A high molecular weight homopolymer polypropylene resin, its preparation method and application
By using a catalyst system of α-cyanosuccinate and aminophenol compounds in propylene polymerization, the problem of poor flowability of ultra-high molecular weight polypropylene resin was solved, achieving high flowability and processability, and improving the physicochemical properties of polypropylene.
Patent Information
- Application Number
- CN202510638261.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, ultra-high molecular weight polypropylene has poor flowability, making it difficult to process.
By using α-cyanosuccinate and/or substituted α-cyanosuccinate as internal electron donors in a catalyst, combined with aminophenol compounds and a phosphorus-free catalyst system, propylene polymerization was carried out under low hydrogen concentration to prepare ultra-high molecular weight homopolymer polypropylene resin with high viscosity-average molecular weight and good flowability.
The prepared ultra-high molecular weight homopolymer polypropylene resin has good fluidity, can be processed and used normally, meets the melt flow rate requirements, and has excellent physicochemical properties.
Smart Images

Figure CN123106959A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polypropylene preparation technology, specifically relating to an ultra-high molecular weight homopolymer polypropylene resin, its preparation method, and its application. Background Technology
[0002] Polypropylene (PP) is a thermoplastic resin with numerous advantages and a wide range of applications, making it one of the most common general-purpose plastics. PP is lightweight, does not easily absorb moisture, is resistant to chemical corrosion, is foldable, has better heat resistance than polyethylene, and possesses good electrical insulation properties. However, these advantages are not homogeneous; the performance of PP depends on many influencing factors, including molecular weight and molecular weight distribution, crystallinity, the type and ratio of comonomers, and the isotactic index. Different types of PP exhibit different properties.
[0003] Ultra-high molecular weight polypropylene (UHMWPP) possesses extremely long molecular chains and excellent physicochemical properties, exhibiting superior strength, abrasion resistance, and oxidation resistance compared to ordinary polypropylene. However, its practical applications are limited by its inherent processing difficulties. This is reflected in melt flow index (MFI) testing; using UHMWPP resin for MFI testing may result in unsatisfactory results. Summary of the Invention
[0004] Based on the above analysis, the present invention aims to provide an ultra-high molecular weight homopolymer polypropylene resin, its preparation method and application, in order to solve the technical problem that ultra-high molecular weight polypropylene has poor flowability and is difficult to process in the prior art.
[0005] The objective of this invention is mainly achieved through the following technical solutions.
[0006] In a first aspect, the present invention provides an ultra-high molecular weight homopolymer polypropylene resin, wherein the viscosity-average molecular weight (Mv) of the ultra-high molecular weight homopolymer polypropylene resin is ≥11.8×10 5 g / mol; melt mass flow rate (MFR) at 230℃ and 21.6 kg load > 1 g / 10 min; in gel permeation chromatography (GPC) curves with x-axis as logMW and y-axis as dw / dlogM, the ratio of the left half-width to the right half-width of the peak position is greater than 1, and the ratio of the left half-width to the right half-width of the baseline at the peak position is greater than 2.1.
[0007] According to some embodiments of the present invention, the viscosity-average molecular weight (Mv) of the ultra-high molecular weight homopolymer polypropylene resin is 12 × 10⁻⁶. 5 ~20×10 5 g / mol.
[0008] According to some embodiments of the present invention, the melt flow rate (MFR) of the ultra-high molecular weight homopolymer polypropylene resin at 230°C and a load of 21.6 kg is 2-6 g / 10 min.
[0009] According to some embodiments of the present invention, in the gel permeation chromatography (GPC) curve of the ultra-high molecular weight homopolymer polypropylene resin with x-axis as logMW and y-axis as dw / dlogM, the ratio of the left half-width to the right half-width of the peak position is 1.1 to 1.2.
[0010] According to some embodiments of the present invention, in the gel permeation chromatography (GPC) curve of the ultra-high molecular weight homopolymer polypropylene resin with logMW on the x-axis and dw / dlogM on the y-axis, the ratio of the width to the right of the baseline at the peak position is greater than 2.2 to 3.
[0011] According to some embodiments of the present invention, the ultra-high molecular weight homopolymer polypropylene resin is a microsphere with a diameter of 50 to 1000 μm.
[0012] According to some embodiments of the present invention, the ultra-high molecular weight homopolymer polypropylene resin is a microsphere with a diameter of 50 to 200 μm.
[0013] According to some embodiments of the present invention, the ultra-high molecular weight homopolymer polypropylene resin is a microsphere with a diameter of 100-180 μm.
[0014] According to some embodiments of the present invention, the surface of the microsphere has spherical secondary particles connected to fibrous particles, which can give the microsphere a larger specific surface area.
[0015] According to some embodiments of the present invention, the ultra-high molecular weight homopolymer polypropylene resin contains cyano succinate.
[0016] According to some embodiments of the present invention, the content of cyanosuccinate in the ultra-high molecular weight homopolymer polypropylene resin is 1 to 100 ppm, preferably 2 to 20 ppm.
[0017] According to some embodiments of the present invention, the specific surface area of the ultra-high molecular weight homopolymer polypropylene resin is >90 m². 2 ·g -1 .
[0018] According to some embodiments of the present invention, the specific surface area of the ultra-high molecular weight homopolymer polypropylene resin is 95-130 m². 2 ·g -1 .
[0019] According to some embodiments of the present invention, the oxidation induction time of the ultra-high molecular weight homopolymer polypropylene resin is greater than 3 min.
[0020] According to some embodiments of the present invention, the oxidation induction time of the ultra-high molecular weight homopolymer polypropylene resin is 5 to 30 min (e.g., 5 min, 6 min, 7 min, 8 min, 10 min, 12 min, 15 min, 16 min, 18 min, 20 min, 22 min, 25 min, 27 min, 30 min, and any two of the above).
[0021] According to some embodiments of the present invention, the ultra-high molecular weight homopolymer polypropylene resin does not contain a detectable amount of P.
[0022] In a second aspect, the present invention provides a method for preparing the ultra-high molecular weight homopolymer polypropylene resin described in the first aspect, comprising: polymerizing propylene in the presence of a catalyst and optionally an aminophenolic compound to obtain the ultra-high molecular weight homopolymer polypropylene resin.
[0023] The catalyst includes a main catalyst, a co-catalyst, and an optional external electron donor;
[0024] The main catalyst includes magnesium, titanium, and an internal electron donor, wherein the internal electron donor includes α-cyanosuccinate and / or substituted α-cyanosuccinate.
[0025] The catalyst does not contain P;
[0026] The hydrogen concentration in the propylene is 0 to 10 ppm, preferably 0 to 3 ppm.
[0027] The preparation method provided by this invention uses α-cyanosuccinate and / or substituted α-cyanosuccinate as the internal electron donor of the catalyst, while limiting the catalyst to not containing components containing detectable amounts of P element. Under the condition that the hydrogen concentration is only 0 to 3 ppm, an ultra-high molecular weight homopolymer polypropylene resin with good flowability is prepared, so that the ultra-high molecular weight homopolymer polypropylene resin can be processed and used normally.
[0028] In this invention, "catalyst without P" means that the catalyst does not contain a detectable amount of phosphorus. In the preparation method provided by this invention, if the catalyst contains P, the molecular weight of the prepared product will decrease, making it impossible to obtain ultra-high molecular weight polypropylene.
