A weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin and its preparation method

By copolymerizing composite epoxy resin with functional monomers and using a ketone-hydrazine crosslinking system, a weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin was prepared, which solved the problems of weather resistance, storage stability and adhesion of coatings, and achieved a high-performance coating protection effect.

CN123107002APending Publication Date: 2026-11-17GUANGDONG TUOPU SYNTHETIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611151336.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing waterborne acrylic resin coatings suffer from defects such as low film-forming crosslinking degree, poor water resistance, insufficient hardness, and easy re-adhesion at high temperatures. Furthermore, traditional additives are prone to migration and volatilization, failing to provide long-term weather protection. Self-crosslinking technology presents a contradiction between storage stability and film-forming crosslinking properties.

Method used

A weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin was prepared by copolymerizing a composite epoxy resin (alicyclic and bisphenol F epoxy resin), a functional monomer (7-(cinnamoxy)-4-methylcoumarin), and methacryloyloxy POSS, combined with a ketone-hydrazine crosslinking system of diacetone acrylamide and adipic acid dihydrazide, through a pre-emulsification-semi-continuous seed emulsion polymerization process, avoiding the use of organic solvents.

Benefits of technology

It achieves low yellowing, high gloss retention, strong adhesion and high hardness of the coating under ultraviolet irradiation and high temperature environment, and has long-term weather resistance and storage stability, meeting environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of coatings, specifically to a weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin and its preparation method. The epoxy-modified acrylic resin comprises the following components: 20-30 parts of composite epoxy resin, 35-45 parts of acrylic mixed monomers, 2-5 parts of functional monomers, 1-3 parts of methacryloyloxy (POSS), 4.3-10.5 parts of crosslinking agent, 1.5-2.5 parts of water-soluble initiator, 2-4 parts of neutralizing agent, 1-3 parts of reactive emulsifier, and 50-65 parts of deionized water. This invention utilizes free radical copolymerization to chemically bond the functional monomer 7-(cinnamoxy)-4-methylcoumarin to the resin backbone. Compared to conventional additive UV absorbers, the polymeric functional monomer reduces migration, volatilization, and extraction losses at the source, resulting in long-lasting weather protection. Even under prolonged outdoor exposure and immersion conditions, it effectively delays coating chalking, gloss loss, and cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coatings, specifically to a weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin and its preparation method. Background Technology

[0002] With increasingly stringent global environmental regulations, low-VOC and zero-VOC waterborne coatings are gradually replacing solvent-based coatings and becoming the mainstream of industry development. Waterborne acrylic resins are one of the most widely used film-forming substances in waterborne coatings due to their light color, good gloss and color retention, and mature synthesis process. However, pure linear acrylic resins have defects such as low film crosslinking degree, poor water resistance, insufficient hardness, and easy re-tack at high temperatures, making it difficult to meet the needs of high-performance protective scenarios.

[0003] Epoxy-modified acrylic resin combines the high adhesion and excellent corrosion resistance of epoxy resin with the weather resistance and decorative properties of acrylic resin, representing an important technical approach to improve the overall performance of waterborne coatings. In existing technologies, epoxy-modified waterborne acrylic resins often use bisphenol A type epoxy resin as the modification skeleton. While this can improve coating adhesion and chemical resistance, the bisphenol A structure contains a large number of benzene ring conjugated systems, which are prone to photo-oxidative degradation under long-term ultraviolet irradiation, leading to yellowing, loss of gloss, and chalking of the coating, and its weather resistance cannot meet the requirements for long-term outdoor use. While using alicyclic epoxy resin alone for modification improves weather resistance, it results in insufficient adhesion to the substrate, low crosslinking density, and limited protective performance.

[0004] To improve the weather resistance of waterborne acrylic coatings, the conventional approach is to add small-molecule UV absorbers, light stabilizers, and other additives to the system. However, these additives are prone to migration, volatilization, and water extraction during long-term use of the coating, resulting in a continuous decline in weather resistance and an inability to provide long-term protection. Some additives may even degrade the coating's water resistance and adhesion.

