A method for preparing an ethylene-norbornene copolymer
By using a mixed solvent system of toluene and methylcyclohexane in the copolymerization of ethylene and norbornene, the problem of balancing polymerization activity and glass transition temperature in the prior art has been solved, achieving a high-efficiency performance improvement and expanding the application range of cyclic olefin copolymers.
Patent Information
- Application Number
- CN202611520533.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to find a balance between improving the polymerization activity and glass transition temperature of ethylene-norbornene copolymerization, and single solvent systems often fail to simultaneously achieve these two key indicators.
A mixed solvent system of toluene and methylcyclohexane was used as the reaction solvent to carry out the solution polymerization of ethylene-norbornene in the presence of a metallocene catalyst. By adjusting the solvent ratio to optimize the microenvironment of the active center, the polymerization activity and glass transition temperature were synergistically improved.
While maintaining high polymerization activity, the glass transition temperature of the copolymer was significantly improved, and the molecular weight distribution could be flexibly controlled, providing a new process route for performance optimization.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer material synthesis technology, specifically relating to a method for preparing an ethylene-norbornene copolymer. Background Technology
[0002] Cyclic olefin copolymers are a class of amorphous thermoplastic resins obtained by coordination copolymerization of ethylene and cyclic olefins (such as norbornene, tetracyclododecene, etc.) under the catalysis of metallocene catalysts. Due to their high transparency, low birefringence, low water absorption and good heat resistance, they have been widely used in optical lenses, display devices and medical packaging.
[0003] In existing technologies, researchers have focused primarily on two aspects to improve the performance of cyclic olefin copolymers: the molecular structure design of catalysts and the functionalization modification of monomers. Regarding catalysts, fine-tuning of polymerization activity and copolymer microstructure is achieved by adjusting the bridging groups, substituent structures, and central metal types of metallocene complexes. Regarding monomers, the refractive index of copolymers is increased by introducing large conjugated aromatic groups such as carbazole, naphthyl, and fluorene, or highly polarizable elements such as sulfur atoms, onto the norbornene ring. However, the influence of polymerization solvents on the polymerization reaction and product properties has been relatively limited in existing research.
[0004] Currently, solution polymerization of ethylene-norbornene typically uses a single solvent as the reaction medium. Commonly used solvents include aromatic hydrocarbons (such as toluene) and alkanes or cycloalkanes (such as n-hexane and cyclohexane). Toluene is widely used in industrial production and laboratory research due to its good solubility for various metallocene catalysts and cycloolefin monomers. Alkane solvents are also used in some polymerization systems due to their low polarity and specific stabilizing effect on the active sites of catalysts. Existing studies have shown that different solvents have different effects on polymerization activity and the glass transition temperature of the product, but a single solvent system often cannot simultaneously achieve both of these key indicators. For example, aromatic hydrocarbon solvents have a better solubility and stabilizing effect on the active sites of catalysts, which is beneficial to improving polymerization activity; while alkane solvents may affect the insertion of norbornene monomers by adjusting the coordination environment of the active sites, thereby affecting the performance of the cycloolefin copolymer. (Zhang Hao et al., *Elastomers*, Vol. 24, No. 4, 2014, "The Effect of Solvents on the Influence ... rac -Et[Ind]2ZrCl2 / MMAO The effect of the catalytic system on the copolymerization of ethylene and norbornene ring When using a toluene / benzene mixed solvent with a volume ratio of 80 / 20, the polymerization activity reaches its maximum, but the glass transition temperature of the product is relatively low. Summary of the Invention
[0005] To address the issue in existing reports that high polymerization activity and high glass transition temperature cannot be simultaneously achieved, this invention provides a novel method for preparing ethylene-norbornene copolymers. By employing a toluene / methylcyclohexane mixed solvent system, this method can improve polymerization activity while maintaining or even increasing the polymer's glass transition temperature, thus achieving a synergistic improvement in both.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing an ethylene-norbornene copolymer involves using a mixed solvent of toluene and methylcyclohexane as the reaction solvent in the presence of a metallocene catalyst to perform solution polymerization of ethylene and norbornene to obtain the ethylene-norbornene copolymer.
