained by an aeration process.

[0014] WO2014 / 090856 specifically relates to the degassing of powdered polyolefin particles with a nitrogen stream, followed by granulation. However, this document does not mention any information regarding the VOC value (i.e., VOC content value) (VDA 278, October 2011) or FOG value (i.e., FOG content value) of the produced product (VDA 278, October 2011).

[0015] EP3126408 relates to a method for manufacturing a polypropylene material with a target melt flow rate of 10 to 200 g / min, and reducing the FOG value to a preferred approximately 250 μg / g by holding the polymer composition at a high temperature for a sufficient time. This document only speculates on the use of airflow to remove volatiles, but does not discuss the aeration process in the examples section. Furthermore, this document does not address the reduction of VOCs in the polypropylene composition.

[0016] Therefore, none of the aforementioned literature specifically addresses compositions having low levels of VOC (VDA278, October 2011) typically below about 60 μg / g and low levels of FOC (VDA 278, October 2011) typically below about 350 μg / g, wherein the composition contains relatively high levels of slip agents (e.g., erucamide). The present invention also specifically relates to compositions obtained by aeration treatment. Preferably, these compositions contain high levels of "slip agents" (e.g., erucamide); typically, the process is an integrated process; no other slip agents are added to the polypropylene composition after the polypropylene material has been aerated. Articles used in automotive applications require low levels of VOC and FOG because this is important for: on the one hand, protecting passengers from unpleasant or even toxic volatile substances (VOC fraction); on the other hand, preventing the condensation of medium molecular weight oligomers or additives on the windshield (FOG fraction).

[0017] Therefore, the automotive industry requires materials with specific emission characteristics and low VOC and FOG levels. Obtaining such materials using an aeration process is particularly desirable because it is a post-polymerization process that can be used to treat many polymers after polymerization. Summary of the Invention

[0018] This invention provides a propylene composition comprising:

[0019] A semi-volatile organic condensable oligomer (FOG, VDA 278, October 2011) comprising approximately 50 μg / g to approximately 400 μg / g of the total polypropylene composition; and

[0020] Volatile organic compounds (VOC, VDA 278, October 2011) contained less than 80 μg / g of the total polypropylene composition.

[0021] The weight ratio of the semi-volatile organic condensable oligomer to the volatile organic compound is greater than about 5.0.

[0022] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene composition is greater than 10 g / 10 min;

[0023] The flexural modulus of the polypropylene composition (ISO 178, measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996) is from 1000 MPa to 6000 MPa; and

[0024] The total amount of the lubricant is at least 500 ppm.

[0025] The term "composition" may refer to a homopolymer or copolymer, which may optionally contain other components and / or additives.

[0026] The terms "volatile organic compound content" or "VOC content" refer to the toluene equivalent content in a material sample as measured according to the China Association of Automobile Manufacturers (CAAM) recommendation VDA278 (October 2011). Volatile organic compound content is a measure of the emissions from plastic materials (such as low-density plastics), determined by the low molecular weight components (typically carbon chains with a carbon chain length of at most C) in the polymer material. 20 This is caused by alkanes. These low-molecular-weight components can be residual monomers, oligomers, additives, plasticizers, and / or degradation products.

[0027] The term "semi-volatile organic condensable content (FOG, VDA 278, October 2011)" refers to the hexadecane equivalent content in a material sample measured according to the China Association of Automobile Manufacturers (CAAM) recommendation VDA-278 in October 2011. Semi-volatile organic compound content is a measure of emissions from plastic materials, caused by medium molecular weight components (e.g., oligomers) with boiling points in the range of °C. 14 -C 32 Within the range of alkanes.

[0028] As used herein, the term "aeration" or "aeration process" refers to a process or step in which a compound is subjected to an airflow. This process takes place in an aeration container.

[0029] As used herein, the term "aeration gas" refers to any gas suitable for heating to at least 50 °C and for removing volatile organic compounds (VOCs) and semi-volatile organic condensables (FOGs) from polyolefin compositions. Suitable gases include, for example, nitrogen, air, or mixtures thereof. However, any inert gas can be used in principle. For economic reasons, air is the most preferred gas for the method of this invention.

[0030] According to the present invention, by filling with a contact diameter of The Reynolds number of a fluid (gas) flow in a packed bed of particles (m) (where the apparent velocity is...). (m / s) is defined as:

[0031]

[0032] In the formula:

[0033] - Density of aeration gas at operating temperature (kg / m³) 3 );

[0034] - : Dynamic viscosity of aeration gas at operating temperature (kg / m·s);

[0035] - Superficial velocity is defined as follows: ,in, The volumetric flow rate of the aeration gas (m) 3 / s), A is the cross-sectional area (m²) 2 ).

[0036] By definition, diameter (m) should be the median particle size d50 (in meters) obtained by sieve analysis according to ISO 3310 and determination according to ISO 9276-2.

[0037] The laminar flow condition applies to Re=10, and fully turbulent flow begins at Re=2000.

[0038] The Reynolds number (Re) is an important dimensionless quantity in fluid mechanics, used to predict flow patterns under different fluid flow conditions.

[0039] The Reynolds number is used to scale flow conditions that are similar but different in size, such as scaling an aircraft model in a wind tunnel to its full-scale version. The ability to predict turbulence and calculate scaling effects can be used to help predict fluid behavior at larger scales. In other words, when the size (scale) of the equipment in which the flow occurs changes, the Reynolds number can be used to ensure that similar flow conditions are maintained.

[0040] The term “weight flow rate of polypropylene composition” as used in this article refers to the total weight of polypropylene composition flowing into the aeration container per hour.

[0041] As used herein, the term "granule" refers to a polyolefin composition in granular and / or granular material form. Granules or granular materials are typically obtained by pelletizing or granulation. For example, granules can be formed by forcing a polyolefin composition to melt through a die and granulating it using an underwater pelletizer. The granules of this invention can be rectangular, wherein the length of the granule is greater than its width and height.

[0042] "Fatty acid amide" is used to refer to amides formed from fatty acids and amines. These compounds are also called N-acylethanolamines and they contain the functional group RC(O)N(H)CH2CH2OH.

[0043] The term "random" indicates that the comonomers of a propylene copolymer are randomly distributed within the propylene copolymer. The term "random" can be understood according to IUPAC (Basic Terminology of Polymer Science; IUPAC Recommendation 1996).

[0044] There are two types of multiphase propylene copolymers:

[0045] HECO is a multiphase copolymer with polypropylene homopolymer as the matrix phase. Due to their good mechanical properties (especially impact strength), these materials are widely used in a variety of applications, including domestic applications and automotive bumpers.

[0046] - RAHECO is a multiphase copolymer containing a random copolymer of polypropylene as the matrix phase. These materials are commonly used in soft fibers and films.

[0047] Preferably, the present invention provides a polypropylene composition, which can be obtained by:

[0048] In the presence of additives, the following components are blended to obtain a blend:

[0049] - Polypropylene

[0050] - Packing material

[0051] - Lubricant

[0052] - Optional HDPE

[0053] - Optional plastic body

[0054] - Optional pigments;

[0055] The blend is then subjected to a process including the following steps:

[0056] a) Provide an aeration container, said aeration container having:

[0057] - At least one aeration gas inlet;

[0058] - At least one exhaust gas outlet;

[0059] - Inlet of polypropylene composition raw material at the top of the aeration container;

[0060] - The outlet of the polypropylene composition at the bottom of the aeration container;

[0061] The polypropylene composition exists as a packed bed.

[0062] b) Initiate countercurrent flow between the polypropylene composition and the aeration gas;

[0063] c) Perform the following operations:

[0064] - The polypropylene composition feedstock is fed from the top into the aeration vessel, the polypropylene composition feedstock having a volatile organic compound content (VOC, VDA 278, October 2011) greater than about 150 µg / g and a semi-volatile organic condensable content (FOG, VDA 278, October 2011) greater than about 350 µg / g.