[0005] Regarding self-crosslinking technology, existing systems generally suffer from a contradiction between storage stability and film-forming crosslinking: some crosslinking monomers can react during the emulsion storage stage, leading to gelation and delamination of the system; some crosslinking systems require high-temperature baking to trigger crosslinking, making room-temperature film-forming self-crosslinking impossible, increasing construction energy consumption and limitations. In addition, traditional emulsion polymerization uses small-molecule emulsifiers, which migrate to the coating surface after film formation, deteriorating the coating's adhesion, water resistance, and density; some processes still require the addition of organic solvents for dissolution, which does not meet environmental protection requirements.

[0006] Therefore, developing a solvent-free waterborne epoxy-modified acrylic resin that combines excellent weather resistance, room temperature self-crosslinking properties, good storage stability, good adhesion, and good chemical resistance is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0007] To address the problems existing in the prior art, the purpose of this invention is to provide a weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin and its preparation method.

[0008] The objective of this invention is achieved through the following technical solution: In a first aspect, the present invention provides a weather-resistant, self-crosslinking, waterborne epoxy-modified acrylic resin, comprising the following components by weight: The composition includes 20-30 parts of composite epoxy resin, 35-45 parts of acrylic mixed monomers, 2-5 parts of functional monomers, 1-3 parts of methacryloyloxy POSS, 4.3-10.5 parts of crosslinking agent, 1.5-2.5 parts of water-soluble initiator, 2-4 parts of neutralizing agent, 1-3 parts of reactive emulsifier, and 50-65 parts of deionized water.

[0009] Preferably, the composite epoxy resin is prepared by compounding alicyclic epoxy resin and low molecular weight bisphenol F epoxy resin in a mass ratio of 1:1.5~2.5.

[0010] Preferably, the alicyclic epoxy resin is at least one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate and diglycidyl hexahydrophthalic acid, with an epoxy equivalent of 120~180 g / eq.

[0011] Preferably, the acrylic acid mixed monomer is composed of hard monomers, soft monomers, and carboxyl functional monomers in a mass ratio of 12~18:15~20:5~8.

[0012] Preferably, the hard monomer is at least one of cyclohexyl methacrylate, styrene, and tert-butyl acrylate; the soft monomer is at least one of isooctyl acrylate and lauryl acrylate; and the carboxyl functional monomer is at least one of acrylic acid and itaconic acid.

[0013] Preferably, the functional monomer is 7-(cinnamoyloxy)-4-methylcoumarin.

[0014] Preferably, the method for preparing the functional monomer includes: Under nitrogen protection, 7-hydroxy-4-methylcoumarin and triethylamine were added to anhydrous dichloromethane. The mixture was stirred in an ice bath under nitrogen protection, and a dichloromethane solution of cinnamyl chloride was slowly added dropwise. After the addition was complete, the temperature was raised to room temperature and the reaction was carried out for 8-12 hours. After the reaction was completed, the reaction solution was poured into 5-10 times its volume of ice water under vigorous stirring. The pH was adjusted to 2-3 with dilute hydrochloric acid, and a solid product was precipitated. The product was then filtered, washed with a large amount of deionized water until neutral, and the crude product was purified by recrystallization from a 50% aqueous ethanol solution and dried under vacuum to obtain 7-(cinnamyloxy)-4-methylcoumarin.

[0015] Preferably, the mass ratio of 7-hydroxy-4-methylcoumarin, cinnamyl chloride and triethylamine is 1:1.05~1.25:0.70~0.90.

[0016] More preferably, the mass ratio of 7-hydroxy-4-methylcoumarin, cinnamyl chloride and triethylamine is 1:1.14:0.86.

[0017] Preferably, methacryloyloxyPOSS is a methacryloyloxypropyl cage-type silsesquioxane. Preferably, the crosslinking agent is composed of diacetone acrylamide and adipate dihydrazide in a mass ratio of 3~5:1~2.

[0018] Preferably, the water-soluble initiator is at least one of azobisisobutyramidine hydrochloride and ammonium persulfate; Preferably, the neutralizing agent is at least one of N,N-dimethylethanolamine and triethylamine; Preferably, the reactive emulsifier is at least one of sodium allyl hydroxypropyl sulfonate and sodium alkylphenol ether sulfosuccinate.