[0029] According to some embodiments of the present invention, the ratio of the main catalyst to the liquid component in the polymerization reaction system is (0.1-20) mg:1 L, preferably (1-15) mg:1 L.
[0030] In this invention, the amount of catalyst is calculated based on the liquid components in the polymerization reaction system, which generally include liquid propylene and possible solvents.
[0031] According to some embodiments of the present invention, the aminophenol compound has the structural formula R'(NH2-C6H3-OH), wherein R' is selected from C1 to C6 alkyl or H.
[0032] According to some embodiments of the present invention, aminophenol compounds include at least one of 2-hydroxyaniline, 3-hydroxyaniline, 4-hydroxyaniline, and 3-methyl-2-hydroxyaniline.
[0033] According to some embodiments of the present invention, the molar ratio of the aminophenolic compound to the catalyst (based on Ti) is 0.001 to 5 (e.g., 0.001, 0.002, 0.005, 0.008, 0.01, 0.02, 0.03, 0.05, 0.08, 0.1, 0.15, 0.2, 0.26, 0.3, 0.33, 0.39, 0.4, 0.5, 0.55, 0.6, 0.65, ... The range is 0.7, 0.72, 0.77, 0.81, 0.85, 0.9, 0.95, 1, 1.1, 1.15, 1.2, 1.35, 1.5, 1.6, 1.7, 1.85, 1.9, 2, 2.2, 2.4, 2.5, 2.6, 2.8, 3, 3.3, 3.5, 3.8, 4, 4.4, 4.4, 4.5, 5, and any two of the above points), preferably 0.01 to 2.
[0034] According to some embodiments of the present invention, the molar ratio of the internal electron donor to magnesium is (0.01 to 0.2):1 (for example, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.15:1, 0.2:1, and any two of the above ranges), preferably (0.03 to 0.15):1.
[0035] According to some embodiments of the present invention, the α-cyanosuccinate and / or substituted α-cyanosuccinate are selected from at least one of the compounds shown in formula (III):
[0036]
[0037] In equation (III), R a R b Each is independently selected from C1 to C2. 14 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; Rc and R d Each is independently selected from H, C1 to C1. 14 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; R c and R d They can be optionally bonded together to form one or more fused ring structures.
[0038] According to some embodiments of the present invention, in formula (III), R a R b Each is independently selected from C1 to C2. 10 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; R c and R d Each is independently selected from C1 to C2. 10 Alkyl, C3-C 10 cycloalkyl, C6-C 20 Aryl, C7~C 20 Alkyl or C7~C 20 Aromatic group.
[0039] In this invention, the hydrogen atom on the aromatic ring (such as the benzene ring) of the aryl, alkylaryl, or aromatic hydrocarbon group can be optionally replaced by other atoms.
[0040] In this invention, "alkyl" includes straight-chain alkyl or branched-chain alkyl.
[0041] According to some embodiments of the present invention, the α-cyanosuccinate and / or substituted α-cyanosuccinate comprises at least one selected from: diethyl 2,3-diisopropyl-2-cyanosuccinate, diethyl 3-methyl-2-isopropyl-2-cyanosuccinate, diethyl 3-ethyl-2-isopropyl-2-cyanosuccinate, diethyl 3-propyl-2-isopropyl-2-cyanosuccinate, diethyl 3-butyl-2-isopropyl-2-cyanosuccinate, diethyl 3-phenyl-2-isopropyl-2-cyanosuccinate, diethyl 2,3-dicyclohexyl-2-cyanosuccinate, dibutyl 2,3-diisopropyl-2-cyanosuccinate, and diethyl 2-diisopropyl-3-cyclopentyl-2-cyanosuccinate.
[0042] According to some embodiments of the present invention, the internal electron donor further includes a dialkoxy-substituted alkane.
[0043] According to some embodiments of the present invention, the dialkoxy-substituted alkane is selected from (R 7 (R) 8 )C(OR 9 (OR) 10 At least one of ), wherein R 7 and R 8 Each is independently selected from hydrogen, C1 to C2. 20 Alkyl groups, C3-C 20 cycloalkyl, C6-C 20 aryl, C7~C 20 Aryl groups or C7-C 10 alkylaryl, R 7 and R 8 The links can be optionally keyed into a loop, R 9 and R 10 Each is independently selected from C1 to C2. 20 Alkyl groups; more preferably, R 7 and R 8 Each is independently selected from hydrogen, C1 to C2. 10 Alkyl groups, C3-C 10 cycloalkyl, C6-C 10 aryl, C7~C 10 Aryl groups or C7-C 10 alkylaryl, R 7 and R 8 The links can be optionally keyed into a loop; R 9 and R 10 Each is independently selected from C1 to C2. 10 Alkyl groups.
[0044] According to some embodiments of the present invention, the dialkoxylated alkane is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2,2 -Dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexylethyl)-1,3- Dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2 At least one of sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane, and 9,9-dimethoxymethylfluorene, for example selected from 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and / or 9,9-dimethoxymethylfluorene.
[0045] In this invention, the content of the dialkoxy-substituted alkanes can be either a partial replacement of α-cyanosuccinate and / or a substitution of α-cyanosuccinate, or an additional amount of dialkoxy-substituted alkanes can be added to the above-mentioned content of α-cyanosuccinate and / or a substitution of α-cyanosuccinate.
[0046] According to some embodiments of the present invention, the molar ratio of the diekoxy-substituted alkane to magnesium is (0.001 to 0.15):1 (for example, 0.001:1, 0.005:1, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.15:1, and any two of the above ranges), preferably (0.005 to 0.1):1.
[0047] According to some embodiments of the present invention, the magnesium element is derived from a magnesium-containing carrier. Various magnesium-containing carriers commonly used in the art can be used in the preparation method of the ultra-high molecular weight homopolymer polypropylene resin provided by the present invention.
[0048] According to some embodiments of the present invention, the magnesium-containing support includes a magnesium chloride alcohol support and / or an alkoxy magnesium support.
[0049] According to some embodiments of the present invention, the magnesium-containing carrier is spherical.
[0050] According to some embodiments of the present invention, the magnesium chloride alcohol carrier comprises the components shown in formula (I).
[0051] MgY 1 Y 2 ·mR'OH formula (I)
[0052] In equation (I), Y 1 Selected from halogens, preferably from chlorine or bromine; Y 2 Selected from halogens, alkyl groups, alkoxy groups, aryl groups, or aryloxy groups, preferably from chlorine, bromine, C1-C6 groups. 14 Alkyl, C1-C 14 Alkoxy, C6~C 14 Aryl or C6~C 14 Aryloxy group; R' is selected from one of halogenated or unsubstituted alkyl, halogenated or unsubstituted cycloalkyl, and halogenated or unsubstituted aralkyl, preferably from halogenated or unsubstituted C1 to C1. 12 Alkyl, halogen-substituted or unsubstituted C3-C 10 Cycloalkyl, halogen-substituted or unsubstituted C7-C 10 One of the aralkyl groups; m is 1 to 5 (e.g., 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, and any two of the above).
