A maleimide-based copolymer fluorescent material containing a urea / thiourea structure and its preparation method
Maleimide-based copolymers containing urea/thiourea structures were prepared by free radical copolymerization of maleimide derivatives and allyl urea monomers. This solved the problem of non-traditional fluorescent polymers emitting light concentrated in the blue light region, achieving multicolor fluorescence emission, which can be applied to Fe3+ detection and fluorescent thin films.
Patent Information
- Application Number
- CN202611635753.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing non-traditional fluorescent polymers emit light primarily in the blue light region. Designing and synthesizing non-traditional polymers that emit light at long wavelengths remains a challenge, especially the design and synthesis of polymers that emit green, yellow, or even red fluorescence.
Maleimide-based derivative monomers and allyl urea monomers are subjected to free radical copolymerization. By adjusting the molar ratio and type of monomers, maleimide-based copolymers containing urea/thiourea structures are formed. The urea groups are used to form intramolecular or intermolecular hydrogen bonds to enhance spatial interactions and achieve a redshift in emission wavelength.
The prepared copolymer can emit green, orange-red, or red multicolor fluorescence in solution, and can be applied to the fields of Fe3+ detection and fluorescent thin films. The synthesis process is simple and the conditions are mild.
Smart Images

Figure CN123106987A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer luminescent materials, and relates to a maleimide-based copolymer fluorescent material and its preparation method, specifically a maleimide-based copolymer fluorescent material with a urea / thiourea structure and its preparation method. Background Technology
[0002] In recent years, non-traditional fluorescent polymers lacking large π-conjugated units have attracted widespread attention from researchers due to their unique photophysical properties. These luminescent materials typically contain electron-rich heteroatoms such as N, O, S, and P, as well as non-conjugated structural units such as amides, esters (-COOR), carbonyl groups (C=O), cyano groups (C=N), carbon-carbon double bonds (C=C), and imine bonds (C=N). Therefore, they possess advantages such as easily tunable structures, environmental friendliness, and excellent biocompatibility, making them promising candidates for applications in fields such as bioimaging, data anti-counterfeiting, and metal ion detection. However, the luminescence of non-conjugated polymers is concentrated in the blue light region, and the design and synthesis of non-traditional polymers exhibiting green, yellow, or even red fluorescence emission remains a key challenge in this field.
[0003] Maleimide, as one of the most important nitrogen-containing heterocycles in organic synthesis, can have one or more hydrogen atoms replaced by different chemical groups to form substituted maleimides. Substituted maleimides, while maintaining the integrity of the double bonds within the heterocycle, provide more functional modification sites, expanding their application range in organic coupling. Liu et al. (Advanced Functional Materials, 2024, 34 (38): 2402578.) introduced alkyl side chains onto the maleimide ring as a flexible "protective layer" to stabilize the clusters formed by polymaleimide. The polymer exhibited effective cluster luminescence, where the introduction of hexyl side chains balanced the rigidity and flexibility of the copolymer structure, achieving a high quantum yield. Zhang et al. (Macromolecules, 2024, 57 (7): 3121-3130) synthesized a series of maleimide-based polymers through free radical copolymerization of electron-withdrawing maleimide derivatives and electron-donating monomers. These polymers all exhibited significant fluorescence emission, covering a range from blue to red. The van der Waals forces between carbonyl groups and the hydrogen bonds between donor and acceptor groups jointly drive the formation of spatially conjugated DA clusters, resulting in a redshift in emission. Since non-traditional luminescent polymers lack large π-conjugated structures, designing and preparing non-traditional luminescent polymers with long-wavelength emission remains a core challenge in this field.
[0004] Therefore, this invention develops a maleimide-based copolymer fluorescent material containing a urea / thiourea structure and its preparation method, achieving an effective redshift of the emission wavelength. Summary of the Invention
[0005] To overcome the shortcomings of existing materials, this invention provides a maleimide-based copolymer fluorescent material containing a urea / thiourea structure and its preparation method. The method involves a free radical copolymerization reaction of a maleimide-based derivative monomer with an allyl urea monomer to prepare a maleimide-based copolymer containing a urea / thiourea structure. The urea group can form multiple intramolecular or intermolecular hydrogen bonds, thereby enhancing spatial interactions and causing a red shift in the emission wavelength of the maleimide-based copolymer. Solutions of the maleimide-based copolymer containing a urea / thiourea structure synthesized by this method can emit multicolor fluorescence (including green, orange-red, or red).
