A photopolymerizable 3D printing conductive hydrogel and precursor composition, its preparation method and application

By using phosphoric acid as a solvent for diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in the hydrogel precursor, the problem of its low solubility in hydrogels was solved, realizing a hydrogel with efficient photocuring and high mechanical properties, suitable for flexible wearable sensors.

CN123106983APending Publication Date: 2026-11-17SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611006666.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve a high and uniform dissolution of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in hydrogels, resulting in low efficiency of photopolymerization 3D printing, poor mechanical properties of hydrogels, and a tendency for pore defects.

Method used

Phosphoric acid was used as the solvent for diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. Through strong intermolecular forces, it was able to achieve uniform dissolution in the hydrogel precursor and form strong intermolecular forces with the polyacrylamide network, thereby enhancing the crosslinking density.

Benefits of technology

It achieves efficient photopolymerization, significantly improves printing efficiency, enhances the fracture strength, Young's modulus and toughness of hydrogels, and improves ionic conductivity and long-term stability, making it suitable for flexible wearable sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106983A_ABST
    Figure CN123106983A_ABST
Patent Text Reader

Abstract

This invention discloses a photopolymerizable 3D printing conductive hydrogel and its precursor composition, preparation method, and applications. The composition comprises acrylamide monomer, polyethylene glycol diacrylate crosslinking agent, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator, and phosphoric acid. Phosphoric acid is used as the solvent for the photoinitiator, achieving uniform dissolution of the photoinitiator without the addition of surfactants. This invention overcomes the problem of poor water solubility of traditional photoinitiators by utilizing the strong intermolecular forces between phosphoric acid and the photoinitiator, achieving molecular-level dispersion and rapid photopolymerization of high-content photoinitiator. Simultaneously, the intermolecular forces formed by the phosphoric acid and polyacrylamide network significantly enhance the mechanical properties of the hydrogel and impart high ionic conductivity and excellent long-term moisture stability to the material. This precursor has high printing precision and can prepare hydrogel structures with complex geometries, showing broad application prospects in fields such as flexible sensors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photopolymer 3D printing materials technology, specifically to a conductive hydrogel precursor composition for photopolymer 3D printing, its preparation method, a 3D printing method using the composition, and the conductive hydrogel obtained therefrom and its application in flexible wearable sensors. Background Technology

[0002] Photopolymerization 3D printing technology for hydrogels has broad application prospects in fields such as soft robotics, flexible sensors, and tissue engineering. In the process of photopolymerization 3D printing, the photoinitiator needs to be uniformly dissolved in the aqueous precursor to ensure a rapid and uniform free radical polymerization reaction under ultraviolet light irradiation.

[0003] Diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide is a commonly used photoinitiator in photopolymerization 3D printing due to its high reactivity and good absorption properties under ultraviolet light. However, the extremely low solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in pure water (approximately 3.13 mg / L at 25°C) severely limits its direct application in hydrogel systems.

