A high-transmittance, low-yellowing, and non-pilling 3D printing resin material, its preparation method and application

By compounding high-transparency polyurethane acrylate with light stabilizers and fluorescent whitening agents into 3D printing resin materials, the problems of over-curing and yellowing that easily occur in high-transparency photocurable resins during the printing process are solved, achieving a printing effect with high transparency, low yellowing and balanced mechanical properties.

CN123106993APending Publication Date: 2026-11-17GUANGZHOU BAHE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611472088.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-transmittance photocurable resins are prone to over-curing and material buildup during the printing process, yellowing after curing, and difficulty in balancing mechanical properties.

Method used

A 3D printing resin material with high light transmittance, low yellowing, and low material accumulation was prepared by compounding difunctional, trifunctional, and hexafunctional aliphatic polyurethane acrylates with high transparency and low yellowing, combined with light stabilizers and fluorescent whitening agents.

Benefits of technology

It increases the crosslinking density of the single-layer curing film, shortens the curing time, improves printing details and edge exposure clarity, enhances the bending and tensile strength of the finished product, reduces overexposure and yellowing, and ensures the finished product is colorless and transparent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106993A_ABST
    Figure CN123106993A_ABST
Patent Text Reader

Abstract

This application provides a high-transmittance, low-yellowing, and non-over-curing 3D printing resin material, its preparation method, and its application, relating to the field of photocurable 3D printing materials technology. In this application, firstly, difunctional polyurethane acrylate, trifunctional polyurethane acrylate, and hexafunctional aliphatic polyurethane acrylate are compounded to form the main resin; secondly, monofunctional and difunctional free radical acrylate monomers are used as reactive diluents; then, a photoinitiator, colorant, and additives including light stabilizers and fluorescent whitening agents are added; finally, the photocurable resin material is formed through stepwise mixing and stirring. Based on the above, this method can improve the problems in the prior art where high-transmittance resins easily cause over-curing and material buildup in densely supported areas during printing, are prone to yellowing after curing, and have difficulty balancing mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photopolymer 3D printing materials technology, and in particular to a 3D printing resin material with high light transmittance, low yellowing, and resistance to material buildup, as well as its preparation method and application. Background Technology

[0002] Photopolymer 3D printing technology, especially the molding processes based on Digital Light Processing (DLP) and StereoLithography Apparatus (SLA), has become one of the most precise and surface-quality technologies in the additive manufacturing field. Among the many photopolymerization systems, free radical photopolymerization dominates the 3D printing photosensitive resin market due to its advantages such as fast reaction speed, mature material systems, and wide process window.

[0003] Existing photosensitive resins used for high-transparency printing typically use polyurethane acrylate resins as the main resin, combined with acrylate reactive diluent monomers and photoinitiators to form a photocuring system. To achieve high light transmittance, these resin systems generally do not introduce pigments, fillers, or other components with light-absorbing or light-blocking effects; the curing light emitted by the printing light source can easily penetrate the liquid resin layer.

[0004] However, precisely because of its high light transmittance, the curing light can penetrate the current cured layer and enter non-target areas during printing, causing over-curing in densely supported areas of the model. This leads to resin buildup at the support points, resulting in a material accumulation problem. When printing thin horizontal pipe structures, the pipes can easily become blocked by over-cured resin. Furthermore, existing high-transmittance resins generally exhibit some degree of yellowing after complete curing, making it difficult to achieve a colorless and transparent state. Moreover, it is difficult to balance the crosslinking density and curing speed of the resin system with the strength and toughness of the cured product, making it challenging to simultaneously meet the requirements for both surface precision and mechanical properties.

[0005] In other words, in the existing technology, there are problems such as high light transmittance photocurable resins being prone to over-curing and material buildup during the printing process, yellowing after curing, and difficulty in balancing mechanical properties. Summary of the Invention

[0006] In view of this, the purpose of this application is to provide a high-transmittance, low-yellowing, and non-over-curing 3D printing resin material, its preparation method, and its application, so as to improve the problems of high-transmittance photocurable resins in the prior art that are prone to over-curing and over-curing during the printing process, easy yellowing after curing, and difficulty in balancing mechanical properties.