[0019] Secondly, the present invention provides a method for preparing a weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin, comprising the following steps: Step 1: Preparation of the oil phase mixture: The composite epoxy resin is added to the acrylic mixed monomers according to the formula, and stirred and dissolved at 50~60℃ to obtain an epoxy resin-monomer solution; after cooling to below 30℃, the functional monomer, methacryloyloxy POSS and diacetone acrylamide are added to the epoxy resin-monomer solution and stirred until completely dissolved to obtain an oil phase mixture. Step 2: Preparation of the aqueous phase mixture: Dissolve the reactive emulsifier in 60% to 80% of the formulation amount of deionized water, stir until homogeneous, add 40% to 60% of the formulation amount of water-soluble initiator, stir until dissolved, and obtain an aqueous phase mixture. Step 3: Pre-emulsification and seed initiation: The aqueous phase mixture is heated to 75-82°C. 5%-10% of the oil phase mixture obtained in step 1 is added to the reaction vessel under stirring. After the system shows a blue phase and the temperature stabilizes, it is kept at this temperature for 10-15 minutes to obtain the seed emulsion. Step 4: Monomer addition and polymerization: The remaining oil phase mixture was added dropwise to the seed emulsion at a uniform rate over 3-4 hours, maintaining the system temperature at 78-84℃ during the addition. Simultaneously, a mixed solution of the remaining water-soluble initiator and remaining deionized water was added dropwise, with the addition time extended by 30-60 minutes compared to monomer addition. Step 5: Post-elimination and cooling: After the addition is complete, heat to 85-88℃ and maintain the temperature for 1-1.5 hours. Then cool to 60-65℃, add the neutralizing agent, and stir for 15-30 minutes. Step 6: Adding and discharging the crosslinking agent: Cool the temperature to below 40℃, slowly add adipic acid dihydrazide to the reactor while stirring, continue stirring for 20-30 minutes, filter and discharge to obtain weather-resistant self-crosslinking waterborne epoxy modified acrylic resin.

[0020] The beneficial effects of this invention are as follows: 1. This invention uses a combination of alicyclic epoxy resin and bisphenol F epoxy resin as a grafting skeleton. The alicyclic epoxy resin, with its saturated alicyclic structure as the main component and lacking a benzene ring conjugated system, is intrinsically inert to ultraviolet light, fundamentally inhibiting photo-oxidative yellowing and endowing the resin with excellent weather resistance. The bisphenol F epoxy resin, rich in epoxy groups and aromatic ether bonds, provides strong adhesion to metal substrates and a high crosslinking density. The synergistic effect of these two components allows the coating to maintain low yellowing and high gloss retention under aging environments such as ultraviolet irradiation and temperature alternation, while also maintaining high-strength adhesion and protective performance, overcoming the shortcomings of traditional single epoxy resins that struggle to simultaneously achieve both weather resistance and adhesion.

[0021] 2. This invention utilizes free radical copolymerization to chemically bond the functional monomer 7-(cinnamoyloxy)-4-methylcoumarin to the resin backbone. This monomer simultaneously contains a coumarin ring and a cinnamic ester structure, exhibiting strong absorption capabilities in the ultraviolet band. It can harmlessly dissipate absorbed light energy through photophysical processes, significantly reducing photodegradation of the coating matrix. Compared to conventional additive ultraviolet absorbers, the polymerized functional monomer reduces migration, volatilization, and extraction losses at the source, resulting in long-lasting weather protection. Even under prolonged outdoor exposure and immersion conditions, it effectively delays coating chalking, gloss loss, and cracking.

[0022] 3. Methacryloxy POSS participates in copolymerization in the form of a polymerizable cage-like silsesquioxane. Its rigid siloxane cage-like framework is covalently anchored to the polymer chain, forming nanoscale organic-inorganic hybrid reinforcement domains at the molecular scale. This hybrid structure domain can significantly improve the microphase rigidity and density of the coating, giving the coating higher hardness and chemical resistance. At the same time, the siloxane cage structure of POSS has excellent thermal stability and oxidation resistance, which can increase the thermal decomposition temperature of the coating and maintain the integrity and protective ability of the coating under high-temperature baking or high-temperature environments.

