A method for regulating the activity and molecular weight of rare-earth catalytic meta-halostyrene polymerization by modifying CGC-type ligands

By modifying CGC-type ligands to regulate the Lewis acidity of rare earth catalysts, the problems of efficient polymerization and molecular weight control of meta-halostyrene were solved, achieving highly selective and highly active homopolymerization and copolymerization of meta-halostyrene, resulting in high molecular weight copolymers with unimodal distribution.

CN123106955APending Publication Date: 2026-11-17BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611480705.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve efficient coordination polymerization of meta-halostyrene and control the polymer molecular weight, especially due to the low charge density of the C=C double bond and the weak coordination ability of the metal center, resulting in low activity of rare earth catalysts and difficulty in controlling the molecular weight.

Method used

By modifying the electronic and steric effects of CGC-type ligands, the Lewis acidity of rare earth metal centers is adjusted, and different Lewis basicity of meta-halostyrene monomers are matched. A catalytic system is formed by combining specific CGC-type rare earth catalysts with organoborates and alkylaluminum co-catalysts to carry out homopolymerization and copolymerization reactions of meta-halostyrene.

Benefits of technology

High syndiotactic selectivity homopolymerization of m-halostyrene (rrrr>99%) was achieved. By controlling the monomer content in the copolymer, a high molecular weight polymer was obtained. The copolymer exhibited a unimodal distribution and excellent crystallinity and thermal properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention belongs to the field of olefin coordination polymerization catalyst technology, specifically relating to a method for regulating the activity and molecular weight of rare-earth catalytic meta-halostyrene polymerization by modifying CGC-type ligands. This invention provides a series of catalysts with the general formula (L)Ln(CH2SiMe3)2(THF). n The invention utilizes a CGC-type rare earth catalyst, where L is either a fluorenyl ligand R1-Flu-CH2CH2NMe2 or an indoxindole ligand 5-R2-IndCH2CH2NMe2. By systematically modifying the electronic and steric effects of the CGC-type ligands, the Lewis acidity of the rare earth metal center is adjusted, achieving highly syndiotactic selectivity homopolymerization (rrrr>99%) of meta-halostyrene (m-F / Cl / Br / ISt) and methoxyhalostyrene, as well as copolymerization with styrene. A fluorenyl yttrium catalyst C((2,7-) containing electron-donating groups is employed. t When Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF catalyzes the homopolymerization of m-fluorostyrene, the activity can reach 2.28×10. 6 g·mol cat ‑1 ·h ‑1 Scandium catalyst A (2,7-) was used. t Bu2-FluCH2CH2NMe2)Sc(CH2SiMe3)2 can achieve a number-average molecular weight as high as 526.86×10 4 g·mol ‑1 This invention yields ultra-high molecular weight polymers. It achieves effective control over the polymerization reactivity and molecular weight of m-halostyrene, resulting in polymers with high syndiotactic selectivity, high molecular weight, and good thermal properties, showing broad application prospects in corrosion-resistant materials, flame-retardant materials, and low dielectric constant materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of olefin coordination polymerization catalyst technology, specifically relating to a method for regulating the activity and molecular weight of rare earth catalytic inter-halostyrene polymerization by modifying constrained-geometry-configuration (CGC) ligands, as well as the CGC-type rare earth catalyst used in this method, its preparation method, and its application. Background Technology

[0002] Halogen-containing polystyrene has attracted widespread attention due to its excellent corrosion resistance, flame retardancy, low dielectric constant, and low surface energy. However, high stereoselectivity is generally difficult to achieve in polyhalostyrene obtained by free radical polymerization. The reason for the low activity of transition metal-catalyzed coordination polymerization is that, compared with electron-donating groups such as oxygen-containing and sulfur-containing groups in polar styrene, halogen groups with electron-withdrawing effects reduce the charge density of the C=C double bond in halostyrene, thereby reducing its coordination insertion ability and leading to reduced or even no polymerization activity.

[0003] Rare earth group III metal catalysts possess strong Lewis acidity, and their f orbitals at the metal center endow them with high coordination numbers, typically reaching 6–9. High coordination numbers allow heteroatoms to coordinate cooperatively with C=C double bonds, promoting coordination-insertion of the C=C double bond. Alternatively, selecting appropriate ligands can regulate the electronic and steric effects of the metal center, preventing it from being poisoned by heteroatoms and encouraging coordination-insertion with the C=C double bond. Rare earth group III metal catalysts can achieve highly active and highly regio / stereoselective polymerization of polar olefins. Their copolymerization reactions with nonpolar olefins exhibit high activity, tunable polar monomer insertion rates, and tunable sequence distribution. Therefore, rare earth group III metal catalysts represent a highly promising catalytic system for the (co)polymerization of polar olefins, urgently requiring industrial development.

[0004] In recent years, restricted geometry (CGC) rare earth catalysts have made significant progress in the polymerization of halostyrene. However, research has mainly focused on ortho- and para-substituted halostyrene, with few reports on the polymerization of meta-substituted halostyrene. This is because the electron-withdrawing effect of halogen atoms at the meta position of styrene is stronger than that at the ortho and para positions, resulting in the lowest charge density on the C=C double bond and the weakest coordination ability between the double bond and the metal center, making polymerization the most difficult to achieve. Furthermore, the electronic and steric effects exhibited by disubstituted polar styrene during polymerization are more complex than those of monosubstituted styrene. Studying the relationship between the high molecular weight / high activity polymerization of disubstituted polar styrene and the electronic / steric effects of monomers and rare earth catalysts is an extremely challenging topic.