[0053] According to some embodiments of the present invention, in formula (I), Y 1 It is chlorine; Y 2 Selected from chlorine, bromine, C1-C5 alkyl, C1-C5 alkoxy, C6-C 10 Aryl or C6~C 10 Aryloxy group; R' is selected from halogen-substituted or unsubstituted C1-C8 alkyl groups, halogen-substituted or unsubstituted C3-C8 cycloalkyl groups, preferably from halogen-substituted or unsubstituted C1-C6 alkyl groups (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or n-hexyl); m is 1.2-3.5 (e.g., 1.5-2.8).
[0054] According to some embodiments of the present invention, MgY in formula (I) 1 Y 2 It is magnesium dichloride.
[0055] According to some embodiments of the present invention, the preparation of the magnesium chloride alcohol carrier is not particularly limited and can be carried out by any method disclosed in the prior art.
[0056] According to some embodiments of the present invention, the magnesium chloride alcohol carrier does not contain a detectable amount of P, and preferably does not contain a detectable amount of phosphate ester.
[0057] According to some embodiments of the present invention, the alkoxymagnesium support comprises the component shown in formula (II):
[0058] [R1O] m’ Mg[OCH(CHXR2)(R3)] n Equation (II);
[0059] In formula (II), R1 is selected from one of alkyl or halogen-substituted alkyl, cycloalkyl or halogen-substituted cycloalkyl; R2 and R3 are each independently one of hydrogen, alkyl or halogen-substituted alkyl; X is halogen; m' is 0.1 to 1.9, n is 0.1 to 1.9, and m'+n=2.
[0060] According to some embodiments of the present invention, in formula (II), R1 is selected from one of C1-C8 alkyl or halogen-substituted alkyl, C3-C8 cycloalkyl or halogen-substituted cycloalkyl; R2 and R3 are each independently one of hydrogen, C1-C5 alkyl or halogen-substituted alkyl; X is chlorine or bromine; m' is 0.8-1.2, n is 0.8-1.2, and m'+n=2.
[0061] According to some embodiments of the present invention, the alkoxymagnesium support does not contain a detectable amount of P, and preferably does not contain a detectable amount of phosphate ester.
[0062] The preparation of the alkoxymagnesium support shown in formula (II) of this invention is not particularly limited and can be carried out by any method disclosed in the prior art.
[0063] In this invention, the preparation of microspheres (e.g., particle diameter of 50–200 μm) of ultra-high molecular weight homopolymer polypropylene resin generally requires the use of a magnesium-containing carrier with uniform particle size and small particle size. For example, a magnesium-containing carrier can be prepared using the following method:
[0064] The preparation method of the magnesium-containing support includes the following steps:
[0065] S1: Magnesium halide with the general formula MgX"Y and a first alcohol compound with the general formula R7OH are subjected to a first contact and emulsification to obtain the first product;
[0066] S2: A second contact is made between an ethylene oxide compound having the structure shown in formula (II) and the first product to obtain a second product;
[0067] S3: Includes formula R 10 OH- halogenated alcohols, with the general formula R 11 The second alcoholic compound of OH undergoes a third contact with the second product to yield the third product;
[0068] S4: Spray dry the third product to obtain a magnesium-containing support.
[0069] According to some embodiments of the present invention, as a specific embodiment of the present invention, in S1, in the general formula MgX"Y, X" is selected from fluorine, chlorine, bromine or iodine; Y is selected from fluorine, chlorine, bromine, iodine, C1-C6 alkyl, C1-C6 alkoxy, C6-C 14 aryl or C6~C 14 aryloxy groups.
[0070] According to some embodiments of the present invention, X" is selected from chlorine or bromine, and Y is selected from chlorine, bromine, and C. 1-5 Alkyl groups, C1-C5 alkoxy groups, C6-C 10 aryl or C6~C 10 aryloxy groups.
[0071] According to some embodiments of the present invention, the magnesium halide is selected from at least one of magnesium chloride, magnesium bromide, magnesium phenoxychloride, magnesium isopropoxychloride, and magnesium n-butoxychloride, preferably magnesium chloride.
[0072] According to some embodiments of the present invention, in the formula R7OH, R7 is C1 to C2. 10 Alkyl groups.
[0073] According to some embodiments of the present invention, in step S2, the ethylene oxide compound has the structural formula shown in formula (II).
[0074]
[0075] Among them, R8 and R9 are each independently selected from H, C1 to C1. 10 Alkyl groups, C1-C1 groups substituted with 1 to 10 halogen atoms 10 The haloalkyl group; preferably, R8 and R9 are each independently selected from H, C1 to C5 alkyl groups, and C1 to C5 haloalkyl groups substituted with 1 to 10 halogen atoms.
[0076] According to some embodiments of the present invention, the ethylene oxide compound is selected from at least one of ethylene oxide, propylene oxide, butane oxide, epichlorohydrin, chlorobutane, bromopropane, and bromobutane.
[0077] According to some embodiments of the present invention, in S3, the formula R 10 In OH, R 10 Choose C1 to C2 atoms that are substituted with at least one halogen atom. 10 Halogenated alkyl groups, C6-C6 groups substituted with at least one halogen atom 20 Halogenated aryl groups.
[0078] According to some embodiments of the present invention, the haloalcohol can be a monohaloalcohol or a polyhaloalcohol, preferably a chloroalcohol, a bromoalcohol, or an iodoalcohol, such as 2,2,2-trichloroethanol, 2,2-dichloroethanol, 2-chloroethanol, 3-chloro-1-propanol, 6-chloro-1-hexanol, 3-bromo-1-propanol, 5-chloro-1-pentanol, 4-chloro-1-butanol, 2-chlorocyclohexanol, 1,2-dichloroethanol, 1,3-dichloropropanol, 1,4-dichlorobutanol, or 2-iodoethanol, etc.
[0079] However, in order to obtain a catalyst support with better performance, according to some embodiments of the present invention, in formula R... 10 In OH, R 10 Choose C1 to C2 atoms that are substituted with at least two halogen atoms. 10 Halogenated alkyl groups, C6-C6 groups substituted with at least two halogen atoms 20 The halogenated aryl group, wherein the halogen atom is selected from at least one of chlorine, bromine and iodine atoms.
[0080] According to some embodiments of the present invention, the haloalcohol is selected from at least one of 2,2,2-trichloroethanol, 2,2-dichloroethanol, 1,2-dichloroethanol, 1,3-dichloropropanol, and 1,4-dichlorobutanol.
[0081] According to some embodiments of the present invention, the formula R 11 In OH, R 11 It is an alkyl group from C1 to C5.
[0082] In this invention, the second alcohol compound is ethanol, methanol, n-propanol, isopropanol, n-butanol, or isobutanol. However, in order to obtain a catalyst support with better performance, according to some embodiments of the present invention, in formula R... 11 In OH, R 11 It is a C1 to C2 alkyl group, that is, the second alcohol compound is methanol and / or ethanol.
[0083] According to some embodiments of the present invention, the amount of the haloalcohol used is 0.05 to 6.5 mol relative to 1 mol of the magnesium halide, and the amount of the second alcohol compound used is 5 to 100 mol.
[0084] When the amount of haloalcohols and alcohols is too large, the resulting catalyst support will clump together and cannot be used for subsequent operations.
[0085] According to some embodiments of the present invention, the amount of the first alcohol compound is 1 to 30 mol relative to 1 mol of the magnesium halide, and the amount of the ethylene oxide compound is 1 to 10 mol.
