A fluorine-free hydrophobic additive, its preparation method and its application

By using a vinyl-terminated PDMS-based terpolymer fluorine-free hydrophobic additive, the environmental protection and compatibility issues of fluorine-containing additives in ArF immersion lithography were solved, achieving stable film formation and development performance of high-precision photoresist, suitable for ArF immersion lithography processes at the 7–28 nm node.

CN123107003APending Publication Date: 2026-11-17JIANGSU JICUI POLYMER NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611450849.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing ArF immersion lithography processes, fluorinated hydrophobic additives have problems such as strong bioaccumulation, high cost, poor compatibility with the main photoresist resin, easy phase separation, and development residue, which cannot meet the requirements of high-precision lithography processes.

Method used

By using vinyl-terminated PDMS-based terpolymers with fluorine-free hydrophobic additives and precisely controlling the copolymerization ratio of the three monomers, a hydrophobic copolymer with interfacial self-enrichment, structural self-anchoring, and in-situ crosslinking and shaping is constructed. High hydrophobicity, heat resistance, and developability are achieved by utilizing the low surface energy properties of Vi-PDMS, the rigid alicyclic structure of IBOMA, and the polar groups of GBLMA lactone.

Benefits of technology

It achieves the environmental friendliness of fluorine-free hydrophobic additives, good compatibility with the main resin of photoresist, stability and high-precision film formation, solves the environmental protection and compatibility problems of traditional fluorine-containing additives, improves the heat resistance and development stability of photoresist, and reduces line edge roughness and development residue defects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention addresses the problems of existing ArF immersion lithography additives, such as environmental limitations of fluorinated hydrophobic additives, insufficient hydrophobicity in fluorine-free systems, poor compatibility with acrylate resins, and easy interface failure during post-baking and development stages. It provides a terpolymer additive, which is obtained by free radical copolymerization of divinyl-terminated polydimethylsiloxane, isoborneol methacrylate, and γ-butyrolactone methacrylate, with a molar ratio of (10~25):(45~75):(15~30). After being added to the ArFi photoresist substrate resin, the additive is pre-baked at 60~80℃ to enrich the PDMS chain interface and form a hydrophobic layer. Subsequent post-baking at 100~120℃ triggers hydrogen bond recombination and covalent crosslinking of residual double bonds, achieving permanent interface shaping. This invention is entirely fluorine-free, with a receding contact angle of 79.5°~83.1°, and combines high hydrophobicity, resin compatibility, alkali resistance, developability, and process stability, making it suitable for 7~28 nm node ArF immersion lithography processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor photoresist functional materials technology, and particularly relates to a fluorine-free interface self-enriched hydrophobic additive suitable for ArF immersion lithography (ArFi) process, its preparation method and application. Background Technology

[0002] Argon fluoride excimer laser immersion lithography (ArF immersion lithography) is a core exposure process in advanced semiconductor manufacturing. This process uses pure water as the exposure medium and has extremely strict requirements on the surface hydrophobicity, interface stability, water penetration resistance, and development compatibility of the photoresist film.

[0003] To address issues such as film swelling, disrupted photoacid diffusion, watermark defects, and pattern distortion caused by immersion in pure water, the industry commonly employs fluorinated hydrophobic additives to achieve hydrophobic protection at the photoresist interface. Currently, commercially available hydrophobic additives are per- and polyfluoroalkyl substances (PFAS) polymers. While PFAS polymers exhibit excellent hydrophobic properties and meet the basic requirements for immersion exposure, they still possess several inherent drawbacks: (1) Fluorine-containing materials are highly bioaccumulative and difficult to degrade naturally. Due to the strict restrictions of global environmental protection policies, there is an urgent need to replace fluorine-containing materials. (2) The high cost and supply chain constraints of fluorine-containing raw materials are not conducive to the localization and large-scale production of photoresist; (3) Fluorine groups have very low polarity and poor compatibility with acrylate photoresist main resins. They are prone to phase separation and precipitation during long-term storage, and defects such as shrinkage cavities and pinholes are likely to occur after film formation. In addition, the residue of fluorine groups can easily cause process problems such as developing residue and equipment contamination.