[0005] To date, a variety of classic regulatory strategies have been developed, including changing or modifying the anionic or neutral supporting ligands of transition metal catalysts, changing the metal center, and changing the main group metal co-catalysts, thereby realizing the coordination (co)polymerization reaction of various polar olefins containing heteroatom functional groups.

[0006] Therefore, developing a method to effectively regulate the activity and molecular weight of rare earth-catalyzed metahalostyrene polymerization, especially through ligand structure modification to achieve precise control of polymerization performance, has significant academic and application value. Summary of the Invention

[0007] To address the technical challenges of achieving efficient coordination polymerization of meta-halostyrene due to the low charge density of the C=C double bond and weak coordination ability with the metal center, as well as the shortcomings of existing CGC-type rare earth catalysts in the polymerization of meta-halostyrene with low activity and difficulty in controlling the polymer molecular weight, this invention provides a method for controlling the activity and molecular weight of rare earth catalytic meta-halostyrene polymerization by modifying CGC-type ligands.

[0008] This invention modifies the electronic (electron-donating / electron-withdrawing groups) and steric effects of CGC-type ligands to regulate the Lewis acidity of rare earth metal centers, thereby achieving matched catalysis of meta-halostyrene monomers with different Lewis basicities, and thus controlling the polymerization reaction activity and polymer molecular weight.

[0009] To achieve the above objectives, the present invention adopts the following technical solution:

[0010] This invention provides a CGC-type rare earth catalyst, which has the following general formula: Formula I: (L)Ln(CH2SiMe3)2(THF) n Due to the different L-ligands, its structural formulas can be either I or II: (I) (II)

[0011] Wherein, L is selected from any of the following ligands: (1) Fluorenyl ligand: R1-Flu-CH2CH2NMe2, wherein R1 is selected from the same or different groups, and is one of hydrogen atom, methyl, ethyl, isopropyl, tert-butyl, n-butyl, alkoxy, diethylamino, amino, chlorine atom, fluorine atom, iodine atom, bromine atom, nitro, phenyl, benzyl, naphthyl; (2) Indene-indole ligand: 5-R2-10-(N,N-dimethylethylamine)-decahydroindene[1,2-b]indole (5--R2-IndCH2CH2NMe2), wherein R2 is selected from the same or different groups, and is one of hydrogen atom, methyl, ethyl, isopropyl, tert-butyl, n-butyl, alkoxy, diethylamino, amino, chlorine atom, fluorine atom, iodine atom, bromine atom, nitro, phenyl, benzyl, naphthyl.

[0012] Ln is selected from one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, or lutetium.

[0013] Where n is 0 or 1.

[0014] Preferably, the catalyst is selected from any one of the following compounds: Catalyst A: (2,7- t Bu2-FluCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst B: (2,7- t Bu2-FluCH2CH2NMe2)Lu(CH2SiMe3)2THF; Catalyst C: (2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF; Catalyst D: (FluCH2CH2NMe2)Y(CH2SiMe3)2THF; Catalyst E: (FluCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst F: (5-Me-IndCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst G: (5-Me-IndCH2CH2NMe2)Y(CH2SiMe3)2THF.

[0015] This invention provides a method for preparing the above-mentioned CGC-type rare earth catalyst, comprising the following steps: (1) Under inert gas protection, CGC type ligand L is reacted with n-butyllithium at -78℃ to -10℃ to generate ligand lithium salt; (2) The lithium ligand obtained in step (1) is reacted with the rare earth metal trialkyl compound Ln(CH2SiMe3)3(THF). n The reaction is carried out in an organic solvent, and the CGC-type rare earth catalyst is obtained after post-treatment.

[0016] This invention provides a method for controlling the homopolymerization activity and molecular weight of meta-halostyrene, comprising the following steps: (1) Under the protection of an inert gas, the above-mentioned CGC rare earth metal complex main catalyst, organoborate co-catalyst and alkylaluminum co-catalyst are mixed in an organic solvent to form a catalytic system; (2) Add meta-halostyrene monomer or methoxyhalostyrene monomer to the above catalytic system and carry out homopolymerization reaction at room temperature; (3) After the polymerization reaction is completed, a terminator is added to terminate the reaction. The reaction mixture is poured into a precipitant containing a polymerization inhibitor to precipitate and obtain syndiotactic poly(m-halostyrene).

[0017] Preferably, (2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF, i.e., CGC type rare earth catalyst C.

[0018] Furthermore, the organoborate cocatalyst is triphenylcarbazo(pentafluorophenyl)borate, namely [Ph3C][B(C6F5)4].

[0019] Furthermore, the alkylaluminum co-catalyst is triisobutylaluminum, i.e., Al i Bu3.

[0020] Furthermore, the molar ratio of the main catalyst, the organoborate co-catalyst, and the alkylaluminum co-catalyst is 1:(0.5-2):(5-200), more preferably 1:1:10.

[0021] Furthermore, the meta-halostyrene monomer is one or more of the following: m-fluorostyrene (mFSt), m-chlorostyrene (mClSt), m-bromostyrene (mBrSt), and m-iodostyrene (mISt).