[0086] According to some embodiments of the present invention, relative to 1 mol of the magnesium halide, the amount of the first alcohol compound is 6 to 22 mol, the amount of the ethylene oxide compound is 2 to 6 mol, the amount of the haloalcohol is 1 to 5 mol, and the amount of the second alcohol compound is 8 to 80 mol, more preferably 31 to 50 mol.
[0087] It should be noted that the trace amounts of water carried in the above reactants will also participate in the reaction to form the spherical carrier. Therefore, the prepared spherical carrier may contain trace amounts of water from the reactants and reaction medium. This should not be construed as a limitation of the present invention by those skilled in the art.
[0088] According to some embodiments of the present invention, the first contact in S1 is carried out under stirring conditions, the conditions of which include: a temperature of 80 to 120°C and a time of 0.5 to 5 hours.
[0089] According to some embodiments of the present invention, in S1, the conditions for the first contact include: a temperature of 80 to 100°C and a time of 0.5 to 3 hours.
[0090] In S1, the present invention does not particularly limit the specific operation method of emulsification, and methods known to those skilled in the art can be used. For example, emulsification can be performed using low-speed shearing or high-speed shearing. According to some embodiments of the present invention, when using low-speed shearing, the stirring rate of the low-speed shearing is 400-800 rpm. The method of high-speed shearing is known to those skilled in the art, for example, using the high-speed stirring speed disclosed in CN1330086A. In addition, the emulsification operation can also be performed with reference to the methods disclosed in the following patent applications, such as the rotary dispersion of a solution containing liquid magnesium halide compounds in a hypergravity bed (rotation speed of 100-3000 rpm) disclosed in CN1580136A; another example is the output of a solution containing liquid magnesium halide adducts in an emulsifier at a speed of 1500-8000 rpm disclosed in CN1463990A; and yet another example is the emulsification of a solution containing liquid magnesium halide adducts by spraying method disclosed in US6020279A.
[0091] According to some embodiments of the present invention, in S2, the conditions for the second contact include: a temperature of 50 to 120°C and a time of 20 to 60 minutes; preferably, the conditions for the second contact include: a temperature of 80 to 100°C and a time of 20 to 50 minutes.
[0092] According to some embodiments of the present invention, step S3 further includes washing the second product with an inert solvent and then reacting it with a product containing the general formula R. 10 OH- halogenated alcohols, with the general formula R 11 The third contact is carried out by a second alcohol compound of OH; preferably, the inert solvent is selected from at least one of pentane, hexane, heptane, petroleum ether and gasoline.
[0093] The present invention does not impose any particular restrictions on the specific conditions of the third contact in S3, as long as it enables the contact containing the general formula R. 10 OH- halogenated alcohols, with the general formula R 11 The second alcohol compound of OH and the second product need to be able to come into sufficient contact to form a fluid. However, in order to have a catalyst support with better performance, according to some embodiments of the present invention, in S3, the conditions for the third contact include: being carried out under stirring conditions, at a temperature of 0 to 120°C, and for a time of 0.5 to 6 hours.
[0094] The present invention does not particularly limit the specific manner of the third contact in S3. The haloalcohol and the second alcohol compound can be mixed and contacted with the second component simultaneously, or the haloalcohol and the second alcohol compound can be contacted with the second component separately and sequentially.
[0095] According to some embodiments of the present invention, in step S4, the spray drying conditions can employ existing conditions capable of forming catalyst supports for olefin polymerization. However, in order to obtain a catalyst support with better performance, according to a preferred embodiment of the present invention, the spray drying is carried out in a sprayer having an atomizing nozzle comprising a material conduit and a nozzle head. The third product is led into the nozzle head through the material conduit and sprayed through the nozzle head into a tower containing an inert medium within the sprayer for solidification. Preferably, the temperature of the third product in the material conduit is between 0 and 80°C, and the temperature of the third product in the nozzle head is between 80 and 180°C; more preferably, the temperature of the third product in the nozzle head is between 120 and 180°C.
[0096] According to some embodiments of the present invention, in S4, the conditions for spray drying include a temperature of 60–200°C, more preferably 90–150°C. In this invention, the spray drying temperature refers to the temperature of the inert medium in the sprayer.
[0097] According to some embodiments of the present invention, the inert medium may include a protective gas medium and / or an inert liquid medium. There is no particular limitation on the type of protective gas medium; for example, it may be nitrogen, an inert gas medium such as helium, or other suitable gases such as carbon dioxide. The inert liquid medium is any liquid medium commonly used in the art that does not chemically react with reactants and reaction products. Preferably, the inert liquid medium is silicone oil and / or an inert liquid hydrocarbon solvent. More preferably, the inert liquid medium is selected from at least one of kerosene, paraffin oil, petrolatum oil, white oil, methyl silicone oil, ethyl silicone oil, methylethyl silicone oil, phenyl silicone oil, and methylphenyl silicone oil, and even more preferably, white oil.
[0098] According to some embodiments of the present invention, the amount of inert liquid medium in the sprayer can be selected according to the amount of magnesium halide with the general formula MgX"Y, preferably 0.8 to 10 L, more preferably 2 to 8 L.
[0099] According to some embodiments of the present invention, the preparation method of the present invention further includes post-treatment means conventional in the art, such as solid-liquid separation, washing, and drying, and there is no particular limitation on these in the present invention. The solid-liquid separation may adopt various existing methods capable of realizing the separation of a solid phase and a liquid phase, for example, suction filtration, pressure filtration or centrifugal separation, etc. Under preferred conditions, the solid-liquid separation method is a pressure filtration method. The present invention has no particular limitation on the pressure filtration conditions, as long as the separation of the solid phase and the liquid phase is achieved as sufficiently as possible. The washing may be performed on the obtained solid phase product by a method well known to those skilled in the art, for example, an inert hydrocarbon solvent (such as pentane, hexane, heptane, petroleum ether and gasoline) may be used to wash the obtained solid phase product. The present invention has no particular limitation on the specific drying conditions, for example, the drying temperature may be 20 to 70°C, the drying time may be 0.5 to 10 hours, and the drying may be carried out under normal pressure or reduced pressure conditions.
[0100] The magnesium-containing carrier with uniform particles and small particle size prepared by the above preparation method has a structure represented by formula (III);
[0101]
[0102] In formula (III), R1 is C1~C 10 alkyl;
[0103] R2 and R3 are the same or different, and are each independently H, C1~C 10 alkyl or C1~C substituted by 1 to 10 halogen atoms 10 haloalkyl;
[0104] R4 is C1-C5 alkyl;
[0105] R5 is C1~C substituted by at least one halogen atom 10 haloalkyl or C6~C substituted by at least one halogen atom 20 haloaryl;
[0106] X is fluorine, chlorine, bromine or iodine;
[0107] m is 0.1 to 1.9, n is 0.1 to 1.9, and m+n=2; preferably, m is 0.8 to 1.2, n is 0.8 to 1.2;
[0108] 0<q<0.2; 0<a<0.1; preferably, 0.005≤q≤0.2; 0.001<a<0.05.
[0109] According to some embodiments of the present invention, the average particle diameter of the magnesium-containing carrier is 2 to 100 μm, and the particle size distribution is less than 2; preferably, the average particle diameter of the magnesium-containing carrier is 2 to 19 μm, and the particle size distribution is 0.6 to 1.6; more preferably, the average particle diameter of the magnesium-containing carrier is 2 to 10 μm, and the particle size distribution is 0.6 to 1.