[0006] This invention provides a maleimide-based copolymer containing a urea / thiourea structure, synthesized by free radical copolymerization of maleimide-based derivative monomers and allyl urea monomers in a specific molar ratio. By adjusting the molar ratio of the two monomers and the type of maleimide-based derivative monomer, different maleimide-based copolymers with urea / thiourea structures can be prepared. The urea or thiourea groups in the copolymer structure form intramolecular or intermolecular hydrogen bonds, which helps enhance the fluorescence of the polymer. The prepared luminescent copolymer can be used in Fe... 3+ Applications include detection and luminescent thin films.
[0007] This invention provides a maleimide-based copolymer fluorescent material containing a urea / thiourea structure, which is prepared by free radical polymerization of maleimide-based derivative monomers and allyl urea monomers. The structural formula of the copolymer fluorescent material is as follows:
[0008] In the formula, R1 is one of hydrogen, methyl, ethyl, phenyl, propionic acid, benzyl, and p-hydroxyphenyl; R2 is one of urea, thiourea, and hydantoin; x and y represent the degree of polymerization of the corresponding repeating unit, with x ranging from 10 to 50 and y ranging from 10 to 50.
[0009] Further, the molar ratio of the maleimide derivative monomer to the allylurea monomer is 2:1 to 1:2. The allylurea monomer is one of allylurea, allyl thiourea, or 1-allyl hydantoin. The maleimide derivative monomer is one of maleimide, N-methylmaleimide, N-ethylmaleimide, N-phenylmaleimide, N-benzylmaleimide, 4-maleimide-phenol, and 3-maleimide-propionic acid.
[0010] This invention provides a method for preparing the above-mentioned maleimide-based copolymer fluorescent material containing a urea / thiourea structure, comprising the following steps: Step 1: Dissolve maleimide derivative monomers and allyl urea monomers in an organic solvent at a molar ratio of 2:1 to 1:2 to prepare a solution with a total monomer concentration of 0.2 mol / L to 2.0 mol / L. Step 2: Add a free radical initiator to the above solution and bubble with N2 for 15-30 minutes to remove oxygen. Under N2 atmosphere, heat the reaction mixture to 60-90°C and stir magnetically for 20-28 hours. Step 3: After the reaction is complete, the solution is poured into a precipitant to precipitate, then allowed to stand, filtered, washed, and dried in a vacuum oven at 60°C for 8-12 hours to obtain the maleimide copolymer.
[0011] Further, the organic solvent is one of 1,4-dioxane, tetrahydrofuran, and N,N-dimethylformamide; the free radical initiator is azobisisobutyronitrile (AIBN), and the amount of free radical initiator is 0.5 mol% to 1 mol% of the total monomers. Further, the precipitant is one of n-hexane, petroleum ether, and methanol; the amount of precipitant is 5 to 10 times the volume of the solution after the reaction.
[0012] The copolymer solution emits green fluorescence under UV excitation at 254 and 365 nm; orange-red fluorescence under excitation at 460 nm; and red fluorescence under excitation wavelengths at 520 and 560 nm; with the maximum emission wavelength range being 500–600 nm. The copolymer powder (solid) emits red or green fluorescence under 365 nm UV irradiation.
[0013] This invention provides the above-mentioned maleimide-based copolymer fluorescent material containing a urea / thiourea structure in Fe 3+ Applications in detection. Preparation of solutions containing different concentrations of Fe. 3+ The copolymer solution was tested, and its fluorescence properties were evaluated.
[0014] This invention provides the application of the above-mentioned maleimide-based copolymer fluorescent material containing a urea / thiourea structure in fluorescent films. The specific application process is as follows: 0.4 g of polyvinyl alcohol is added to 20 mL of water and stirred at 100°C until dissolved, obtaining a 0.02 g / mL polyvinyl alcohol solution. 1 mL of the maleimide-based copolymer solution and 5 mL of the prepared polyvinyl alcohol solution are measured and mixed. After mixing evenly, the mixture is stirred for 0.5 to 1 hour, poured into a circular mold, and placed in an oven at 50°C to 80°C for 2 to 5 hours, successfully obtaining a PVA film doped with the copolymer.
[0015] Furthermore, the concentration of the maleimide copolymer solution is 0.5 mg / mL to 2 mg / mL.