[0022] Further, the methoxyhalostyrene is one or more of 4-fluoro-2-methoxystyrene (2,4-FMOS), 5-fluoro-2-methoxystyrene (2,5-FMOS), 6-fluoro-2-methoxystyrene (2,6-FMOS), 5-chloro-2-methoxystyrene (2,5-ClMOS), 5-bromo-2-methoxystyrene (2,5-BrMOS), and 5-iodo-2-methoxystyrene (2,5-IMOS).

[0023] Furthermore, the molar ratio of the meta-halostyrene monomer or methoxyhalostyrene monomer to the main catalyst is (200~600):1.

[0024] Furthermore, the polymerization reaction temperature is preferably 20~30℃, more preferably 20℃, and the reaction time is 0.3~72 hours.

[0025] Furthermore, the organic solvent is selected from any one of toluene, n-hexane, and dichloromethane, preferably toluene.

[0026] Furthermore, the terminating agent is a methanol solution.

[0027] Furthermore, the precipitant is a methanol solution.

[0028] The polymers described are all highly syndiotactic selectivity (rrrr>99%), with a number average molecular weight ( M n It can reach 0.4×10 4 ~526.86×10 4 g·mol -1 .

[0029] This invention provides a method for regulating the copolymerization reaction of meta-halostyrene and styrene, comprising the following steps:

[0030] (1) Under the protection of an inert gas, the above-mentioned CGC rare earth metal complex C, organoborate cocatalyst and alkyl aluminum cocatalyst are mixed in an organic solvent to form a catalytic system.

[0031] (2) Add a mixture of meta-halostyrene monomer and styrene or a mixture of methoxyhalostyrene monomer and styrene to the above catalytic system and carry out a copolymerization reaction at room temperature.

[0032] (3) After the polymerization reaction is completed, a terminator is added to terminate the reaction, and the reaction mixture is poured into a precipitant to precipitate and obtain the polymer.

[0033] Furthermore, the rare earth metal complex main catalyst is a CGC-type rare earth metal dialkyl complex C, with the structure shown in the formula (2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF.

[0034] Furthermore, the organoborate cocatalyst is triphenylcarbazo(pentafluorophenyl)borate, namely [Ph3C][B(C6F5)4].

[0035] Furthermore, the alkylaluminum co-catalyst is triisobutylaluminum, i.e., Al i Bu3.

[0036] Furthermore, the molar ratio of the main catalyst, the organoborate co-catalyst, and the alkylaluminum co-catalyst is 1:1:10.

[0037] Furthermore, the meta-halostyrene monomer is one or more of the following: m-fluorostyrene (mFSt), m-chlorostyrene (mClSt), m-bromostyrene (mBrSt), and m-iodostyrene (mISt).

[0038] Further, the methoxyhalostyrene is one or more of 4-fluoro-2-methoxystyrene (2,4-FMOS), 4-chloro-2-methoxystyrene (2,4-ClMOS), 4-bromo-2-methoxystyrene (2,4-BrMOS), and 4-iodo-2-methoxystyrene (2,4-IMOS).

[0039] Furthermore, the molar ratio of the meta-halostyrene monomer to the styrene monomer is 1:5 to 5:1.

[0040] Furthermore, the molar ratio of the methoxyhalostyrene monomer to the styrene monomer is 1:5 to 5:1.

[0041] Furthermore, the molar ratio of the meta-halostyrene monomer to the main catalyst is (100-500):1.

[0042] Furthermore, the molar ratio of the methoxyhalostyrene monomer to the main catalyst is (100-500):1.

[0043] Furthermore, the polymerization reaction temperature is preferably 20~30℃, more preferably 25℃, and the reaction time is 1 min~180 min.

[0044] Furthermore, the organic solvent is selected from any one of toluene, n-hexane, and dichloromethane, preferably toluene.

[0045] Furthermore, the terminating agent is a methanol solution.

[0046] Furthermore, the precipitant is a methanol solution. Beneficial effects

[0047] (1) Highly efficient and highly syndiotactic selective polymerization of meta-halostyrene was achieved for the first time: This invention modifies the electronic effect of CGC-type ligands to adjust the Lewis acidity of the rare earth metal center, so that the Lewis acidity of the metal center matches the weak Lewis basicity of the meta-halostyrene monomer, thus achieving for the first time highly syndiotactic selective homopolymerization (rrrr>99%) of meta-substituted halostyrene (mF / Cl / Br / ISt). Among them, a yttrium catalyst C((2,7-) containing an electron-donating group (2,7-di-tert-butyl) fluorenyl ligand is used. t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF), due to the weakest Lewis acidity of its metal center, exhibits the strongest coordination ability with the weakly Lewis basic meta-halostyrene, thus displaying the highest polymerization activity—achieving a conversion rate of 94% within 1 hour at 200 equivalents of mFSt, with an activity of 2.28 × 10⁻⁶. 6 g·molcat -1 ·h -1 When catalyzed at 600 equivalent mFSt, the conversion rate reached 86% within 1 hour, and the polymer molecular weight reached 16.9 × 10⁻⁶. 4 g·mol -1 .

