Materials, devices and preparation methods based on hyperbranched polyurethane acrylate
By using hyperbranched polyurethane acrylate resin with a suitable urethane bond density, the problem of balancing transmission haze and diffraction efficiency of HPDLC materials under high light intensity was solved, achieving high-efficiency optical performance stability and device optimization.
Patent Information
- Application Number
- CN202611601026.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing HPDLC materials based on hyperbranched acrylates struggle to balance high diffraction efficiency and low transmission haze under high light intensity exposure conditions. Current technologies present a challenge in balancing production efficiency with reducing transmission haze.
Hyperbranched polyurethane acrylate with a suitable urethane bond density is used as the main photocurable resin in the HPDLC system. By combining specific components and preparation methods, intermolecular interactions are formed, and the phase separation process is optimized.
Under high exposure intensity conditions, low transmission haze and high diffraction efficiency were achieved. The material system exhibited good performance stability over a wide exposure intensity range, taking into account both liquid crystal cell filling and device performance optimization.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of holographic projection display technology, and more specifically, to a material, device, and preparation method based on hyperbranched polyurethane acrylate. Background Technology
[0002] Holographic polymer-dispersed liquid crystal (HPDLC) gratings utilize laser interference light to induce photopolymerization and phase separation in a polymer / liquid crystal hybrid system, forming a one-dimensional periodic refractive index modulation structure with alternating polymer-rich and liquid crystal-rich regions. This structure exhibits Bragg diffraction for light of characteristic wavelengths, and the diffraction efficiency can be controlled under an applied electric field. It holds significant application value in fields such as transparent displays, augmented reality (AR / VR) optical waveguides, electrically controlled optical switches, and holographic sensors.
[0003] To obtain high-diffraction-efficiency HPDLC gratings, researchers generally prefer to use acrylate monomers with high functionality and rapid photopolymerization. Among them, hyperbranched acrylates have attracted widespread attention due to their low intrinsic viscosity caused by their three-dimensional spherical topology, which is beneficial for liquid crystal cell filling and formulation optimization. At the same time, their high functionality enables the rapid formation of cross-linked networks in the early stages of photopolymerization, effectively locking the phase separation process.
[0004] However, existing HPDLC materials based on hyperbranched acrylates may still face problems such as increased transmission haze and decreased optical transparency under high-intensity, rapid exposure conditions. This may be related to factors such as excessively fast polymerization rates, local shrinkage during network formation, and inhomogeneity in the phase separation process, thus affecting the overall optical performance of the device. To improve these problems, existing technologies typically employ methods such as reducing exposure intensity, extending exposure time, or adding post-processing steps. However, a balance remains to be struck between improving production efficiency and reducing transmission haze. Therefore, there is still a need in the field for an HPDLC material system that can achieve both high diffraction efficiency and low transmission haze under high exposure intensity conditions. Summary of the Invention
[0005] The present invention aims to provide a material, device and preparation method based on hyperbranched polyurethane acrylate, so as to improve the problem that the existing HPDLC system is difficult to balance diffraction efficiency and transmission haze under high exposure light intensity conditions.
[0006] One object of the present invention is to provide a holographic polymer-dispersed liquid crystal material based on hyperbranched polyurethane acrylate, comprising, by weight: 30-70 parts of hyperbranched polyurethane acrylate, 5-20 parts of active monomer diluent Nematic liquid crystal 30-45 parts, Photoinitiator 0.1~1 part, Total initiator 0.5~2 parts, Other auxiliary agents, 1-2 parts The hyperbranched polyurethane acrylate is a hyperbranched polyurethane oligomer containing multiple acrylate terminal groups, and its urethane bond density is 1.0~7.0 mmol / g, preferably 4.0~7.0 mmol / g.
