A method for hydrogenation pretreatment of nitrile butadiene rubber and the hydrogenated nitrile butadiene rubber obtained therefrom
By employing a combined pretreatment method involving molecular sieves, adsorption resins, ion exchange resins, and chelating resins, the problem of incomplete impurity removal during the hydrogenation process of nitrile rubber in existing technologies has been solved, achieving efficient hydrogenation and improved product quality.
Patent Information
- Application Number
- CN202611190624.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-06
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to effectively remove impurities from nitrile rubber, leading to a decrease in the activity of the hydrogenation catalyst and affecting the quality and performance of hydrogenated nitrile rubber.
A combined pretreatment method using molecular sieves, adsorption resins, ion exchange resins, and chelating resins is employed to deeply remove moisture, organic impurities, and metal ions from nitrile rubber solutions, preventing catalyst poisoning and side reactions.
It significantly improves the hydrogenation saturation and uniformity of nitrile rubber, enhances product quality and performance, reduces side reactions, and extends catalyst life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of rubber hydrogenation modification technology, and in particular to a method for hydrogenation pretreatment of nitrile butadiene rubber and the hydrogenated nitrile butadiene rubber obtained therefrom. Background Technology
[0002] In the testing and production process of hydrogenated nitrile butadiene rubber (NBR), the most crucial step is the hydrogenation reaction: the NBR solution or emulsion is selectively hydrogenated in a high-pressure reactor under the action of a catalyst (such as Grubbs catalyst, rhodium-based catalyst, etc.) and additives. However, catalysts, being precious metals, are expensive and highly sensitive to moisture, various organic impurities, and metal ions, easily becoming poisoned and losing some or all of their activity. Therefore, removing impurities from the raw materials is of paramount importance.
[0003] In actual production and testing of nitrile rubber (NBR), residual acrylonitrile monomers remain. Various additives are added during polymerization, including emulsifiers, initiators, molecular weight regulators, chain transfer agents, and terminators. Furthermore, substances such as calcium chloride and sodium hydroxide are added during post-processing. Therefore, NBR contains impurities such as rubber residues, polar impurities, metal ions, low-molecular-weight byproducts, and unreacted monomers. In addition, the solvents used for hydrogenation of NBR solutions in industrial production are generally industrial grade, with high moisture and impurity content. These impurities directly adhere to and poison the hydrogenation catalyst, covering active sites and causing rapid catalyst activity decay and shortened lifespan. They also easily trigger increased side reactions during hydrogenation, leading to increased catalyst dosage for NBR hydrogenation and side effects such as uneven saturation and decreased mechanical and weather resistance properties of the product.
[0004] Water, being a polar ligand, adsorbs onto the surface of precious metal catalysts, competing for adsorption sites on the carbon-carbon double bonds in rubber molecules. This prevents the double bonds from approaching the metal for hydrogenation, significantly reducing catalytic activity. Furthermore, water induces numerous harmful side reactions, damaging the rubber molecular structure and leading to decreased product quality. Organic impurities harm catalysts in two ways: chemical poisoning (sulfur, amines, phosphorus, mostly irreversible) and physical deactivation (polymers, tar, soaps, regenerable by solvents). Sulfur-based organic compounds are the most destructive impurities; even trace amounts can permanently destroy the activity of precious metals. Basic amines and organophosphorus compounds damage the ligand structure of homogeneous catalysts. Macromolecules and phenols primarily clog the pores of heterogeneous catalysts. Impurity metal ions cause a decrease in hydrogenation catalyst activity, even permanent deactivation, through four main pathways: alloy poisoning, site competition, electronic modification, and support blockage. Simultaneously, they catalyze side reactions such as cyano hydrolysis, molecular chain scission, and oxidative discoloration, increasing precious metal consumption and severely damaging the mechanical and aging resistance properties of hydrogenated nitrile rubber products.