[0048] (2) Precise control of monomer content in meta-halostyrene-styrene copolymers is achieved: This invention uses CGC-type yttrium catalyst C((2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF) catalyzes the copolymerization reaction of m-halostyrene (mF / Cl / Br / ISt) with styrene (St), exhibiting high copolymerization activity (up to 4.4 × 10⁻⁶). 5 ~3.6×10 6 g·mol cat -1 ·h -1 The content of the intermediate halogenated styrene in the copolymer can be adjusted within the range of 5–79 mol% according to the feed ratio. The resulting copolymer has a high molecular weight ( M n = 6.6 × 10 4 ~16.9×10 4 g·mol -1 ) and a narrower molecular weight distribution ( M w / M n <2), and the unimodal distribution proves that the obtained product is a copolymer rather than a simple blend of homopolymers.

[0049] (3) Ultra-high molecular weight polymerization of methoxyhalostyrene was achieved: This invention discovered that using CGC-type scandium catalyst A ((2,7- t Bu2-FluCH2CH2NMe2)Sc(CH2SiMe3)2, due to the strong Lewis acidity of its scandium center, its small ionic radius, and the steric hindrance effect generated by its large-volume ligands, effectively suppresses the chain growth stage. β -H elimination yielded ultra-high molecular weight polyoxymethyl halogenated styrene with a number average molecular weight of 255.14 × 10⁻⁶. 4 ~526.86×10 4 g·mol -1 .

[0050] (4) The invention reveals the law governing the regulation of polymerization performance by ligand electronic effects: Through systematic research on the polymerization behavior of meta-halostyrene catalyzed by a series of CGC-type rare earth catalysts with different electron-donating capabilities, the following law was revealed: For meta-halostyrene with weak Lewis basicity, reducing the Lewis acidity of the metal center is beneficial to improving polymerization activity; while for monomers with strong Lewis basicity, it is necessary to appropriately enhance the Lewis acidity of the metal center. This discovery provides theoretical guidance for the rational design of rare earth catalysts suitable for monomers with different polarities.

[0051] (5) High syndiotactic selectivity of the polymer: The poly(m-halostyrene) and m-halostyrene-styrene copolymers obtained in this invention both exhibit excellent syndiotactic selectivity (rrrr>99%), endowing the polymers with excellent crystallinity and thermal properties. The glass transition temperature of the polymer ( T g ) and melting point ( T m The amount can be adjusted by the type and content of the comonomer. Attached Figure Description

[0052] Figure 1 Catalyst C in Example 3 + Reaction energy diagram for catalytic insertion of the first molecule mFSt monomer.

[0053] Figure 2 Catalyst C in Example 3 + Reaction energy diagram of the first three mFSt monomer insertions catalyzed.

[0054] Figure 3 This describes the polymerization mechanism of methoxyhalostyrene catalyzed by rare earth catalyst C in Example 4. Detailed Implementation

[0055] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described below in conjunction with embodiments.

[0056] Example 1: Synthesis of CGC rare earth metal catalysts A / E / F.

[0057] First, the reactor was placed in a glove box, and ScCl3(THF)3 (3.76 g) was dissolved in THF solution (-30℃) to obtain mixture a; Further, cold THF solvent was added to LiCH2SiMe3 (2.83 g, 3 equiv.) to obtain mixture b; Further, mixture b is slowly added dropwise to mixture a under stirring conditions to obtain mixture c, and the reaction continues for 2 hours; Furthermore, the solvent is removed under vacuum; Further, the product was extracted with n-hexane and recrystallized to obtain crystal d; Further, crystal d (0.92 g) was dissolved in THF solution to obtain mixture e; Further, [Et3NH][BPh4] (0.68 g, 1 equiv.) was added to mixture e to obtain mixture f, and the reaction was continued for 12 h; Further, the solvent was removed under vacuum and the mixture was extracted with anhydrous diethyl ether, then dried to obtain g of solid. Further, solid g (0.7 g) was dissolved in THF solution to obtain mixture h; Furthermore, the fluorene ligand (2,7- t Bu2-FluCH2CH2NMe2 or FluCH2CH2NMe2) or indene-indole ligand (5-Me-IndCH2CH2NMe2) (1 equiv.) was dissolved in THF solution (-30℃) to give mixture i; Furthermore, the mixture h is slowly added dropwise to the mixture i under stirring conditions, and the reaction continues for 6 h; Finally, the product was extracted with toluene and recrystallized to obtain the CGC rare earth metal catalyst A / F / E described in this invention.

[0058] Example 2: Synthesis of CGC rare earth metal catalysts B / C / D / G.

[0059] First, place the reactor in a glove box and add the fluorene ligand (2,7- t Bu2-FluCH2CH2NMe2 or FluCH2CH2NMe2) or indene-indole ligand (5-Me-IndCH2CH2NMe2) is dissolved in Et2O solution (-30℃) to give mixture a; Further, under stirring conditions, 1.1 equivalents of n-butyllithium were slowly added dropwise to mixture a to obtain mixture b, and the reaction was continued for 2 h. Further, the solvent was removed under vacuum, and cold toluene solvent (-30℃) was added to obtain mixture c; Further, cold toluene solvent is added to LuCl3(THF). 3.5 Or YCl3(THF) 3.5 In the middle, we obtain mixture d; Further, mixture c was slowly added dropwise to mixture d, and the reaction was continued with stirring for 6 hours. After the reaction was completed, it was cooled to -30 °C to obtain mixture e. Further, cold toluene solvent was added to LiCH2SiMe3 (5.0 mmol) to obtain mixture f; Furthermore, mixture e was slowly added dropwise to mixture f, and the reaction was continued with stirring for 6 hours; Furthermore, the solvent is removed under vacuum; Finally, the CGC rare earth metal catalyst B / C / D / G of the present invention was obtained by recrystallization from a mixed solution of n-hexane and toluene at -30°C.