[0065] - Aeration gas is fed into the aeration container through at least one inlet at the bottom;

[0066] - Exhaust gas is discharged through the exhaust outlet;

[0067] - The aerated polypropylene composition is discharged through the outlet at the bottom of the aeration container;

[0068] d) Maintain the aeration gas flow for an aeration time of 3 to 96 hours;

[0069] The gas temperature is between 100 ℃ and 140 ℃, and the Reynolds number of the gas flow is between 5 and 150.

[0070] In a preferred aspect of the invention, the blending step includes blending multiphase polypropylene with other polypropylene homopolymers and / or polypropylene copolymers.

[0071] In a preferred aspect of the invention, the polypropylene composition comprises at least 500 ppm of a slip agent, wherein the slip agent is a fatty acid amide. The slip agent is preferably erucamide or oleamide, and most preferably erucamide.

[0072] Preferably, the VDA 277 of the polypropylene composition of the present invention is less than 3, and more preferably less than 1.

[0073] In a preferred aspect of the invention, the atomized weight of the polypropylene composition is less than 1.1, preferably less than 1, and / or the VDA270 is less than 4, preferably less than 3.

[0074] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene composition of the present invention is preferably 5 to 160 g / 10 min, more preferably 8 to 50 g / 10 min, and most preferably 10 to 130 g / 10 min.

[0075] In a preferred aspect of the invention, the flexural modulus of the polypropylene composition (ISO 178, measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996) is from 1000 MPa to 6000 MPa, preferably from 1200 MPa to 5500 MPa, and more preferably from 1300 to 5000 MPa.

[0076] The puncture energy (ISO 6603-2) of the polypropylene composition of the present invention is preferably 3 J to 60 J, more preferably 4 J to 50 J, and most preferably 5 J to 45 J.

[0077] In a preferred aspect of the invention, the polypropylene composition has a melting point of 155°C to 170°C, for example, 160°C to 167°C.

[0078] In a preferred aspect of the invention, the multiphase polypropylene component raw material added to the blend prior to the aeration step is a multiphase propylene copolymer (HECO). The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the multiphase propylene copolymer (HECO) is preferably 5 to 150 g / 10 min, more preferably 10 to 120 g / 10 min. Furthermore, the xylene-soluble content (ISO 6427, 23 °C) of the multiphase propylene copolymer (HECO) is preferably 8 to 30 wt%, more preferably 10 to 25 wt%. Additionally, the total content of ethylene-derived units in the multiphase propylene copolymer (HECO) is preferably 4 wt% to 20 wt%, more preferably 6 wt% to 15 wt% (as determined by NMR).

[0079] In a preferred aspect of the invention, the other polypropylene homopolymer or polypropylene copolymer component raw material added to the blend prior to the aeration step is a polypropylene homopolymer. Optionally, the MFR2 (ISO 1133, 230 °C, 2.16 kg) of this homopolymer is preferably 20 to 160 g / 10 min, preferably 50 to 100 g / 10 min, most preferably 60 to 80 g / 10 min, for example about 75 g / 10 min. Alternatively, the other polypropylene homopolymer or polypropylene copolymer component added to the blend prior to the aeration step can be a polypropylene copolymer. The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene copolymer raw material is preferably 5 g / 10 min to 120 g / 10 min, and / or the xylene-soluble (ISO 16152) content is 8 wt% to 20 wt%, and / or the total content of ethylene-derived units is 4 wt% to 10 wt% (as determined by NMR).

[0080] The polypropylene composition of the present invention preferably contains filler, wherein the filler may be selected from talc, glass and mixtures thereof.

[0081] In a preferred aspect of the invention, the polypropylene composition comprises a plastomer, preferably an ethylene-octene plastomer.

[0082] In a preferred aspect, the polypropylene composition of the present invention comprises a pigment, preferably a black pigment, such as carbon black pigment.

[0083] The polypropylene composition of the present invention is preferably produced by an integrated process, wherein no slip agent is added after the aeration step. Attached Figure Description

[0084] Figure 1 FOG / VOC ratio before and after aeration (based on VDA278, October 2011). Detailed Implementation

[0085] Surprisingly, the aerated polypropylene compositions of the present invention exhibit acceptable levels of VOC and FOG and contain more than 500 ppm of slip agent. This is advantageous because it means that the polypropylene composition is easily released from the mold after the injection molding process. Furthermore, the presence of a slip agent (e.g., erucamide) enhances the scratch resistance of the polypropylene composition. Adding the slip agent to the composition before the aeration process is important because it results in a desired and uniform distribution of the slip agent within the polypropylene composition, whereas compositions in which erucamide is added after the aeration step exhibit a less uniform distribution of the slip agent.

[0086] In a first preferred embodiment of the invention, the polypropylene composition contains greater than 500 ppm of the slip agent erucamide. This embodiment is particularly suitable for polypropylene compositions intended for injection molding because the presence of erucamide ensures that the polypropylene composition does not adhere to the mold walls. This means that the molded product can be easily removed from the mold without leaving any residue, which is important for the molding process.

[0087] In this regard, a first preferred embodiment of the present invention relates to a polypropylene composition comprising:

[0088] The oligomer contains a semi-volatile organic condensable (FOG, VDA278, October 2011) content of 50 µg / g to 400 µg / g of the total polypropylene composition and a volatile organic compound (VOC, VDA 278, October 2011) content of less than 80 μg / g of the total polypropylene composition.

[0089] The weight ratio of the semi-volatile organic condensable to the volatile matter is greater than about 5.0;

[0090] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene composition is greater than 5 g / 10 min;

[0091] The flexural modulus of the polypropylene composition (ISO 178, measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996) is from 1000 MPa to 6000 MPa; and

[0092] The total amount of the slip agent erucamide is at least 500 ppm;

[0093] The polypropylene composition can be obtained as follows:

[0094] In the presence of additives, the following components are blended to obtain a blend:

[0095] - Polypropylene

[0096] - Packing material

[0097] - Lubricant

[0098] - Optional HDPE

[0099] - Optional plastic body

[0100] - Optional pigments;

[0101] The blend is further subjected to a process including the following steps:

[0102] a) Provide an aeration container, said aeration container having:

[0103] - At least one aeration gas inlet;

[0104] - At least one exhaust gas outlet;

[0105] - Inlet of polypropylene composition raw material at the top of the aeration container;

[0106] - The outlet of the polypropylene composition at the bottom of the aeration container;

[0107] The polypropylene composition exists as a packed bed.

[0108] b) Initiate countercurrent flow between the polypropylene composition and the aeration gas;

[0109] c) Perform the following operations:

[0110] - The polypropylene composition feedstock is fed from the top into the aeration container, wherein the volatile organic compound content (VOC, VDA 278, October 2011) of the polypropylene composition feedstock is greater than about 150 µg / g and the semi-volatile organic condensable content (FOG, VDA 278, October 2011) is greater than about 350 µg / g.

[0111] - Aeration gas is fed into the aeration container through at least one inlet at the bottom;

[0112] - Exhaust gas is discharged through the exhaust outlet;

[0113] - The aerated polypropylene composition is discharged through the outlet at the bottom of the aeration container;

[0114] d) Maintain the aeration gas flow for an aeration time of 3 to 96 hours;

[0115] The gas temperature is between 100 ℃ and 140 ℃, and the Reynolds number of the gas flow is between 5 and 150.

[0116] In a second preferred embodiment, the polypropylene composition has a high flexural modulus of 1200 MPa to 5500 MPa (ISO 178, measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996), a high puncture energy greater than 4 J, and an MFR2 greater than 8 g / 10 min (ISO 1133, 230 °C, 2.16 kg). This embodiment targets a relatively rigid and flexurally resistant polypropylene composition that can withstand point impacts and is suitable for injection molding applications. Such a material can be used, for example, in automotive interior applications.