[0007] In this technical solution, the urethane bond density of the hyperbranched polyurethane acrylate is preferably 4.0~7.0 mmol / g. Preferably, the hyperbranched polyurethane acrylate accounts for 30%~70% of the total mass of the hyperbranched polyurethane acrylate and the reactive monomer diluent, and other additives are preferably leveling agents.
[0008] In one or more embodiments of the present invention, the number-average molecular weight of the hyperbranched polyurethane acrylate may be about 2000 to 6000, and the functionality may be about 6 to 14.
[0009] Hyperbranched polyurethane acrylate (HPUA) molecules contain urethane bonds (-NH-COO-), which enable intermolecular interactions. The inventors have discovered that using hyperbranched polyurethane acrylate with a suitable urethane bond density as the main photocurable resin in HPDLC systems helps to achieve lower transmission haze and higher diffraction efficiency under high exposure intensity conditions. According to embodiments of the present invention, under exposure conditions of 50–150 mW / cm², the grating devices obtained in some embodiments can exhibit a transmission haze of less than 3.0% and a diffraction efficiency of more than 85%.
[0010] Furthermore, the preparation method of the hyperbranched polyurethane acrylate includes: Using polyisocyanate and branching unit precursor as raw materials, wherein the branching unit precursor has OH and / or NH2 functional groups, and controlling the equivalent ratio of NCO to OH or NH2 functional groups to be 1.5:1 to 3.5:1, a polyurethane core with a hyperbranched topology is prepared; then, the peripheral end groups of the polyurethane core are converted into photopolymerizable acrylate double bonds using an end-capping agent containing acrylate groups.
[0011] Controlling the functional group equivalent ratio of NCO to OH or NH2 can be understood as controlling the functional group equivalent ratio of NCO to OH, or controlling the functional group equivalent ratio of NCO to NH2.
[0012] Furthermore, the polyisocyanate is selected from at least one of isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), and dicyclohexylmethane diisocyanate (HMDI). The branching unit precursor contains three or more active hydrogen atoms, and the branching unit precursor is selected from at least one of polyols, polyamines, or alkanolamines.
[0013] Furthermore, the branching unit precursor is selected from at least one of trimethylolpropane, pentaerythritol, glycerol, and triethanolamine.
[0014] Furthermore, the active monomer diluent is selected from at least one of trimethylolpropane triacrylate (TMPTA), isobornyl acrylate (IBOA), 1,6-hexanediol diacrylate (HDDA), and pentaerythritol tetraacrylate (PETA).
[0015] Furthermore, the nematic liquid crystal is a mixture of cyanobiphenyl or fluorinated biphenyl liquid crystals. Preferably, the nematic liquid crystal is a nematic liquid crystal with positive dielectric anisotropy.
[0016] Furthermore, the photoinitiator is selected from one or more of rose red (RB) and its ester derivatives, erythrosine B (B), and eosin Y (Y); The co-initiator is selected from one or more of N-phenylglycine (NPG), triethanolamine (TEOA), and N-methyldiethanolamine (MDEA).
[0017] The other additives are leveling agents.
[0018] Preferably, the leveling agent is selected from one or more of silicone leveling agents, polyacrylate leveling agents, and fluorocarbon compound leveling agents; specifically, the leveling agent is selected from one or more of Tego Glide 432, BYK-333, BYK-354, BYK-361, BYK-UV 3500, Tego Flow 370, and Efka SL 3258.
[0019] Another object of the present invention is to provide a holographic grating device, wherein the holographic grating device is made of any of the holographic polymer-dispersed liquid crystal materials described above.
[0020] Furthermore, this includes the following steps: S1. Under light-protected conditions, mix all components of the holographic polymer-dispersed liquid crystal material. S2. Pour the mixed components into the liquid crystal cell; S3. Expose the liquid crystal cell under the interference light field formed by the dual-beam light source; S4. Place the exposed liquid crystal cell in a dark place and then irradiate it with uniform light for post-curing to obtain the holographic grating device.