[0060] Example 3: Modifying CGC-type ligands to regulate the homopolymerization activity and molecular weight of meta-halostyrene.

[0061] The reactor was placed in a glove box, and 10 μmol of catalyst, 10 μmol of [Ph3C][B(C6F5)4], and 100 μmol of Al were added sequentially to the flask. i Bu3 and 0.8 mL toluene were stirred for 2 minutes. Then meta-halostyrene was added, and after reacting for a certain time, the reaction was terminated by removing the glove box and rinsing with methanol solution. The product was then vacuum dried at 40 °C to constant weight to obtain poly(meta-halostyrene) (P(mF / Cl / Br / ISt)s).

[0062] Table 1: Serial Number monomer catalyst Monomer / Catalyst Time (h) Yield (%) <![CDATA[Activity (10 4 g·mol cat -1 ·h -1 )]]> rrrr(%) <![CDATA[ M n (10 4 )]]> <![CDATA[ M w / M n ]]> <![CDATA[ T g (℃)]]> 1 mFSt E 200:1 72 trace — — — — — 2 mFSt F 200:1 72 trace — — — — — 3 mFSt A 200:1 48 55 0.03 99 0.5 1.59 — / 258 4 mFSt D 200:1 12 41 0.08 99 0.4 2.14 — / 257 5 mFSt G 200:1 12 88 0.18 99 0.5 1.85 — / 256 6 mFSt C 200:1 1 94 2.28 99 1.0 2.44 — / 270 7 mFSt C 600:1 1 86 6.06 99 16.9 1.60 — / 275 8 mClSt C 200:1 1 100 2.80 99 3.6 2.80 90 / — 9 mClSt C 600:1 1 88 7.36 99 7.6 2.13 89 / — 10 mBrSt C 200:1 1 100 3.66 99 4.3 2.99 101 / 311 11 mBrSt C 600:1 1 82 8.95 99 29.4 2.11 98 / — 12 mISt C 200:1 3 100 1.53 99 1.4 3.00 105 / 240 13 mISt C 600:1 3 81 3.72 99 4.1 3.29 88 / —

[0063] Using a modified supporting ligand regulation strategy, a series of CGC-type rare earth catalysts (A, C, E, F, G, and H) with different electron-donating abilities were investigated for the homopolymerization of meta-fluorostyrene (mFSt). Although these rare earth catalysts all exhibited high syndiotactic selectivity (rrrr>99%) for the homopolymerization of mFSt, catalyst C showed the highest polymerization activity. This is because the metal center of rare earth catalyst C possesses the weakest Lewis acidity and the strongest coordination ability with the weakly Lewis basic m-fluorostyrene. Furthermore, catalyst C also achieved hypersyndiotactic polymerization of other meta-halostyrene (m-Cl / Br / ISt).

[0064] Example 4: Modifying CGC-type ligands to regulate the homopolymerization activity and molecular weight of methoxyhalostyrene.

[0065] The reactor was placed in a glove box, and 10 μmol of catalyst, 10 μmol of [Ph3C][B(C6F5)4], and 100 μmol of Al were added sequentially to the flask. i Bu3 and 1.5 mL of toluene were stirred for 2 minutes. Then, methoxyhalostyrene was added, and after reacting for a certain period of time, the reaction was terminated by removing the glove box and rinsing with methanol solution. The mixture was then vacuum dried at 40 °C to constant weight to obtain poly(methoxyhalostyrene) (P(2,4- / 2,5- / 2,6-FMOS, 2,5-Cl / Br / IMOS)s).

[0066] Table 2: Serial Number monomer catalyst Monomer / Catalyst Time (h) Yield (%) <![CDATA[activity (10 4 g·mol cat -1 ·h -1 )]]> rrrr(%) <![CDATA[ M n (10 4 )]]> <![CDATA[ M w / M n ]]> <![CDATA[ T g (℃)]]> 1 2,4-FMOS A 200:1 1 77 2.3 99 255.1 1.91 92 / 244 2 2,6-FMOS A 200:1 1 73 2.2 99 ndf ndf 122 / — 3 2,5-FMOS A 200:1 1 66 2.0 99 526.9 1.44 92 / 244 4 2,4-FMOS B 200:1 2 57 0.8 99 1.5 1.67 90 / — 5 2,6-FMOS B 200:1 2 71 1.1 99 1.5 1.77 117 / — 6 2,5-FMOS B 200:1 1.3 74 1.7 99 1.5 1.17 86 / 203 7 2,4-FMOS C 200:1 2 80 1.2 99 1.0 1.59 89 / 238 8 2,6-FMOS C 200:1 2 93 1.4 99 3.6 1.26 122 / — 9 2,5-FMOS C 200:1 0.3 94 8.6 99 3.6 1.31 92 / — 10 2,5-FMOS C 600:1 0.3 75 20.5 99 7.1 1.28 94 / — 11 2,5-CIMOS C 200:1 1.5 86 2.1 99 1.4 2.38 111 / 230 12 2,5-CIMOS C 600:1 1.5 77 5.1 99 3.4 3.17 112 / 228 13 2,5-BrMOS C 200:1 4 76 0.8 99 0.6 2.30 122 / 241 14 2,5-BrMOS C 600:1 4 72 2.3 99 1.4 3.25 125 / 257 15 2,5-IMOS C 200:1 4 71 0.9 99 0.4 3.11 127 / — 16 2,5-IMOS C 600:1 4 66 2.6 99 1.3 3.72 132 / —