[0117] In this regard, a second preferred embodiment of the present invention relates to a polypropylene composition comprising:

[0118] The oligomer has a semi-volatile organic condensable (FOG, VDA278, October 2011) content of 50 µg / g to 400 µg / g of the total polypropylene composition and a volatile organic compound (VOC, VDA 278, October 2011) content of less than 80 μg / g of the total polypropylene composition.

[0119] The weight ratio of the semi-volatile organic condensable to the volatile matter is greater than about 5.0;

[0120] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene composition is greater than 8 g / 10 min;

[0121] The flexural modulus of the polypropylene composition (ISO 178, measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996) is from 1200 MPa to 5500 MPa; and

[0122] The total amount of the lubricant is at least 500 ppm.

[0123] The following scope applies to all embodiments of the present invention.

[0124] Properties of Polypropylene Compositions

[0125] The polypropylene compositions of this invention are commonly used in the production of molded articles for automobiles. Emissions of volatile organic compounds (VOCs, VDA 278, October 2011) are generally undesirable; therefore, producing compositions with low VOC levels is important. Emissions of semi-volatile organic condensables (FOGs, VDA 278, October 2011) are caused by longer-chain oligomers in the polypropylene compositions, which often condense on the windshield, causing fogging. This is obviously undesirable while driving. Fogging can be measured by the “fogging weight” described in the experimental section below; for automotive applications, a lower fogging weight level is better.

[0126] The FOG content of the polypropylene composition of the present invention is 350 µg / g or less, preferably 300 µg / g or less, more preferably 250 µg / g or less, even more preferably 200 µg / g or less, and most preferably 170 µg / g or less. Furthermore, the VOC content of the polypropylene composition obtained by the method of the present invention can be 80 µg / g or less, or 60 µg / g or less, preferably 40 µg / g or less, and most preferably 20 µg / g or less.

[0127] Preferably, the FOG / VOC ratio of the polypropylene composition of the present invention is 3 or more, more preferably 5 or more, and more preferably 10 or more.

[0128] The VDA 277 of the polypropylene composition of the present invention can be from 0 µgC / g to 10 µgC / g, for example, less than 10 µgC / g, preferably less than 5 µgC / g, more preferably less than 2 µgC / g, and most preferably less than 1 µgC / g. Furthermore, this method can achieve an atomized weight of less than 1.2, preferably less than 1.1, and most preferably less than 1.

[0129] Furthermore, the VDA 270 (Automotive Industry Association) of the polypropylene composition of the present invention is minimized. VDA 270 is a measure of how consumers perceive the unpleasant odor of a particular polymer material. The VDA 270 of the polypropylene composition of the present invention is 4 or less, preferably 3 or less.

[0130] In a preferred aspect of the invention, the polypropylene is relatively rigid, with a flexural modulus of 1200 MPa to 5500 MPa, preferably about 1300 MPa to 5000 MPa. In another preferred aspect, the polypropylene composition of the invention can be used to produce injection-molded articles, particularly molded articles for automotive applications. For articles used in automobiles, the rigidity of the polypropylene material is important, and therefore a relatively high flexural modulus value is also important.

[0131] The polypropylene compositions of this invention are also relatively resistant to pinhole impact punctures. This is very important if the material is used to produce injection-molded parts (particularly for automotive applications). Recently, there has been a strong focus on reducing the weight of polypropylene components in automotive applications. Therefore, these impact-resistant parts are important, as they would otherwise be easily damaged or punctured during everyday consumer use of the vehicle.

[0132] Furthermore, the MFR2 (ISO 1133, 230 °C, 2.16 kg) of the polypropylene composition is preferably from 5 g / 10 min to 200 g / 10 min, more preferably from 8 g / 10 min to 150 g / 10 min, and most preferably from 10 g / 10 min to 130 g / 10 min. The MFR2 of the polypropylene composition is particularly preferably from 15 g / 10 min to 20 g / 10 min. A reasonable MFR2 (i.e., greater than 10 g / 10 min) is important for the polypropylene composition because it means that it can flow relatively efficiently and is therefore suitable for injection molding.

[0133] Raw material components of polypropylene composition

[0134] Prior to aeration, the polypropylene composition of the present invention preferably comprises the following raw material components:

[0135] - Polypropylene;

[0136] - Slip agent;

[0137] - Packing material;

[0138] - Optional HDPE;

[0139] - Optional plastic body;

[0140] - Optional pigments.

[0141] In a preferred aspect, the polypropylene exists in the form of multiphase polypropylene and other polypropylene homopolymers and / or polypropylene copolymers.

[0142] polypropylene

[0143] Preferably, in the polypropylene composition of the present invention, the total content of polypropylene derivative units is at least 50 wt%, more preferably at least 55 wt%, most preferably at least 64 wt%, and optionally at most 90 wt%.

[0144] The polypropylene composition of the present invention preferably comprises at least one multiphase polypropylene copolymer and other polypropylene homopolymers or polypropylene copolymers.

[0145] Preferably, the polypropylene composition of the present invention:

[0146] - FOG content less than 350 µg / g; and

[0147] - VOC content is less than 80 μg / g;

[0148] The polypropylene composition can be obtained by a method comprising the following steps:

[0149] a) Polymerizing propylene and optional other C4-C by solution polymerization in at least one polymerization reactor. 12 α-olefins are raw materials for the production of polypropylene polymers.

[0150] b) Recover the polymer feedstock from at least one polymerization reactor, feed the polymer feedstock mixture into at least one flash vessel, thereby at least partially removing the solvent, unreacted monomers and unreacted comonomers, to produce the polymer feedstock;

[0151] c) The polymer is mixed with a series of other components, optionally including HDPE, fillers, and carbon nanoparticles, preferably by means of an extruder or a static mixer;

[0152] d) Recycle polypropylene composition raw materials, wherein the propylene composition raw materials are:

[0153] - VOC content is less than 150 µg / g; and

[0154] - FOG content is less than 350 µg / g;

[0155] e) subjecting the polypropylene composition raw material to a gas flow of 5 to 150 in an aeration container for a continuous aeration time of 3 to 96 hours; wherein the temperature of the gas is at least 100 °C;

[0156] f) Recycle the polypropylene composition.

[0157] Multiphase polypropylene

[0158] Two different multiphase polypropylene copolymers are known in the art:

[0159] - Multiphase copolymers containing polypropylene random copolymer (RAHECO) as the matrix phase; and

[0160] - A multiphase copolymer containing propylene homopolymer (HECO) as the matrix phase.

[0161] In a preferred aspect of the invention, the composition comprises at least one, preferably at least two, different multiphase polypropylene materials. Preferably, the composition comprises at least one HECO or at least two different HECOs or at least one HECO and a random multiphase polypropylene (RAHECO).

[0162] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the RAHECO of the present invention is preferably 1 to 100 g / 10 min, preferably 1 to 50 g / 10 min, most preferably 5 to 20 g / 10 min, and / or the content of xylene solubles (ISO 6427, 23 °C) is 10 to 50 wt%, preferably 20 to 40 wt%, most preferably 25 to 35 wt%, and / or the total content of units derived from ethylene is 2 to 40 wt%, preferably 5 to 25 wt% (as determined by NMR).

[0163] The MFR2 (ISO 1133, 230 °C, 2.16 kg) of the HECO of the present invention is preferably 5 to 150 g / 10 min, preferably 10 to 120 g / 10 min, and / or the xylene soluble content (ISO 16152) is 8 to 30 wt%, preferably 10 to 25 wt%, and / or the total content of ethylene-derived units is 4 wt% to 20 wt%, preferably 6 wt% to 15 wt% (as determined by NMR).