[0007] To achieve the above objectives, this application adopts the following technical solution: In a first aspect, this application provides a 3D printing photocurable resin material with high light transmittance, low yellowing, and minimal material buildup, comprising the following components by weight: 10-30 parts of difunctional polyurethane acrylate, 10-30 parts of trifunctional polyurethane acrylate, 5-10 parts of hexafunctional aliphatic polyurethane acrylate, 30-50 parts of monofunctional free radical acrylate monomer, 20-50 parts of difunctional free radical acrylate monomer, 1-10 parts of photoinitiator, 0.01-1 parts of colorant, and 0.01-1 parts of additives, wherein the additives include light stabilizers and fluorescent whitening agents.

[0008] In a preferred embodiment of this application, the difunctional polyurethane acrylate in the aforementioned 3D printing photocurable resin material is a difunctional polyurethane acrylate resin with high transparency, low yellowing, and good toughness, and the difunctional polyurethane acrylate includes one or more of Bahe BWL 8404A, Bahe BWL 426D, Bahe BWL 423, and Bahe BWL 435.

[0009] In a preferred embodiment of this application, the trifunctional polyurethane acrylate in the aforementioned 3D printing photocurable resin material is a trifunctional tough polyurethane acrylate resin with high surface hardness and high light transmittance, and the trifunctional polyurethane acrylate includes one or more of Bahe BWL 475, Bahe BW 8006, Bahe BW 8008 and Bahe BWL 471.

[0010] In a preferred embodiment of this application, the hexafunctional aliphatic polyurethane acrylate in the aforementioned 3D printing photocurable resin material is a hexafunctional aliphatic polyurethane acrylate resin with low yellowing after curing and a flexural strength of 90 MPa. The hexafunctional aliphatic polyurethane acrylate includes one or more of Bahe BW 8291, Bahe BW L8044, Bahe BWL8400, and Bahe BW L8298.

[0011] In a preferred embodiment of this application, in the aforementioned 3D printing photocurable resin material, the monofunctional radical acrylate monomer includes one or more of acrylmorpholine, hydroxyethyl methacrylate, isobornyl acrylate, and cyclotrimethylolpropane methyl acetal acrylate; the difunctional radical acrylate monomer includes one or more of 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and bisphenol A diacrylate ethoxylate.

[0012] In a preferred embodiment of this application, the photoinitiator in the aforementioned 3D printing photocurable resin material comprises one or more of (2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone.

[0013] In a preferred embodiment of this application, the light stabilizer in the aforementioned 3D printing photocurable resin material includes one or more of Tinuvin 400, BW A21, and Tinuvin 479; the fluorescent whitening agent includes one or more of Tinopal NFWLIQ, Tinopal OB CO, and Tinopal SFP; and the colorant includes one or more of BWA42-20 colorant and ULOMBU1154 colorant.

[0014] Secondly, this application also provides a method for preparing the above-mentioned 3D printing photocurable resin material, comprising: mixing an amount of additive, photoinitiator, monofunctional free radical acrylate monomer and difunctional free radical acrylate monomer, and performing a first stirring to form a monomer composition; mixing an amount of difunctional polyurethane acrylate, trifunctional polyurethane acrylate and hexafunctional aliphatic polyurethane acrylate with the monomer composition, and performing a second stirring with heating to form the 3D printing photocurable resin material.

[0015] In a preferred embodiment of this application, in the above preparation method, the stirring time of the first stirring is 30-60 min, the stirring speed of the first stirring is 600-700 rpm; the stirring time of the second stirring is 30-60 min, the stirring speed of the second stirring is 500-700 rpm, and the stirring temperature of the second stirring is 80-90℃.

[0016] Thirdly, this application also provides an application of the above-mentioned 3D printing photocurable resin material in digital light processing 3D printing or ultraviolet mask curing 3D printing.