[0005] Currently, the industry primarily uses simple static filtration and conventional distillation pretreatment methods for nitrile rubber (NBR) solutions. These methods have limited ability to remove fine polar impurities, and conventional concentration easily leads to NBR molecular chain breakage and NBR aging and deterioration, affecting the quality of the finished product. Simply using heating and vacuum concentration only concentrates the material and cannot effectively remove harmful impurities; these impurities accumulate during concentration. These factors still severely restrict the overall effect of NBR hydrogenation modification, making it difficult to meet the production requirements of high-quality hydrogenated NBR. Furthermore, the current industry practice of hydrogenating NBR first and then removing impurities, while improving product purity, cannot eliminate the toxic effects of impurities in the NBR solution on the hydrogenation catalyst. Summary of the Invention
[0006] This invention provides a method for hydrogenation pretreatment of nitrile butadiene rubber (NBR) and the hydrogenated NBR obtained therefrom. After dissolving the NBR in a solvent, it is first passed through a molecular sieve to deeply remove moisture from the solution, preventing catalyst hydrolysis and cyano hydrolysis. Then, it is passed through an adsorption resin to remove peroxides and organic impurities from the solution, avoiding interference with subsequent ion exchange. Next, it is passed through an ion exchange resin to remove high-content metal ions from the solution, preventing catalyst consumption and side reactions. A chelating resin is connected in series at the end to remove trace amounts of precious metals not captured by the ion exchange resin. This method can significantly reduce the covering and poisoning effects of harmful impurities on the active sites of the hydrogenation catalyst, reduce the occurrence of side reactions during hydrogenation, and effectively improve the hydrogenation saturation and uniformity of the NBR.
[0007] In a first aspect, this application provides a method for hydrogenation pretreatment of nitrile rubber, comprising the following steps: S1. Cut and crush nitrile rubber into pieces, add solvent, heat and stir to dissolve, and obtain nitrile rubber solution; S2. The adsorption resin, ion exchange resin and chelating resin are pre-wetted and displacement activated with solvent to obtain pretreated adsorption resin, ion exchange resin and chelating resin. S3. The nitrile rubber solution obtained in step S1 is passed sequentially through a purification device containing a molecular sieve, the pretreated adsorption resin obtained in step S2, an ion exchange resin, and a chelating resin to obtain a purified nitrile rubber solution. S4. The purified nitrile rubber solution obtained in step S3 is sent to a concentration device and concentrated under high temperature and negative pressure conditions to obtain concentrated nitrile rubber solution. S5. The concentrated nitrile rubber solution obtained in step S4 is allowed to stand and homogenize, then introduced into a hydrogenation reactor, a catalyst is added, and a hydrogenation reaction is carried out.
[0008] By adopting the above technical solution, this application provides a method for the pretreatment of nitrile rubber for hydrogenation, which can improve the degree of hydrogenation of nitrile rubber. This is likely because, after dissolving the nitrile rubber in a solvent, it is first passed through a molecular sieve to deeply remove water from the rubber solution, preventing catalyst hydrolysis and cyano hydrolysis; then, it is passed through an adsorption resin to remove peroxides and organic impurities from the rubber solution, avoiding interference with subsequent ion exchange; next, it is passed through an ion exchange resin to remove high-content metal ions from the rubber solution, preventing catalyst consumption and side reactions; finally, a chelating resin is connected in series at the end to remove trace amounts of precious metals not captured by the ion exchange resin. This method can significantly reduce the coverage and poisoning effect of harmful impurities on the active sites of the hydrogenation catalyst, reduce the occurrence of side reactions during the hydrogenation process, effectively improve the hydrogenation saturation and uniformity of nitrile rubber, and comprehensively optimize the quality, experimental and production stability of the hydrogenated nitrile rubber product.
[0009] Optionally, in step S3, the molecular sieve is selected from at least one of type 3A molecular sieve, type 4A molecular sieve, and type 5A molecular sieve.
[0010] By adopting the above technical solution, the molecular sieve has regular and uniform nanopores inside, and exchangeable cations are distributed in the pores to form extremely strong polar electrostatic adsorption sites. The inner wall of the molecular sieve pores is filled with negatively charged silicon-aluminum-oxygen framework and cations, forming a local electric field. Polar water molecules are firmly adsorbed into the active sites in the pores by the electrostatic force of dipole-ion interaction, thereby achieving the purpose of water removal.
[0011] Preferably, the molecular sieve is selected from type 3A molecular sieve.
[0012] Optionally, in step S2, the adsorption resin includes styrene-based adsorption resin and acrylate-based adsorption resin.