[0004] To avoid the drawbacks of perfluorinated / polyfluorinated polymer materials, the industry has gradually developed fluorine-free hydrophobic modification technologies. The mainstream fluorine-free hydrophobic modification technologies in the industry include: long-chain alkyl-modified resins and common polydimethylsiloxane (PDMS) blend modification systems. Among them: a) Alkyl acrylate systems have weak hydrophobicity, low water retreat angle, and insufficient resistance to pure water wetting and penetration, making them unsuitable for the high-precision process of high-end ArF immersion lithography. b) Conventional PDMS modified systems, while possessing the advantage of low surface energy and hydrophobicity, have poor thermodynamic compatibility with acrylate resins, are prone to disordered migration and surface oil precipitation, and exhibit poor film-forming stability. In addition, conventional PDMS modified systems lack interface anchoring structures, resulting in fragile pre-formed hydrophobic layer structures. After high-temperature baking in the photoresist process (Post-Exposure Bake, PEB) and alkaline development and rinsing, problems such as interface reconstruction, detachment, and swelling are likely to occur. Conventional PDMS modified systems cannot simultaneously achieve hydrophobic stability during immersion exposure and structural stability during post-baking and development.

[0005] In summary, existing ArFi lithography fluorine-free hydrophobic modification technologies suffer from the following common technical bottlenecks: they cannot achieve segmented, controllable interface forming, and cannot meet the high-precision, low-defect production requirements of advanced lithography processes. 1) The hydrophobic layer formed by low-temperature pre-baking has no locking structure and is prone to failure during the post-baking and developing stages; 2) The high-temperature cross-linking and shaping system has the problem of insufficient hydrophobic enrichment before exposure, making it difficult to adapt to the pure water immersion exposure process; 3) Existing fluorine-free hydrophobic modification systems lack the synergistic regulation of rigid structure and polar hydrogen bonds, resulting in poor film heat resistance, dimensional stability, and swelling resistance, and are prone to problems such as high pattern roughness and numerous defects. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a fluorine-free interface self-enriched hydrophobic additive (vinyl-terminated PDMS-based ternary copolymer fluorine-free hydrophobic additive), its preparation method, and its application suitable for ArF immersion lithography (ArFi) processes.

[0007] A fluorine-free hydrophobic additive, comprising the following raw material components: Vinyl-terminated polydimethylsiloxane (Vi-PDMS) Isobornyl methacrylate (IBOMA) γ-Butyrolactone methacrylate (GBLMA); IBOMA and GBLMA are comonomers; The molar ratio of dimethylsiloxane, isoborneol methacrylate, and γ-butyrolactone methacrylate is (10-25):(45-75):(15-30). With appropriate polymerization process and auxiliary agent system, a novel hydrophobic copolymer with interfacial self-enrichment, structural self-anchoring, and in-situ crosslinking and shaping characteristics can be constructed. This invention precisely controls the copolymerization ratio of the three monomers and relies on the low surface energy characteristics of Vi-PDMS to endow the polymer with surface enrichment ability. The siloxane bond and side methyl group in its main structure make the whole has strong hydrophobicity. The rigid alicyclic structure of IBOMA is used to improve the heat resistance, development resistance and miscibility with the photoresist main resin. At the same time, the lactone polar group of GBLMA is used to suppress the disordered migration and precipitation defects of PDMS chain segments.