[0016] The beneficial effects of this invention are: (1) This invention proposes a maleimide-based copolymer fluorescent material containing urea / thiourea structure. By adjusting the type of maleimide-based derivative monomer and the molar ratio of maleimide-based monomer to urea- or thiourea-based monomer, maleimide-based copolymers containing urea or thiourea structure can be prepared. (2) The maleimide copolymer containing urea / thiourea structure obtained by the present invention has mild reaction conditions, simple synthesis process and is easy to realize; (3) The maleimide copolymer containing urea / thiourea structure prepared in this invention emits fluorescence in both powder and solution states. In solution, it can achieve multicolor fluorescence emission of green, orange-red, or red, and is used in Fe... 3+ Applications include detection and fluorescent thin films. Attached Figure Description
[0017] Figure 1 A schematic diagram of the synthetic route for maleimide copolymers containing urea / thiourea structures; Figure 2 The images show the solid-state fluorescence spectra of the copolymer fluorescent materials prepared in Examples 1 and 2, as well as their fluorescence photographs under sunlight and different excitation lights; wherein, A is the poly(N-phenylmaleimide-allylurea) prepared in Example 1, and B is the poly(N-phenylmaleimide-allylthiourea) prepared in Example 2. Figure 3 The fluorescence spectra of the copolymer fluorescent materials prepared in Examples 1 and 2 are obtained in DMF solutions of different concentrations; where A is the poly(N-phenylmaleimide-allylurea) prepared in Example 1 and B is the poly(N-phenylmaleimide-allylthiourea) prepared in Example 2. Figure 4 Fluorescence images of the poly(N-phenylmaleimide-allylurea) solutions prepared in Example 1 and the poly(N-phenylmaleimide-allylthiourea) solutions prepared in Example 2 under sunlight and different excitation light; Figure 5 The poly(N-phenylmaleimide-allylurea) prepared in Example 1 reacts with different metal ions and different concentrations of Fe. 3+ The fluorescence detection spectrum; where A represents different metal ions and B represents different iron ion concentrations; Figure 6 Application of the copolymer fluorescent materials prepared in Examples 1 and 2 in polyvinyl alcohol luminescent films. Detailed Implementation
[0018] The present invention will be further illustrated by the following embodiments, but is not limited to the following embodiments.
[0019] This invention provides a maleimide copolymer containing a urea / thiourea structure, synthesized by free radical copolymerization of maleimide derivative monomers and allyl urea monomers in a molar ratio of 2:1 to 1:2. Different types of maleimide copolymers containing urea / thiourea structures can be prepared by adjusting the molar ratio of the two monomers and changing the types of monomers. The urea or thiourea groups form intramolecular or intermolecular hydrogen bonds, which helps to enhance the fluorescence properties of the polymer. Therefore, the maleimide copolymer containing a urea / thiourea structure prepared by this invention has the characteristics of simple synthesis process, tunable structure, and multicolor fluorescence emission, and can be used in Fe... 3+ Applications include fluorescence detection and luminescent thin films.
[0020] Example 1: Preparation of poly(N-phenylmaleimide-allylurea) (P1) The specific method is as follows: N-phenylmaleimide (0.01 mol) and allyl urea (0.01 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and azobisisobutyronitrile (AIBN) (0.0001 mol) was added as an initiator. The polymerization reaction was carried out at 70 °C under a N2 atmosphere for 24 h. After the reaction was completed, the polymerization solution was poured into n-hexane to precipitate, the precipitate was collected by filtration, and then washed three times with tetrahydrofuran. The product was dried to constant weight in a vacuum oven.
[0021] Example 2: Preparation of poly(N-phenylmaleimide-allyl thiourea) (P2) The specific method is as follows: N-phenylmaleimide (0.01 mol) and allyl thiourea (0.01 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and AIBN (0.0001 mol) was added as an initiator. The polymerization reaction was carried out at 70 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane to precipitate, the precipitate was collected by filtration, and then washed three times with chloroform. The obtained product was dried to constant weight in a vacuum oven.
[0022] Example 3: Preparation of poly(3-maleimide propionate-1-allyl hydantoin) (P3) The specific method is as follows: 0.01 mol of 3-maleimide propionic acid and 0.02 mol of 1-allyl hydantoin were dissolved in 10 mL of ultra-dry 1,4-dioxane, and 0.00024 mol of AIBN was added as an initiator. The polymerization reaction was carried out at 80 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane to precipitate the product. The precipitate was collected by filtration and then washed three times with tetrahydrofuran. The resulting product was dried to constant weight in a vacuum oven.
[0023] Example 4: Preparation of poly(4-maleimide-phenol-1-allylhydantoin) (P4) The specific method is as follows: 4-maleimide-based phenol (0.02 mol) and 1-allylhydantoin-allylurea (0.01 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and AIBN (0.00015 mol) was added as an initiator. The polymerization reaction was carried out at 90 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane to precipitate, the precipitate was collected by filtration, and then washed three times with tetrahydrofuran. The product was dried to constant weight in a vacuum oven.