[0021] Furthermore, the mixing temperature of the components is 20–40°C; and / or, The thickness of the liquid crystal cell is 8~12μm; and / or, The irradiation power of the interference exposure is 50~150 mW / cm²; and / or, The time spent in the dark is 20-40 minutes; and / or, The post-curing time is 4 to 10 minutes.
[0022] Preferably, the inner surface of the liquid crystal cell is coated with an ITO transparent electrode.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention uses hyperbranched polyurethane acrylate with a suitable urethane bond density as the main photocurable resin in the HPDLC system, which helps to achieve both high diffraction efficiency and low transmission haze under high exposure light intensity conditions. In one or more embodiments of the present invention, under exposure conditions of 50 to 150 mW / cm², the transmission haze of the obtained grating device can be lower than 3.0%, and the diffraction efficiency can be higher than 85%.
[0024] (2) The material system of the present invention exhibits good performance stability over a wide range of exposure intensity. In one or more embodiments of the present invention, the obtained device maintains high diffraction efficiency and low transmission haze within an exposure intensity range of 50–150 mW / cm².
[0025] (3) The hyperbranched polyurethane acrylate used in this invention has both a branched structure and photopolymerizable double bonds, which can meet the needs of liquid crystal cell filling, rapid exposure forming and device performance optimization.
[0026] (4) The embodiments and comparative examples of the present invention show that the carbamate bond density is one of the important structural factors affecting the overall performance of HPDLC devices; when it is within a suitable range, it is more conducive to obtaining lower transmission haze and higher diffraction efficiency. Detailed Implementation
[0027] To enable those skilled in the art to better understand this solution, the present invention will be further described in detail below with reference to specific embodiments. Unless otherwise specified, the process methods used in the embodiments are conventional methods; and unless otherwise specified, the materials used are commercially available.
[0028] Table 1
[0029] Synthesis Example 1 (Synthesis of hyperbranched polyurethane acrylate HPUA-8) This synthetic example provides a method for synthesizing hyperbranched polyurethane acrylate HPUA-8, comprising: Step 1: Preparation of NCO-terminated hyperbranched polyurethane core Under dry nitrogen protection, add the following materials to a 1000 mL three-necked flask equipped with a stirrer, thermometer, reflux condenser, and constant pressure dropping funnel: Isophorone diisocyanate (IPDI): 66.7 g, dried butyl acetate: 80.0 g, catalyst dibutyltin dilaurate (DBTDL): 0.08 g (0.1 wt% of the total feed in step 1). Stirring was started, and dry nitrogen gas was introduced for protection. The temperature was raised to 60°C. 13.4 g (0.1 mol) of trimethylolpropane (TMP) was dissolved in 10 mL of butanone (approximately 8 g) to obtain a clear solution. This TMP solution was transferred to a constant-pressure dropping funnel and slowly added dropwise to the reaction flask with stirring, controlling the dropping rate to keep the reaction system temperature below 70°C (dropping completed in approximately 30 minutes). After the addition was complete, the reaction was maintained at 70°C for 4 hours to obtain a hyperbranched polyurethane core (hPU-NCO) solution with NCO end groups.
[0030] Step 2: Acrylic end capping Cool the solution obtained in step 1 to 50°C, then add: p-Methoxyphenol (polymerization inhibitor): 0.06 g (approximately 500 ppm of the final product mass), hydroxyethyl acrylate (HEA): 36.6 g. The reaction was carried out with continuous stirring at 50°C. The NCO content was monitored by titration using the di-n-butylamine method. The reaction was stopped when the NCO mass fraction was <0.1% (approximately 3-4 hours).
[0031] Post-treatment (precipitation and dissolution): The reaction solution was slowly poured into 500 mL of n-hexane under vigorous stirring, resulting in a viscous precipitate. The precipitate was collected by filtration and redissolved in approximately 30 mL of butyl acetate. This redissolved precipitate was then poured into 500 mL of n-hexane again under stirring. This dissolution-precipitation process was repeated twice. The precipitate was collected and dried under vacuum at 40°C for 24 hours to obtain a pale yellow viscous solid, which is the hyperbranched polyurethane acrylate, designated HPUA-8.