[0008] The preparation method of this fluorine-free hydrophobic additive includes the following steps: Step 1: Add the vinyl-terminated polydimethylsiloxane, isoborneol methacrylate and γ-butyrolactone methacrylate to the solvent, stir and pre-disperse, then introduce an inert gas to replace the oxygen and water vapor in the reaction system, maintain the reaction system at a slight positive pressure, raise the temperature of the reaction system and stir at a constant temperature. Step 2: Add the free radical initiator and chain transfer agent to the mixture from Step 1, and stir in the dark until completely dissolved; under a slightly positive pressure inert atmosphere, carry out a controlled free radical copolymerization reaction at 95~115℃ with stirring and segmented temperature control; This invention innovatively designs a differentiated temperature-controlled reaction mechanism, wherein the synthesis stage is a controlled linear chain growth reaction, used to construct the linear backbone of the ternary copolymer, so that the prepared copolymer can be stably dissolved in PGMEA and the matching coating solvent, and uniformly form a film, reserving sufficient active reaction sites for the subsequent PEB stage interface shaping and covalent crosslinking. The specific functional divisions are as follows: Vi-PDMS provides low surface energy properties, endowing the material interface with directional enrichment and hydrophobic and water-repellent capabilities; the high proportion of IBOMA alicyclic structure provides the copolymer with excellent heat resistance, rigidity, and developability, significantly improving compatibility with the photoresist acrylate main resin and eliminating defects such as precipitation, cratering, and phase separation; the lactone polar groups carried by GBLMA can form an intermolecular hydrogen bond network, realizing the interfacial anchoring of PDMS chain segments and inhibiting their disordered migration and high-temperature precipitation. Oxygen must be isolated throughout the polymerization process, as oxygen will quench free radicals and terminate polymerization, leading to low monomer conversion and uneven product molecular weight; during segmented temperature-controlled reactions, the heating rate must be strictly controlled, rapid heating is strictly prohibited, and a uniform heating rate must be maintained to avoid system burst polymerization and local gelation; initiators and chain transfer agents must be prepared and used immediately at low temperature and away from light to prevent premature decomposition and inactivation of the initiator; Step 3: After the reaction is complete, cool down (naturally cool to room temperature to prevent the polymer chain segments from agglomerating suddenly due to excessive cooling). Then, purify the reaction solution by sedimentation, allow it to stand to precipitate, and filter the mixture of precipitate and reaction solution to obtain a solid product. During the sedimentation process, the reaction solution should be added dropwise slowly to ensure that impurities are fully removed and to improve the purity of the copolymer and the uniformity of film formation. Step 4: The solid product obtained in Step 3 is repeatedly washed with solvent and then further purified by sedimentation and filtration to completely remove residual monomers, free auxiliaries and oligomer impurities, and obtain the purified solid product. Step 5: Dry the solid product obtained in Step 4 to constant weight, completely remove residual solvent and ethanol, and obtain a colorless and transparent non-fluorinated hydrophobic additive (solid non-fluorinated hydrophobic terpolymer) with high purity, uniform molecular weight and stable storage.

[0009] As a preferred option, the solvent in step 1 is propylene glycol monomethyl ether acetate (PGMEA). PGMEA is a photoresist-specific solvent with excellent compatibility with the photoresist's main resin system. It can completely avoid the problems of poor compatibility and residual solvent affecting film quality that exist with traditional toluene solvents. At the same time, it effectively avoids excessive aggregation and phase separation of PDMS, ensuring a uniform copolymer structure and a narrow molecular weight distribution.

[0010] As a preferred embodiment, based on 100 parts by weight of divinyl-terminated polydimethylsiloxane, the propylene glycol methyl ether acetate added in step 1 is 350 to 500 parts by weight.

[0011] As a preferred option: the free radical initiator in step 2 is azobisisobutyronitrile (2,2-diisobutyronitrile). -Azobis(2-methylpropionitrile), AIBN), the chain transfer agent in step 2 is n-dodecyl mercaptan.

[0012] As a preferred embodiment, based on 100 parts by weight of divinyl-terminated polydimethylsiloxane, the amount of azobisisobutyronitrile added in step 2 is 0.5 to 0.8 parts, and the amount of n-dodecyl mercaptan added is 0.3 to 0.5 parts.

[0013] Preferably, steps 1 to 5 are as follows: Step 1: Add the vinyl-terminated polydimethylsiloxane, isoborneol methacrylate and γ-butyrolactone methacrylate to the solvent, stir and pre-disperse, then introduce an inert gas to replace the oxygen and water vapor in the reaction system (to prevent oxygen from causing polymerization inhibition and raw material oxidation and deterioration), maintain the reaction system at a slight positive pressure, heat the reaction system to 95°C at a uniform rate, and stir at a constant temperature for 30 minutes to ensure that the reaction system is completely homogeneous and transparent; Step 2: Add the free radical initiator and chain transfer agent to the mixture from Step 1 (the free radical initiator and chain transfer agent should be prepared fresh and added to the reaction system dropwise at a uniform rate in one go to avoid the problem of excessively wide molecular weight distribution caused by local enrichment of the additives), and stir in the dark until completely dissolved; under a slightly positive pressure inert atmosphere, heat the reaction system to 105°C at a heating rate of 1°C / min and react at a constant temperature in a sealed environment for 4 hours (to ensure that the monomer undergoes a stable free radical chain growth reaction). After the reaction is completed, continue to heat to 115°C and react at a constant temperature for 1 hour (to controllably retain 8% to 15% of the residual active carbon double bonds, so as to reserve sufficient crosslinking active sites for the subsequent heat setting of the fluorine-free hydrophobic additive in the photoresist process). Step 3: After the reaction is complete, cool down (naturally cool down to room temperature to prevent the polymer chain segments from agglomerating suddenly due to excessive cooling). Then, slowly add excess anhydrous methanol to the reaction solution for precipitation and purification. Let it stand to precipitate a white flocculent copolymer precipitate. Filter the mixture of precipitate and reaction solution to obtain a solid product. Step 4: The solid product obtained in Step 3 is repeatedly washed with solvent (electronic grade PGMEA), then anhydrous methanol is added for precipitation and purification, and then the product is separated by filtration to completely remove residual monomers, free auxiliaries and oligomer impurities, and obtain the purified solid product. Step 5: Dry the solid product obtained in Step 4 to constant weight in a vacuum oven at 60℃ to completely remove residual solvent and ethanol, and obtain a colorless and transparent non-fluorinated hydrophobic additive (solid non-fluorinated hydrophobic terpolymer) with high purity, uniform molecular weight and stable storage.