[0017] Beneficial effects: This application provides a high-transmittance, low-yellowing, and non-accumulating 3D printing resin material, its preparation method, and its application. First, by introducing a trifunctional polyurethane acrylate into a difunctional polyurethane acrylate system for compounding, the crosslinking density of the monolayer cured film is increased and the curing time is shortened. Second, the introduction of a hexafunctional aliphatic polyurethane acrylate with low yellowing and high flexural strength after curing improves the problem of unclear printing details and edge exposure, and enhances the flexural and tensile strength of the cured product, resulting in clearer surface texture. Third, the introduction of a light stabilizer increases the resin's critical exposure energy and reduces the exposure depth, suppressing overexposure caused by the resin's high transmittance and the penetration of curing light into non-target areas. Fourth, the introduction of a fluorescent whitening agent absorbs ultraviolet light penetrating into the resin liquid and converts it into fluorescence, thereby reducing the accumulation problem in densely packed printing supports. Finally, the use of a colorant to neutralize the resin's yellowing results in a colorless and transparent finished product after complete curing.

[0018] Based on the above, the synergistic blending of trifunctional and hexafunctional aliphatic polyurethane acrylates in a conventional difunctional formulation system allows the resin system to maintain high light transmittance while balancing crosslinking density, curing speed, and strength and toughness. This improves the surface accuracy and mechanical properties of the printed parts. Simultaneously, the light stabilizer and fluorescent whitening agent work together to suppress over-curing in non-target areas by increasing the critical exposure energy and absorbing transmitted ultraviolet light, respectively. This reduces the resin's exposure depth and material buildup, resulting in clear and complete molding effects in densely supported areas and fine tubular structures. Furthermore, the neutralizing effect of the pigment on resin yellowing further ensures the colorless and transparent appearance of the cured product, thus improving the problems of over-curing and material buildup, yellowing after curing, and difficulty in balancing mechanical properties associated with high-transmittance UV-curable resins in existing technologies.

[0019] Furthermore, based on the performance test results described in the embodiments of this application, the resin material of Example 1, using the complete formulation, has an exposure depth Dp of 0.216, a critical exposure energy Ec of 10.74, an elongation at break of 15.6%, a flexural strength of 48 MPa, a Shore hardness of 83D, an impact strength of 49 J / m, a yellowing value Δb of 1.5, and no material buildup at the printing support. In contrast, Comparative Examples 1 to 5, which use only a single type of polyurethane acrylate as the main resin, all exhibited material buildup at the support and struggled to simultaneously achieve strength, toughness, and low yellowing. Comparing Examples 4 and 5, it can be seen that the critical exposure energy Ec of the resin increased from 7.17 to 11.03 after adding the light stabilizer, and the material buildup phenomenon was significantly reduced. Comparing Examples 5 and 2, it can be seen that the exposure depth Dp of the resin decreased from 0.3513 to 0.194 after adding the fluorescent whitening agent, and the light penetration in the material was significantly reduced. Comparing Examples 3 and 5, it can be seen that the Dp and Ec of the resin did not change significantly after adding the color paste, but the yellowing value Δb after curing decreased from 9.3 to 5.5. The above data show that the combination of the main resin compound system, light stabilizer, fluorescent whitening agent and color paste in this application produces a synergistic technical effect in suppressing material buildup, reducing yellowing and balancing mechanical properties. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in this invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.

[0021] Figure 1 This is an enlarged view of the 3D printed sample of the photocurable resin material in Embodiment 1 of this application, showing no material buildup at densely supported areas. Figure 2 An enlarged view showing material buildup in densely supported areas on the printed sample for comparison; Figure 3 This is a comparison diagram of the yellowing test samples of the embodiments and comparative examples of this application. Detailed Implementation

[0022] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. It should also be noted that, to make the embodiments more comprehensive, the following embodiments are the best and preferred embodiments, and those skilled in the art can use other alternative methods to implement some well-known technologies; moreover, the accompanying drawings are only for more specific description of the embodiments and are not intended to specifically limit the present invention.

[0023] This application provides a resin formulation for a photocurable resin material for 3D printing. The key feature is the combination of difunctional polyurethane acrylate, trifunctional polyurethane acrylate, and hexafunctional aliphatic polyurethane acrylate with an active diluent, so that the material has both high transparency and low yellowing properties, and is not prone to material buildup during the printing process, thereby meeting the application requirements of high-transparency resins for 3D printing.