[0164] Multiphase propylene copolymers comprise: polypropylene as a matrix, and an elastomeric propylene copolymer dispersed within the matrix. Thus, the polypropylene matrix contains (finely) dispersed inclusions (not part of the matrix), which comprise the elastomeric propylene copolymer. The term "inclusions" indicates that the matrix and inclusions form distinct phases within the multiphase propylene copolymer, and these inclusions can be observed, for example, by a high-resolution microscope (e.g., electron microscopy or scanning force microscopy).

[0165] In addition to propylene, the multiphase propylene copolymer also contains comonomers. Preferably, the multiphase propylene copolymer also contains ethylene and / or C4-C in addition to propylene. 12 α-olefins. Therefore, the term "propylene copolymer" in this invention should be understood as polypropylene comprising units derived from, and preferably composed of, units derived from:

[0166] a) Propylene; and

[0167] b) Ethylene and / or C4-C 12 α-olefins.

[0168] Multiphase propylene copolymer materials can be produced by melt blending and / or reactor blending. "Reactor blending" means that the various fractions of the polymer are produced in a subsequent stage in the presence of the product from the previous stage. For example, the matrix and dispersed phase of multiphase polypropylene can be produced in this subsequent stage.

[0169] In addition, the melt blend may contain more than two fractions of propylene, for example, by melt blending multiphase propylene copolymers with other propylene (e.g., propylene homopolymers or propylene random copolymers).

[0170] Therefore, the propylene copolymers (i.e., multiphase propylene copolymer elastomers) of the present invention include monomers that can be copolymerized with propylene, such as comonomers (e.g., ethylene and / or C4-C). 12 (α-olefin). Preferably, the propylene copolymer of the present invention comprises a monomer that can copolymerize with propylene, said monomer being selected from ethylene, 1-butene, and 1-hexene. More specifically, in addition to propylene, the propylene copolymer of the present invention comprises units derived from ethylene and / or 1-butene. In a preferred embodiment, the propylene copolymer of the present invention comprises only units derived from ethylene and propylene.

[0171] Therefore, the elastomer propylene copolymer (EC) is preferably ethylene propylene rubber (EPR), and the matrix polypropylene is a random propylene copolymer or propylene homopolymer.

[0172] In cases where the matrix contains one or more polypropylene monomers that are random propylene copolymers, it should be understood that the random propylene copolymers contain monomers that can be copolymerized with propylene, such as comonomers (e.g., ethylene and / or C4-C). 12 α-olefins, particularly ethylene and / or C4-C8 α-olefins, such as 1-butene and / or 1-hexene. Preferably, the random propylene copolymer of the present invention comprises monomers copolymerizable with propylene, said monomers being selected from ethylene, 1-butene, and 1-hexene. More specifically, in addition to propylene, the random propylene copolymer of the present invention comprises units derived from ethylene and / or 1-butene. In a preferred embodiment, the random propylene copolymer comprises units derived from ethylene.

[0173] Multiphase polypropylene can be prepared by reactor blending, melt blending, or a combination thereof. These processes are known in the art.

[0174] The multiphase polypropylene of the present invention is preferably produced using a multi-stage process known in the art, wherein the matrix is ​​produced in at least one slurry reactor, and subsequently the elastomer copolymer is produced in at least one gas-phase reactor.

[0175] Therefore, the polymerization system may include one or more conventional stirred slurry reactors and / or one or more gas-phase reactors. Preferably, the reactors used are selected from loop reactors and gas-phase reactors, and in particular, the process employs at least one loop reactor and at least one gas-phase reactor. It is also possible to use multiple reactors of each type, for example, one loop reactor and two or three gas-phase reactors in series, or two loop reactors and one or two gas-phase reactors.

[0176] Preferably, as described below, the process further includes prepolymerization using a selected catalyst system, which includes a Ziegler-Natta pro-catalyst, an external donor, and a co-catalyst.

[0177] In a preferred aspect, the prepolymerization is carried out in liquid propylene in the form of bulk slurry polymerization, i.e., the liquid phase mainly comprises propylene and small amounts of other reactants and optional inert components dissolved therein.

[0178] The prepolymerization reaction is usually carried out at a temperature of 0 to 50 °C, preferably 10 to 45 °C, and more preferably 15 to 40 °C.

[0179] The pressure in the prepolymerization reactor is not critical, but it must be high enough to keep the reaction mixture in the liquid phase. Therefore, the pressure can be from 20 to 100 bar, for example, 30 to 70 bar.

[0180] Preferably, all catalyst components are introduced in the prepolymerization step. However, where the solid catalyst component (i) and the cocatalyst (ii) can be fed separately, only a portion of the cocatalyst can be introduced in the prepolymerization stage, with the remainder introduced in the subsequent polymerization stage. Again, in this case, so much catalyst must be introduced into the prepolymerization stage to achieve sufficient polymerization reaction.

[0181] Other components may be added during the prepolymerization stage. Therefore, as is known in the art, hydrogen may be added to the prepolymerization stage to control the molecular weight of the prepolymer. Furthermore, antistatic additives may be used to prevent particles from adhering to each other or to the reactor walls.

[0182] Precise control of prepolymerization conditions and reaction parameters is within the scope of the art.

[0183] A slurry reactor refers to any reactor, such as a continuous stirred tank reactor, a simple batch stirred tank reactor, or a loop reactor, that operates in bulk or slurry form and in which the polymer is formed in particulate form. "Bulk" means that the reaction medium contains at least 60 wt% monomer. According to a preferred embodiment, the slurry reactor includes a bulk loop reactor.

[0184] "Gas-phase reactor" refers to any mechanically mixed or fluidized bed reactor. Preferably, the gas-phase reactor includes a mechanically stirred fluidized bed reactor, wherein the gas velocity is at least 0.2 m / s.

[0185] A particularly preferred embodiment of the present invention for preparing multiphase polypropylene includes a polymerization process comprising a combination of one ring reactor and one or two gas-phase reactors, or a combination of two ring reactors and one or two gas-phase reactors.

[0186] The preferred multi-stage process is the slurry-gas phase process, such as the Borstar process developed by Borealis. ® The technology of the process. In this respect, reference is made to EP 0 887 379 A1, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479 and WO 00 / 68315, the contents of which are incorporated herein by reference.

[0187] Another suitable slurry-gas phase process is Basell's Spheripol. ® Process.

[0188] Preferably, the multiphase polypropylene of the present invention is obtained by using Spheripol... ® Or Borstar ® The PP process uses a special Ziegler-Natta main catalyst and special external donors, as is known to those skilled in the art.

[0189] Therefore, a preferred multi-stage process may include the following steps:

[0190] - In a first slurry reactor and an optional second slurry reactor (both slurry reactors use the same polymerization conditions), a polypropylene matrix is ​​produced in the presence of a selected catalyst system known to those skilled in the art, the catalyst system comprising a special Ziegler-Natta main catalyst (i), an external donor (iii), and a co-catalyst (ii).

[0191] - Transfer the slurry reactor product to at least one first gas phase reactor (e.g., a gas phase reactor or first and second gas phase reactors in series);

[0192] - In the at least first gas-phase reactor, an elastomer copolymer is produced in the presence of a polypropylene matrix and a catalyst system;

[0193] - Recover polymer products for further processing.

[0194] For the above-mentioned preferred slurry-gas phase process, the following general information regarding process conditions can be provided.

[0195] The temperature is preferably 40 to 110 °C, more preferably 50 to 100 °C, particularly 60 to 90 °C, and the pressure is 20 to 80 bar, more preferably 30 to 60 bar. Hydrogen may be added optionally to control the molecular weight in a manner known per se.