[0014] A method for applying a fluorine-free hydrophobic additive includes the following steps: A fluorine-free hydrophobic additive is added to the ArFi photoresist base resin. After uniformly mixing the fluorine-free hydrophobic additive with the ArFi photoresist base resin, the mixture is spin-coated into a film. By mass percentage, the amount of the fluorine-free hydrophobic additive added is 3% to 6% of the total amount of the ArFi photoresist base resin. Then, pre-baking is carried out at 60℃~80℃ (the solvent is evaporated during the photoresist film formation stage, and the spin-coated film is shaped), forming a hydrophobic interface on the surface of the spin-coated film (the copolymer does not undergo chemical reaction, and at the same time, the PDMS segments are oriented to enrich the air interface by thermal motion, and a uniform and stable hydrophobic interface is formed in advance before exposure). Immersion exposure is performed (the hydrophobic interface can effectively prevent pure water from penetrating into the film during immersion exposure, avoiding resin swelling, photo-acid disorder, watermark defects and pattern distortion, and ensuring the stable progress of the immersion exposure process). After exposure, a photoresist process (Post-Exposure Bake, PEB) is performed. During the post-baking stage of the photoresist process at 100℃~120℃, the hydrophobic interface is permanently shaped and cured (completing the secondary directional enrichment of PDMS segments). The high temperature triggers the hydrogen bond recombination and shaping of the GBLMA lactone groups, while the residual active double bonds of the copolymer undergo covalent cross-linking to form a stable hydrophobic interface structure. This structure completely solves the problems of easy peeling, easy migration, and poor alkali resistance and developability of traditional fluorine-free hydrophobic layers, significantly improving the dimensional stability of the photoresist film, reducing line edge roughness, and reducing residual defects in development.

[0015] As a preferred method, pre-dry at 60℃~80℃ for 60s.

[0016] Preferably, the receding contact angle of the ArFi photoresist spin-coated film with added fluorine-free hydrophobic additives and a hydrophobic interface is 79.5° to 83.1°.

[0017] The beneficial effects of this invention are: (1) This invention completely abandons the traditional fluorine-containing PFAS hydrophobic system. The fluorine-free hydrophobic additive of this invention achieves fluorine-free composition, which is very environmentally friendly. It avoids the disadvantages of traditional fluorine-containing PFAS materials, such as environmental restrictions, high cost and poor compatibility. The fluorine-free hydrophobic additive prepared can meet the requirements of green mass production of semiconductors.

[0018] (2) The fluorine-free hydrophobic additive of the present invention is essentially a colorless, transparent, solid vinyl-terminated PDMS-based terpolymer monomer (i.e., Vi-PDMS / IBOMA / GBLMA terpolymer monomer); the various parts of the terpolymer monomer work synergistically to take into account hydrophobic properties, resin compatibility, heat resistance and development resistance, and there is no precipitation, no agglomeration and no interface defects. (3) The unique segmented interface forming mechanism (a hydrophobic interface is formed on the surface of the film obtained by spin coating during pre-baking, and the hydrophobic interface is permanently fixed and cured in the post-baking stage of the photoresist process), which is precisely matched with the ArFi lithography process. It first meets the hydrophobic protection requirements of immersion exposure, and then realizes the interface structure fixation, perfectly balancing the exposure stability and the post-baking and development structure stability; it solves the industry pain points of poor compatibility, easy exudation, unstable hydrophobic layer structure, and many residual defects in the traditional PDMS modified system. The prepared hydrophobic additive has excellent performance with high interface stability, high water retreat contact angle, low swelling, and low line edge roughness. It does not require additional top hydrophobic coating and can be widely used in 7-28nm process ArF immersion lithography process (mainly used for the construction of hydrophobic interface on the surface of ArFi photoresist at 7-28nm node), with excellent industrial mass production and environmental protection application value; (4) The preparation process is simple and controllable, the reaction conditions are mild, the raw materials are readily available, and it can be mass-produced on a large scale. It is compatible with high-end ArF immersion lithography process and has significant advantages in domestic substitution (it can replace traditional perfluorinated hydrophobic materials and is compatible with the complete lithography process system of immersion exposure, post-baking and shaping, and alkaline development). Detailed Implementation