[0024] In the embodiments of this application, the difunctional polyurethane acrylate is a polyurethane acrylate material with high transparency, low yellowing, and good toughness. For example, BWL 8404A, BWL 426D, BWL 423, BWL435, etc. from Bahe can be selected. The difunctional polyurethane acrylate serves as the base resin of the formulation system, providing basic transparency and flexibility to the cured film.

[0025] In this embodiment, the trifunctional polyurethane acrylate is a trifunctional tough polyurethane acrylate with high surface hardness and high light transmittance. Exemplarily, BWL 475, BW 8006, BW 8008, and BWL471 from Bahe can be selected. By replacing a conventional difunctional formulation system with a large amount of trifunctional polyurethane acrylate resin, the crosslinking density of the single-layer cured film can be increased and the curing time shortened, thereby achieving higher hardness and precision on the surface of the printed parts.

[0026] In this embodiment, the hexafunctional aliphatic polyurethane acrylate is a high-strength, low-yellowing hexafunctional aliphatic polyurethane acrylate with low yellowing after curing and a flexural strength of 90 MPa. Exemplary examples include BW 8291, BW L8044, BW L8400, and BW L8298 from Bahe. The addition of a low-yellowing hexafunctional resin can improve printing details and address issues of unclear edge exposure, while also increasing the overall flexural and tensile strength of the cured product. Furthermore, due to the high overall functionality of the resin system, the surface texture of the printed product is very clear.

[0027] In the embodiments of this application, the monofunctional radical acrylate monomer is one or more selected from acrylmorpholine, hydroxyethyl methacrylate, isobornyl acrylate, and cyclotrimethylolpropane methyl acetal acrylate. The monofunctional radical acrylate monomer acts as a reactive diluent to adjust the viscosity of the resin system and participates in the free radical polymerization reaction under light irradiation.

[0028] In the embodiments of this application, the difunctional radical acrylate monomer is one or more selected from 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and bisphenol A diacrylate ethoxylate. The difunctional radical acrylate monomer can improve the degree of crosslinking of the cured film while diluting the resin system, thereby balancing flowability and cured strength.

[0029] In the embodiments of this application, the photoinitiator is one or more of (2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone. Exemplarily, (2,4,6-trimethylbenzoyl)phenylphosphine oxide is designated as TPO, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide is designated as 819.

[0030] In the embodiments of this application, the additives include light stabilizers and optical brighteners. It should be noted that the auxiliary components in the formulation of this application include light stabilizers, color pastes, and optical brighteners, with the color paste listed as a separately measured component. For example, light stabilizers can be Tinuvin 400, BW A21, Tinuvin 479, etc.; optical brighteners can be Tinopal NFW LIQ, Tinopal OB CO, Tinopal SFP, etc.; and color pastes can be BWA42-20, ULOMBU1154, etc. Introducing a light stabilizer into the formulation can increase the critical exposure energy of the cured resin and reduce the exposure depth, thereby reducing overexposure caused by the resin's high transparency and the penetration of curing light into other areas. Adding an optical brightener can absorb ultraviolet light penetrating into the resin liquid and convert it into fluorescence, thereby reducing material buildup problems in densely printed support areas. Adding color paste can neutralize the yellowing of the resin itself, thereby ensuring that the finished product is colorless and transparent after complete curing.

[0031] This application also provides a method for preparing the above-mentioned 3D printing photocurable resin material. The specific process of this preparation method is described in detail below.

[0032] S1, the formulation amounts of additives, photoinitiator, monofunctional free radical acrylate monomers and difunctional free radical acrylate monomers are mixed and stirred for the first time to form a monomer composition.

[0033] In this embodiment, the formulated amounts of additives and photoinitiators are first mixed with monofunctional and difunctional free radical acrylate monomers. The monomers dissolve and disperse the additives and photoinitiators to form a homogeneous monomer composition. Exemplarily, the first stirring time is 30-60 minutes, and the stirring speed is 600-700 rpm, until all components are completely dissolved and uniformly dispersed. It should be noted that dispersing the additives and photoinitiators in the monomers before adding the main resin avoids uneven dispersion of the additives in the high-viscosity resin, thereby ensuring the consistency of curing behavior throughout the resin system.