[0004] To overcome the solubility problem of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in water, existing technologies typically use surfactants such as sodium dodecyl sulfate to disperse diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide into a nano-suspension aqueous solution, which significantly improves the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in water (1.0%) (Ge Q, Chen Z, Cheng J, Zhang B, Zhang YF, Li H, He X, Yuan C, Liu J, Magdassi S, Qu S. 3D printing of highly stretchable hydrogel with diverse UVcurable polymers[J]. Science Advances, 2021, 7(2): eaba4261.). However, surfactants can block photoinitiators, reduce the efficiency of free radical polymerization, and easily generate bubbles at the liquid-gas interface during printing, leading to pore defects in the printed structure, which damages the mechanical integrity and molding accuracy of the structure. Another technique involves dissolving diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in the crosslinking agent polyethylene glycol diacrylate, and then mixing the intermediate solution with water. However, this technique only allows for extremely low photoinitiator loading (less than 0.1%), which significantly reduces the efficiency of photopolymer 3D printing (Zhang H, Wang P, Zhang H, Chen G, Wang K, Chen X, Chen Z, Jiang M, Yang J, Chen M, Li J. One-Step Digital Light Processing 3D Printing of Robust, Conductive, Shape-Memory Hydrogel for Customizing High-PerformanceSoft Devices[J]. ACS Applied Materials & Interfaces, 2024, 16(49): 68131~68143.).Other methods, such as chemical modification, macromolecular modification, or coating dispersion, may introduce problems such as high migration rate, coating layer rupture, or crystallization, which complicate the preparation process. In addition, increasing the content of diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide in pursuit of high printing speed often leads to incomplete cross-linking of the hydrogel and shorter polymer chains, thereby reducing the mechanical properties of the hydrogel (Ma C, Zhang H, Xie W, Liu W. Ultralow-Concentration-Initiator-Enabled Acrylamide-Phosphoric Acid Ionic Hydrogel with High Toughness and LowHysteresis for Multiple-Function Flexible Sensors[J]. ACS Applied PolymerMaterials, 2026, 8(9): 6818~6829.).

[0005] Therefore, there is an urgent need to develop a new precursor system that can achieve uniform dissolution of high-content diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide without the use of surfactants, while ensuring that the hydrogel still has good mechanical properties during rapid curing and meeting the requirements of precursor flowability for photopolymerization 3D printing. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a conductive hydrogel precursor composition for photopolymerization 3D printing, which uses phosphoric acid as a solvent for diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator to achieve uniform dissolution without surfactant.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned precursor composition.

[0008] Another object of the present invention is to provide a 3D printing method using the above-described precursor composition and a conductive hydrogel obtained therefrom.

[0009] To achieve the above objectives, the present invention provides the following technical solution: A conductive hydrogel precursor composition for photopolymerizable 3D printing comprises an acrylamide monomer, a polyethylene glycol diacrylate crosslinking agent, a diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator, and phosphoric acid, wherein the phosphoric acid serves as a solvent for the photoinitiator, enabling the composition to achieve uniform dissolution of the photoinitiator without the addition of a surfactant.

[0010] Furthermore, the phosphoric acid in the composition has a mass fraction of 15% to 60%.

[0011] Furthermore, the mass of the photoinitiator is 0.5% to 2% of the mass of the acrylamide monomer.

[0012] Furthermore, the mass of the crosslinking agent is 0.1% to 2.5% of the mass of the acrylamide monomer.

[0013] A method for preparing a conductive hydrogel precursor for photopolymerization 3D printing includes: simultaneously adding acrylamide monomer, polyethylene glycol diacrylate crosslinking agent and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator to a phosphoric acid solution, stirring at room temperature in the dark until completely dissolved, and obtaining a homogeneous precursor solution in one step.

[0014] A method for preparing a photopolymerizable 3D printed conductive hydrogel involves placing the precursor solution under ultraviolet light irradiation and curing it into a conductive hydrogel using a predetermined curing and molding step.

[0015] Furthermore, the wavelength of ultraviolet light is 380–420 nm, and the XY axis resolution is 20–80 micrometers.

[0016] Further, the curing and molding step is as follows: the precursor solution is poured into a liquid tank with a release film at the bottom, the volume of the solution is increased by 2-3 mL from the calculated volume of the printed model, and the slicing parameters of the printed model are: layer height of 0.025-0.1 mm, layer curing time of 3-8 s, lifting distance of 5-10 mm, and lifting speed of 60-120 mm / min.

[0017] A conductive hydrogel, formed by curing using the above method, comprises a polyacrylamide network, phosphoric acid, and a uniformly distributed component derived from diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

[0018] The application of the above-described conductive hydrogel precursor composition or the conductive hydrogel in flexible wearable sensors.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) In this invention, phosphoric acid is used as a solvent for diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. By utilizing the strong intermolecular forces between phosphoric acid and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, the uniform dissolution of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide at the molecular level is achieved, thus avoiding the use of surfactants.