[0110] According to some embodiments of the present invention, the titanium element is derived from a titanium compound, wherein the titanium compound is selected from Ti(OR) 4 ) 4-n X' n At least one of the compounds shown, wherein R 4 Selected from C1 to C 20 The hydrocarbon group is preferably from C1 to C2. 14 The aliphatic hydrocarbon groups, the repeating X' are the same or different, and each is independently selected from F, Cl or Br, and n is an integer from 0 to 4.
[0111] According to some embodiments of the present invention, the titanium compound is selected from one or a mixture thereof, preferably titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxy, titanium tetraethoxy, titanium monochlorotributoxy, titanium dichlorodibutoxy, titanium trichlorobutoxy, titanium monochlorotriethoxy, titanium dichlorodiethoxy, titanium trichloroethoxy, titanium trichloride, or titanium trichloride.
[0112] According to some embodiments of the present invention, the molar ratio of titanium to magnesium is (0.01 to 0.3):1 (for example, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.15:1, 0.2:1, 0.24:1, 0.28:1, 0.3:1, and any two of the above ranges), preferably (0.06 to 0.15):1.
[0113] According to some embodiments of the present invention, the preparation method of the main catalyst includes: mixing a magnesium-containing support, titanium halide, and an internal electron donor.
[0114] According to some embodiments of the present invention, the molar ratio of titanium halide (calculated as Ti), magnesium-containing support (calculated as Mg), and internal electron donor is (5-100):1:(0.01-0.2), preferably (15-40):1:(0.03-0.15).
[0115] According to some embodiments of the present invention, the method of mixing a magnesium-containing support, titanium halide, and an internal electron donor includes: (1) mixing the magnesium-containing support with the titanium halide; and (2) mixing the system of step (1) with the internal electron donor.
[0116] According to some embodiments of the present invention, the mixing in step (1) is carried out at -30 to 0°C, preferably at -25 to -15°C. For example, the mixing in step (1) can be carried out at -30°C, -20°C, -10°C, 0°C, or 5°C. The mixing method in step (1) is not particularly limited, for example, it can be stirring. The mixing time in step (1) can be 1 to 600 min.
[0117] According to some embodiments of the present invention, in step (2), a heating treatment is performed first, and the internal electron donor is added during the heating process; more preferably, the temperature is raised to 80–120°C, preferably 90–115°C. For example, the temperature is raised to 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, or 120°C. The mixing method in step (2) is not particularly limited, for example, it can be stirring. The mixing time in step (2) can be 30–900 min.
[0118] According to some embodiments of the invention, in step (2), the mixture is filtered and optionally washed and dried. In a further preferred embodiment, the mixture is first washed with the titanium halide and then with an alkane solvent (e.g., hexane).
[0119] According to some embodiments of the present invention, the method includes:
[0120] (1) Add titanium halide to the reaction vessel, cool to -30℃~0℃, then add magnesium-containing support to the reaction vessel, and stir at -30℃~0℃ for 1~600min (preferably 10~60min).
[0121] (2) Heat the reaction vessel to 0-1°C (preferably 80-120°C) and add an internal electron donor during the heating process. Then, after maintaining the temperature at this point for 30-900 min (preferably 10-60 min), filter off the liquid. Then, wash with titanium tetrachloride, and finally wash with hexane. After drying, the catalyst component is obtained.
[0122] According to some embodiments of the present invention, the co-catalyst comprises alkylaluminum.
[0123] The alkylaluminum described in this invention can be a commonly used alkylaluminum with activating properties in the art. According to some embodiments of the invention, the alkylaluminum contains 1 to 3 alkyl groups, and the number of carbon atoms in the alkyl groups is C1 to C8. Preferably, the alkylaluminum is selected from at least one of triethylaluminum, tripropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-octylaluminum, diethylaluminum hydrogen, diisobutylaluminum hydrogen, diethylaluminum chloride, diisobutylaluminum chloride, sesquiethylaluminum chloride, and diethylaluminum chloride.
[0124] The external electron donor described in this invention can be any external electron donor commonly used in the art. According to some embodiments of the invention, the external electron donor is selected from at least one silicon-containing compound, preferably from at least one of methylcyclohexyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane, and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
[0125] According to some embodiments of the present invention, the molar ratio of the main catalyst to the co-catalyst is 1:(15-718) (for example, 1:15, 1:50, 1:100, 1:150, 1:200, 1:250, 1:300, 1:350, 1:400, 1:450, 1:500, 1:550, 1:600, 1:650, 1:700 or 1:718, and any two of the above ranges), wherein the molar amount of the main catalyst is expressed as the molar amount of Ti.
[0126] According to some embodiments of the present invention, the molar ratio of the main catalyst to the external electron donor is 1:(1 to 111) (for example, 1:1, 1:5, 1:6, 1:7, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100 or 1:110, and any two of the above ranges), wherein the molar amount of the main catalyst is expressed as the molar amount of Ti.
[0127] According to some embodiments of the present invention, the polymerization reaction is bulk polymerization or slurry polymerization.
[0128] According to some embodiments of the present invention, the conditions for bulk polymerization include: a temperature of 10–90°C and a time of 0.1–10 h.
[0129] According to some embodiments of the present invention, the conditions for slurry polymerization include: a temperature of 10–90°C and a time of 0.1–10 h.
[0130] According to some embodiments of the present invention, the solvent for the slurry polymerization includes at least one of hexane, heptane, and toluene.
[0131] According to some embodiments of the present invention, the slurry polymerization system also includes an antioxidant.
[0132] According to some embodiments of the present invention, the mass ratio of the antioxidant to the main catalyst is (10-200):1.
[0133] According to some embodiments of the present invention, the antioxidant is selected from at least one of hindered phenolic antioxidants (e.g., antioxidant 1010, antioxidant 1076, etc.), phosphite antioxidants (e.g., antioxidant 168, antioxidant 627AV, etc.), and thioether antioxidants (e.g., antioxidant DSTDP, antioxidant 412S, etc.).
[0134] Thirdly, the present invention provides the application of the ultra-high molecular weight homopolymer polypropylene resin described in the first invention or the ultra-high molecular weight homopolymer polypropylene resin prepared by the preparation method described in the second aspect in 3D printing and resin filling.
[0135] Compared with the prior art, the present invention can achieve at least the following beneficial effects:
[0136] The ultra-high molecular weight homopolymer polypropylene resin provided by this invention has special molecular chain structure properties, which can have a certain degree of fluidity while having ultra-high molecular weight, making the processing and application of ultra-high molecular weight homopolymer polypropylene resin possible; in addition, the ultra-high molecular weight homopolymer polypropylene resin provided by this invention has a higher specific surface area, which can endow polypropylene particles with better reactivity in later modification. Attached Figure Description
[0137] Figure 1 The GPC curve of the polypropylene prepared in Example 1 is shown.
[0138] Figure 2 The image shows a scanning electron microscope (SEM) image of the polypropylene prepared in Example 1.
[0139] Figure 3 The image shows a scanning electron microscope (SEM) image of the polypropylene prepared in Example 1.