[0007] Furthermore, the metallocene catalyst is any one of rac-ethylenebis(1-indenyl)zirconia, rac-dimethylsilylbis(1-indenyl)zirconia, diphenylmethylene(cyclopentadiene)(9-fluorenyl)zirconia, and diphenylmethylenecyclopentadiene(2,7-di-tert-butyl-fluorenyl)zirconia.
[0008] Furthermore, the volume ratio of toluene to methylcyclohexane used is 1:3 to 3:1.
[0009] Furthermore, the temperature of the solution polymerization reaction is 30-120 °C, preferably 90 °C.
[0010] Furthermore, the solution polymerization reaction takes 5-120 minutes, preferably 20 minutes.
[0011] Furthermore, the obtained ethylene-norbornene copolymer has a molecular weight distribution of 2.0-2.2 and a glass transition temperature of 165-192 °C.
[0012] This invention mixes toluene and methylcyclohexane in an appropriate ratio. The use of toluene ensures the complete dissolution of the catalyst and monomer and guarantees high polymerization activity, while methylcyclohexane promotes the insertion of norbornene by regulating the microenvironment of the active sites. The synergistic effect of the two mixtures simultaneously enhances the polymerization activity and the glass transition temperature of the product. Furthermore, by varying the ratio of the two mixtures, the polarity and solubility of the polymerization system can be flexibly adjusted, thereby achieving effective control over the polymerization activity, molecular weight, and glass transition temperature.
[0013] The significant advantages of this invention are: (1) The present invention applies the mixed solvent system of toluene and methylcyclohexane to the copolymerization reaction of ethylene-norbornene, which can expand the range of polymer solvents and provide a new process for the preparation of cyclic olefin copolymers.
[0014] (2) The present invention uses a metallocene catalyst as the main catalyst. During the polymerization reaction, the main catalyst has excellent copolymerization catalytic ability, thereby making the polymerization reaction of the present invention have high reactivity. Attached Figure Description
[0015] Figure 1 The image shows the GPC diagram of the copolymer prepared in Example 3.
[0016] Figure 2 The image shows the DSC diagram of the copolymer prepared in Example 9. Detailed Implementation
[0017] To make the content of this invention easier to understand, the technical solution of this invention will be further described below with reference to specific embodiments, but this invention is not limited thereto.
[0018] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0019] Examples 1-8: Preparation of ethylene-norbornene copolymer
[0020] Step 1: Preparation of norbornene solution Norbornene was dissolved in the corresponding solvent used in the reaction to prepare an NB solution with a mass fraction of 75%.
[0021] Step 2: Reactor Pretreatment The high-pressure polymerization reactor was vacuum dried at 110 °C for 1 hour, and the process was repeated three times with vacuuming and nitrogen purging, followed by three purgings with ethylene to ensure that the reaction system was free of water and oxygen.
[0022] Step 3: Polymerization reaction Under an inert atmosphere, MAO (Al / Zr = 1000), 80 mL of different solvents, and NB solution were added to the reactor and stirred until homogeneous. Diphenylmethylene (cyclopentadiene)(9-fluorenyl)zirconium dichloride (3.0 μmol) was dissolved in 2 mL of toluene and injected into the reactor using a syringe. After sealing the reactor, ethylene was introduced under rapid stirring and the pressure was maintained at 3 bar. The temperature was raised to 90 °C, and the reaction was allowed to proceed for 20 minutes. The reaction was then terminated by adding 200 mL of hydrochloric acid-ethanol solution. The mixture was filtered and dried under vacuum to obtain the product.
[0023] The specific solvent systems, norbornene dosage, and reaction results for each case are shown in Table 1.
[0024] Table 1. Effects of solvent system and norbornene dosage on the copolymerization of ethylene and norbornene.
[0025] Results Analysis: Examples 1-5 (40 mL NB feed) and Examples 6-10 (20 mL NB feed) show that when the volume ratio of toluene to methylcyclohexane is 1:3 (Example 4), the polymer... T g It has reached its maximum molecular weight, which is higher than that of pure toluene and pure methylcyclohexane, and its polymerization activity is also higher than that of pure toluene.