[0023] 4. This invention employs a ketone-hydrazine crosslinking system constructed from diacetone acrylamide and adipic acid dihydrazide. During emulsion storage, the adipic acid dihydrazide is stably dispersed in the aqueous phase, while the ketone groups of the diacetone acrylamide are embedded within the polymer particles. The two are effectively isolated from each other, preventing crosslinking reactions and ensuring the long-term storage stability of the emulsion. After coating and film formation, with moisture evaporation and changes in system pH, the adipic acid dihydrazide and ketone groups undergo a condensation reaction to generate hydrazones, achieving room-temperature self-crosslinking. This significantly improves the crosslinking density, hardness, water resistance, and anti-blocking properties of the final coating. The optimized crosslinking agent ratio balances the film flexibility and crosslinking effect, allowing the coating to maintain good impact resistance while possessing high hardness.

[0024] 5. This method utilizes a water-soluble initiator and a reactive emulsifier, prepared through a pre-emulsification-semi-continuous seed emulsion polymerization process. No organic solvents are involved throughout the process, resulting in near-zero VOCs and meeting environmental protection requirements. The reactive emulsifier is covalently anchored to the latex particle surface, completely avoiding the adhesion degradation and water resistance reduction caused by the migration of traditional small-molecule emulsifiers to the coating surface. The resulting resin has uniform particle size and, after adjustment with a neutralizing agent, exhibits excellent water dilution and mechanical stability. It does not separate or clump under room temperature or 50°C heat storage conditions, fully meeting the needs of industrial mass production and long-term storage and transportation. Detailed Implementation

[0025] To better understand the above technical solutions, exemplary embodiments of the present invention are described in more detail below. While exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the invention to those skilled in the art.

[0026] The raw materials used in the embodiments and comparative examples of this invention include: Alicyclic epoxy resin: 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, epoxy equivalent 132 g / eq; low molecular weight bisphenol F epoxy resin: epoxy equivalent 168 g / eq; bisphenol A type epoxy resin: E-51, epoxy equivalent 185 g / eq (for comparative example); hard monomer: cyclohexyl methacrylate; soft monomer: isooctyl acrylate; carboxyl monomer: acrylic acid; functional monomer: 7-(cinnamoyloxy)-4-methylcoumarin Methacryloxypropyl POSS: Methacryloxypropyl cage-like silsesquioxane; Diacetone acrylamide (DAAM), Adipate dihydrazide (ADH); UV absorber UV-327 (for comparative example); N-hydroxymethylacrylamide (for comparative example); Water-soluble initiator: Azobisisobutyramidine hydrochloride (AIBA); Neutralizing agent: N,N-dimethylethanolamine (DMEA); Reactive emulsifier: Sodium allyloxyhydroxypropylsulfonate (SR-10).

[0027] The present invention will be further described below with reference to the following embodiments.

[0028] Example 1 A weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin, with the following component ratio by weight: The composition includes 20 parts of composite epoxy resin (alicyclic epoxy: bisphenol F epoxy = 1:1.5), 35 parts of acrylic mixed monomers (hard monomer: soft monomer: carboxyl monomer = 12:15:5), 2 parts of functional monomers, 1 part of methacryloyloxy POSS, 4.3 parts of crosslinking agent (DAAM:ADH = 3:1), 1.5 parts of water-soluble initiator, 2 parts of neutralizing agent, 1 part of reactive emulsifier, and 50 parts of deionized water.

[0029] The preparation steps of the above-mentioned weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin are as follows: Step 1: Add the composite epoxy resin to the acrylic mixed monomers according to the ratio, heat to 50°C, and stir until completely dissolved to obtain an epoxy resin-monomer solution; cool to 28°C, add the functional monomer, methacryloyloxy POSS and diacetone acrylamide, and stir until completely dissolved to obtain an oil phase mixture.

[0030] Step 2: Dissolve the reactive emulsifier in 60% of the formula amount of deionized water, stir to dissolve, then add 40% of the formula amount of water-soluble initiator, stir evenly to obtain an aqueous phase mixture.

[0031] Step 3: Add the aqueous phase mixture to the reactor, heat to 75°C, and stir at 200 r / min; slowly add 5% of the oil phase mixture to the reactor, keep warm until the system shows a blue phase and the temperature stabilizes, and continue to keep warm for 10 min to obtain the seed emulsion.