[0020] (2) Diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide has extremely high solubility in phosphoric acid, which allows for the addition of high content of photoinitiator in the precursor, thereby achieving rapid photocuring and significantly improving printing efficiency.

[0021] (3) While promoting the dissolution of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phosphoric acid has abundant phosphate groups that can form strong intermolecular forces with the amide groups in the polyacrylamide network, thereby enhancing the crosslinking density of the hydrogel network and significantly improving the fracture strength, Young's modulus and toughness of the hydrogel, thus overcoming the problem of poor mechanical properties of traditional fast-curing hydrogels.

[0022] (4) The introduction of phosphoric acid endows the hydrogel with high ionic conductivity and excellent long-term stability, which can effectively solve the problem of conductivity decay caused by water loss in traditional ionic conductive hydrogels.

[0023] (5) The conductive hydrogel prepared by the method of the present invention can be used in flexible wearable sensors and has high sensitivity (>465.59 kPa). -1 With advantages such as short response time (<200ms) and good repeatability (0~40% strain), it can be used in scenarios such as human pulse monitoring, joint motion monitoring, and repeated pressure force monitoring. Attached Figure Description

[0024] Figure 1 This is a schematic diagram comparing the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in water and phosphoric acid solution.

[0025] Figure 2 Fourier transform infrared spectra of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide powder, aqueous phosphoric acid solution, phosphoric acid solution saturated with diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, aqueous solution saturated with diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and polyacrylamide-phosphoric acid hydrogel.

[0026] Figure 3 The graph shows the solubility curves of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in solutions with different phosphoric acid contents at room temperature.

[0027] Figure 4 The graph shows the relationship between phosphoric acid content and gelation time for hydrogels with different phosphoric acid contents in Examples 1-5.

[0028] Figure 5 The graphs show the Young's modulus and fracture strength of hydrogels with different phosphate contents in Examples 1-5.

[0029] Figure 6 The graph shows the conductivity data of hydrogels with different phosphate contents in Examples 1-5.

[0030] Figure 7 The graph shows the changes in residual mass and conductivity of hydrogels with different phosphate contents in Examples 1 and 5 over 30 days.

[0031] Figure 8 The images show the physical and digital models of the lattice structure printed by the photopolymerization 3D printing conductive hydrogel proposed in this invention.

[0032] Figure 9 This is an optical micrograph of a microstructure sample printed using the conductive hydrogel produced by photopolymerization 3D printing according to the present invention.

[0033] Figure 10 The graph shows the sensitivity, response time, and repeatability data of conductive hydrogels used in flexible wearable sensors.

[0034] Figure 11 This image shows the application effect of the photopolymerized 3D printed conductive hydrogel proposed in this invention in flexible sensing. Detailed Implementation

[0035] To better understand the present invention, specific embodiments are given below for further explanation. It should be noted that the following embodiments should not be construed as limiting the scope of protection of the present invention, that is, the present invention is not limited to the following embodiments.

[0036] Example 1 A precursor for dispersing a photoinitiator using a surfactant comprises the following components by mass: 3g acrylamide, 7g deionized water, 0.018g polyethylene glycol diacrylate, 0.03g diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.21g sodium dodecyl sulfate, and 0.02g tartrazine, a light absorber.

[0037] Preparation steps: First, dissolve sodium dodecyl sulfate in deionized water. Then, add acrylamide, polyethylene glycol diacrylate, and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide to the above-mentioned deionized water solution containing sodium dodecyl sulfate. Stir at room temperature (25°C) for 2 hours until all solids are completely dissolved. Then, add lemon yellow and continue stirring for 15 minutes to obtain a uniform and transparent precursor solution.