[0034] S2, the formulated amounts of difunctional polyurethane acrylate, trifunctional polyurethane acrylate and hexafunctional aliphatic polyurethane acrylate are mixed with the monomer composition and heated and stirred a second time to form the 3D printing photocurable resin material.

[0035] In this embodiment, the stirring time of the second stirring is 30-60 minutes, the rotation speed is 500-700 rpm, and the stirring temperature is 80-90℃. Heating and stirring reduce the viscosity of the polyurethane acrylate resin, ensuring that the three main resins and monomer composition are thoroughly and uniformly mixed until completely and uniformly dispersed, thus obtaining the 3D printing photocurable resin material.

[0036] It should be noted that, in order to facilitate a direct comparison of the effects of each additive on the printing effect, the ratio of the main resin to the monomer in the following examples and comparative examples remains fixed, and only the type and amount of additives are adjusted. Therefore, the sum of the proportions of each component is not 100 parts. If you need to convert to a total of 100 parts, you can calculate it according to the relative proportions of each component.

[0037] Example 1 The formulation of Example 1, by weight, is as follows: 15 parts of difunctional polyurethane acrylate with brand name BWL 426D, 20 parts of trifunctional polyurethane acrylate with brand name BWL 475, 5 parts of hexafunctional aliphatic polyurethane acrylate with brand name BWL8298, 20 parts of acrylamide morpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BWA21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of color paste BWA42-20.

[0038] The preparation process is as follows: the photoinitiator and additives are mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 r / min for 30 min until completely dissolved to obtain a monomer composition; BWL 426D, BWL 475 and BW L8298 are added to the uniformly mixed monomer composition above, and dispersed at 600 r / min for 30 min at 80°C until completely uniformly dispersed to obtain the 3D printing resin of Example 1.

[0039] Example 2 The formulation of Example 2, by weight, is as follows: 15 parts of a difunctional polyurethane acrylate with brand name BWL 426D, 20 parts of a trifunctional polyurethane acrylate with brand name BWL 475, 5 parts of a hexafunctional aliphatic polyurethane acrylate with brand name BWL8298, 20 parts of acrylamide morpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, and 0.04 parts of fluorescent whitening agent Tinopal OB CO.

[0040] The preparation process is as follows: the photoinitiator and fluorescent whitening agent are mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 r / min for 30 min until completely dissolved to obtain a monomer composition; BWL 426D, BWL 475 and BW L8298 are added to the uniformly mixed monomer composition above, and dispersed at 600 r / min for 30 min at 80°C until completely uniformly dispersed to obtain the 3D printing resin of Example 2.

[0041] Example 3 By weight, the formulation of Example 3 is as follows: 15 parts of difunctional polyurethane acrylate with brand name BWL 426D, 20 parts of trifunctional polyurethane acrylate with brand name BWL 475, 5 parts of hexafunctional aliphatic polyurethane acrylate with brand name BWL8298, 20 parts of acrylamide morpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, and 0.3 parts of color paste BWA42-20.

[0042] The preparation process is as follows: the photoinitiator and pigment are mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 r / min for 30 min until completely dissolved to obtain a monomer composition; BWL 426D, BWL 475 and BW L8298 are added to the uniformly mixed monomer composition above, and dispersed at 600 r / min for 30 min at 80°C until completely uniformly dispersed to obtain the 3D printing resin of Example 3.

[0043] Example 4 By weight, the formulation of Example 4 is as follows: 15 parts of difunctional polyurethane acrylate with brand name BWL 426D, 20 parts of trifunctional polyurethane acrylate with brand name BWL 475, 5 parts of hexafunctional aliphatic polyurethane acrylate with brand name BWL8298, 20 parts of acrylamide morpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, and 0.2 parts of light stabilizer BWA21.