[0196] The reaction products of slurry polymerization, preferably carried out in a loop reactor, are then transferred to a subsequent gas-phase reactor, wherein the temperature is preferably 50 to 130 °C, more preferably 60 to 100 °C, and the pressure is 5 to 50 bar, preferably 8 to 35 bar, and hydrogen is optionally added to control the molecular weight in a manner known per se.

[0197] The average residence time in the reaction zone can be varied. In one embodiment, the average residence time in a slurry reactor (e.g., a ring reactor) is 0.5 to 5 hours (e.g., 0.5 to 2 hours), while the average residence time in a gas-phase reactor is typically 1 to 8 hours.

[0198] If desired, polymerization can be carried out in a slurry reactor (preferably a ring reactor) under supercritical conditions and / or in a gas-phase reactor in a condensation mode in a known manner.

[0199] Polypropylene homopolymer

[0200] In a preferred aspect of the invention, the polypropylene composition comprises RAHECO or HECO and a propylene homopolymer. The propylene homopolymer has a melt flow rate MFR2 (230 °C, 2.16 kg) as measured according to ISO 1133 of 20 to 1000 g / 10 min, preferably 50 to 800 g / 10 min, and most preferably 60 to 700 g / 10 min.

[0201] Throughout this invention, the expression for propylene homopolymer refers to polypropylene consisting essentially of (i.e., equal to or greater than 99.9 wt%) propylene units. In a preferred embodiment, only propylene units are detectable in the propylene homopolymer.

[0202] In terms of molecular weight, propylene homopolymers can be multimodal or bimodal, with bimodal being the preferred type.

[0203] Preferably, the propylene homopolymer is isotactic. Therefore, it should be understood that the propylene homopolymer has a considerably high pentad concentration, i.e., above 80%, more preferably above 85%, further more preferably above 90%, further more preferably above 92%, and even more preferably above 93%, for example above 95%.

[0204] Preferably, the density of the propylene homopolymer, as measured according to ISO 1138, is at least 890 kg / m³. 3More preferably, at least 900 kg / m 3 More preferably, it is 900 to 915 kg / m 3 .

[0205] The propylene homopolymer of the present invention can be produced in a slurry reactor and / or a gas-phase reactor.

[0206] A preferred multi-stage process is the slurry-gas phase process, such as the Borstar process developed by Borealis. ® The technical process. In this regard, see EP 0 887 379 A1, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479 and WO 00 / 68315, the contents of which are incorporated herein by reference.

[0207] Another suitable slurry-gas phase process is Basell's Spheripol. ® Process.

[0208] In a preferred embodiment, prepolymerization is carried out in the form of bulk slurry polymerization in liquid propylene, i.e., the liquid phase mainly comprises propylene and small amounts of other reactants and optional inert components dissolved therein.

[0209] The prepolymerization reaction is usually carried out at a temperature of 0 to 50 °C, preferably 10 to 45 °C, and more preferably 15 to 40 °C.

[0210] The pressure in the prepolymerization reactor is not critical, but it should be high enough to keep the reaction mixture in the liquid phase; therefore, the pressure can be 20 to 100 bar, for example, 30 to 70 bar.

[0211] Preferably, all catalyst components are introduced in the prepolymerization step. However, where the solid catalyst component (i) and the cocatalyst (ii) can be fed separately, only a portion of the cocatalyst can be introduced in the prepolymerization stage, with the remainder introduced in the subsequent polymerization stage. Again, in this case, so much catalyst must be introduced into the prepolymerization stage to achieve sufficient polymerization reaction.

[0212] Other components may be added during the prepolymerization stage. Therefore, as is known in the art, hydrogen may be added to the prepolymerization stage to control the molecular weight of the prepolymer. Furthermore, antistatic additives may be used to prevent particles from adhering to each other or to the reactor walls.

[0213] Precise control of prepolymerization conditions and reaction parameters is within the technical scope of those skilled in the art.

[0214] A slurry reactor refers to any reactor, such as a continuous stirred tank reactor, a simple batch stirred tank reactor, or a ring reactor, that operates in bulk or slurry form and in which the polymer is formed in particulate form.

[0215] Suitable catalyst systems are described in EP591 224.

[0216] Lubricant

[0217] During polypropylene production, slip agents are typically added to polypropylene blends to reduce the coefficient of friction of these polypropylene materials. The preferred aspects of this invention and the most commonly used slip agents in industry are derived from the chemical groups of fatty acid amides (e.g., erucamide). When the slip agent is mixed with the polypropylene polymer melt, it is absorbed by the amorphous regions of the polypropylene polymer.

[0218] Upon cooling, due to the difference in surface energy between the two materials, the slip agent becomes incompatible with the polypropylene material and migrates to the material surface. The migration rate depends on the difference in surface energy between the polypropylene and the slip agent (the greater the difference, the faster the migration). This initially leads to the formation of a monolayer on the polymer surface, followed by subsequent layer deposition as new slip agent molecules arrive at the surface, resulting in the formation of a bilayer. Because the bonds between the fatty acid amide layers are weak, materials produced from polypropylene containing fatty acid amides tend to slide against each other. The presence of the slip agent layer also reduces the friction on the surface of the polypropylene composition. This property is also important, for example, when producing injection-molded articles, as slip agents can be used to help demold the injection-molded articles from the mold. When the polypropylene cools, the fatty acid amides arrive at the surface of the polypropylene article; therefore, the coefficient of friction between the polypropylene article and the mold is reduced. This means that only relatively small forces are needed to remove the polypropylene article from the mold, and when the molded article is released, no polypropylene adheres to the mold. Many slip agents (especially fatty acid amides, such as erucamide) are relatively volatile, so care must be taken to avoid these materials escaping during the processing steps of polymer production.

[0219] Despite being processed, the polypropylene compositions of the present invention retain a high level of slip agents. The slip agents are preferably added before the aeration step, as this results in a more uniform distribution of the slip agents throughout the material; conversely, if the slip agents are added after the aeration step, they may not be able to smoothly coat the polypropylene articles produced by injection molding, meaning that these articles are not easy to slide out of the mold. Furthermore, compounds such as erucamide serve a dual purpose; they are also responsible for the scratch resistance of the polypropylene composition. For good scratch resistance, uniform distribution of these compounds throughout the composition is important.

[0220] filler

[0221] The polypropylene composition of the present invention may further contain filler in an amount of up to 40 wt%, preferably up to 30 wt%, based on the total amount of the polypropylene composition. Generally, the filler content is 1.0 wt% or more, more preferably 5.0 wt% or more, and most preferably 7.0 wt% or more, based on the total amount of the polypropylene composition.

[0222] The filler can be selected from: glass fiber, talc, carbon fiber, siliceous silicate, mica, wollastonite, or mixtures thereof. Preferably, the filler is selected from glass fiber and talc. Most preferably, the filler is talc or glass fiber.

[0223] HDPE

[0224] High-density polyethylene (HDPE) is well known in the art and is defined as polyethylene that is essentially unbranched (i.e. has a linear structure).

[0225] Preferably, the density of high-density polyethylene (HDPE) is at least 930 kg / m³. 3 More preferably 940 kg / m 3 More preferably 930 kg / m 3 Up to 975 kg / m 3 A further preferred value is 940 kg / m 3 Up to 968 kg / m 3 For example, 950 kg / m 3 Up to 965 kg / m 3 .

[0226] Preferably, the melt flow rate of high-density polyethylene (HDPE) is quite low. According to a preferred embodiment, the melt flow rate MFR2 (190 °C / 2.16 kg) of high-density polyethylene (HDPE) is not more than 10.0 g / 10 min, more preferably not more than 5.0 g / 10 min, and even more preferably from 0.01 g / 10 min to 10.0 g / 10 min, for example from 0.1 g / 10 min to 5.0 g / 10 min.