[0032] Step 4: Add the remaining oil phase mixture at a uniform rate over 3 hours, with the addition temperature controlled at 78±1℃; simultaneously add the mixture of the remaining initiator and the remaining deionized water over 3.5 hours.

[0033] Step 5: After the addition is complete, heat to 85℃ and keep warm for 1 hour; cool down to 60℃, add neutralizing agent, and stir for 15 minutes.

[0034] Step 6: Cool down to 38℃, add adipic acid dihydrazide to the system, stir for 20 minutes; filter through a 100-mesh filter to discharge the material.

[0035] Example 2 A weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin, with the following component ratio by weight: The composition includes 25 parts of composite epoxy resin (alicyclic epoxy: bisphenol F epoxy = 1:2), 40 parts of acrylic mixed monomers (hard monomer: soft monomer: carboxyl monomer = 15:17.5:6.5), 3.5 parts of functional monomers, 2 parts of methacryloyloxy POSS, 7.5 parts of crosslinking agent (DAAM:ADH = 4:1.5), 2 parts of water-soluble initiator, 3 parts of neutralizer, 2 parts of reactive emulsifier, and 58 parts of deionized water.

[0036] The preparation steps of the above-mentioned weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin are as follows: Step 1: Add the composite epoxy resin to the acrylic mixed monomers according to the ratio, heat to 55°C, and stir until completely dissolved to obtain an epoxy resin-monomer solution; cool to 25°C, add the functional monomer, methacryloyloxy POSS and diacetone acrylamide, and stir until completely dissolved to obtain an oil phase mixture.

[0037] Step 2: Dissolve the reactive emulsifier in 70% of the formula amount of deionized water, stir to dissolve, then add 50% of the formula amount of water-soluble initiator, stir evenly to obtain an aqueous phase mixture.

[0038] Step 3: Add the aqueous phase mixture to the reactor, heat to 79°C, and stir at 220 r / min; slowly add 7.5% of the oil phase mixture to the reactor, keep warm until the system shows a blue phase and the temperature stabilizes, and continue to keep warm for 12 min to obtain the seed emulsion.

[0039] Step 4: Add the remaining oil phase mixture at a uniform rate over 3.5 hours, with the addition temperature controlled at 81±1℃; simultaneously add the mixture of the remaining initiator and the remaining deionized water over 4 hours.

[0040] Step 5: After the addition is complete, heat to 86℃ and keep warm for 1.25 hours; cool down to 62℃, add neutralizing agent, and stir for 22 minutes.

[0041] Step 6: Cool down to 35℃, add adipic acid dihydrazide to the system, stir for 25 minutes; filter through a 100-mesh filter to discharge the material.

[0042] Example 3 A weather-resistant, self-crosslinking waterborne epoxy-modified acrylic resin, with the following component ratio by weight: The composition includes 30 parts of composite epoxy resin (alicyclic epoxy: bisphenol F epoxy = 1:2.5), 45 parts of acrylic mixed monomers (hard monomer: soft monomer: carboxyl monomer = 18:20:8), 5 parts of functional monomers, 3 parts of methacryloyloxy POSS, 10.5 parts of crosslinking agent (DAAM:ADH = 5:2), 2.5 parts of water-soluble initiator, 4 parts of neutralizing agent, 3 parts of reactive emulsifier, and 65 parts of deionized water.

[0043] The preparation steps of the above-mentioned weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin are as follows: Step 1: Add the composite epoxy resin to the acrylic mixed monomers according to the ratio, heat to 60°C, and stir until completely dissolved to obtain an epoxy resin-monomer solution; cool to 28°C, add the functional monomer, methacryloyloxy POSS and diacetone acrylamide, and stir until completely dissolved to obtain an oil phase mixture.

[0044] Step 2: Dissolve the reactive emulsifier in 80% of the formula amount of deionized water, stir to dissolve, then add 60% of the formula amount of water-soluble initiator, stir evenly to obtain an aqueous phase mixture.

[0045] Step 3: Add the aqueous phase mixture to the reactor, heat to 82℃, and stir at 250 r / min; slowly add 10% of the oil phase mixture to the reactor, keep warm until the system shows a blue phase and the temperature stabilizes, and continue to keep warm for 15 min to obtain the seed emulsion.