[0019] The present invention will be further described below with reference to embodiments. The description of the embodiments below is only for the purpose of helping to understand the present invention. It should be noted that those skilled in the art can make several modifications to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

[0020] Example 1 Weigh 24.00 g of Vi-PDMS (Mn=10000), 16.42 g of IBOMA, and 5.45 g of GBLMA into a clean, dry container. Add 104.7 g of the measured solvent PGMEA. Set the stirring speed to 300 r / min and pre-disperse the mixture at room temperature for 10 min. Then, continuously purge with high-purity nitrogen for 15 min to completely remove oxygen and moisture from the reaction system. Maintain a slight positive pressure nitrogen atmosphere throughout the process to prevent oxygen from inhibiting polymerization and causing oxidation and deterioration of the raw materials. After purging, uniformly raise the temperature to 95℃ and stir at a constant temperature for 30 min to ensure the reaction system is completely homogeneous and transparent.

[0021] Dissolve 0.16 g of AIBN initiator and 0.1 g of n-dodecyl mercaptan chain transfer agent in a small amount of PGMEA, stir in the dark until completely dissolved, and use immediately. Add the solution dropwise to the reaction system at a uniform rate in one go to avoid the problem of excessively wide molecular weight distribution caused by local enrichment of the additives. After the additives are added, the temperature is increased to 105℃ at a uniform gradient of 1℃ / min, and the mixture is polymerized at a constant temperature in a closed system for 4 hours to ensure that the monomer undergoes a stable free radical chain growth reaction. After the polymerization is completed, continue to heat to 115℃ and cure at a constant temperature for 1 hour to controllably retain 8% to 15% of the residual active carbon double bonds, reserving sufficient crosslinking active sites for subsequent PEB heat setting.

[0022] After the reaction, the mixture was allowed to cool naturally to room temperature to prevent rapid aggregation of polymer chains due to excessive cooling. The reaction solution was then slowly added dropwise to excess anhydrous methanol for precipitation and purification. A white flocculent copolymer precipitate formed upon standing. The solid product was separated by filtration, dissolved in electronic-grade PGMEA, and precipitated again in anhydrous methanol by filtration. This process was repeated twice to thoroughly remove residual monomers, free additives, and oligomer impurities. Finally, the purified solid product was dried in a 60°C vacuum oven to constant weight to completely remove residual solvents and ethanol, yielding a high-purity, uniformly molecular weight, and stably stored colorless, transparent, fluorine-free, hydrophobic terpolymer.

[0023] Example 2 Weigh 20.00 g of Vi-PDMS (Mn=12000), 19.80 g of IBOMA, and 4.16 g of GBLMA and place them in a clean, dry container. Add 96.8 g of the measured solvent PGMEA and process according to Example 1.

[0024] Weigh 0.16g of AIBN initiator and 0.1g of n-dodecyl mercaptan chain transfer agent and dissolve them in a small amount of PGMEA. Then react and treat them in the same way as in Example 1 to finally obtain a colorless, transparent, solid, fluorine-free, hydrophobic terpolymer.

[0025] Example 3 Weigh 30.00 g of Vi-PDMS (Mn=15000), 15.69 g of IBOMA, and 6.12 g of GBLMA and place them in a clean, dry container. Add 118.78 g of the measured solvent PGMEA and process according to Example 1.

[0026] Weigh 0.16g of AIBN initiator and 0.1g of n-dodecyl mercaptan chain transfer agent and dissolve them in a small amount of PGMEA. Then react and treat them in the same way as in Example 1 to finally obtain a colorless, transparent, solid, fluorine-free, hydrophobic terpolymer.

[0027] Example 4 Weigh 16.42g of IBOMA and 5.45g of GBLMA and place them in a clean, dry container. Add 128.7g of the measured solvent PGMEA and process according to Example 1.