[0227] plastic body

[0228] In the context of this invention, the plastic body used is preferably an ethylene copolymer. A suitable ethylene copolymer can be any ethylene and C6-C... 12 A copolymer of an α-olefin, wherein the α-olefin possesses the aforementioned properties. Preferably, the ethylene copolymer is selected from ethylene-based plastics. Suitable ethylene-based plastics are commercially available, for example, from Borealis under the trade name Queo.

[0229] Preferably, the density of the plastic body is 860 kg / m³. 3 Up to 930 kg / m3 More preferably 865 kg / m 3 Up to 920 kg / m 3 For example, 868 kg / m 3 Up to 910 kg / m 3 More preferably, the melt flow rate (MFR) of the plasmid (190 °C / 2.16 kg) is from 0.1 g / 10 min to 40.0 g / 10 min, more preferably from 0.3 g / 10 min to 35 g / 10 min, for example from 0.4 g / 10 min to 32 g / 10 min.

[0230] In a preferred aspect of the invention, the plastic body is an ethylene-octene plastic body.

[0231] The ethylene-based plastic body can be prepared by known processes (e.g., one-stage or two-stage polymerization processes) in the presence of suitable catalysts known to those skilled in the art (e.g., vanadium oxide catalysts or single-center catalysts, such as metallocene or defined geometry catalysts), including solution polymerization, slurry polymerization, gas-phase polymerization, and combinations thereof.

[0232] Preferably, these ethylene-based plastics are prepared in the presence of a single-center catalyst via a one-stage or two-stage solution polymerization process (especially a high-temperature solution polymerization process at temperatures above 100 °C).

[0233] This process is essentially based on polymerizing monomers and suitable comonomers in a liquid hydrocarbon solvent (in which the resulting polymer is soluble). Polymerization is typically carried out at a temperature above the polymer's melting point, thereby obtaining a polymer solution. This solution is then flash-evaporated to separate the polymer from the unreacted monomers and solvent. The solvent is subsequently recovered and recycled during the process.

[0234] Preferably, the solution polymerization process is a high-temperature solution polymerization process, using a polymerization temperature higher than 100 °C. Preferably, the polymerization temperature is at least 110 °C, more preferably at least 150 °C. The polymerization temperature can be as high as 250 °C.

[0235] The pressure for this solution polymerization process is preferably 10 bar to 100 bar, more preferably 15 bar to 100 bar, and even more preferably 20 bar to 100 bar.

[0236] The liquid hydrocarbon solvent used is preferably unsubstituted C5-C. 12 Hydrocarbons or C5-C hydrocarbons substituted with C1-C4 alkyl groups 12 Hydrocarbons, such as pentane, methylpentane, hexane, heptane, octane, cyclohexane, methylcyclohexane, and hydrogenated naphtha. More preferably, unsubstituted C6-C hydrocarbons are used. 10 Hydrocarbon solvent.

[0237] Suitable, the ethylene copolymer contains 10 wt% to 50 wt% linear C6-C 12 α-olefin comonomer units, preferably 20 wt% to 45% linear C6-C 12 α-olefin comonomer units, preferably 30 wt% to 40 wt% of linear C6-C 12 α-olefin comonomer unit.

[0238] Preferably, the linear α-olefin comonomer unit is selected from 1-octene and / or 1-hexene; most preferably, the linear α-olefin comonomer unit is 1-octene. Preferably, the composition of the present invention uses a copolymer of ethylene and 1-octene.

[0239] pigment

[0240] Optionally, the polypropylene composition comprises a pigment. Suitable pigments are known in the art.

[0241] Preferably, a black pigment, such as carbon black, or Black Pearls purchased from Cabot Corporation, is used. ® .

[0242] Based on the total weight of the polypropylene composition, the total amount of pigment in the polypropylene composition of the present invention is preferably 0.1 wt% to 15 wt%, more preferably 0.5 wt% to 10 wt%, and most preferably 0.5 wt% to 8 wt%.

[0243] additive

[0244] The polypropylene composition may also contain other additives. These additives can help process the polypropylene composition or help improve the final properties of the composition, such as MFR2. The polypropylene composition of the present invention may contain additives selected from antioxidants, processing aids, and acid removers (e.g., calcium stearate, lubricants).

[0245] The total amount of additives is preferably 0.05 to 5.0 wt%, more preferably 0.10 to 3.5 wt%, and most preferably 0.25 to 2.5 wt%.

[0246] Production process of polypropylene composition

[0247] As described above, the present invention relates to polypropylene compositions, which can be obtained by:

[0248] In the presence of additives, the following components are blended to obtain a blend:

[0249] - Polypropylene

[0250] - Packing material

[0251] - Lubricant

[0252] - Optional HDPE

[0253] - Optional plastic body

[0254] - Optional pigments;

[0255] The blend is then subjected to a process including the following steps:

[0256] a) Provide an aeration container, said aeration container having:

[0257] - At least one aeration gas inlet;

[0258] - At least one exhaust gas outlet;

[0259] - Inlet of polypropylene composition raw material at the top of the aeration container;

[0260] - The outlet of the polypropylene composition at the bottom of the aeration container;

[0261] The polypropylene composition exists as a packed bed.

[0262] b) Initiate countercurrent flow between the polypropylene composition and the aeration gas;

[0263] c) Perform the following operations:

[0264] - The polypropylene composition feedstock is fed from the top into the aeration vessel, the polypropylene composition feedstock having a volatile organic compound content (VOC, VDA 278, October 2011) greater than about 150 µg / g and a semi-volatile organic condensable content (FOG, VDA 278, October 2011) greater than about 350 µg / g.

[0265] - Aeration gas is fed into the aeration container through at least one inlet at the bottom;

[0266] - Exhaust gas is discharged through the exhaust outlet;

[0267] - The aerated polypropylene composition is discharged through the outlet at the bottom of the aeration container;

[0268] d) Maintain the aeration gas flow for an aeration time of 3 to 96 hours;

[0269] The gas temperature is between 100 ℃ and 140 ℃, and the Reynolds number of the gas flow is between 5 and 150.

[0270] The above process is preferably carried out for less than about 24 hours, or less than about 12 hours, or less than about 10 hours, for example, 3 to 9 hours. Generally, aeration time is inversely proportional to gas temperature, meaning that an equilibrium must be reached between the two to prevent the pellets from melting and sticking together. According to EP2005 / 056962, the typical temperature and residence time for polypropylene is 80 to 110 °C, lasting 10 to 50 hours. It is believed that under the conditions described here, extending the aeration time to more than 5 hours results in a plateau in VOC reduction; conversely, within an aeration time of 0 to 5 hours, the dependence of FOG on aeration time is relatively small. This is believed to be due to the fact that, relative to the <C> factor affecting VOC emissions... 20 The rapid diffusion of alkanes affects the emissions of higher molecular weight alkanes (C60-C60) from FOG. 16 -C 32 The spread of ) is relatively slow.

[0271] Typically, the polypropylene composition is preferably not mechanically mixed or moved throughout the treatment process. Therefore, during aeration, the polypropylene composition is essentially stationary (except for its vertical passage through the aeration container). Consequently, the present invention preferably excludes the process of agitating the polymer composition during aeration.

[0272] Preferably, the aeration process is carried out using polypropylene granules. Furthermore, the process is typically conducted in a secluded treatment container (preferably a secluded silo). The silo can be, for example, a steel silo.

[0273] The polypropylene compositions obtained through the above process have a specific structure, which means that they exhibit MRF2 values ​​suitable for injection molding, relatively high puncture energy values, high scratch resistance and high hardness, as well as other properties.

[0274] Experimental Section

[0275] The following examples illustrate certain aspects and implementations of the invention as described in the claims. However, those skilled in the art will understand that the following description is merely illustrative and should not be construed as limiting the invention in any way.

[0276] Detection methods

[0277] Sample preparation

[0278] After preparing samples consisting of injection-molded plates according to EN ISO 19069-2:2016, the VOC, FOG, and TVOC values ​​were determined as described below. These plates were immediately packaged in aluminum composite foil after preparation, and the foil was then sealed.