[0032] Product structural parameters (theoretical estimates): The number-average molecular weight is approximately 4800.
[0033] The functionality (number of double bonds per acrylate molecule) is approximately 8.
[0034] The carbamate bond density was theoretically estimated based on the stoichiometric relationship of the feed ingredients. Each molecule of IPDI contains two NCO atoms, which, upon complete reaction, generate two carbamate bonds. When the amount of IPDI added is 0.3 mol (66.7 g, i.e., 0.3 mol), the theoretical total amount of carbamate bonds is 0.6 mol. Combining this with the theoretical total mass of the product to estimate the carbamate bond content per unit mass of product, it can be deduced that the number of millimoles of carbamate bonds per gram of product is approximately 5.2 mmol / g.
[0035] Synthesis Example 2 (Synthesis of hyperbranched polyurethane acrylate HPUA-12) This synthesis example provides a method for synthesizing hyperbranched polyurethane acrylate HPUA-12, which differs from Synthesis Example 1 in that IPDI is replaced with 50.5 g of hexamethylene diisocyanate (HDI) and TMP is replaced with 13.6 g of pentaerythritol (PENTA). The feed ratio of HDI to PENTA was 3:1, resulting in HPUA-12. Based on the feed ratio, the functionality was estimated to be approximately 12, the carbamate bond density to be approximately 6.9 mmol / g, and the molecular weight to be approximately 5600.
[0036] Synthesis Example 3 (Synthesis of hyperbranched polyurethane acrylate HPUA-6) This synthetic example provides a method for synthesizing hyperbranched polyurethane acrylate HPUA-6. The difference from Synthesis Example 1 is that IPDI is replaced with 52.3 g of toluene diisocyanate (TDI), and TMP is replaced with 9.2 g of glycerol. The feed ratio of TDI to glycerol is 3:1, ultimately yielding HPUA-6. Based on the feed ratio, the functionality is estimated to be approximately 6, the urethane bond density approximately 6.2 mmol / g, and the molecular weight approximately 3200.
[0037] Synthesis Example 4 (Synthesis of hyperbranched polyurethane acrylate HPUA-10) This synthetic example provides a method for synthesizing hyperbranched polyurethane acrylate HPUA-10. The difference from Synthesis Example 1 is that IPDI is replaced with 78.7 g of dicyclohexylmethane diisocyanate (HMDI), and TMP is replaced with 14.9 g of triethanolamine. The feed ratio of HMDI to triethanolamine is 3:1, ultimately yielding HPUA-10. Based on the feed ratio, the functionality is estimated to be approximately 10, the urethane bond density is approximately 4.7 mmol / g, and the molecular weight is approximately 4800.
[0038] Comparative Synthesis Example 1 (Synthesis of hyperbranched polyester acrylate HPEA-8, without urethane bonds) This comparative synthesis example provides a method for synthesizing hyperbranched polyester acrylate HPEA-8, including: Step 1: Melt condensation polymerization of hydroxyl-terminated hyperbranched polyester core (HPE-OH-4) To a 500 mL three-necked flask equipped with a mechanical stirrer, nitrogen inlet, and condenser, add: 13.4 g of trimethylolpropane (TMP), 53.6 g of 2,2-dimethylolpropionic acid (bis-MPA), and 0.47 g of p-toluenesulfonic acid (p-TSA). Under nitrogen protection, heat to 140°C with stirring to allow the mixture to melt. A vacuum (-0.09 MPa) is continuously applied to promote the forward esterification reaction. The reaction is stopped after 3 hours and cooled to room temperature to obtain a pale yellow, transparent, viscous solid, HPE-OH-4. GPC determination yielded Mn≈4200, and hydroxyl titration showed an average functionality of ≈8.