[0028] Weigh 0.16g of AIBN initiator and 0.1g of n-dodecyl mercaptan chain transfer agent and dissolve them in a small amount of PGMEA. Then react and treat them in the same way as in Example 1 to finally obtain a colorless, transparent, solid, fluorine-free, hydrophobic binary copolymer.

[0029] Example 5 Weigh 24.00g of Vi-PDMS (Mn=12000) and 16.42g of IBOMA and place them in a clean, dry container. Add 104.7g of the measured solvent PGMEA and process according to Example 1.

[0030] Weigh 0.16g of AIBN initiator and 0.1g of n-dodecyl mercaptan chain transfer agent and dissolve them in a small amount of PGMEA. Then react and treat them in the same way as in Example 1 to finally obtain a colorless, transparent, solid, fluorine-free, hydrophobic binary copolymer.

[0031] In summary, the fluorine-free hydrophobic additive of the present invention is fluorine-free and environmentally friendly, possesses stable exposure performance and excellent resin compatibility, and its hydrophobic interface can be stably formed before exposure, achieving dual locking and shaping of hydrogen bonds and covalent networks in the photoresist process stage; when applied to photoresist, the fluorine-free hydrophobic additive does not precipitate and is resistant to development.

[0032] The precautions for Examples 1 to 5 are as follows: (1) Oxygen must be isolated throughout the polymerization process. Oxygen will quench free radicals and terminate the polymerization, resulting in low monomer conversion and uneven molecular weight of the product. (2) The heating rate must be strictly controlled. Rapid heating is strictly prohibited. The heating rate should be kept uniform to avoid system agglomeration and local gel clumping. (3) Initiators and chain transfer agents should be prepared and used immediately at low temperature and away from light to prevent premature decomposition and failure of AIBN; (4) The reaction solution should be added slowly during the sedimentation process to ensure that impurities are fully removed and to improve the purity of the copolymer and the uniformity of film formation.

[0033] Photolithography Application: The fluorine-free hydrophobic additives prepared in Examples 1 to 5 were added to the ArFi photoresist base resin system (the addition amount was 3%~6% according to the formulation requirements), and after uniform mixing, they were spin-coated into a film; 60℃, 60 s pre-baking only evaporated the solvent, the copolymer did not react chemically, the PDMS segments were enriched at the directional air interface, and a uniform hydrophobic interface was formed before exposure (characterized by simultaneous TGA-DSC thermal analysis, the sample at 60℃ only showed endothermic weight loss behavior corresponding to the evaporation of organic solvent, and no chemical reaction characteristic peaks or mass abrupt changes such as crosslinking, polymerization, chemical bond decomposition, etc. were observed, only solvent evaporation was achieved, no chemical reaction was observed, the film was stable and the homogeneous structure was stabilized); the interface structure was stable during the immersion exposure process, with no water seepage or film swelling defects; after exposure, the film was exposed to 100~120℃. Post-baking with PEB completes the secondary directional enrichment of PDMS segments, the shaping of the GBLMA hydrogen bond interface, and the in-situ covalent crosslinking of residual double bonds, forming a stable interface (based on the synergistic effect of thermodynamic surface energy and molecular chain motion characteristics: the surface energy of PDMS segments is significantly lower than that of the copolymer matrix and photoresist resin phase, and the molecular chain motion capability is enhanced at high temperature. Driven by the minimization of interfacial free energy, they spontaneously migrate and aggregate towards the free air interface of the film; the rigid alicyclic structure of IBOMA anchors the main skeleton of the copolymer, and the dynamic hydrogen bond network formed by the lactone groups of GBLMA restricts the disordered aggregation and excessive exudation of PDMS, ultimately achieving controllable and directional enrichment of PDMS segments on the surface).