[0140] Figure 4 The image shows a scanning electron microscope (SEM) image of the polypropylene prepared in Comparative Example 1. Detailed Implementation
[0141] To make the technical problem to be solved, the technical solution, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely for illustrating this patent and do not limit the scope of protection of this invention in any way.
[0142] Unless otherwise defined, the technical terms used in the following embodiments have the same meaning as commonly understood by those skilled in the art. Unless otherwise specified, the reagents used in the following embodiments are conventional biochemical reagents; the raw materials, instruments, and equipment used in the following embodiments can all be obtained commercially or by existing methods; unless otherwise specified, the reagent dosages are those used in routine experimental operations; unless otherwise specified, the experimental methods are conventional methods.
[0143] In the various embodiments and comparative examples of the present invention, the performance data were tested according to the following test methods:
[0144] (1) Average particle diameter and particle size distribution of catalyst support, and average particle diameter of polypropylene: were measured using a Masters Sizer 2000 particle size analyzer (manufactured by Malvern Instruments Ltd).
[0145] (2) GPC curve and viscosity-average molecular weight (Mv) of polypropylene: The results were obtained using a PL-GPC 220 gel permeation chromatograph from Polymer Laboratories, UK, with an IR5 infrared detector. The temperature was 150℃, the chromatographic column was three PLgel 13μm Olexis columns, the mobile phase was 1,2,4-trichlorobenzene (with 0.025% by mass of antioxidant 2,6-dibutyl-p-cresol), the flow rate was 1.0 mL / min, and the sample mass concentration was approximately 1 mg / mL. The results were universally calibrated using EasiCalPS-1 narrow distribution polystyrene standard from PL.
[0146] (3) Polypropylene melt flow rate (MFR): Measured in accordance with GB / T3682.1-2018.
[0147] (4) Content of cyanosuccinate: The content of α-cyanosuccinate and / or substituted α-cyanosuccinate was tested by gas chromatography with diamyl phthalate as an internal standard.
[0148] (5) Specific surface area of polypropylene: The specific surface area of the sample was measured using an ASAP2020 adsorption instrument manufactured by Micromeritics, USA, and the BET method was used to calculate the specific surface area of the sample.
[0149] (6) Appearance morphology of polypropylene: Tested using an optical microscope of Nikon Eclipse E200.
[0150] (7) Oxidation induction time of polypropylene: Tested according to GB / T 19466.6-2009, the test temperature is 200℃.
[0151] In the various embodiments and comparative examples of the present invention, the triethylaluminum used is a hexane solution of triethylaluminum, wherein the concentration of triethylaluminum is 0.5 mmol / mL.
[0152] Example 1
[0153] (1) Preparation of magnesium-containing carrier
[0154] S1: In a 0.6L reactor, 0.08mol magnesium chloride and 1.7mol ethanol (the first alcohol compound) are added sequentially. The mixture is heated to 90℃ with stirring and reacted at a constant temperature for 1h to carry out the first contact. Then, emulsification is carried out to obtain the first product.
[0155] S2: The first product is subjected to a second contact with 0.48 mol of epichlorohydrin to obtain a second product. The conditions for the second contact are: temperature of 90°C and time of 30 min.
[0156] S3: After the second product is filtered by pressure, it is thoroughly mixed and stirred with 2.5 mol of ethanol (second alcohol compound) and 0.35 mol of 1,3-dichloropropanol (halogenated alcohol) to form a third fluid and obtain the third product;
[0157] S4: The third product is sprayed into the spray tower of the sprayer tower at 100°C using a sprayer B-290 containing a nozzle head and a material conduit for spray drying. The temperature of the third product in the material conduit is 15°C and the temperature in the nozzle head is 120°C, to obtain a magnesium-containing carrier Z1.
[0158] The structure and composition of the magnesium-containing support Z1 were determined by gas chromatography-mass spectrometry, nuclear magnetic resonance (NMR) and elemental analysis as follows:
[0159]
[0160] The magnesium-containing carrier Z1 has an average particle diameter (D50) of 4 μm and a particle size distribution ((D90-D10) / D50) of 0.9.
[0161] Observations showed that the magnesium-containing carrier Z1 particles had relatively regular morphology, smooth surfaces, and were mostly spherical. The particle size distribution was relatively concentrated, and there were basically no irregularly shaped particles.
[0162] (2) Preparation of the main catalyst
[0163] In a 300 mL reaction flask, 0.91 mol of titanium tetrachloride was added and cooled to -20 °C. 0.04 mol (calculated as Mg) of magnesium-containing support Z1 was added and stirred at -20 °C for 30 min. Then, the temperature was slowly increased to 110 °C. During the heating process, 1.5 mmol of diethyl 2,3-diisopropyl-2-cyanosuccinate was added. The temperature was maintained at 110 °C for 30 min, and the liquid was filtered off. The mixture was then washed twice with boiling titanium tetrachloride and finally washed three times with hexane. After drying, the main catalyst a was obtained.
[0164] (3) Propylene polymerization reaction
[0165] In a 5L stainless steel high-pressure reactor, nitrogen gas was used for purging. Then, 1 mmol of triethylaluminum, 0.05 mmol of methylcyclohexyldimethoxysilane, 10 mL of anhydrous hexane, 10 mg of the above-mentioned main catalyst a (containing 0.008 mmol of titanium), and 2.5 L of liquid propylene (hydrogen concentration of 0 ppm) were introduced into the nitrogen gas stream. The temperature was raised to 70°C and reacted at this temperature for 1 h. The mixture was then cooled, depressurized, discharged, and dried to obtain polypropylene powder.
[0166] The polypropylene powder prepared in this embodiment exhibits a good spherical morphology.
[0167] like Figure 2 and Figure 3 As shown, the polypropylene powder particles exhibit a good spherical shape, and the connection between spherical secondary particles and fibrous particles can be clearly observed.
[0168] Example 2
[0169] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0170] (2) The preparation of the main catalyst is as described in Example 1.
[0171] (3) The propylene polymerization reaction is the same as in Example 1, except that the hydrogen concentration in the propylene is 1 ppm.
[0172] Example 3
[0173] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0174] (2) The preparation of the main catalyst is as described in Example 1.
[0175] (3) The propylene polymerization reaction is the same as in Example 1, except that the hydrogen concentration in the propylene is 3 ppm.
[0176] Example 4
[0177] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0178] (2) The preparation of the main catalyst is as described in Example 1.
[0179] (3) The propylene polymerization reaction was carried out in accordance with Example 1, except that the same amount of 2,3-diisopropyl-2-cyanosuccinate and 2-isopropyl-2-isopentyl-1,3-dimethoxypropane (molar ratio of 10:3) were used instead of 2,3-diisopropyl-2-cyanosuccinate.
[0180] Example 5
[0181] (1) The preparation of the magnesium-containing carrier is described in Example 4.
[0182] (2) The preparation of the main catalyst is described in Example 4.
[0183] (3) The propylene polymerization reaction is the same as in Example 4, except that the hydrogen concentration in the propylene is 1 ppm.
[0184] Example 6
[0185] (1) The preparation of the magnesium-containing carrier is described in Example 4.
[0186] (2) The preparation of the main catalyst is described in Example 4.
[0187] (3) The propylene polymerization reaction is the same as in Example 4, except that the hydrogen concentration in the propylene is 3 ppm.
[0188] Example 7
[0189] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0190] (2) The preparation of the main catalyst is as described in Example 1.