[0067] Using a modified supporting ligand regulation strategy, a series of disubstituted methoxyhalostyrene (2,4- / 2,5- / 2,6-FMOS, 2,5-Cl / Br / IMOS) were achieved through ultra-high molecular weight, highly syndiotactic selectivity homopolymerization (rrrr>99%) with a series of CGC-type rare earth catalysts A, B, and C. This was because the electronic effect of the strong Lewis acid at the scandium center, as well as the steric hindrance effect generated by the small ionic radius and large ligand, suppressed the chain growth stage. β The elimination of -H yields polymers with ultra-high molecular weights.

[0068] The electron-withdrawing effect of halogen groups at the meta position of the styrene benzene ring is stronger than that at the ortho and para positions. Therefore, the Lewis basicity of 2,5-FMOS vinyl groups is weaker than that of 2,4-FMOS and 2,6-FMOS. The coordination interaction between the weakly Lewis-based lutetium catalyst B and yttrium catalyst C and 2,5-FMOS is stronger than that of 2,4-FMOS and 2,6-FMOS, thus 2,5-FMOS exhibits higher polymerization activity under the catalysis of lutetium catalyst B and yttrium catalyst C. Conversely, the strongly basic scandium catalyst A exhibits slightly higher polymerization activity than 2,5-FMOS when catalyzing the C=C double bond of the relatively strong Lewis basic 2,4-FMOS and 2,6-FMOS.

[0069] Example 5: Catalyst C catalyzes the copolymerization reaction of meta-halostyrene with styrene.

[0070] Place the reactor in a glove box and add 10 μmol of catalyst C, 10 μmol of [Ph3C][B(C6F5)4], and 100 μmol of Al to the flask in sequence. i Bu3 and 1.0 mL of toluene were stirred for 2 minutes. Then, a mixture of meta-halostyrene monomer (mXSt) and styrene monomer (St) (total monomer amount 6000 μmol) was added. After reacting for a certain period of time, the reaction was terminated by removing the glove box and rinsing with methanol solution. The copolymer was then dried under vacuum at 40 °C to constant weight to obtain copolymer P(mF / Cl / Br / ISt-co-St)s.

[0071] Table 3: Serial Number meta-halostyrene meta-halo-styrene / styrene Time (h) Yield (%) <![CDATA[activity (10 5 g·mol cat -1 ·h -1 )]]> Meta-halostyrene content (%) <![CDATA[ M n (10 4 )]]> <![CDATA[ M w / M n ]]> <![CDATA[ T g (℃)]]> 1 mFSt 100:500:1 1 79 30.6 7 11.5 1.94 100 / 268 2 mFSt 200:400:1 1 75 32.4 19 14.5 1.70 98 / 259 3 mFSt 300:300:1 3 73 10.4 35 12.8 1.61 98 / 253 4 mFSt 400:200:1 3 64 10.0 52 16.9 1.55 97 / 250 5 mFSt 500:100:1 8 83 4.4 78 14.8 1.57 93 / 271 6 mClSt 100:500:1 1 91 36.0 15 12.1 1.44 100 / 254 7 mClSt 200:400:1 1 78 32.3 21 12.7 1.56 98 / 240 8 mClSt 300:300:1 2 72 15.7 31 11.0 1.88 97 / 250 9 mClSt 400:200:1 10 67 3.1 33 6.6 1.61 96 / 250 10 mClSt 500:100:1 15 70 2.2 55 9.9 1.74 95 / 251 11 mBrSt 100:500:1 1 72 30.2 5 14.4 1.78 100 / 255 12 mBrSt 200:400:1 1 70 33.1 9 13.7 1.70 102 / 239 13 mBrSt 300:300:1 3 68 11.6 18 18.2 1.71 101 / — 14 mBrSt 400:200:1 10 95 5.3 48 6.4 3.33 101 / — 15 mBrSt 500:100:1 15 94 3.8 67 9.9 2.64 109 / — 16 mISt 100:500:1 1 84 37.9 20 9.9 1.86 101 / 242 17 mISt 200:400:1 1 85 44.9 28 14.2 1.59 107 / — 18 mISt 300:300:1 5 99 12.0 49 7.0 2.69 101 / — 19 mISt 400:200:1 10 99 6.72 59 4.4 3.07 105 / — 20 mISt 500:100:1 30 86 2.2 79 5.5 2.62 109 / —

[0072] Table 3 shows that the content of mFSt in the copolymer can be adjusted within the range of 7–78 mol% according to the feed ratio. The copolymerization activity is significantly higher than that of mFSt, which may be because styrene has higher polymerization activity, thus increasing the copolymerization activity. The content of mClSt in the copolymer can be adjusted within the range of 15–55 mol%, the content of mBrSt in the copolymer can be adjusted within the range of 5–67 mol%, and the content of mISt in the copolymer can be adjusted within the range of 20–79 mol%.

[0073] Example 6: Catalyst C catalyzes the copolymerization reaction of methoxyhalostyrene and styrene.