[0046] Step 4: Add the remaining oil phase mixture at a uniform rate over 4 hours, with the addition temperature controlled at 84±1℃; simultaneously add the mixture of the remaining initiator and the remaining deionized water over 5 hours.

[0047] Step 5: After the addition is complete, heat to 88℃ and keep warm for 1.5 hours; cool down to 65℃, add neutralizing agent, and stir for 30 minutes.

[0048] Step 6: Cool down to 38℃, add adipic acid dihydrazide to the system, stir for 30 minutes; filter through a 100-mesh filter to discharge the material.

[0049] Comparative Example 1 The only difference between this comparative example and Example 2 is that the composite epoxy resin is replaced with an equal mass of bisphenol A type epoxy resin E-51, while the other components and preparation methods are the same as in Example 2.

[0050] Comparative Example 2 The only difference between this comparative example and Example 2 is that the functional monomer is replaced with an equal mass of additive UV absorber UV-327, which is added to the system before discharge in step 6. The remaining components and preparation methods are the same as in Example 2.

[0051] Comparative Example 3 The only difference between this comparative example and Example 2 is that no methacryloyloxy POSS is added; all other components and preparation methods are the same as in Example 2.

[0052] Comparative Example 4 The only difference between this comparative example and Example 2 is that the crosslinking agent is replaced with an equal mass of N-hydroxymethylacrylamide, an oil phase mixture is added in step 1, and the adipic acid dihydrazide addition operation in step 6 is not performed. The remaining components and preparation methods are the same as in Example 2.

[0053] Performance Testing and Result Analysis The resin emulsions obtained in Example 2 and Comparative Examples 1-4, and the coatings prepared therefrom, were subjected to performance tests. The test standards and methods are as follows: Solid content testing shall refer to GB / T 1725-2007; pencil hardness testing shall refer to GB / T 6739-2006.

[0054] Adhesion testing refers to the cross-cut test in GB / T 9286-1998; impact resistance testing refers to GB / T 1732-1993.

[0055] Storage stability: Store at a constant temperature of 50℃ in a sealed container for 30 days, and visually inspect for stratification, clumping, or gelation. Water resistance: Immerse in deionized water at room temperature for 168 hours and observe the coating condition; Weather resistance: QUV accelerated aging test (UVB-313 lamp, irradiance 0.63W / m²) 2 The test was conducted after 1000 hours of testing, including a cycle of 4 hours of light exposure at 60℃ and 4 hours of condensation at 50℃. The results showed the gloss retention rate and yellowing index Δb.

[0056] The test results are shown in the table below:

[0057] The test results above show that: Example 2 exhibits excellent overall performance, with stable emulsion storage and a coating exhibiting high hardness, good adhesion, and outstanding water and weather resistance. Compared to Comparative Example 1, Example 2 shows a 31.1% increase in gloss retention after QUV aging and an 82.1% decrease in the yellowing index, demonstrating that the introduction of alicyclic epoxy significantly improves weather resistance, while the compounded bisphenol F epoxy retains excellent adhesion. Compared to Comparative Example 2, Example 2 shows a 19.7% increase in gloss retention after aging, a 70.7% decrease in the yellowing index, and superior water resistance, demonstrating that the polymeric functional monomers do not migrate or precipitate, resulting in more durable weather protection. Compared to Comparative Example 3, Example 2 shows an increase in pencil hardness from HB to 2H and a certain improvement in weather resistance, demonstrating that the POSS hybrid structure effectively enhances the coating's hardness and thermo-oxidative stability. Compared to Comparative Example 4, Example 2 demonstrates superior storage stability, water resistance, and weather resistance, proving that the ketone-hydrazine crosslinking system can simultaneously achieve excellent storage stability and room-temperature self-crosslinking performance.

[0058] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. The illustrative expressions of the above terms in this specification should not be construed as necessarily referring to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.