[0039] Step 2: Acrylic end capping Subsequently, HPE-OH-4 (42.0 g, approximately 0.01 mol, containing approximately 0.08 mol of hydroxyl groups) was dissolved in 400 mL of anhydrous dichloromethane, and 97.0 g (0.96 mol) of triethylamine was added as an acid-binding agent. The mixture was cooled to 0–5°C in an ice-water bath. A solution of 87.0 g (0.96 mol) of acryloyl chloride in dichloromethane (approximately 50 mL) was slowly added dropwise with stirring, controlling the temperature to not exceed 5°C (the addition was completed in approximately 1 hour). After the addition was complete, the reaction was allowed to proceed overnight at room temperature (12 hours). After the reaction was complete, the organic phase was washed three times with 300 mL of deionized water, dried overnight with anhydrous magnesium sulfate, filtered, and then the dichloromethane solvent was removed by rotary evaporation under reduced pressure (40°C, -0.08 MPa) to obtain the terminal acrylate hyperbranched polyester (HPEA-8).
[0040] Product structural parameters (estimated theoretically based on feed ratio): Number average molecular weight: estimated at approximately 4600 based on the feed ratio.
[0041] Functionality: estimated at approximately 8 based on the feed ratio.
[0042] Carbamate bond density: 0 mmol / g (main chain contains only ester bonds, no -NH-COO-).
[0043] Comparative Synthesis Example 2 (low urethane density hyperbranched polyurethane acrylate HPUA-8-L, urethane bond density 0.87 mmol / g) This comparative synthesis example provides a method for synthesizing low-urethane-density hyperbranched polyurethane acrylate HPUA-8-L, comprising: Step 1: Preparation of a hyperbranched polyurethane core with NCO end groups containing flexible PPG long chains Under dry nitrogen protection, 22.2 g of isophorone diisocyanate (IPDI) and 200 g of polypropylene glycol (PPG-4000) with a number average molecular weight of 4000 were dissolved in 224 g of dry butyl acetate and reacted at 60°C for 2 hours to obtain an NCO-terminated prepolymer. Subsequently, 2.24 g of trimethylolpropane (TMP) and 0.22 g of dibutyltin dilaurate (DBTDL) were added to the prepolymer, and the reaction was continued at 70°C for 4 hours to complete the branching and chain extension.
[0044] Step 2: Acrylic end capping Cool to 50°C, add 0.03 g of p-methoxyphenol and 5.8 g of hydroxyethyl acrylate (HEA), and react at 50°C until NCO < 0.1% (monitored by the di-n-butylamine method, approximately 2-3 hours).
[0045] Post-treatment: The reaction solution was slowly poured into 800 mL of n-hexane to precipitate the precipitate. The precipitate was collected by filtration and redissolved in approximately 30 mL of butyl acetate. The precipitate was then poured into 800 mL of n-hexane again. This process was repeated three times. The precipitate was collected and dried under vacuum at 40°C for 48 hours to obtain HPUA-8-L.
[0046] Product structural parameters (estimated theoretically based on feed ratio): Number average molecular weight: estimated at approximately 5500 based on the feed ratio.
[0047] Functionality: estimated at approximately 8 based on the feed ratio.
[0048] Carbamate bond density: Due to the dilution of the urethane bond concentration by the introduction of the PPG-4000 flexible chain segment, the concentration is approximately 0.87 mmol / g based on the feed ratio.
[0049] HPUA-8-L has the same functionality (8) and similar molecular weight (5500 vs 4800) as HPUA-8, and is also a hyperbranched polyurethane backbone, but its urethane bond density is only 0.87 mmol / g, which is lower than the critical value of this invention.