[0191] (3) Propylene polymerization reaction
[0192] In a 5L stainless steel high-pressure reactor, the reactor was purged with a nitrogen stream. Then, 2.2 mmol of triethylaluminum, 0.115 mmol of methylcyclohexyldimethoxysilane, 0.02 mmol of 2-hydroxyaniline, 22 mL of anhydrous hexane, and 22 mg of the above-mentioned main catalyst a (containing 0.018 mmol of titanium) and 2.5 L of liquid propylene (hydrogen concentration of 0 ppm) were introduced into the nitrogen stream. The temperature was raised to 70°C and the reaction was carried out at this temperature for 1 h. The reactor was then cooled, depressurized, discharged, and dried to obtain polypropylene powder.
[0193] The polypropylene powder prepared in this embodiment exhibits a good spherical morphology.
[0194] Example 8
[0195] (1) The preparation of the magnesium-containing carrier is described in Example 7.
[0196] (2) The preparation of the main catalyst is described in Example 7.
[0197] (3) The propylene polymerization reaction is the same as in Example 7, except that 2-hydroxyaniline is not added.
[0198] The polypropylene powder prepared in this embodiment suffered from severe agglomeration, making discharge difficult.
[0199] By comparing Examples 8 and 7, it is shown that adding aminophenol compounds such as 2-hydroxyaniline to the preparation method of ultra-high molecular weight homopolymer polypropylene resin provided by the present invention can increase the catalyst concentration in the polymerization reaction system under the same reaction scale, thereby achieving the effect of producing more polymers in a single run and effectively improving production efficiency.
[0200] Example 9
[0201] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0202] (2) The preparation of the main catalyst is as described in Example 1.
[0203] (3) The propylene polymerization reaction is the same as in Example 1, except that 2L of anhydrous hexane is added to the components introduced in the nitrogen gas stream to carry out the slurry polymerization reaction.
[0204] Example 10
[0205] (1) The preparation of the magnesium-containing carrier is described in Example 9.
[0206] (2) The preparation of the main catalyst is described in Example 9.
[0207] (3) The propylene polymerization reaction was carried out in accordance with Example 9, except that 0.4g of antioxidant 1010 was added before discharge.
[0208] Example 11
[0209] (1) Preparation of magnesium-containing carrier
[0210] In a 150L reactor with stirring, 10kg of anhydrous magnesium chloride and 12.6kg of ethanol were added to 60L of white oil with a viscosity of 30 centipoise (20°C), and the reaction was carried out at 125°C for 2 hours. The resulting mixture of the molten adduct and white oil was then transferred to a methyl silicone oil medium preheated to 125°C; the methyl silicone oil had a viscosity of 300 centipoise (20°C), and the amount of methyl silicone oil used was 120L. The mixture was stirred at 200 rpm for 20 minutes to obtain a final mixture. This mixture was then introduced into a rotating bed for dispersion, and under stirring conditions, the dispersed mixture was introduced into a hexane medium preheated to -35°C, with 1200L of hexane used. The magnesium chloride / alcohol adduct melt, dispersed as small droplets, was cooled and solidified into spherical solid particles. Solid particles were filtered out from the suspension obtained after rapid cooling. The particles were washed with hexane at room temperature, with 100 L of hexane per wash, for a total of 5 washes. The magnesium-containing support Z2 was obtained by vacuuming at 40 °C.
[0211] The structural formula of magnesium-containing support Z2 was determined by gas chromatography-mass spectrometry, nuclear magnetic resonance and elemental analysis as: MgCl2·2.6C2H5OH.
[0212] The magnesium-containing carrier Z2 has an average particle diameter (D50) of 52 μm and a particle size distribution ((D90-D10) / D50) of 1.1.
[0213] Observations showed that the magnesium-containing carrier Z2 had a relatively regular particle morphology, a relatively smooth surface, and a relatively concentrated particle size distribution.
[0214] (2) The preparation of the main catalyst is the same as in Example 1, except that 0.04 mol (calculated as Mg) magnesium-containing support Z1 is replaced with 0.04 mol (calculated as Mg) magnesium-containing support Z2.
[0215] (3) The propylene polymerization reaction is described in Example 1.
[0216] Comparative Example 1
[0217] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0218] (2) The preparation of the main catalyst is the same as in Example 1, except that the same molar amount of diisobutyl phthalate is used instead of diethyl 2,3-diisopropyl-2-cyanosuccinate.
[0219] (3) The propylene polymerization reaction is described in Example 1.
[0220] like Figure 4 As shown, no obvious spherical secondary particles or fibrous particles could be observed on the surface of the polypropylene powder particles obtained in this comparative example.
[0221] Comparative Example 2
[0222] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0223] (2) The preparation of the main catalyst is the same as in Example 1, except that the same amount of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane is used instead of diethyl 2,3-diisopropyl-2-cyanosuccinate.
[0224] (3) The propylene polymerization reaction is described in Example 1.
[0225] No obvious spherical secondary particles or fibrous particles could be observed on the surface of the polypropylene powder particles obtained in this comparative example.
[0226] Comparative Example 3
[0227] (1) The preparation of the magnesium-containing carrier is as described in Example 1.
[0228] (2) The preparation of the main catalyst is as described in Example 1.
[0229] (3) The propylene polymerization reaction is the same as in Example 1, except that the hydrogen concentration in the propylene is 100 ppm.
[0230] The performance of the polypropylene prepared in each example and comparative example was tested, and the results are shown in Table 1.
[0231] Table 1
[0232]
[0233] The oxidation induction time of the polypropylene prepared in Examples 9 and 10 was tested, and the results are shown in Table 2.
[0234] Table 2
[0235] Group Oxidation induction time (min) Example 9 1 Example 10 6.6
[0236] The results above show that, compared with bulk polymerization, antioxidants can be added online during slurry polymerization, which can significantly prolong the oxidation induction time of polypropylene.
[0237] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.
Claims
1. A type of ultra-high molecular weight homopolymer polypropylene resin, characterized in that, The ultra-high molecular weight homopolymer polypropylene resin has a viscosity-average molecular weight ≥ 11.8 × 10⁻⁶. 5 g / mol; melt mass flow rate at 230℃ and 21.6kg load > 1g / 10min; in the gel permeation chromatography curve with x-axis as logMW and y-axis as dw / dlogM, the ratio of the left half-width to the right half-width of the peak position is greater than 1, and the ratio of the left half-width to the right half-width of the baseline of the peak position is greater than 2.
1.
2. The ultra-high molecular weight homopolymer polypropylene resin according to claim 1, characterized in that, The ultra-high molecular weight homopolymer polypropylene resin is a microsphere with a diameter of 50-1000 μm; preferably, the surface of the microsphere has spherical secondary particles connected with fibrous particles. And / or, the ultra-high molecular weight homopolymer polypropylene resin contains cyano succinate; And / or, the specific surface area of the ultra-high molecular weight homopolymer polypropylene resin is >90 m². 2 ·g -1 ; And / or, the oxidation induction time of the ultra-high molecular weight homopolymer polypropylene resin is greater than 3 min.