[0013] By employing the above technical solution, the adsorption resin is a cross-linked polymer porous microsphere. In the organic system, the resin's hydrophobic framework repels the solvent, and it adsorbs organic impurities by van der Waals and hydrogen bonds, fixing them within the micropores. Non-polar resins (styrene-based) can adsorb non-polar and weakly polar organic substances (aromatics, rubber oligomers, oils, and olefins); moderately polar resins (acrylate-based) can adsorb polar and weakly polar substances.
[0014] Preferably, the adsorbent resin is an acrylate-based adsorbent resin.
[0015] Optionally, in step S2, the ion exchange resin includes macroporous sulfonic acid cation exchange resin and gel-type sulfonic acid cation exchange resin.
[0016] By adopting the above technical solution, residual metal ions in the adhesive solution diffuse into the resin channels, where metal cations replace hydrogen ions on the resin, thus fixing the metal onto the resin. This significantly reduces the metal content of the effluent, eliminating the need for extensive water washing and reducing the risk of wastewater and cyanide hydrolysis. Molecular sieves and macroporous adsorption resins rely solely on physical adsorption and have almost no retention capacity for dissolved metal ions. Water washing and filtration can only remove suspended catalyst particles, not metal ions dissolved in the adhesive solution. Cation exchange resins, however, can deeply remove dissolved precious metals.
[0017] Preferably, the ion exchange resin is a macroporous sulfonic acid-based cation exchange resin.
[0018] Optionally, in step S2, the chelating resin includes aminophosphonic acid chelating resin, thiourea-type chelating resin, and mercapto-type chelating resin.
[0019] By employing the above technical solution, the chelating resin is a functionalized adsorption resin with a framework of polystyrene-divinylbenzene macroporous cross-linked microspheres, on which multidentate coordination functional groups are bonded and grafted. These multidentate coordination functional groups contain at least one of nitrogen, sulfur, and oxygen atoms, which can act as coordinating atoms to form stable chelates with metal ions using five- or six-membered ring structures. This chelation effect is based on coordination bonds, and its binding strength is higher than that of ion exchange resins based on electrostatic interactions. It also exhibits selectivity for coexisting ions and carboxylic acid compounds. In the gel solution pretreated with ion exchange resin, the residual concentration of metal ions is reduced to the ppm level; after further treatment with chelating resin, the residual concentration can be further reduced to the ppb level. Simultaneously, due to the high stability of the chelate coordination bonds, after column chromatography at room temperature to medium temperature, the hydrogenated product will not experience slow precipitation of metal ions during long-term storage.
[0020] Preferably, the chelating resin is an aminophosphonic acid chelating resin.
[0021] Optionally, in step S1, the nitrile rubber includes ordinary nitrile rubber and / or nitrile rubber derivatives.
[0022] Optionally, the ordinary nitrile rubber is a binary copolymer of butadiene and acrylonitrile, and its acrylonitrile content, Mooney viscosity and polymer molecular weight can be selected according to actual needs. For example, any one or more of low, medium and high acrylonitrile contents can be selected.
[0023] Optionally, the nitrile rubber derivative includes carboxylated nitrile rubber and / or nitrile rubber incorporating a third ester of ester.
[0024] Optionally, in step S1, the solvent includes chlorobenzene, dichloromethane, acetone, tetrahydrofuran, and N-methylpyrrolidone.
[0025] Preferably, the solvent is chlorobenzene.
[0026] Optionally, in step S1, the stirring speed is 100 rpm to 200 rpm, the heating temperature is 50℃ to 100℃, and the dissolution time is 3 to 8 hours.
[0027] Optionally, in step S1, the mass concentration of nitrile rubber is 2-6%.
[0028] Optionally, in step S3, the flow rate of the nitrile rubber liquid through the purification device is 1~3 BV / h, and the temperature is 30~60℃.
[0029] Optionally, in step S3, after the adsorption resin and ion exchange resin have been used for a period of time, they can be regenerated and eluted with hydrochloric acid to achieve the recycling and reuse of the resin; the mass concentration of the hydrochloric acid is 2~6%, preferably 4%.
[0030] Optionally, in step S4, the concentration temperature of the purified nitrile rubber solution is 60~100℃, the concentration pressure is -70kPa~-90kPa, and the single residence time in the concentration device is 5~20s.