[0038] Printing steps: Inject the above precursor solution into the resin tank of the digital light processing 3D printer, and set the printing parameters as follows: ultraviolet light wavelength 405 nm, exposure power density 4 mW / cm². 2 The single-layer thickness is 0.05 mm, the single-layer curing time is 4 s, and the molding platform descends / ascends at a speed of 90 mm / min. After layer-by-layer curing is completed, the sample is taken out and rinsed with deionized water to remove residual precursors on the surface. It is then placed in a UV curing chamber for 2 minutes of post-curing to obtain a hydrogel using a surfactant-dispersed photoinitiator.

[0039] Example 2 A phosphoric acid-promoted dissolution conductive hydrogel precursor comprises, by weight, the following components: 3 g acrylamide, 1.5 g phosphoric acid, 5.5 g deionized water, 0.018 g polyethylene glycol diacrylate, 0.03 g diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and 0.02 g tartrazine light absorber.

[0040] Preparation steps: Acrylamide, polyethylene glycol diacrylate and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide were added to a phosphoric acid solution (concentration 15 wt%) composed of phosphoric acid and deionized water. The mixture was stirred at room temperature (25℃) for 2 hours until all solids were completely dissolved. Then, lemon yellow was added and stirring was continued for 15 minutes to obtain a uniform and transparent precursor solution.

[0041] Printing steps: Inject the above precursor solution into the resin tank of the digital light processing 3D printer, and set the printing parameters as follows: ultraviolet light wavelength 405 nm, exposure power density 4 mW / cm². 2 The single-layer thickness is 0.05 mm, the single-layer curing time is 4 s, and the molding platform descends / ascends at a speed of 90 mm / min. After layer-by-layer curing is completed, the sample is taken out and rinsed with deionized water to remove residual precursors on the surface. It is then placed in a UV curing chamber for 2 minutes of post-curing to obtain conductive hydrogel.

[0042] Example 3 A phosphoric acid-promoted dissolution conductive hydrogel precursor comprises, by weight, the following components: 3g acrylamide, 3g phosphoric acid, 4g deionized water, 0.018g polyethylene glycol diacrylate, 0.03g diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and 0.02g tartrazine light absorber.

[0043] Preparation steps: Acrylamide, polyethylene glycol diacrylate and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide were added to a phosphoric acid solution (concentration 30 wt%) composed of phosphoric acid and deionized water. The mixture was stirred at room temperature (25℃) for 2 hours until all solids were completely dissolved. Then, lemon yellow was added and stirring was continued for 15 minutes to obtain a uniform and transparent precursor solution.

[0044] Printing steps: Inject the above precursor solution into the resin tank of the digital light processing 3D printer, and set the printing parameters as follows: ultraviolet light wavelength 405 nm, exposure power density 4 mW / cm². 2 The single-layer thickness is 0.05 mm, the single-layer curing time is 4 s, and the molding platform descends / ascends at a speed of 90 mm / min. After layer-by-layer curing is completed, the sample is taken out and rinsed with deionized water to remove residual precursors on the surface. It is then placed in a UV curing chamber for 2 minutes of post-curing to obtain conductive hydrogel.

[0045] Example 4 A phosphoric acid-promoted dissolution conductive hydrogel precursor comprises, by weight, the following components: 3 g acrylamide, 4.5 g phosphoric acid, 2.5 g deionized water, 0.018 g polyethylene glycol diacrylate, 0.03 g diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and 0.02 g tartrazine light absorber.

[0046] Preparation steps: Acrylamide, polyethylene glycol diacrylate and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide were added to a phosphoric acid solution (concentration 45 wt%) composed of phosphoric acid and deionized water. The mixture was stirred at room temperature (25℃) for 2 hours until all solids were completely dissolved. Then, lemon yellow was added and stirring was continued for 15 minutes to obtain a uniform and transparent precursor solution.

[0047] Printing steps: Inject the above precursor solution into the resin tank of the digital light processing 3D printer, and set the printing parameters as follows: ultraviolet light wavelength 405 nm, exposure power density 4 mW / cm². 2 The single-layer thickness is 0.05 mm, the single-layer curing time is 4 s, and the molding platform descends / ascends at a speed of 90 mm / min. After layer-by-layer curing is completed, the sample is taken out and rinsed with deionized water to remove residual precursors on the surface. It is then placed in a UV curing chamber for 2 minutes of post-curing to obtain conductive hydrogel.