[0074] Place the reactor in a glove box and add 10 μmol of catalyst C, 10 μmol of [Ph3C][B(C6F5)4], and 100 μmol of Al to the flask in sequence. i Bu3 and 1.0 mL of toluene were stirred for 2 minutes. Then, a mixture of methoxyhalostyrene (2,5-XMOS) and styrene monomer (St) (total monomer amount 600 μmol) was added. After reacting for a certain period of time, the reaction was terminated by removing the glove box and rinsing with methanol solution. The mixture was then vacuum dried at 40 °C to constant weight to obtain copolymer P(2,5-F / Cl / Br / IMOS-co-St)s.

[0075] Table 4: Serial Number Methoxyhalostyrene Methoxyhalostyrene / styrene Time (h) Yield (%) <![CDATA[Activity (10 4 g·mol cat -1 ·h -1 )]]> Methoxylated halostyrene content (%) <![CDATA[ M n (10 4 )]]> <![CDATA[ M w / M n ]]> <![CDATA[ T g (℃)]]> 1 2,5-FMOS 100:500:1 90 90 4.0 15 9.7 1.73 98 / 252 2 2,5-FMOS 200:400:1 90 98 4.7 32 9.9 1.69 97 / 251 3 2,5-FMOS 300:300:1 120 93 3.6 49 9.9 1.32 95 / 252 4 2,5-FMOS 400:200:1 120 98 4.0 64 6.7 1.99 96 / 250 5 2,5-FMOS 500:100:1 120 96 4.1 82 11.4 1.28 95 / — 6 2,5-CIMOS 100:500:1 60 95 6.6 14 8.8 1.79 101 / 250 7 2,5-CIMOS 200:400:1 60 97 7.1 32 7.0 1.87 102 / 250 8 2,5-CIMOS 300:300:1 180 88 2.4 49 4.6 2.47 106 / 250 9 2,5-CIMOS 400:200:1 180 99 2.9 66 5.3 2.25 108 / — 10 2,5-CIMOS 500:100:1 180 99 3.1 81 5.3 2.14 111 / — 11 2,5-BrMOS 100:500:1 45 91 8.9 16 5.1 1.84 104 / — 12 2,5-BrMOS 200:400:1 60 84 7.0 33 4.4 2.18 108 / — 13 2,5-BrMOS 300:300:1 180 97 3.0 49 5.3 1.99 114 / — 14 2,5-BrMOS 400:200:1 180 88 3.1 67 5.2 1.83 118 / — 15 2,5-BrMOS 500:100:1 180 82 3.2 91 4.9 1.88 125 / — 16 2,5-IMOS 100:500:1 50 86 8.0 15 4.6 2.28 104 / — 17 2,5-IMOS 200:400:1 90 92 5.8 31 3.8 2.37 109 / — 18 2,5-IMOS 300:300:1 180 98 3.6 50 3.1 2.46 — / — 19 2,5-IMOS 400:200:1 180 92 3.8 66 3.3 2.14 124 / — 20 2,5-IMOS 500:100:1 180 96 4.5 82 2.3 2.68 — / —

[0076] The copolymerization results under different feed ratios showed that the content of 2,5-FMOS in the copolymer could be adjusted within the range of 14–91 mol%, and the copolymerization activity was 3.6 × 10⁻⁶. 4 ~4.7×10 4 g·mol cat -1 ·h -1 number-average molecular weight of copolymers M n = 6.7 × 10 4 ~11.4×10 4 g·mol -1 .

[0077] This invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.

Claims

1. A method for regulating the activity and molecular weight of rare-earth catalytic meta-halostyrene polymerization by modifying CGC-type ligands, characterized in that, Includes the following steps: A series of CGC-type rare earth catalysts having the general formula (L)Ln(CH2SiMe3)2(THF) n are provided, wherein L is a fluorenyl ligand R1-Flu-CH2CH2NMe2 (R1 is the same or different group, each being one of a hydrogen atom, a methyl group, an ethyl group, an iso-propyl group, a tert-butyl group, a n-butyl group, an alkoxy group, a diethylamino group, an amino group, a chlorine atom, a fluorine atom, an iodine atom, a bromine atom, a nitro group, a phenyl group, a benzyl group, a naphthyl group) or an indenoindol ligand 5-R2-IndCH2CH2NMe2 (R2 is the same or different group, each being one of a hydrogen atom, a methyl group, an ethyl group, an iso-propyl group, a tert-butyl group, a n-butyl group, an alkoxy group, a diethylamino group, an amino group, a chlorine atom, a fluorine atom, an iodine atom, a bromine atom, a nitro group, a phenyl group, a benzyl group, a naphthyl group), and Ln is one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium or lutetium. By adjusting the electron-donating ability of the ligand L and / or changing the type of metal center Ln, the Lewis acidity of the rare earth metal center is controlled to match the Lewis basicity of the m-halostyrene monomer. In the presence of a co-catalyst, the CGC-type rare earth catalyst is used to catalyze the homopolymerization of meta-halostyrene monomers or their copolymerization with styrene, thereby enabling the regulation of the polymerization activity and the molecular weight of the resulting polymer.