[0031] Optionally, in step S4, the concentration device includes a falling film evaporator, a flash tank, and a screw extruder; preferably, it is a falling film evaporator.
[0032] Optionally, in step S4, the mass concentration of the concentrated nitrile rubber solution is 6-10%.
[0033] Optionally, in step S5, the hydrogenation reaction is carried out under the following conditions: 115~125℃ and 5.5~6.5MPa for 6.5~7.5h.
[0034] In a second aspect of this application, this application provides a method for preparing hydrogenated nitrile rubber from the nitrile rubber hydrogenation pretreatment method described in the first aspect of this application.
[0035] Optionally, the hydrogenated nitrile rubber has virtually no metal ion residue and can be directly applied to electronic fields such as lithium-ion batteries, photovoltaic cells, and semiconductors.
[0036] In summary, the present invention has at least one of the following beneficial technical effects: 1. This application provides a method for hydrogenation pretreatment of nitrile rubber. The method involves sequentially passing through molecular sieves, adsorption resins, ion exchange resins, and chelating resins. The four impurity removal substances are arranged in a reasonable order and cooperate with each other, overcoming the shortcomings of existing hydrogenation pretreatment processes for nitrile rubber, such as incomplete impurity removal and poor hydrogenation improvement effect.
[0037] 2. This application provides a method for hydrogenation pretreatment of nitrile rubber. This pretreatment method effectively removes various organic impurities and metal ions from the rubber solution, which not only improves the hydrogenation effect of the rubber solution, but also reduces the side reactions caused by impurities, thereby improving product quality and performance, and improving the mechanical strength, oil resistance and heat aging resistance of the rubber.
[0038] 3. This application provides a hydrogenated nitrile butadiene rubber (NBR) with virtually no metal ion residue, which can be directly applied in electronic fields such as lithium-ion batteries, photovoltaic cells, and semiconductors. When this low-metal-residue hydrogenated NBR is applied in electronic fields such as lithium-ion batteries, photovoltaic cells, and semiconductors, it can effectively avoid problems such as insulation failure, electrochemical migration short circuits, corrosion failure, and accelerated aging caused by metal ion migration, significantly improving device safety and service life.
[0039] 4. This application provides a method for hydrogenation pretreatment of nitrile rubber. This method is not limited by the acrylonitrile monomer content, Mooney viscosity, polymerization molecular weight, or whether the nitrile rubber contains a third monomer. It can comprehensively cover the hydrogenation pretreatment test and production of nitrile rubber solutions with low acrylonitrile, medium acrylonitrile, and high acrylonitrile, and has extremely strong versatility and adaptability. Detailed Implementation
[0040] The embodiments of the present invention will be described in detail below with reference to the examples. However, those skilled in the art will understand that the following examples are only for illustrating the present invention and should not be regarded as limiting the scope of the present invention. Specific conditions not specified in the examples shall be carried out according to conventional conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0041] Ordinary nitrile butadiene rubber was purchased from Zhenjiang Nandi Chemical Co., Ltd. (3650), carboxyl nitrile butadiene rubber was purchased from Zhenjiang Nandi Chemical Co., Ltd. (3245C), acrylate-based adsorption resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (LXA501), styrene-based adsorption resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (LX-10), macroporous sulfonic acid-based cation exchange resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (D001), aminophosphonic acid chelating resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (LSC500), gel-type sulfonic acid-based cation exchange resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (LSC101), and thiourea-type chelating resin was purchased from Xi'an Lanxiao Technology New Material Co., Ltd. (LSC200).