[0048] Example 5 A phosphoric acid-promoted dissolution conductive hydrogel precursor comprises, by weight: 3 g acrylamide, 6 g phosphoric acid, 1 g deionized water, 0.018 g polyethylene glycol diacrylate, 0.03 g diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and 0.02 g tartrazine light absorber.

[0049] Preparation steps: Acrylamide, polyethylene glycol diacrylate and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide were added to a phosphoric acid solution (concentration 60 wt%) composed of phosphoric acid and deionized water. The mixture was stirred at room temperature (25℃) for 2 hours until all solids were completely dissolved. Then, lemon yellow was added and stirring was continued for 15 minutes to obtain a uniform and transparent precursor solution.

[0050] Printing steps: Inject the above precursor solution into the resin tank of the digital light processing 3D printer, and set the printing parameters as follows: ultraviolet light wavelength 405 nm, exposure power density 4 mW / cm². 2 The single-layer thickness is 0.05 mm, the single-layer curing time is 4 s, and the molding platform descends / ascends at a speed of 90 mm / min. After layer-by-layer curing is completed, the sample is taken out and rinsed with deionized water to remove residual precursors on the surface. It is then placed in a UV curing chamber for 2 minutes of post-curing to obtain conductive hydrogel.

[0051] Example 6 The precursor solutions and printed hydrogels prepared in the above embodiments and comparative examples were evaluated as follows: (1) Gelization time: The gelation time was determined by using an optical rheometer under ultraviolet irradiation (4 mW / cm²). 2 In-situ monitoring was conducted to record the time corresponding to the intersection of the energy storage modulus and the loss modulus.

[0052] (2) Tensile mechanical properties: in accordance with GB / T2567 The 2008 testing standard requires that hydrogel samples printed in the shape of dumbbells be subjected to tensile testing according to standard methods to obtain fracture strength, Young's modulus, and toughness.

[0053] (3) Ionic conductivity: The ionic conductivity of the hydrogel was measured using the AC impedance method.

[0054] (4) Long-term stability: The hydrogel sample was placed in an environment with room temperature and 50% relative humidity. After 30 days, the mass retention rate and conductivity changes were measured.

[0055] The following is in conjunction with the appendix Figure 1-7 Table 1 further illustrates the relevant performance of the samples in each embodiment.

[0056] Table 1

[0057] Figure 1 This is a schematic diagram comparing the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in water and phosphoric acid solution. As shown in the figure, the chemical structures of the raw materials of the acrylamide-polyethylene glycol diacrylate (PT-AP) ionic hydrogel with phosphoric acid-coated diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide are illustrated, along with the traditional preparation process and the one-step preparation process and UV curing mechanism of this invention. The raw materials of the system include acrylamide (AAm), photoinitiator TPO, crosslinking agent polyethylene glycol diacrylate (PEGDA), and phosphoric acid (PA), which can ionize to generate hydrogen ions and dihydrogen phosphate ions. In the traditional process, TPO is difficult to dissolve in pure water, and sodium dodecyl sulfate (SDS) surfactant must be added to obtain a uniform precursor. However, this invention can directly dissolve TPO powder in phosphoric acid solution to achieve complete dissolution, and then add AAM and PEGDA to obtain a surfactant-free, uniform PT-AP precursor in one step. The components in the precursor are uniformly dispersed by hydrogen bonds. After the precursor undergoes a free radical polymerization reaction under UV irradiation, a transparent PT-AP ionic hydrogel containing anionic and cationic crosslinking networks of ionized phosphoric acid is formed, which is suitable for photocuring 3D printing molding processes.