[0044] The preparation process is as follows: the photoinitiator and light stabilizer are mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 r / min for 30 min until completely dissolved to obtain a monomer composition; BWL 426D, BWL 475 and BW L8298 are added to the uniformly mixed monomer composition above, and dispersed at 600 r / min for 30 min at 80°C until completely uniformly dispersed to obtain the 3D printing resin of Example 4.

[0045] Example 5 By weight, the formulation of Example 5 is as follows: 15 parts of difunctional polyurethane acrylate with brand name BWL 426D, 20 parts of trifunctional polyurethane acrylate with brand name BWL 475, 5 parts of hexafunctional aliphatic polyurethane acrylate with brand name BWL8298, 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, and 2 parts of photoinitiator TPO.

[0046] The preparation process is as follows: A photoinitiator is mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 rpm for 30 minutes until completely dissolved to obtain a monomer composition. BWL426D, BWL 475, and BWL8298 are added to the uniformly mixed monomer composition, and dispersion continues at 80°C and 600 rpm for 30 minutes until completely uniform, thus obtaining the 3D printing resin of Example 5. It should be noted that Example 5 does not contain light stabilizers, fluorescent whitening agents, or color pastes, serving as a control example to examine the effects of each additive.

[0047] Comparative Example To illustrate the role of each component in the resin system of this application, the following comparative examples are also provided in the embodiments of this application.

[0048] Comparative Example 1: By weight, the formulation of Comparative Example 1 is as follows: 40 parts of difunctional polyurethane acrylate (brand name BWL 426D), 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BWA21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of colorant BWA42-20. The preparation process is as follows: The photoinitiator and additives are mixed with acryloylmorpholine, dipropylene glycol diacrylate, and cyclotrimethylolpropane methyl acetal acrylate, and dispersed at 600 rpm for 30 minutes until completely dissolved; BWL 426D is added to the uniformly mixed liquid, and dispersion continues at 80°C and 600 rpm for 30 minutes until completely uniform, thus obtaining the 3D printing resin of Comparative Example 1.

[0049] Comparative Example 2: By weight, the formulation of Comparative Example 2 was as follows: 40 parts of a difunctional polyurethane acrylate (brand name BWL 8404A), 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BWA21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of color paste BWA42-20. The preparation process was the same as that of Comparative Example 1, except that the main resin was replaced with BWL 8404A.

[0050] Comparative Example 3: By weight, the formulation of Comparative Example 3 was as follows: 40 parts of trifunctional polyurethane acrylate (brand name BW 8008), 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BW A21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of color paste BWA42-20. The preparation process was the same as that of Comparative Example 1, except that the main resin was replaced with BW 8008.

[0051] Comparative Example 4: By weight, the formulation of Comparative Example 4 was as follows: 40 parts of hexafunctional aliphatic polyurethane acrylate (brand name BW L8298), 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BW A21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of color paste BWA42-20. The preparation process was the same as that of Comparative Example 1, except that the main resin was replaced with BW L8298.

[0052] Comparative Example 5: By weight, the formulation of Comparative Example 5 was as follows: 40 parts of trifunctional polyurethane acrylate (brand name BWL 475), 20 parts of acryloylmorpholine, 20 parts of dipropylene glycol diacrylate, 20 parts of cyclotrimethylolpropane methyl acetal acrylate, 2 parts of photoinitiator TPO, 0.2 parts of light stabilizer BWA21, 0.04 parts of fluorescent whitening agent Tinopal OB CO, and 0.3 parts of color paste BWA42-20. The preparation process was the same as that of Comparative Example 1, except that the main resin was replaced with BWL 475.

[0053] Performance Testing and Results Analysis The resin materials prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were subjected to printing tests and performance tests. Tensile properties were tested according to GB / T1040.1-2018 "Determination of Tensile Properties of Plastics", with elongation at break expressed as %, and tensile strength expressed as MPa. Flexural strength was determined according to GB / T1449-2005 "Test Method for Flexural Properties of Fiber Reinforced Plastics", with flexural strength expressed as MPa. Hardness was tested according to GB / T2411-2018 "Determination of Indentation Hardness of Plastics and Hard Rubber Using a Hardness Tester", with the hardness unit determined based on the hardness tester used; in this application, Shore hardness D was used.