[0042] Example 1 Example 1 provides a method for hydrogenation pretreatment of nitrile rubber, comprising the following steps: S1. Cut and crush ordinary nitrile rubber into pieces, add chlorobenzene, control the mass concentration of nitrile rubber at 4%, and stir at 150 rpm at 75°C for 5.5 hours to dissolve and obtain nitrile rubber solution. S2. 3A-type molecular sieves, acrylate-based adsorption resin, macroporous sulfonic acid-based cation exchange resin, and aminophosphonic acid chelating resin are packed from top to bottom into four tandem chromatography columns installed from top to bottom. Each column is made of glass, with an inner diameter of 1 cm and a height of 29 cm. The acrylate-based adsorption resin, macroporous sulfonic acid-based cation exchange resin, and aminophosphonic acid chelating resin in the chromatography columns are completely immersed in chlorobenzene solvent for 1 hour. Then, they are rinsed at a rate of 2 BV / h for 1 hour to activate the acrylate-based adsorption resin, macroporous sulfonic acid-based cation exchange resin, and aminophosphonic acid chelating resin. Finally, the air inside the chromatography columns is removed to complete the pretreatment and the columns are ready for use. S3. The nitrile rubber solution obtained in step S1 is loaded into the material conveying pump. The flow rate of the nitrile rubber solution is controlled at 2BV / h and the adsorption temperature is 45℃. Nitrogen gas is used for protection throughout the process. The nitrile rubber solution flows uniformly from top to bottom through the 3A molecular sieve, the pretreated acrylate adsorption resin, the macroporous sulfonic acid cation exchange resin and the aminophosphonic acid chelating resin in step S2 to obtain purified nitrile rubber solution. S4. Start the falling film evaporator unit, preheat the purified nitrile rubber solution to 130°C, start the vacuum unit, stabilize the vacuum degree of the falling film evaporator at -70kPa and the temperature at 100°C; feed the purified nitrile rubber solution obtained in step S3 into the falling film evaporator at a uniform speed, control the single residence time of the purified nitrile rubber to 12s, remove the solvent, increase the solid content of the purified nitrile rubber solution to 6%, and obtain concentrated nitrile rubber solution. S5. The concentrated nitrile rubber solution obtained in step S5 is sent to a buffer tank and allowed to stand and homogenize for 30 minutes. Then it is introduced into a hydrogenation reactor and 150 ppm (based on the mass of nitrile rubber) of catalyst GrubbsII is added to complete the catalytic hydrogenation reaction. The reaction temperature is 120℃, the reaction time is 7 hours, and the reaction pressure is 6 MPa.
[0043] Example 2
[0044] Example 2 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S1, ordinary nitrile rubber is replaced with carboxylated nitrile rubber.
[0045] The other steps are the same as in Example 1.
[0046] Example 3
[0047] Example 3 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that chlorobenzene is replaced with tetrahydrofuran in step S1.
[0048] The other steps are the same as in Example 1.
[0049] Example 4
[0050] Example 4 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the 3A molecular sieve is replaced with the 4A molecular sieve.
[0051] The other steps are the same as in Example 1.
[0052] Example 5
[0053] Example 5 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the acrylate-based adsorption resin is replaced with a styrene-based resin.
[0054] Example 6
[0055] Example 6 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the macroporous sulfonic acid cation exchange resin is replaced with a gel-type sulfonic acid cation exchange resin.
[0056] The other steps are the same as in Example 1.
[0057] Example 7
[0058] Example 7 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the aminophosphonic acid chelating resin is replaced with a thiourea-type chelating resin.
[0059] The other steps are the same as in Example 1.
[0060] Comparative Example 1 Comparative Example 1 provides a method for hydrogenation pretreatment of nitrile rubber. The difference from Example 1 is that steps S2, S3, and S4 are omitted, that is, the nitrile rubber solution is directly subjected to hydrogenation test without any treatment.
[0061] The specific steps are as follows: S1. Cut and crush ordinary nitrile rubber into pieces, add chlorobenzene, control the mass concentration of nitrile rubber at 4%, and stir at 150 rpm at 75°C for 5.5 hours to dissolve and obtain nitrile rubber solution. S2. The nitrile rubber solution obtained in step S1 is introduced into a hydrogenation reactor, and 150 ppm (based on the mass of nitrile rubber) of GrubbsII catalyst is added to complete the catalytic hydrogenation reaction; the reaction temperature is 120℃, the reaction time is 7h, and the reaction pressure is 6MPa.
[0062] Comparative Example 2 Comparative Example 2 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the chromatography column packed with type 3A molecular sieve is removed.
[0063] The other steps are the same as in Example 1.
[0064] Comparative Example 3 Comparative Example 3 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the chromatography column packed with acrylate-based adsorption resin is removed.
[0065] The other steps are the same as in Example 1.
[0066] Comparative Example 4 Comparative Example 4 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the chromatography column packed with macroporous sulfonic acid cation exchange resin is removed.
[0067] The other steps are the same as in Example 1.