[0058] Figure 2Fourier transform infrared (FTIR) spectra of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide powder (TPO powder), phosphoric acid aqueous solution (PA solution), phosphoric acid solution saturated with diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TPO-saturated PA Solution), aqueous solution saturated with diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (TPO-saturated aqueous solution), and polyacrylamide-phosphine hydrogel (PAAm-PA60% Hydrogel). The FTIR spectrum of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide powder is in the wavenumber range of 3000 to 2800 cm⁻¹. -1 An absorption peak for the stretching vibration of the aromatic ring and methyl group appears in the range of 1662 to 1436 cm⁻¹. -1 There are multiple absorption peaks corresponding to benzene ring vibrations within the range, especially between 1116 and 1193 cm⁻¹. -1 A strong absorption peak attributable to the stretching vibration of the phosphorus-oxygen double bond appears in the range, and these spectral characteristics are consistent with the chemical structure of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. Compared with pure phosphoric acid solution, phosphoric acid solution containing saturated diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide shows a higher absorption peak in the range of 3000 to 2800 cm⁻¹. -1 1100 to 1600 cm -1 The presence of more sharp absorption peaks in the region confirms the presence of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide in the system. Notably, compared to pure phosphoric acid solution, the absorption peak of the asymmetric stretching vibration of the phosphorus-oxygen bond in the phosphoric acid solution containing saturated diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide exhibits a slight red shift, with the peak value decreasing from approximately 1003 cm⁻¹. -1 Offset to approximately 1001 cm -1 This phenomenon demonstrates the existence of hydrogen-bonded intermolecular interactions between the two. In contrast, the infrared spectrum of an aqueous solution containing saturated diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide largely overlaps with that of pure water, and no sharp characteristic peaks attributed to diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide were observed. This spectral evidence confirms the low solubility of this substance in water and its stable solubility in phosphoric acid systems. The infrared spectrum of the polyacrylamide-phosphoric acid hydrogel simultaneously contains the characteristic absorption peaks of the amide in polyacrylamide, the phosphorus-oxygen bond absorption peaks of phosphoric acid, and the characteristic peaks of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, indicating that irreversible destruction of functional groups did not occur during gel formation. A significant red shift was observed in the absorption peak of the asymmetric stretching vibration of the phosphorus-oxygen bond, with the peak value decreasing from approximately 1003 cm⁻¹. -1 Offset to 998 cm -1This study demonstrates that strong hydrogen bonds are formed between the nitrogen-hydrogen bonds and phosphorus-oxygen bonds between the phosphate hydroxyl groups and the amide groups of polyacrylamide. These strong hydrogen bonds significantly enhance the Young's modulus and fracture strength of the hydrogel.

[0059] Figure 3 The figure shows the relationship between the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and the phosphoric acid content. As shown, the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide gradually increases with increasing phosphoric acid content, reaching its maximum at a phosphoric acid content of 60 wt%. The solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide is approximately four orders of magnitude higher than that of the precursor solution with 0 wt% phosphoric acid. Furthermore, Figure 3 The results indicate that when the phosphoric acid content is 45%, the rate of change in the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide has begun to approach stability. After that, further increasing the phosphoric acid content to 60% does not significantly improve the solubility of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and the photoinitiation efficiency also tends to stabilize.

[0060] Combining the data in Table 1 and Figure 4 It can be seen that in Example 1, sodium dodecyl sulfate was used to disperse diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. The precursor gelled for more than 8 seconds under UV irradiation, resulting in slow curing speed, which could not meet the requirements of high-speed photopolymerization 3D printing. Examples 2-5 did not use surfactants, but only phosphoric acid as the solvent for diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide. As the phosphoric acid content increased from 15% to 60%, the gelation time gradually decreased from about 7.5 seconds to 3.3 seconds (Example 5), which was more than twice that of Example 1. This shows that when the phosphoric acid content is 60% of the precursor solution mass fraction (the solution also contains 30% acrylamide monomer, 10% crosslinking agent, initiator and water), the diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide is most fully dissolved and dispersed, and the photoinitiation efficiency is the highest, thus significantly accelerating the photopolymerization speed.