[0050] Example 1 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a fabrication method, specifically including the following steps: (1) Preparation of holographic polymer-dispersed liquid crystal materials Under light-protected conditions, 40 parts of HPUA-8, 10 parts of TMPTA, 10 parts of IBOA, 38 parts of liquid crystal E7, 0.5 parts of photoinitiator RB, 1.0 part of co-initiator NPG, and 1.0 part of leveling agent BYK-361 provided in Synthesis Example 1 were weighed out. The above components were mixed and stirred at 25°C until uniform and transparent to obtain the holographic polymer-dispersed liquid crystal material.
[0051] (2) Fabrication of HPDLC grating devices Holographic polymer-dispersed liquid crystal material was capillarily injected into an 8μm thick liquid crystal cell. Exposure was performed using 532nm dual-beam interference, with the interference angle corresponding to a grating period of 450nm. The exposure intensity was set to 50mW / cm², and the exposure time was 60 seconds. After exposure, the device was placed in the dark for 30 minutes, and then post-cured for 5 minutes under uniform light at 405nm (50 mW / cm²) to obtain the HPDLC grating device.
[0052] (3) Performance testing First-order diffraction efficiency test: Using a 532 nm continuous laser as the light source, incident on the grating at the Bragg angle, the intensity I of the first-order diffracted light was measured. diff and zero-order transmitted light intensity I trans , according to η = I diff / (I diff +I trans The correction value is obtained by calculating and subtracting the reflection loss of the glass substrate.
[0053] Transmission haze test: According to GB / T 2410 standard, the grating area is tested at a wavelength of 550 nm using a haze meter, and the results have been subtracted from the inherent haze of the same glass substrate.
[0054] Example 2 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method thereof. The difference from Embodiment 1 is that the exposure intensity is set to 100 mW / cm². Performance tests are performed using the same testing methods as in Embodiment 1.
[0055] Example 2 - Batch Repeat 1 A second batch of HPUA-8 was synthesized using the same feed ratio and operating conditions as in Example 1. The formulation and preparation conditions were identical to those in Example 2. Performance tests were conducted using the same methods as in Example 1. The results showed that at 100 mW / cm², η = 90.1% and H = 1.9%.
[0056] Example 2 - Batch Repeat 2 A third batch of HPUA-8 was synthesized using the same feed ratio and operating conditions as in Example 1. The formulation and preparation conditions were identical to those in Example 2. Performance tests were conducted using the same methods as in Example 1. The results showed that at 100 mW / cm², η = 89.8% and H = 1.8%.
[0057] The data above show that the haze of the gratings prepared by the three batches of HPUA-8 is within the range of 1.8% to 2.0%, and the diffraction efficiency is within the range of 89% to 91%, with minimal fluctuation. This fully demonstrates that the HPUA products obtained according to the feed ratio and synthesis steps given in this invention have good batch-to-batch reproducibility in achieving the grating performance, and the consistency of the product structure is effectively verified by the final performance.
[0058] Example 3 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method thereof. The difference from Embodiment 1 is that the exposure intensity is set to 150 mW / cm². Performance tests were conducted using the same testing methods as in Embodiment 1.
[0059] The test results of Examples 1, 2 and 3 are summarized in Table 2.
[0060] Table 2
[0061] Example 4 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method thereof. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-12, which is provided by Synthesis Example 2. Performance tests were performed using the same testing methods as in Example 1.
[0062] Example 5 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method thereof. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-6, and the exposure intensity is 100 mW / cm². The HPUA-6 is provided by Synthesis Example 3. Performance tests are performed using the same testing methods as in Example 1.
[0063] Example 6 This embodiment provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method thereof. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-10, and the exposure intensity is 145 mW / cm². The HPUA-10 is provided by Synthesis Example 4. Performance tests are performed using the same testing methods as in Example 1.
[0064] The test results of Examples 4, 5 and 6 are summarized in Table 3.
[0065] Table 3
[0066] As shown in Tables 2 and 3, HPUA prepared with different combinations of isocyanates and polyols / polyamines exhibits high diffraction efficiency and low transmission haze in the range of 50–150 mW / cm², provided that the urethane bond density falls within the range of 4.0–7.0 mmol / g. According to the data from the examples, under the tested conditions, η≥85% and H not higher than 2.0% can be achieved.