[0054] The printing test used a Jianchuang S10 3D printer with a light intensity of 6000 μW / cm². The printing process parameters were: single-layer slice thickness 0.05 mm, single-layer penetration depth 0.1 mm, bottom layer exposure time 12 s, number of bottom layer exposures 3, number of transition layer exposures 5, linear transition method, static time 0 s, lift distance 5 mm, lift speed 200 mm / min, return distance 5 mm, and return speed 200 mm / min.

[0055] It should be noted that, in the embodiments of this application, the exposure depth Dp and the critical exposure energy Ec can be determined using the photocuring working curve method commonly used in the art, that is, by measuring the thickness of the cured layer at different exposure energies and fitting it according to the following working curve equation: Cd = Dp·ln(E / Ec) Where Cd represents the thickness of the cured layer, Dp represents the depth of exposure, E represents the exposure energy incident on the resin liquid surface, Ec represents the critical exposure energy, and ln represents the natural logarithm.

[0056] The performance test results of each embodiment and comparative example are shown in the table below.

[0057] The following conclusions can be drawn from the table above. First, the formulation uses a blend of difunctional, trifunctional, and hexafunctional aliphatic polyurethane acrylates, resulting in a reasonable balance between the strength and toughness of the finished product, meeting most application requirements. Furthermore, the addition of trifunctional and hexafunctional aliphatic polyurethane acrylates improves the surface finish of the material. Second, comparing Examples 4 and 5, it was found that adding the light stabilizer BWA21 to the formulation significantly increased the Ec value of the material and significantly reduced the material buildup phenomenon. This indicates that the buildup of high-transmittance resins is affected to some extent by the material's Ec value. Third, comparing Examples 5 and 2, it was found that adding the fluorescent whitening agent Tinopal OBCO to the formulation significantly reduced the exposure depth Dp value of the material, indicating a significant decrease in light penetration within the material, and also improving the buildup phenomenon. Fourth, comparing Examples 3 and 5, it was found that adding the colorant BWA42-20 to the formulation did not significantly change the overall Dp and Ec values ​​of the material, nor did it improve the buildup effect, but it significantly reduced yellowing after curing.

[0058] Combination Figure 1 and Figure 2 , Figure 1 This is an enlarged view of a sample printed using the resin material of Example 1 at a densely supported area. Figure 1As can be seen, the sample surface is flat, and no resin over-curing and accumulation occurred after the support was removed, meaning there was no material buildup. Figure 2 To compare with the enlarged view of the printed sample at the densely supported area, from Figure 2 As can be seen, multiple annular resin over-curing build-up protrusions are visible on the surface of the densely supported areas of the control sample, indicating obvious material accumulation. Figure 1 and Figure 2 The comparison clearly shows that the resin material in this application embodiment can effectively improve the problem of material accumulation in densely printed support areas.

[0059] Combination Figure 3 , Figure 3 This is a comparison image of the yellowing test samples. The top row, from left to right, shows the cured samples of Examples 1 to 5, and the bottom row, from left to right, shows the cured samples of Comparative Examples 1 to 5. Figure 3 As can be seen, the sample from Example 1 is generally colorless and transparent, while the sample from Example 5, which did not contain any colorant or light stabilizer, is noticeably yellowish. Some of the comparative sample samples also show varying degrees of yellowing. Figure 3 The appearance of the sample shown corroborates the test results of the yellowing value Δb in the table above.

[0060] Based on the above conclusions, the optimal combination of this application is Example 1, with a Dp / Ec value of 0.216 / 10.74, an elongation at break of 15.6%, a flexural strength of 48 MPa, a Shore hardness of 83D, an impact strength of 49 J / m, low yellowing, and no material accumulation during printing.

[0061] Application Examples In this embodiment, the aforementioned 3D printing photocurable resin material is suitable for digital light processing 3D printing or ultraviolet mask curing 3D printing processes, and is particularly suitable for desktop printing equipment. For example, by adding the resin material prepared in the above embodiment into the feed tank of a DLP or LCD 3D printing equipment, and printing according to the conventional slice thickness and single-layer exposure parameters of the printing equipment, a printed product with high transparency, low yellowing, and no material buildup in densely supported areas can be obtained. The surface texture of the finished product is clear, and the fine horizontal pipe structure is not easily blocked by over-cured resin.