[0061] Combining the data in Table 1 and Figure 5 It can be seen that the hydrogel printed in Example 1 has a tensile strength of 43 kPa, a Young's modulus of 4.2 kPa, and a toughness of 217 kJ / m. 3 The overall mechanical properties were poor because the presence of sodium dodecyl sulfate introduced interfacial defects, and the uneven dispersion of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide led to incomplete cross-linking. The fracture strength, Young's modulus, and toughness of Examples 2-5 all increased significantly with increasing phosphoric acid content. Example 5 achieved a fracture strength of 430 kPa, a Young's modulus of 137.5 kPa, and a toughness of 1530.71 kJ / m. 3Compared with Example 1, the yields were increased by approximately 893%, 3190%, and 605%, respectively. This is because phosphoric acid ensures the uniform dissolution and efficient initiation of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and on the other hand, the phosphate group forms a strong intermolecular force with the amide group in the polyacrylamide network, which enhances the network crosslinking density and endows the hydrogel with excellent mechanical properties.

[0062] Combining the data in Table 1 and Figure 6 It can be seen that the ionic conductivity of Example 1 is only 0.063 mS / cm, indicating a weak ion transport capacity. The conductivity of Examples 2 to 5 increases significantly with the increase of phosphoric acid content. The conductivity of Example 5 reaches 25.11 mS / cm, which is nearly 400 times that of the comparative sample. Phosphoric acid itself is a proton conductor, and the increase of its content provides richer proton transport pathways inside the hydrogel, thereby greatly improving the ionic conductivity.

[0063] Combining the data in Table 1 and Figure 7 It can be seen that the hydrogel prepared in Example 1, after being placed in an environment of room temperature and 50% relative humidity for 30 days, had a mass retention rate of only about 40%, and its conductivity decreased by nearly an order of magnitude, indicating severe shrinkage due to water loss. The long-term stability of Examples 2 to 5 improved significantly with the increase of phosphoric acid content. In Example 5, the mass retention rate was about 95% after 30 days under the same conditions, and the conductivity decreased only slightly, while the appearance and size remained basically unchanged. This is attributed to the strong intermolecular forces between phosphoric acid and water molecules, which effectively inhibited the evaporation and loss of water, giving the hydrogel excellent moisturizing and long-term stable conductivity.

[0064] Figure 8 The figures show the physical and digital models of the conductive hydrogel lattice structure printed by photopolymerization 3D printing proposed in this invention. The figures show the physical samples of the conductive hydrogel lattice structure prepared by photopolymerization 3D printing technology and their corresponding digital models. The array in the figures presents a variety of lattice designs with different topologies, ranging from porous three-dimensional structures with complex protrusions on the surface to cubic-like structures with different porosities and node connections. The physical samples in each column are highly consistent with the digital models above them, which intuitively proves that the printing method has extremely high forming accuracy and fidelity at the microscale.

[0065] Figure 9The image shows an optical micrograph of the conductive hydrogel microstructure sample printed by photopolymerization 3D printing proposed in this invention. As shown, a series of standard test pieces with protrusions and flow channels were prepared. The width of the structure increases in a gradient of 80 micrometers from left to right. All microstructures within this gradient range can be completely formed without deformation or collapse defects. The measured dimensions of the protrusions and flow channels are highly consistent with the original design model. In terms of digital light processing molding technology, the surface morphology of the molded part is not an irregular structure, but a periodic texture determined by the pixel size of the device. The magnified microscopic image shows clear stripes with a period of 80 micrometers, which perfectly matches the projection resolution of the device. In addition, this invention also prepared a variety of pyramidal microstructures, and the relevant structures were all replicated with high precision, further verifying the manufacturing capability of this invention for small feature sizes. Figure 10 This chart presents the sensitivity, response time, and repeatability data for conductive hydrogel applications in flexible wearable sensors. The relative capacitance change of the sensor exhibits three highly linear intervals with varying applied pressure, with linear correlation coefficients greater than 0.99 in each interval. The corresponding sensing sensitivity is 465.59 kPa in the pressure ranges of 0–0.5 kPa, 0.5–2 kPa, and 2–5 kPa. -1 187.25 kPa -1 , and 92.63 kPa -1 The sensor's pressurization response time is approximately 180 milliseconds, and its depressurization recovery time is approximately 200 milliseconds. The sensor can maintain a stable dynamic response under variable amplitude cyclic loads ranging from 10% to 40%, and can output signal peaks with good repeatability under different strain levels.