[0024] Example 5: Preparation of poly(N-methylmaleimide-allylurea) (P5) The specific method is as follows: N-methylmaleimide (0.015 mol) and allyl urea (0.01 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and AIBN (0.00015 mol) was added as an initiator. The polymerization reaction was carried out at 70 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane to precipitate, the precipitate was collected by filtration, and then washed three times with chloroform. The product was dried to constant weight in a vacuum oven.
[0025] Example 6: Preparation of poly(maleimide-1-allylhydantoin) (P6) The specific method is as follows: Maleimide (0.01 mol) and 1-allylhydantoin (0.01 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and AIBN (0.0002 mol) was added as an initiator. The polymerization reaction was carried out at 70 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane, the precipitate was collected by filtration, and then washed three times with acetone. The product was dried to constant weight in a vacuum oven.
[0026] Example 7: Preparation of poly(N-benzylmaleimide-allylthiourea) (P7) The specific method is as follows: N-benzylmaleimide (0.01 mol) and allyl thiourea (0.02 mol) were dissolved in 10 mL of ultra-dry 1,4-dioxane, and AIBN (0.00024 mol) was added as an initiator. The polymerization reaction was carried out at 70 °C under a N2 atmosphere for 24 h. After the reaction was completed, the reaction solution was slowly poured into n-hexane, the precipitate was collected by filtration, and then washed three times with chloroform. The product was dried to constant weight in a vacuum oven.
[0027] The synthetic route for the maleimide-based copolymer fluorescent material containing a urea / thiourea structure prepared in this invention is as follows: Figure 1 As shown, maleimide derivative monomers with a molar ratio of 2:1 to 1:2 and allyl urea monomers are copolymerized via free radical copolymerization to synthesize maleimide copolymers containing urea / thiourea structures.
[0028] Performance tests were conducted on the products obtained in Examples 1 and 2. For example... Figures 2-6 As shown.
[0029] Figure 2 The fluorescence spectrum and fluorescence photograph of the solid-state copolymer prepared by N-phenylmaleimide with allyl urea / allyl thiourea in a molar ratio of 1:1 are shown in the figure. It can be seen from the figure that under the excitation of 365 nm ultraviolet light, poly(N-phenylmaleimide-propylene urea) (P1) emits red fluorescence, with a maximum excitation wavelength of 460 nm and a maximum emission wavelength of 558 nm; poly(N-phenylmaleimide-propylene thiourea) (P2) emits green fluorescence, with a maximum excitation wavelength of 420 nm and a maximum emission wavelength of 493 nm.
[0030] Figure 3 and Figure 4 The results showed that the fluorescence of the poly(N-phenylmaleimide-allylurea) solution prepared in Example 1 significantly increased with increasing DMF concentration. However, the fluorescence of the poly(N-phenylmaleimide-allylthiourea) solution prepared in Example 2 initially increased gradually with increasing DMF concentration, reaching its peak at 1 mg / mL. Subsequently, the fluorescence intensity decreased with further increases in DMF concentration. This may be due to enhanced self-absorption and exciton-exciton interactions at high concentrations, leading to weakened fluorescence. Under UV irradiation at 254 nm and 365 nm, P1 and P2 emitted orange and yellow-green fluorescence, respectively. When excited by a 460 nm light source, P1 and P2 (concentrations above 0.5 mg / mL) exhibited orange-red and orange fluorescence, respectively. Further increasing the excitation wavelength to 520 nm, both P1 and P2 emitted red fluorescence. Under different excitation light, solutions P1 and P2 could emit multicolor fluorescence, including green, orange, and red.
[0031] Figure 5 This demonstrates that the poly(N-phenylmaleimide-allylurea) prepared in Example 1 can be used to detect Fe in solution. 3+ With Ca 2+ Co 2+ Cr 3+ Cu 2+ Zn 2+ Ni 2+ In comparison, Fe 3+ The addition of Fe significantly reduced the fluorescence of the copolymer. Different concentrations of Fe... 3+ The addition of [a substance] gradually reduced its fluorescence, and when the concentration increased to 4 mmol / L, the fluorescence was completely quenched.