3. The method for preparing the ultra-high molecular weight homopolymer polypropylene resin according to claim 1 or 2, characterized in that, include: Propylene is polymerized in the presence of a catalyst and optional aminophenolic compounds to obtain the ultra-high molecular weight homopolymer polypropylene resin. The catalyst includes a main catalyst, a co-catalyst, and an optional external electron donor; The main catalyst includes magnesium, titanium, and an internal electron donor, wherein the internal electron donor includes α-cyanosuccinate and / or substituted α-cyanosuccinate. The catalyst does not contain P; The hydrogen concentration in the propylene is 0 to 10 ppm, preferably 0 to 3 ppm; Preferably, the ratio of the main catalyst to the liquid component in the polymerization reaction system is (0.1-20) mg:1 L, and more preferably (1-15) mg:1 L.
4. The preparation method according to claim 3, characterized in that, The aminophenol compound has the structural formula R'(NH2-C6H3-OH), wherein R' is selected from C1 to C6 alkyl or H; preferably, the aminophenol compound includes at least one of 2-hydroxyaniline, 3-hydroxyaniline, 4-hydroxyaniline, and 3-methyl-2-hydroxyaniline; And / or, the molar ratio of the aminophenolic compound to the catalyst based on Ti is 0.001 to 5, preferably 0.01 to 2.
5. The preparation method according to claim 3 or 4, characterized in that, The molar ratio of the internal electron donor to magnesium is (0.01–0.2):1, preferably (0.03–0.15):1; And / or, the α-cyanosuccinate and / or substituted α-cyanosuccinate are selected from at least one of the compounds shown in formula (III): In equation (III), R a R b Each is independently selected from C1 to C2. 14 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; R c and R d Each is independently selected from H, C1 to C1. 14 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; R c and R d They can be optionally bonded together to form one or more fused ring structures; Preferably, in formula (III), R a R b Each is independently selected from C1 to C2. 10 Alkyl, C3-C 10 cycloalkyl, C6-C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aryl alkyl; R c and R d Each is independently selected from C1 to C2. 10 Alkyl, C3-C 10 cycloalkyl, C6-C 20 Aryl, C7~C 20 Alkyl or C7~C 20 Aromatic group.
6. The preparation method according to any one of claims 3-5, characterized in that, The internal electron donor also includes dialkoxy-substituted alkanes; Preferably, the dialkoxy-substituted alkane is selected from (R 7 (R) 8 )C(OR 9 (OR) 10 At least one of ), wherein R 7 and R 8 Each is independently selected from hydrogen, C1 to C2. 20 Alkyl groups, C3-C 20 cycloalkyl, C6-C 20 aryl, C7~C 20 Aryl groups or C7-C 10 alkylaryl, R 7 and R 8 The links can be optionally keyed into a loop, R 9 and R 10 Each is independently selected from C1 to C2. 20 Alkyl groups; more preferably, R 7 and R 8 Each is independently selected from hydrogen, C1 to C2. 10 Alkyl groups, C3-C 10 cycloalkyl, C6-C 10 aryl, C7~C 10 Aryl groups or C7-C 10 alkylaryl, R 7 and R 8 The links can be optionally keyed into a loop; R 9 and R 10 Each is independently selected from C1 to C2. 10 Alkyl groups; Preferably, the molar ratio of the dialkoxy-substituted alkane to magnesium is (0.001-0.15):1, more preferably (0.005-0.1):
1.
7. The preparation method according to any one of claims 3-6, characterized in that, The magnesium element is derived from a magnesium-containing carrier; And / or, The titanium element is derived from titanium compounds, which are selected from Ti(OR) 4 ) 4-n X' n At least one of the compounds shown, wherein R 4 Selected from C1 to C 20 The hydrocarbon group is preferably from C1 to C2. 14 The aliphatic hydrocarbon groups, the repeating X' are the same or different, and each is independently selected from F, Cl or Br, and n is an integer from 0 to 4; Preferably, the titanium compound is selected from one or a mixture of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxy, titanium tetraethoxy, titanium monochlorotributoxy, titanium dichlorodibutoxy, titanium trichlorobutoxy, titanium monochlorotriethoxy, titanium dichlorodiethoxy, titanium trichloroethoxy, titanium trichloride, or titanium trichloride, with titanium tetrachloride being the most preferred. And / or, The molar ratio of titanium to magnesium is (0.01-0.3):1, preferably (0.06-0.15):
1.
8. The preparation method according to any one of claims 3-7, characterized in that, The preparation method of the main catalyst includes: mixing a magnesium-containing support, titanium halide, and an internal electron donor; Preferably, the molar ratio of titanium halide (calculated as Ti), magnesium-containing support (calculated as Mg), and internal electron donor is (5-100):1:(0.01-0.2), more preferably (15-40):1:(0.03-0.15); Preferably, the method of mixing the magnesium-containing support, titanium halide, and internal electron donor includes: (1) mixing the magnesium-containing support with the titanium halide; (2) mixing the system of step (1) with the internal electron donor; More preferably, the mixing in step (1) is carried out at -30 to 0°C, preferably at -25 to -15°C; and / or, in step (2), the temperature is raised first, and the internal electron donor is added during the heating process; preferably, the temperature is raised to 80 to 120°C, preferably 90 to 115°C.
9. The preparation method according to any one of claims 3-8, characterized in that, The co-catalyst comprises alkylaluminum; preferably, the number of alkyl groups in the alkylaluminum is 1 to 3, and the number of carbon atoms in the alkyl groups is C1 to C8; more preferably, the alkylaluminum is selected from at least one of triethylaluminum, tripropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-octylaluminum, diethylaluminum monohydrogen, diisobutylaluminum monohydrogen, diethylaluminum monochloro, diisobutylaluminum monochloro, sesquiethylaluminum chloride, and diethylaluminum dichloro. And / or, the external electron donor is selected from at least one of silicon-containing compounds, preferably from at least one of methylcyclohexyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane, and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane; And / or, the molar ratio of the main catalyst to the co-catalyst is 1:(15-718), and / or, the molar ratio of the main catalyst to the external electron donor is 1:(1-111), wherein the molar of the main catalyst is expressed in terms of the molar amount of Ti.
10. The preparation method according to any one of claims 3-9, characterized in that, The polymerization reaction is bulk polymerization or slurry polymerization; Preferred, The conditions for bulk polymerization include: a temperature of 10–90°C and a time of 0.1–10 h; And / or, the conditions for slurry polymerization include: a temperature of 10–90°C and a time of 0.1–10 h; And / or, the solvent for the slurry polymerization includes at least one of hexane, heptane, and toluene; And / or, the slurry polymerization system also includes an antioxidant; preferably, the mass ratio of the antioxidant to the main catalyst is (10-200):1; preferably, the antioxidant is selected from at least one of hindered phenolic antioxidants, phosphite antioxidants, and thioether antioxidants.
11. The application of the ultra-high molecular weight homopolymer polypropylene resin according to claim 1 or 2, or the ultra-high molecular weight homopolymer polypropylene resin prepared by the preparation method according to any one of claims 3-10, in 3D printing and resin filling.
Citation Information
Patent Citations
Spherical catalyst components used for polymerization or copolymerization of olefin and its catalyst
CN1330086A
Process for preparing olefin polymerization ball type catalytic component and carrier
CN1463990A
Magnesium halide / alcohol addition compound and its preparing method and use
CN1580136A
Process for producing a solid catalyst component for olefin polymerization and a process for producing an olefin polymer
US6020279A