[0034] Performance test results: The five embodiments of this invention, by gradient-tuning the ratio of Vi-PDMS hydrophobic segments, IBOMA rigid segments, and GBLMA hydrogen-bonded anchoring segments, establish a clear performance variation pattern. The quantitative analysis of each key indicator is as follows: I. Gradient Changes in Hydrophobic Properties (After Pre-baking): The contact angle receded in Example 1 was 79.5°, in Example 2 it was 81.2°, in Example 3 it was 83.1°, in Example 4 it was 55.8°, and in Example 5 it was 80.7°. The data shows that within a reasonable ratio range, as the proportion and molecular weight of Vi-PDMS increase, the low surface energy characteristics of the copolymer are significantly enhanced, the hydrophobic properties of the film interface improve linearly, and the resistance to pure water wetting and penetration gradually increases. After removing Vi-PDMS, the system completely loses its interfacial gradient enrichment ability and high hydrophobic properties; IBOMA and GBLMA only play auxiliary roles in solubilization, rigid support, and hydrogen bond stabilization. Example 3 exhibits the best hydrophobic properties, can withstand longer periods of immersion exposure in pure water, and effectively inhibits swelling defects caused by water penetration into the film.

[0035] II. Film Compatibility and Surface Defect Control: With the increase in the proportion of IBOMA alicyclic monomers, the compatibility between the copolymer and the photoresist substrate acrylate resin is significantly optimized. Example 2 showed the highest IBOMA content, resulting in the best film uniformity with no pinholes, precipitates, or orange peel defects on the film surface; Example 1 was second best; Example 3 showed a slight decrease in film uniformity due to the reduced IBOMA content and increased silicon content, but it was still far superior to the traditional physically blended PDMS system. This demonstrates that the high-rigidity alicyclic structure can effectively confine the disordered migration of PDMS segments, solving the phase separation and oil precipitation problems commonly found in silicon-based additives.

[0036] III. Structural Stability and Developability: The polar groups of GBLMA lactones provide hydrogen bonds, acting as anchors. With increasing GBLMA ratio, the binding effect of PDMS segments is enhanced, significantly improving interface stability after high-temperature PEB. Example 3: A high GBLMA ratio constructs a high-density hydrogen bond network. Combined with residual double bond thermal crosslinking, the hydrophobic layer exhibits the strongest resistance to alkaline development with 2.38% TMAH, showing no interface detachment or hydrophobic failure. Example 1: A balanced ratio of hydrogen bonds, rigidity, and hydrophobicity results in the best overall stability. Example 2: Due to a lower GBLMA content, the hydrogen bond anchoring density is slightly lower, but relying on the high IBOMA rigidity structure, it exhibits excellent dimensional stability and optimal pattern roughness control. Example 5: Without the binding of GBLMA polar lactone hydrogen bonds, the large polarity difference between the Vi-PDMS hydrophobic segments and the IBOMA rigid alicyclic matrix leads to slight phase separation in the film microstructure after pre-baking, increased film surface haze, and a significant decrease in homogeneous stability.

[0037] IV. Comprehensive Process Adaptability Analysis: The performance patterns of the five sets of examples are significant, and the ternary interactions and cooperation indicate the performance of each component. This proves that the technical solution of the present invention, which involves ternary synergistic modification, segmented interface shaping, and controllable residual double bonds, possesses significant innovation and process advantages.

[0038] This invention addresses the common technical bottlenecks in existing ArF immersion lithography hydrophobic additives, including poor environmental friendliness due to fluorine content, insufficient hydrophobicity in fluorine-free systems, poor compatibility with silicon-based modifiers, easy migration and precipitation at high temperatures, weak hydrophobic interface stability, and easy failure during development. It innovatively designs a Vi-PDMS / IBOMA / GBLMA ternary controllable copolymer system. By precisely controlling the hydrophobic functional segment and rigid support segment through gradient ratio adjustment, a segmented molding mechanism is achieved, involving pre-enrichment of the pre-baking interface, stable barrier at the exposure interface, and dual locking through PEB thermal crosslinking. This invention completely solves the technical contradiction between high hydrophobicity, high compatibility, high temperature and development resistance, and long-term process stability that traditional hydrophobic materials cannot simultaneously achieve. The all-fluorine-free system is green and environmentally friendly, compatible with advanced semiconductor processes, and features a simple and controllable preparation process, a wide parameter window, and strong mass production capability. Different ratio systems can be adapted to high-precision, low-roughness patterning processes and long-term, high-critical immersion exposure mass production processes, possessing strong engineering application value and market promotion prospects.

Claims

1. A fluorine-free hydrophobic additive, characterized in that, Includes the following raw material components: Divinyl-terminated polydimethylsiloxane, Isoborneol methacrylate, γ-Butyrolactone methacrylate; The molar ratio of the dual-vinyl-terminated polydimethylsiloxane, the isoborneol methacrylate and the γ-butyrolactone methacrylate is (10-25):(45-75):(15-30).