[0279] For thermal desorption analysis according to VDA 278 (October 2011), samples were stored uncovered directly at room temperature (maximum 23 °C) for 7 days before the start of the analysis.

[0280] For VDA 277 (January 1995) measurements, no additional capless storage or other conditioning is required. Instead, the injection-molded plate is shredded and ground in a Retsch SM-2000 grinder.

[0281] In both cases (VDA 277 and VDA 278), the production date, arrival time at the laboratory, and analysis date of the injection-molded plate were recorded.

[0282] According to VDA 278 VOC and FOG

[0283] VOC:

[0284] Measured using injection-molded plates according to VDA 278 (October 2011). VDA 278 (October 2011) is used for thermal desorption analysis to characterize organic emissions from automotive non-metallic materials, VDA Automotive Industry Association. According to VDA 278 (October 2011), VOC value is defined as "the total amount of volatile to moderately volatile substances". It is calculated as toluene equivalent. The method described in this recommendation can determine and analyze boiling / elution ranges up to n-pentane (C 25 The following substances.

[0285] FOG:

[0286] Measured using injection-molded plates in October 2011, according to VDA 278. According to VDA 278, in October 2011, the FOG value is defined as "the total amount of low-volatility substances eluted from the retention time of n-octadecyl groups (including both ends)". FOG is calculated as hexadecane equivalents. Substances in the boiling point range of n-alkanes from "C14" to "C32" were identified and analyzed.

[0287] Total emissions, TVOC:

[0288] The total emissions in the granulated polypropylene composition were determined according to VDA 277 in January 1995.

[0289] Atomization:

[0290] Atomization measurements were performed on compression-molded samples (diameter 80 mm + / - 1 mm, thickness < 1 cm) cut from an injection-molded plate according to DIN 75201:2011-11 Method B (gravimetric method). This method determines the mass (in mg) of atomized condensate on the aluminum foil by weighing the foil before and after the atomization test. The term "atomization" refers to the fraction of volatile substances condensing on glass components (e.g., automotive windshields).

[0291] Diameter D:

[0292] Sieve analysis was performed according to ISO 3310. Sieve analysis involved nested sieve columns with wire mesh screens, with the following sieve aperture sizes: >20 µm, >32 µm, >63 µm, >100 µm, >125 µm, >160 µm, >200 µm, >250 µm, >315 µm, >400 µm, >500 µm, >710 µm, >1 mm, >1.4 mm, >2 mm, >2.8 mm, >4 mm. The sample was poured into the top sieve with the largest aperture. The apertures at the bottom of each column were smaller than those at the top (see dimensions above). The receiver was located at the bottom. The column was placed in a mechanical shaker. The shaker was used to shake the column. After shaking, the material on each sieve was weighed. The weight of the sample on each sieve was then divided by the total weight to obtain the percentage retained on each sieve. The particle size distribution and characteristic median particle size d50 were determined based on the sieving analysis results of ISO 9276-2.

[0293] Melt flow rate (MFR2)

[0294] Melt flow rate (MFR2) was measured at 230 °C and a load of 2.16 kg. Melt flow rate is the amount of polymer extruded (in grams) in 10 minutes at 230 °C and a load of 2.16 kg using test equipment standardized according to ISO 1133.

[0295] Xylene cold soluble fraction (XCS wt%)

[0296] The cold soluble fraction (XCS) of xylene was determined at 23 °C according to ISO 6427.

[0297] NMR spectroscopy measurement:

[0298] Quantitative analysis of microstructure using NMR spectroscopy

[0299] Quantitative nuclear magnetic resonance (NMR) spectroscopy is used to quantify the comonomer content and comonomer sequence distribution of polymers. 1 H and 13 C. Using a Bruker Advance III 400 NMR spectrometer, the solution state was recorded at 400.15 MHz and 100.62 MHz, respectively. 13 C { 1 ¹H NMR quantitative spectroscopy. Using… 13The optimal 10mm extended temperature probe was used at 125 °C, with nitrogen used for all atmospheres, to record all spectra. Approximately 200 mg of material was dissolved with chromium acetylacetonate (III) (Cr(acac)3) in 3 mL of 1,2-tetrachloroethane-d2 (TCE-d2) to obtain a 65 mM relaxant solution in solvent (Singh G., Kothari A., Gupta V., Polymer Testing 28 5 (2009), 475). To ensure solution homogeneity, the NMR tube was further heated in a rotary furnace for at least 1 hour after initial sample preparation in a heating block. After inserting the magnet, the tube was rotated at 10 Hz. This setup was chosen primarily for the need to obtain high resolution and accurate quantification of ethylene content. Standard single-pulse excitation without NOE was used, employing an optimal apex cone angle, a 1-second cyclic delay, and a two-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6 k) transient signals were acquired for each spectrum.

[0300] Quantitative analysis was performed using specialized computer software. 13 C{ 1 The ¹H NMR spectra were processed and integrated, and the quantitative properties were determined by integration. The chemical shifts of the solvent were used, with all chemical shifts indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm. This method can be similarly applied even without this structural unit. Characteristic signals corresponding to ethylene incorporation were observed (Cheng, HN, Macromolecules 17 (1984), 1950).

[0301] When characteristic signals corresponding to defects in the 2,1 reddish region are observed (e.g., L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100(4):1253; Cheng, HN, Macromolecules 1984, 17:1950; and W.J. Wang and S. Zhu, MacromoleculesAs described in 2000, 33 1157), the influence of regional defects on the measured properties needs to be corrected. No characteristic signals corresponding to other types of regional defects were observed.

[0302] Using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157), by... 13 C{ 1 The comonomer fraction is quantified by integrating multiple signals across the entire spectral region of the H spectrum. This method is chosen because of its robust nature and ability to address regional defects as needed. The integration region is slightly adjusted to improve applicability across the entire range of comonomer contents encountered.

[0303] For systems where isolated ethylene is observed only in the PPEPP sequence, the method of Wang et al. is adjusted to reduce the influence of non-zero integrals from sites that are known to be absent. This method reduces the overestimation of ethylene content in such systems by reducing the number of sites used to determine absolute ethylene content to the following formula:

[0304]

[0305] By using this set of sites, the corresponding integral equation becomes:

[0306]

[0307] The same notation as used in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) is used. The equation for absolute propylene content is not modified.

[0308] The molar percentage of the incorporated comonomer is calculated from the mole fraction:

[0309]

[0310] The weight percentage of the incorporated comonomer is calculated from the mole fraction:

[0311]

[0312] The distribution of comonomer sequences at the ternary group level was determined using the analytical method of Kakugo et al. (Kakugo, M., Naito, Y., Mizunuma, K., Miyatake, T., Macromolecules 15(1982)1150). This method was chosen because of its stability and the ability to fine-tune the integration region to increase its applicability to a wider range of comonomer contents.

[0313] Polymer-Puncture Plate-Instrument:

[0314] In the drop hammer test according to ISO 6603-2, the puncture energy was measured using a 60×60×1mm injection-molded plate and a clamped, lubricated impact pin with a test speed of 2.2m / s and a diameter of 20mm. The reported puncture energy was obtained by integrating the breaking energy curve measured at (60×60×1mm).

[0315] Flexural modulus:

[0316] According to ISO 178, the flexural modulus is determined by three-point bending using an 80×10×4mm injection molding test bar prepared in accordance with ISO 294-1:1996.

[0317] VDA 270:

[0318] VDA 270 is a method for determining the odor characteristics of automotive trim materials. VDA 270 is measured according to the standard used by the German Industry Association in 1992. Typically, the material is heated for a period of time in a sealed container (with or without deionized water). The container is then removed from the warm environment, and at least three human subjects rate the odor of the specific polymeric material from 1 to 6 according to the categories described below:

[0319] 1: Unaware

[0320] 2: It can be detected, but it doesn't cause discomfort.