[0026] Meanwhile, compared with the examples, Comparative Example 1, using a toluene / benzene mixed solvent, showed higher polymerization activity than the solvent system using toluene alone, but the resulting copolymer had a lower glass transition temperature. This indicates that while the toluene / benzene mixed solvent can improve catalytic activity to some extent, it cannot simultaneously improve polymerization activity and product heat resistance. Comparative Example 2, using a toluene / n-hexane mixed solvent, showed significantly lower polymerization activity than the solvent system using toluene alone, resulting in an unsatisfactory overall polymerization effect. Comparative Example 3, using a cyclohexane / methylcyclohexane mixed solvent, showed a significant decrease in polymerization activity, glass transition temperature, and molecular weight.
[0027] As can be seen above, in terms of polymerization activity, the polymerization activity is significantly higher than that of the pure toluene system when using the toluene / methylcyclohexane mixed solvent, and slightly lower than that of the pure methylcyclohexane system, but the glass transition temperature is significantly increased. This proves that the mixed solvent system can improve the glass transition temperature of the polymer while maintaining high polymerization activity.
[0028] Regarding thermal properties, when using a toluene / methylcyclohexane mixed solvent, the resulting copolymer exhibits [the following characteristics]. T g Compared to the pure toluene system, the glass transition temperature was increased by more than 7 °C, and the glass transition temperatures of all ethylene-norbornene copolymers reached 165-192 °C. Meanwhile, the molecular weight distribution of all products remained within a narrow range of 2.01-2.16, indicating that the copolymerization process was stable and controllable.
[0029] Regarding molecular weight, when using a toluene / methylcyclohexane mixed solvent, the resulting copolymer... M w The values (90500-142500) are generally higher than those of the pure toluene system (80400-124100), indicating that the mixed solvent is beneficial for increasing the molecular weight of the polymer.
[0030] In terms of process economy, by using commercial metallocene catalysts and adjusting the ratio of toluene to methylcyclohexane, the glass transition temperature and weight-average molecular weight of the product can be flexibly controlled within a certain range without the need for complex catalyst synthesis or monomer modification, thus providing process feasibility for producing differentiated products with different performance indicators.
[0031] In summary, this invention provides a novel method for regulating the performance of ethylene-norbornene copolymerization through mixed solvents. This method can achieve a synergistic improvement in polymerization activity and product glass transition temperature without changing the catalyst and monomers. It provides a simple, efficient, and low-cost technical path for optimizing the performance of cyclic olefin copolymer materials, and has broad application prospects in fields such as optical lenses, display devices, and medical packaging.
[0032] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.
Claims
1. A method for preparing an ethylene-norbornene copolymer, characterized in that, In the presence of a metallocene catalyst, ethylene and norbornene were subjected to solution polymerization using a mixed solvent of toluene and methylcyclohexane as the reaction solvent to obtain an ethylene-norbornene copolymer.
2. The method for preparing the ethylene-norbornene copolymer according to claim 1, characterized in that, The metallocene catalyst is any one of rac-ethylenebis(1-indenyl)zirconia, rac-dimethylsilylbis(1-indenyl)zirconia, diphenylmethylene(cyclopentadiene)(9-fluorenyl)zirconia, and diphenylmethylenecyclopentadiene(2,7-di-tert-butyl-fluorenyl)zirconia.
3. The method for preparing the ethylene-norbornene copolymer according to claim 1, characterized in that, The volume ratio of toluene to methylcyclohexane used is 1:3 to 3:
1.
4. The method for preparing the ethylene-norbornene copolymer according to claim 1, characterized in that, The solution polymerization reaction is carried out at a temperature of 30-120 ℃.
5. The method for preparing the ethylene-norbornene copolymer according to claim 1, characterized in that, The solution polymerization reaction takes 5-120 minutes.
6. The method for preparing the ethylene-norbornene copolymer according to claim 1, characterized in that, The molecular weight distribution of the obtained ethylene-norbornene copolymer is 2.0-2.2.