[0066] Figure 11 This paper demonstrates the application effects of a flexible wearable sensor based on photopolymerized 3D-printed conductive hydrogel. The flexible wearable sensor is effectively used for pulse monitoring. Comparison of the sensor capacitance changes with heart rate in resting and active states confirms that the sensor can capture weak physiological signals under weak mechanical stimulation. In joint motion monitoring, the capacitance change during wrist axial rotation is shown, demonstrating the sensor's sensitive response to moderate-amplitude joint movements. In repetitive pressure force monitoring, the capacitance response curves under finger pressing and releasing actions verify the sensor's usability under high compressive load conditions. In summary, the flexible wearable sensor based on photopolymerized 3D-printed conductive hydrogel can simultaneously monitor human physiological activities and limb mechanical movements by relying on precise capacitance change signals.

[0067] In summary, Example 5 exhibits the best performance in terms of curing speed, mechanical properties, electrical conductivity, long-term stability, and printing accuracy, representing the optimal implementation of the present invention. This precursor system achieves rapid photocuring and high mechanical strength without the need for any surfactants, simply by directly dissolving diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide with phosphate. It also possesses high ionic conductivity and excellent long-term moisture retention stability, making it widely applicable in fields such as flexible sensors where high electromechanical performance and structural complexity are required.

[0068] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A conductive hydrogel precursor composition for photopolymerization 3D printing, characterized in that, The composition comprises acrylamide monomer, polyethylene glycol diacrylate crosslinking agent, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator, phosphoric acid, and water, wherein the phosphoric acid serves as a solvent for the photoinitiator, thereby enabling the composition to achieve uniform dissolution of the photoinitiator without the addition of a surfactant.

2. The composition according to claim 1, characterized in that, The phosphoric acid in the composition has a mass fraction of 15% to 60%.

3. The composition according to claim 1, characterized in that, The mass of the photoinitiator is 0.5% to 2% of the mass of the acrylamide monomer.

4. The composition according to claim 1, characterized in that, The mass of the crosslinking agent is 0.1% to 2.5% of the mass of the acrylamide monomer.

5. The method for preparing the conductive hydrogel precursor for photopolymerization 3D printing according to any one of claims 1-4, characterized in that, Diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide photoinitiator, acrylamide monomer, and polyethylene glycol diacrylate crosslinking agent were dissolved in a phosphoric acid solution and stirred until completely dissolved to obtain a homogeneous precursor solution free of surfactants.

6. A method for preparing a photopolymerizable 3D printed conductive hydrogel, characterized in that, Using the composition of any one of claims 1 to 4 as a printing precursor, the mixture is cured layer by layer under ultraviolet light irradiation.

7. The preparation method according to claim 6, characterized in that, The wavelength of the ultraviolet light is 380–420 nm.

8. The preparation method according to claim 6, characterized in that, The curing time for a single layer is 3–8 seconds, and the layer thickness is 0.025–0.1 mm.

9. A conductive hydrogel, characterized in that, The product is formed by curing according to any one of claims 6-8 and comprises a polyacrylamide network, phosphoric acid, and a uniformly distributed component derived from diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

10. The application of the conductive hydrogel precursor composition according to any one of claims 1-4 or the conductive hydrogel according to claim 9 in a flexible wearable sensor.