2. A method for preparing the fluorine-free hydrophobic additive as described in claim 1, characterized in that, Includes the following steps: Step 1: Add the double-vinyl-terminated polydimethylsiloxane, the isoborneol methacrylate and the γ-butyrolactone methacrylate to the solvent, stir and pre-disperse, then introduce an inert gas to replace the oxygen and water vapor in the reaction system, maintain the reaction system at a slight positive pressure, raise the temperature of the reaction system and stir at a constant temperature. Step 2: Add the free radical initiator and chain transfer agent to the mixture from Step 1, and stir in the dark until completely dissolved; carry out the free radical copolymerization reaction by stirring and segmented temperature control at 95~115℃ under a slightly positive pressure inert atmosphere. Step 3: After the reaction is complete, cool down, then purify the reaction solution by sedimentation, let it stand to precipitate, and filter the mixture of precipitate and reaction solution to obtain a solid product. Step 4: The solid product obtained in Step 3 is repeatedly washed with solvent and then further purified by sedimentation and filtration to obtain the purified solid product. Step 5: Dry the solid product obtained in Step 4 to constant weight to obtain a fluorine-free hydrophobic additive.

3. The preparation method according to claim 2, characterized in that: The solvent in step 1 is propylene glycol methyl ether acetate.

4. The preparation method according to claim 3, characterized in that: Based on 100 parts by weight of the dual-vinyl-terminated polydimethylsiloxane, the propylene glycol methyl ether acetate added in step 1 is 350-500 parts by weight.

5. The preparation method according to claim 2, characterized in that: In step 2, the free radical initiator is azobisisobutyronitrile, and the chain transfer agent is n-dodecyl mercaptan.

6. The preparation method according to claim 5, characterized in that: Based on 100 parts by weight of the dual-vinyl-terminated polydimethylsiloxane, the azobisisobutyronitrile added in step 2 is 0.5-0.8 parts and the n-dodecyl mercaptan is 0.3-0.5 parts.

7. The preparation method according to claim 2, characterized in that, Steps 1 to 5 are specifically as follows: Step 1: Add the double-vinyl-terminated polydimethylsiloxane, the isoborneol methacrylate and the γ-butyrolactone methacrylate to the solvent, stir and pre-disperse, then introduce an inert gas to replace the oxygen and water vapor in the reaction system, maintain the reaction system at a slight positive pressure, heat the reaction system to 95°C at a uniform rate, and stir at a constant temperature for 30 min. Step 2: Add the free radical initiator and chain transfer agent to the mixture from Step 1, and stir in the dark until completely dissolved; under a slightly positive pressure inert atmosphere, heat the reaction system to 105°C at a heating rate of 1°C / min, and react at a constant temperature in a sealed environment for 4 hours. After the reaction is completed, continue to heat to 115°C and react at a constant temperature for 1 hour. Step 3: After the reaction is complete, cool down and then slowly add excess anhydrous methanol to the reaction solution for precipitation and purification. Let it stand to precipitate the precipitate, and then filter the mixture of precipitate and reaction solution to obtain a solid product. Step 4: The solid product obtained in Step 3 is washed repeatedly with solvent, then anhydrous methanol is added for precipitation and purification, and then filtered to obtain the purified solid product. Step 5: Dry the solid product obtained in Step 4 to constant weight in a vacuum oven at 60°C to obtain a fluorine-free hydrophobic additive.

8. A method for applying the fluorine-free hydrophobic additive prepared by any one of claims 2-7, characterized in that, Includes the following steps: The fluorine-free hydrophobic additive is added to the ArFi photoresist base resin. After the fluorine-free hydrophobic additive and the ArFi photoresist base resin are uniformly mixed, they are spin-coated into a film. The amount of the fluorine-free hydrophobic additive added accounts for 3% to 6% of the amount of the ArFi photoresist main resin, by weight percentage. Then, pre-baking is carried out at 60℃~80℃ to form a hydrophobic interface on the surface of the spin-coated film. Immersion exposure; After exposure, a photoresist process is performed, and the hydrophobic interface is shaped and cured at 100℃~120℃ during the post-baking stage of the photoresist process.

9. The application method according to claim 8, characterized in that: Pre-bake at 60℃~80℃ for 60 seconds.

10. The application method according to claim 8, characterized in that: The retraction contact angle of the ArFi photoresist spin-coated film with added fluorine-free hydrophobic additives and a hydrophobic interface is 79.5° to 83.1°.