[0059] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A weather-resistant, self-crosslinking, waterborne epoxy-modified acrylic resin, characterized in that, By weight, it includes the following ingredients: The composition includes 20-30 parts of composite epoxy resin, 35-45 parts of acrylic mixed monomers, 2-5 parts of functional monomers, 1-3 parts of methacryloyloxy POSS, 4.3-10.5 parts of crosslinking agent, 1.5-2.5 parts of water-soluble initiator, 2-4 parts of neutralizing agent, 1-3 parts of reactive emulsifier, and 50-65 parts of deionized water. The functional monomer is 7-(cinnamoyloxy)-4-methylcoumarin; methacryloyloxyPOSS is methacryloyloxypropyl cage-type silsesquioxane; and the crosslinking agent is composed of diacetone acrylamide and adipate dihydrazide.

2. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, The composite epoxy resin is composed of alicyclic epoxy resin and low molecular weight bisphenol F epoxy resin in a mass ratio of 1:1.5~2.5, based on parts by weight; wherein the alicyclic epoxy resin is at least one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate and diglycidyl hexahydrophthalic acid.

3. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, The acrylic acid mixed monomers, by weight, consist of hard monomers, soft monomers, and carboxyl functional monomers in a mass ratio of 12~18:15~20:5~8.

4. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, By weight, the hard monomer is at least one of cyclohexyl methacrylate, styrene, and tert-butyl acrylate; the soft monomer is at least one of isooctyl acrylate and lauryl acrylate; and the carboxyl functional monomer is at least one of acrylic acid and itaconic acid.

5. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, The preparation methods of functional monomers, by weight, include: Under nitrogen protection and ice bath conditions, 7-hydroxy-4-methylcoumarin and triethylamine were dissolved in anhydrous dichloromethane, and a dichloromethane solution of cinnamyl chloride was slowly added dropwise. After the addition was complete, the temperature was raised to room temperature and the reaction was carried out for 8-12 hours. After the reaction was completed, the reaction solution was poured into 5-10 times its volume of ice water, and the pH was adjusted to 2-3 with dilute hydrochloric acid, precipitating a solid product. The product was filtered, washed with water until neutral, recrystallized, and dried under vacuum to obtain the functional monomer.

6. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 5, characterized in that, The mass ratio of 7-hydroxy-4-methylcoumarin, cinnamyl chloride and triethylamine, by weight, is 1:1.05~1.25:0.70~0.

90.

7. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, In the crosslinking agent, the mass ratio of diacetone acrylamide to adipate dihydrazide is 3~5:1~2.

8. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, The water-soluble initiator is at least one of azobisisobutyramidine hydrochloride and ammonium persulfate; the neutralizing agent is at least one of N,N-dimethylethanolamine and triethylamine.

9. The weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, The reactive emulsifier is at least one of sodium allyl hydroxypropyl sulfonate and sodium alkylphenol ether sulfosuccinate.

10. A method for preparing the weather-resistant self-crosslinking waterborne epoxy-modified acrylic resin according to claim 1, characterized in that, Includes the following steps: (1) Add the composite epoxy resin to the acrylic mixed monomers according to the ratio, stir and dissolve at 50~60℃ to obtain epoxy resin-monomer solution; cool down to below 30℃, add functional monomer, methacryloyloxy POSS and diacetone acrylamide, stir and dissolve to obtain oil phase mixture. (2) Dissolve the reactive emulsifier in water accounting for 60% to 80% of the total amount of deionized water, add water-soluble initiator accounting for 40% to 60% of the total amount of water-soluble initiator, stir to dissolve, and obtain an aqueous phase mixture; (3) Add the aqueous phase mixture to the reactor, heat it to 75~82℃, add 5%~10% of the oil phase mixture while stirring, keep it warm until the system shows a blue phase and the temperature is stable, continue to keep it warm for 10~15min to obtain the seed emulsion. (4) The remaining oil phase mixture is added dropwise to the seed emulsion at a constant rate over 3-4 hours, and the system temperature is controlled at 78-84℃ during the addition. The remaining water-soluble initiator and the remaining deionized water are added dropwise simultaneously. (5) After the addition is complete, heat to 85~88℃ and keep the temperature for 1~1.5h. Then cool down to 60~65℃, add neutralizing agent and stir for 15~30min. (6) Cool down to below 40°C, add adipic acid dihydrazide, stir for 20-30 minutes, filter and discharge to obtain weather-resistant self-crosslinking waterborne epoxy modified acrylic resin.