[0321] 3: It is noticeable, but still not uncomfortable.

[0322] 4: It's uncomfortable

[0323] 5: It's very uncomfortable

[0324] 6: Unbearable

[0325] experiment

[0326] Table 1: Properties of the base resin used in the composition used in Example 1

[0327]

[0328] 1Random thermoplastic olefins; 2 according to 13 C-NMR spectroscopy was measured

[0329] Table 2: Composition of the various polypropylene compositions used in Example 1

[0330]

[0331] All values ​​are expressed as a weight percentage and rounded to the nearest 0.5%. 1 Ethylene-propylene elastomer. 2 Properties of polypropylene composition raw materials before aeration.

[0332] Example 1

[0333] Granulated polypropylene compositions corresponding to materials A, B, C, D, and E as defined in Table 2 were aerated in batches. Aeration was carried out in insulated cylindrical silos with dimensions of 1.5 m. 3 The median particle size d50 of the pellets is 3.5 mm (ISO 3310, evaluated according to ISO 9276-2). The pellets are at room temperature (approximately 25 °C) before aeration, i.e., no preheating step is applied.

[0334] The aeration process was carried out at 140 °C for 7.5 hours. A 260m³ aeration tank was used. 3 The gas flow rate is 100 kg / h. During this process, the granules are not mixed or stirred, but simply moved vertically in the silo at a speed of 100 kg / h.

[0335] The process was carried out on a scale of 1000 kg. At 1.5 m 3 Inside the silo. Throughout the aeration process, the relative flow rate of the polypropylene composition pellets was maintained at 100 kg / hour.

[0336] The aeration process lasts for 7 hours continuously.

[0337] Table 4 shows the VOC, FOG, VDA 277, and atomized weight for each grade before and after the aeration step.

[0338] Table 3: Overview of the airflow characteristics used in this experiment

[0339]

[0340] The Reynolds number can be calculated using the following formula:

[0341]

[0342] In the formula:

[0343] - Density of aeration gas at operating temperature (kg / m³) 3 );

[0344] - : Dynamic viscosity of aeration gas at operating temperature (kg / m·s);

[0345] - Superficial velocity is defined as follows: ,in, The volumetric flow rate of the aeration gas (m) 3 / s), A is the cross-sectional area (m²) 2 );

[0346] - D: Particle diameter d50 (m) (using sieve analysis according to ISO 3310 and evaluated according to ISO 9276-2).

[0347] The Reynolds number of the gas flow used in Example 1 is 20.

[0348] Table 4: VOC, FOG, VDA 277, atomized weight, VDA 270, and FOG / VOC ratio for polymers A, B, C, D, and E

[0349]

[0350] VOC and FOG values ​​were measured after 7 days according to VDA 278 and VDA 277, and the atomized weight was measured immediately.

[0351] Surprisingly, the total amount of slip enhancer in all polymers A through E after aeration was greater than 500 ppm.

[0352] Table 5: Properties of polypropylene compositions A, B and C after aeration

[0353]

Claims

1. A method for providing a polypropylene composition, wherein, The method includes: In the presence of additives, the following components are blended to obtain a blend that can be used as a raw material for a polypropylene composition: - Polypropylene - Packing material - Lubricant - Optional HDPE - Optional plastic body - Optional pigments; The blend is further subjected to a process including the following steps: a) Provide an aeration container, said aeration container having: - At least one aeration gas inlet; - At least one exhaust gas outlet; - The inlet for the polypropylene composition feedstock is located at the top of the aeration container; - The outlet of the polypropylene composition located at the bottom of the aeration container; The polypropylene composition raw material exists as a packed bed; b) To initiate countercurrent flow between the polypropylene composition raw material and the aeration gas; c) Perform the following operations: - The polypropylene composition feedstock is fed from the top into the aeration vessel, the polypropylene composition feedstock having a volatile organic compound (VOC) content greater than 150 µg / g as measured by VDA 278 in October 2011 and a semi-volatile organic condensable (FOG) content greater than 350 µg / g as measured by VDA 278 in October 2011. - The aeration gas is fed into the aeration container through at least one inlet at the bottom; - Exhaust gas is discharged through the exhaust outlet; - The aerated polypropylene composition is discharged through an outlet at the bottom of the aeration container; d) Maintain the aeration gas flow for an aeration time of 3 to 96 hours; The gas temperature ranges from 100 ℃ to 140 ℃, and the Reynolds number of the gas flow ranges from 5 to 150. The Reynolds number of the aeration gas flow through the packed bed is defined by equation (I): (I) In the formula: - The density of the aeration gas at the operating temperature is expressed in kg / m³. 3 ; - The dynamic viscosity of the aeration gas at the operating temperature is expressed in kg / m·s. - For apparent velocity, it is defined as ,in, The volumetric flow rate of the aeration gas is expressed in meters per second (m). 3 / s, Cross-sectional area, unit is m 2 ; - D is the diameter of the particle, in meters (m); In this case, no more slip agent is added to the composition after the aeration step (d).

2. The method according to claim 1, wherein, The polypropylene composition comprises: Semi-volatile organic condensable oligomer FOG, with a content of 50 µg / g to 170 µg / g of the total polypropylene composition as determined by VDA 278 in October 2011; and The volatile organic compounds (VOCs) content, as determined by VDA 278 in October 2011, is less than 20 μg / g of the total polypropylene composition. Wherein, the weight ratio of the semi-volatile organic condensable oligomer to the volatile organic compound is greater than 5.0; The MFR2 of the polypropylene composition, as measured according to ISO 1133 at 230 °C and 2.16 kg load, is greater than 10 g / 10 min. The polypropylene composition, according to ISO 178, has a flexural modulus of 1000 MPa to 6000 MPa as measured on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996; and The total amount of lubricant is at least 500 ppm.

3. The method according to claim 1, wherein, The lubricant is a fatty acid amide.

4. The method according to claim 3, wherein, The fatty acid amide is erucamide or oleamide.

5. The method according to claim 2, wherein, The VDA 277 of the polypropylene composition is less than 1.

6. The method according to claim 2, wherein, The atomized weight of the polypropylene composition is less than 1.1, and / or the VDA 270 of the polypropylene composition is less than 3.

7. The method according to claim 2, wherein, The MFR2 of the polypropylene composition, as measured according to ISO 1133 at 230 °C and 2.16 kg load, is 10 g / 10 min to 25 g / 10 min.

8. The method according to claim 2, wherein, The flexural modulus of the polypropylene composition, as measured according to ISO 178, on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996, is from 1300 MPa to 5000 MPa.

9. The method according to claim 1, wherein, The blending step includes blending multiphase polypropylene with other polypropylene homopolymers and / or polypropylene copolymers.

10. The method according to claim 2, wherein, The flexural modulus of the polypropylene composition, as measured according to ISO 178, on an 80×10×4 mm injection-molded sample prepared according to ISO 294-1:1996, is from 1200 MPa to 5500 MPa.

11. The method according to claim 2, wherein, The puncture energy of the polypropylene composition is 20 J to 60 J.

12. The method according to claim 1, wherein, The filler is selected from talc, glass, and mixtures thereof.

Citation Information

Patent Citations

  • A procatalyst for polymerization of olefins containing a trans-esterification product of a lower alcohol and a phthalic acid ester

    EP0591224A1

  • Process and apparatus for preparing propylene homopolymers and copolymers

    EP0887379A1

  • Novel polypropylene compositions with low fogging

    EP3260489A1

  • Removing volatile constituents from particulate olefin polymers produced by gas-phase polymerization

    GB1272778A

  • Method for deodorizing polyolefin granulates

    US6218504B1