[0068] Comparative Example 5 Comparative Example 5 provides a method for hydrogenation pretreatment of nitrile rubber, which differs from Example 1 in that, in step S2, the chromatography column packed with aminophosphonic acid chelating resin is removed.
[0069] The other steps are the same as in Example 1.
[0070] Performance testing The degree of hydrogenation of nitrile rubber solutions in Examples 1-7 and Comparative Examples 1-5 was tested according to SH / T 1762-2008, and the results are shown in Table 1.
[0071] Table 1 Degree of hydrogenation of nitrile rubber
[0072] Conclusion Analysis and Summary Based on Examples 1-7 and Table 1, it can be seen that pretreating the nitrile rubber solution sequentially through a molecular sieve, adsorption resin, ion exchange resin, and chelating resin before hydrogenation can increase the degree of hydrogenation. In Examples 3-7, after replacing the solvent with tetrahydrofuran, the molecular sieve with type 4A molecular sieve, the adsorption resin with styrene-based resin, the macroporous ion exchange resin with gel-type ion exchange resin, and the chelating resin with thiourea-type chelating resin, the degree of hydrogenation was slightly lower compared to Examples 1 and 2.
[0073] Based on Example 1, Comparative Examples 1-5, and Table 1, it can be seen that the nitrile rubber solution in Comparative Example 1, which was not pretreated, had the lowest degree of hydrogenation. In Comparative Examples 2-5, removing the molecular sieve or any type of resin, i.e., removing one less impurity, resulted in a lower hydrogenation effect than in Example 1. This is because the residual impurities still have a certain toxic effect on the catalyst. Comparative Example 4 did not have an ion exchange resin, and the chelating resin used later was mainly used to treat trace metal ions, which was easily saturated. This means that the removal of conventional metal ions was not thorough, so the degree of hydrogenation was lower than that of Comparative Examples 2, 3, and 5. This indicates that the large number of metal elements in the nitrile rubber solution had the greatest toxic effect on the catalyst, resulting in the lowest degree of hydrogenation.
[0074] The above are all preferred embodiments of this application and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made to the products, methods and principles of this application should be covered within the scope of protection of this application.
Claims
1. A method for hydrogenation pretreatment of nitrile rubber, characterized in that, Includes the following steps: S1. Cut and crush nitrile rubber into pieces, add solvent, heat and stir to dissolve, and obtain nitrile rubber solution; S2. The adsorption resin, ion exchange resin and chelating resin are pre-wetted and displacement activated with solvent to obtain pretreated adsorption resin, ion exchange resin and chelating resin. S3. The nitrile rubber solution obtained in step S1 is passed sequentially through a purification device containing a molecular sieve, the pretreated adsorption resin obtained in step S2, an ion exchange resin, and a chelating resin to obtain a purified nitrile rubber solution. S4. The purified nitrile rubber solution obtained in step S3 is sent to a concentration device and concentrated under high temperature and negative pressure conditions to obtain concentrated nitrile rubber solution. S5. The concentrated nitrile rubber solution obtained in step S4 is allowed to stand and homogenize, then introduced into a hydrogenation reactor, a catalyst is added, and a hydrogenation reaction is carried out.
2. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S3, the molecular sieve is selected from at least one of type 3A molecular sieve, type 4A molecular sieve, and type 5A molecular sieve.
3. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S2, the adsorption resin includes styrene-based adsorption resin and acrylate-based adsorption resin.
4. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S2, the ion exchange resin includes macroporous sulfonic acid cation exchange resin and gel-type sulfonic acid cation exchange resin.
5. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S2, the chelating resin includes aminophosphonic acid chelating resin, thiourea-type chelating resin, and mercapto-type chelating resin.
6. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S1, nitrile rubber includes ordinary nitrile rubber and / or nitrile rubber derivatives.
7. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S1, the solvent includes chlorobenzene, dichloromethane, acetone, tetrahydrofuran, and N-methylpyrrolidone.
8. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S3, the flow rate of the nitrile rubber liquid through the purification device is 1~3 BV / h, and the temperature is 30~60℃.
9. The method for hydrogenation pretreatment of nitrile rubber according to claim 1, characterized in that, In step S4, the concentration temperature of the purified nitrile rubber solution is 60~100℃, the concentration pressure is -70kPa~-90kPa, and the single residence time in the concentration device is 5~20s.