2. The method according to claim 1, characterized in that, The methods for regulating the Lewis acidity of rare earth metal centers include: (1) Introduce an electron-donating group 2,7-di-tert-butyl to the fluorenyl ligand or replace the fluorenyl ligand with an indene-indole ligand to reduce the Lewis acidity of the metal center; (2) Replace the Lewis acidity of the metal center with Sc, which has a strong Lewis acidity, or Y or Lu, which has a weaker Lewis acidity, to reduce the Lewis acidity of the metal center.

3. The method according to claim 1, characterized in that, For weakly Lewis basic meta-halostyrene monomers, a combined catalyst consisting of a fluorenyl ligand modified with an electron-donating group and a weakly Lewis acidic metal center is used to reduce the Lewis acidity of the metal center and improve polymerization activity. The weakly Lewis basic meta-halostyrene monomer is selected from m-fluorostyrene, m-chlorostyrene, m-bromostyrene, or m-iodostyrene. The organoborate co-catalyst is triphenylcarbazone (pentafluorophenyl)borate. The alkylaluminum co-catalyst is triisobutylaluminum. The organic solvent is selected from toluene, n-hexane, and dichloromethane, preferably toluene. The catalyst is (2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF, i.e., catalyst C; the molar ratio of the CGC-type rare earth catalyst, organoboron salt compound and organoaluminum compound is 1:(0.5-2):(5-200), preferably 1:1:10; the molar ratio of the meta-halostyrene monomer to the catalyst is (200-600):1, the polymerization reaction temperature is 20-30℃, and the reaction time is 0.3-72 hours.

4. The method according to claim 1, characterized in that, For Lewis-based methoxyhalostyrene monomers, a catalyst combining a strongly Lewis acidic scandium metal center and an electron-donating ligand is used to suppress β-H elimination during the chain growth stage, resulting in ultra-high molecular weight polymers. The methoxyhalostyrene is one or more of 4-fluoro-2-methoxystyrene (2,4-FMOS), 5-fluoro-2-methoxystyrene (2,5-FMOS), 6-fluoro-2-methoxystyrene (2,6-FMOS), 5-chloro-2-methoxystyrene (2,5-ClMOS), 5-bromo-2-methoxystyrene (2,5-BrMOS), and 5-iodo-2-methoxystyrene (2,5-IMOS). The catalyst is (2,7- t Bu2-FluCH2CH2NMe2)Sc(CH2SiMe3)2, i.e., catalyst A; the resulting polymer has a number-average molecular weight of up to 526.86 × 10⁻⁶. 4 g·mol -1 .

5. A method for regulating the copolymerization reaction of meta-halostyrene and styrene through ligand modification, characterized in that, Includes the following steps: A CGC-type rare earth catalyst (2,7-) composed of a fluorenyl ligand modified with an electron-donating group 2,7-di-tert-butyl and a yttrium metal center. t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF; In the presence of a co-catalyst, meta-halostyrene monomer and styrene monomer are mixed in an organic solvent at a molar ratio of 1:5 to 5:1 and copolymerized at 20 to 30°C. By adjusting the feed ratio of meta-halostyrene monomer to styrene monomer, the content of meta-halostyrene in the copolymer can be controlled within the range of 5 mol% to 91 mol%. The m-halostyrene monomer is selected from any one of m-fluorostyrene, m-chlorostyrene, m-bromostyrene, or m-iodostyrene; the methoxyhalostyrene is selected from any one of 4-fluoro-2-methoxystyrene, 4-chloro-2-methoxystyrene, 4-bromo-2-methoxystyrene, or 4-iodo-2-methoxystyrene.

6. The method according to claim 5, characterized in that, The molar ratio of the m-halostyrene monomer or methoxyhalostyrene monomer to the catalyst is (100–500):1; the activity of the copolymerization reaction can reach 2.4 × 10⁻⁶. 4 ~3.6×10 6 g·mol cat -1 ·h -1 The number-average molecular weight of the obtained copolymer was 2.3 × 10⁻⁶. 4 ~18.2×10 4 g·mol -1 Molecular weight distribution M w / M n < 3.

4.

7. A CGC-type rare earth catalyst for implementing the method according to any one of claims 1 to 6, characterized in that, It has the following general formula: (L)Ln(CH2SiMe3)2(THF) n Wherein, L is selected from the fluorene ligand R1-Flu-CH2CH2NMe2 (R1 is H or 2,7-). t Bu2) or indole ligand 5-Me-IndCH2CH2NMe2, R1 is selected from H or 2,7-di-tert-butyl; Ln is selected from Sc, Y or Lu; n is 0 or 1, when Ln is Sc n=0, when Ln is Y or Lu n=1.

8. The CGC-type rare earth catalyst according to claim 7, characterized in that, The catalyst is selected from any of the following compounds: Catalyst A: (2,7- t Bu2-FluCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst B: (2,7- t Bu2-FluCH2CH2NMe2)Lu(CH2SiMe3)2THF; Catalyst C: (2,7- t Bu2-FluCH2CH2NMe2)Y(CH2SiMe3)2THF; Catalyst D: (FluCH2CH2NMe2)Y(CH2SiMe3)2THF; Catalyst E: (FluCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst F: (5-Me-IndCH2CH2NMe2)Sc(CH2SiMe3)2; Catalyst G: (5-Me-IndCH2CH2NMe2)Y(CH2SiMe3)2THF.

9. The use of the catalyst according to any one of claims 1 to 8 in the preparation of meta-dimethyl styrene or meta-dimethyl styrene copolymers.