[0062] This invention encompasses any substitutions, modifications, equivalent methods, and solutions made within the spirit and scope of this invention. To provide the public with a thorough understanding of this invention, specific details are described in detail in the following preferred embodiments; however, those skilled in the art will fully understand the invention even without these details. Furthermore, to avoid unnecessary misunderstanding of the essence of this invention, well-known methods, processes, procedures, components, and circuits are not described in detail.

[0063] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A 3D printing photocurable resin material with high light transmittance, low yellowing, and minimal material buildup, characterized in that, The product comprises, by weight, the following components: 10-30 parts of difunctional polyurethane acrylate, 10-30 parts of trifunctional polyurethane acrylate, 5-10 parts of hexafunctional aliphatic polyurethane acrylate, 30-50 parts of monofunctional free radical acrylate monomer, 20-50 parts of difunctional free radical acrylate monomer, 1-10 parts of photoinitiator, 0.01-1 parts of color paste, and 0.01-1 parts of additives, wherein the additives include light stabilizers and fluorescent whitening agents.

2. The 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup as described in claim 1, characterized in that, The difunctional polyurethane acrylate is a difunctional polyurethane acrylate resin with high transparency, low yellowing and good toughness. The difunctional polyurethane acrylate includes one or more of Bahe BWL 8404A, Bahe BWL 426D, Bahe BWL423 and Bahe BWL 435.

3. The 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup as described in claim 1, characterized in that, The trifunctional polyurethane acrylate is a trifunctional tough polyurethane acrylate resin with high surface hardness and high light transmittance, and the trifunctional polyurethane acrylate includes one or more of Bahe BWL 475, Bahe BW 8006, Bahe BW8008 and Bahe BWL 471.

4. The 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup as described in claim 1, characterized in that, The hexafunctional aliphatic polyurethane acrylate is a hexafunctional aliphatic polyurethane acrylate resin with low yellowing after curing and a flexural strength of up to 90 MPa. The hexafunctional aliphatic polyurethane acrylate includes one or more of Bahe BW8291, Bahe BW L8044, Bahe BW L8400 and Bahe BW L8298.

5. The 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup as described in claim 1, characterized in that, The monofunctional radical acrylate monomers include one or more of acrylmorpholine, hydroxyethyl methacrylate, isobornyl acrylate, and cyclotrimethylolpropane methyl acetal acrylate; the difunctional radical acrylate monomers include one or more of 1,6-hexanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and bisphenol A diacrylate ethoxylate.

6. The 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup as described in claim 1, characterized in that, The photoinitiator includes one or more of (2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 1-hydroxycyclohexylphenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone.

7. A 3D printing photocurable resin material with high light transmittance, low yellowing, and resistance to material buildup, as described in any one of claims 1 to 6, characterized in that... The light stabilizer includes one or more of Tinuvin 400, BW A21, and Tinuvin 479; the fluorescent whitening agent includes one or more of Tinopal NFW LIQ, Tinopal OB CO, and Tinopal SFP; and the color paste includes one or more of BWA42-20 and ULOM BU1154.

8. A method for preparing a 3D printing photocurable resin material with high light transmittance, low yellowing, and minimal material buildup, characterized in that, include: The additives, photoinitiator, monofunctional free radical acrylate monomers and difunctional free radical acrylate monomers in the formulation amount are mixed and stirred for the first time to form a monomer composition; The formulation amounts of difunctional polyurethane acrylate, trifunctional polyurethane acrylate, and hexafunctional aliphatic polyurethane acrylate are mixed with the monomer composition and subjected to a second stirring under heating to form the 3D printing photocurable resin material.

9. The preparation method according to claim 8, characterized in that, The stirring time of the first stirrer is 30-60 minutes, and the stirring speed of the first stirrer is 600-700 rpm; the stirring time of the second stirrer is 30-60 minutes, the stirring speed of the second stirrer is 500-700 rpm, and the stirring temperature of the second stirrer is 80-90℃.