[0067] Comparative Example 1 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPEA-8, which was provided by Comparative Synthesis Example 1. Performance tests were performed using the same testing methods as in Example 1.
[0068] Comparative Example 2 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPEA-8, and the exposure intensity is set to 100 mW / cm². The HPEA-8 was provided by Comparative Synthesis Example 1. Performance tests were performed using the same testing methods as in Example 1.
[0069] Comparative Example 3 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPEA-8, and the exposure intensity is set to 150 mW / cm². The HPEA-8 was provided by Comparative Synthesis Example 1. Performance tests were performed using the same testing methods as in Example 1.
[0070] The test results of Comparative Example 1, Comparative Example 2 and Comparative Example 3 are summarized in Table 4.
[0071] Table 4
[0072] Comparing the data in Tables 2 and 4, it can be seen that the comparative example and the embodiment use the same hyperbranched topology, similar functionality, and molecular weight. The main difference lies in the framework chemistry—HPEA-8 does not contain urethane bonds. Under similar exposure conditions, the transmission haze of the device obtained from the HPEA-8 system is significantly higher than that from the HPEA-8 system, and the diffraction efficiency is also reduced. This result indicates that a hyperbranched topology alone is insufficient to guarantee low haze under high exposure intensity; the urethane structure in the polymer framework plays a positive role in improving the overall performance of the device.
[0073] Comparative Example 4 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-8-L, which is provided by comparative synthesis example 2. Performance tests were performed using the same testing methods as in Example 1.
[0074] Comparative Example 5 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-8-L, and the exposure intensity is set to 100 mW / cm². The HPUA-8-L is provided by comparative synthesis example 2. Performance tests were performed using the same testing methods as in Example 1.
[0075] Comparative Example 6 This comparative example provides a holographic polymer-dispersed liquid crystal material, an HPDLC grating device, and a preparation method. The difference from Example 1 is that HPUA-8 in Example 1 is replaced with an equal mass of HPUA-8-L, and the exposure intensity is set to 150 mW / cm². The HPUA-8-L is provided by comparative synthesis example 2. Performance tests were performed using the same testing methods as in Example 1.
[0076] The test results of Comparative Examples 4, 5 and 6 are summarized in Table 5.
[0077] Table 5
[0078] Comparing Tables 2 and 5, it can be seen that HPUA-8-L in the comparative example is a hyperbranched polyurethane acrylate containing urethane bonds, and it has the same functionality, the same backbone type, and a similar molecular weight as HPUA-8. The main difference between the two lies in the urethane bond density: HPUA-8 is approximately 5.2 mmol / g, while HPUA-8-L is approximately 0.87 mmol / g. Under similar exposure conditions, the device obtained from the HPUA-8-L system has significantly higher transmission haze than the HPUA-8 system, and the diffraction efficiency is also lower. This result indicates that not all HPUA containing urethane structures can achieve ideal results. The urethane bond density is one of the important structural factors affecting the overall performance of the device, and within a suitable range, it is more beneficial to reduce transmission haze and maintain high diffraction efficiency.
[0079] The performance of Examples 1-6 and Comparative Examples 1-6 is summarized in Table 6.
[0080] Table 6
[0081] It should be noted that, for those skilled in the art, the structure of HPUA is closely related to the type of synthetic raw materials used, the feed ratio, and the reaction conditions. Some structural parameters in this article, especially the carbamate bond density, can be theoretically estimated based on the stoichiometric relationships of the feed materials; these estimates are based on the reasonable expectation that the polyisocyanate and polyol / polyamine will fully react under the stated reaction conditions. Those skilled in the art can obtain HPUA products with the corresponding structural characteristics by following the raw material specifications, feed ratios, and synthetic steps described in the instructions.