[0032] Figure 6This section describes the application of poly(N-phenylmaleimide-allylurea) prepared in Example 1 and poly(N-phenylmaleimide-allylthiourea) prepared in Example 2 in polyvinyl alcohol (PVA) films. The specific application process is as follows: 0.4 g of polyvinyl alcohol was added to 20 mL of water and stirred at 100 °C until dissolved, yielding a 0.02 g / mL polyvinyl alcohol solution. 1 mL of the polymer solution (2 mg / mL) and 5 mL of the polyvinyl alcohol solution were measured and mixed. After thorough mixing, the mixture was stirred for another 30 minutes, poured into a circular mold, and placed in an oven at 50 °C for 5 hours. The resulting PVA films with doped copolymers were successfully prepared and designated as PVA / P1 and PVA / P2, respectively. As shown in the figure, the poly(N-phenylmaleimide-allylurea) prepared in Example 1 and the poly(N-phenylmaleimide-allylthiourea) prepared in Example 2, when doped into the polyvinyl alcohol network, successfully prepared fluorescent films. The prepared film emitted orange and red fluorescence when excited by a 365 nm UV lamp.
Claims
1. A maleimide-based copolymer fluorescent material containing a urea / thiourea structure, characterized in that, The copolymer fluorescent material is prepared by free radical polymerization of maleimide derivative monomers and allyl urea monomers. The structural formula of the copolymer fluorescent material is as follows: ; In the formula, R1 is one of hydrogen, methyl, ethyl, phenyl, propionic acid, benzyl, and p-hydroxyphenyl; R2 is one of urea, thiourea, and hydantoin; x and y represent the degree of polymerization of the corresponding repeating unit, with x ranging from 10 to 50 and y ranging from 10 to 50.
2. The maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 1, characterized in that, The molar ratio of the maleimide derivative monomer to the allyl urea monomer is 2:1 to 1:
2.
3. The maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 1, characterized in that, The allylurea monomer is one of allylurea, allyl thiourea, or 1-allyl hydantoin; the maleimide derivative monomer is one of maleimide, N-methylmaleimide, N-ethylmaleimide, N-phenylmaleimide, N-benzylmaleimide, 4-maleimide-phenol, or 3-maleimide-propionic acid.
4. The maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 1, characterized in that, The maleimide-based copolymer fluorescent material emits green, orange-red, or red fluorescence in solution under different excitation wavelengths, with a maximum emission wavelength of 500-600 nm; the maleimide-based copolymer fluorescent material emits red or green fluorescence in powder form under 365 nm ultraviolet light irradiation.
5. A method for preparing a maleimide-based copolymer fluorescent material containing a urea / thiourea structure as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Step 1: Dissolve maleimide derivative monomers and allyl urea monomers in an organic solvent at a molar ratio of 2:1 to 1:2 to prepare a solution with a total monomer concentration of 0.2 mol / L to 2.0 mol / L. Step 2: Add a free radical initiator to the above solution and bubble with N2 for 15 to 30 minutes to remove oxygen; under N2 atmosphere, heat the reaction mixture to 60°C to 90°C and stir magnetically for 20 to 28 hours. Step 3: After the reaction is complete, the solution is poured into a precipitant to precipitate, then allowed to stand, filtered, washed, and dried in a vacuum oven at 60°C for 8-12 hours to obtain the maleimide copolymer.
6. The method for preparing the maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 5, characterized in that, The organic solvent is one of 1,4-dioxane, tetrahydrofuran, and N,N-dimethylformamide.
7. The method for preparing the maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 5, characterized in that, The free radical initiator is azobisisobutyronitrile, and the amount of free radical initiator is 0.5 mol% to 1 mol of the total monomer.
8. The method for preparing the maleimide-based copolymer fluorescent material containing a urea / thiourea structure according to claim 5, characterized in that, The precipitant is one of n-hexane, petroleum ether, and methanol; the amount of precipitant used is 5 to 10 times the volume of the solution after the reaction.
9. A maleimide-based copolymer fluorescent material containing a urea / thiourea structure as described in any one of claims 1 to 4 in Fe 3+ Applications in detection.
10. The application of a maleimide-based copolymer fluorescent material containing a urea / thiourea structure as described in any one of claims 1 to 4 in a fluorescent thin film, characterized in that: The application process is as follows: 0.4 g of polyvinyl alcohol is added to 20 mL of water and stirred at 100 °C until dissolved to obtain a 0.02 g / mL polyvinyl alcohol solution; 1 mL of maleimide copolymer solution and 5 mL of the prepared polyvinyl alcohol solution are measured and mixed, stirred for 0.5 h to 1 h after mixing evenly, poured into a circular mold and placed in an oven at 50 °C to 80 °C for 2 h to 5 h to successfully obtain a PVA film doped with copolymer. The concentration of the maleimide copolymer solution is 0.5 mg / mL to 2 mg / mL.