[0082] The above embodiments of the present invention are merely examples for clearly illustrating the technical solutions of the present invention, and are not intended to limit the specific implementation of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the claims of the present invention should be included within the protection scope of the claims of the present invention.
Claims
1. A hyperbranched polyurethane acrylate based holographic polymer dispersed liquid crystal material, characterized in that, By weight, it includes: 30-70 parts of hyperbranched polyurethane acrylate, 5-20 parts of active monomer diluent Nematic liquid crystal 30-45 parts, Photoinitiator 0.1~1 part, Total initiator 0.5~2 parts, Other auxiliary agents, 1-2 parts The hyperbranched polyurethane acrylate is a hyperbranched polyurethane oligomer containing multiple acrylate terminal groups, and its urethane bond density is 1.0~7.0 mmol / g.
2. The hyperbranched polyurethane acrylate-based holographic polymer dispersed liquid crystal material according to claim 1, characterized in that, The preparation method of the hyperbranched polyurethane acrylate includes: Using polyisocyanate and branching unit precursor as raw materials, wherein the branching unit precursor has OH and / or NH2 functional groups, and controlling the equivalent ratio of NCO to OH or NH2 functional groups to be 1.5:1 to 3.5:1, a polyurethane core with a hyperbranched topology is prepared; then, the peripheral end groups of the polyurethane core are converted into photopolymerizable acrylate double bonds using an end-capping agent containing acrylate groups.
3. The hyperbranched polyurethane acrylate-based holographic polymerization dispersed liquid crystal material according to claim 2, characterized in that, The polyisocyanate is selected from at least one of isophorone diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, and dicyclohexylmethane diisocyanate; The branching unit precursor contains three or more active hydrogen atoms, and the branching unit precursor is selected from at least one of polyols, polyamines, and alkanolamines.
4. The hyperbranched polyurethane acrylate-based holographic polymer dispersed liquid crystal material according to claim 2, wherein The branching unit precursor is selected from at least one of trimethylolpropane, pentaerythritol, glycerol, and triethanolamine.
5. The hyperbranched polyurethane acrylate-based holographic polymer dispersed liquid crystal material according to claim 1, wherein, The active monomer diluent is selected from at least one of trimethylolpropane triacrylate, isobornyl acrylate, 1,6-hexanediol diacrylate, and pentaerythritol tetraacrylate.
6. The hyperbranched polyurethane acrylate-based holographic polymer dispersed liquid crystal material according to claim 1, wherein, The nematic liquid crystal is a mixture of cyanobiphenyl or fluorinated biphenyl liquid crystals.
7. The hyperbranched polyurethane acrylate-based holographic polymer dispersed liquid crystal material according to any one of claims 1 to 6, characterized in that, The photoinitiator is selected from one or more of rose red, rose red ester derivatives, erythrosine B, and eosin Y; The co-initiator is selected from one or more of N-phenylglycine, triethanolamine, and N-methyldiethanolamine; The other additives are leveling agents.
8. A holographic grating device, characterized by The holographic grating device is made from the holographic polymer-dispersed liquid crystal material as described in any one of claims 1 to 7.
9. A method for fabricating the holographic grating device according to claim 8, characterized in that, Includes the following steps: S1. Under light-protected conditions, mix all components of the holographic polymer-dispersed liquid crystal material. S2. Pour the mixed components into the liquid crystal cell; S3. Expose the liquid crystal cell under the interference light field formed by the dual-beam light source; S4. Place the exposed liquid crystal cell in a dark place and then irradiate it with uniform light for post-curing to obtain the holographic grating device.
10. The method for fabricating a holographic grating device according to claim 9, characterized in that, The temperature at which the components are mixed is 20–40°C; and / or, The thickness of the liquid crystal cell is 8~12μm; and / or, The irradiation power of the interference exposure is 50~150 mW / cm²; and / or, The time spent in the dark is 20-40 minutes; and / or, The post-curing time is 4 to 10 minutes.