A water-foamed polyurethane polishing pad and its preparation method
By using amino-modified polysiloxane-coated water-in-oil nanodroplets and an open-mold free foaming process, the problems of uneven cell structure and mechanical property gradient in all-water foamed polyurethane polishing pads were solved, and a polyurethane polishing pad that meets the requirements of precision polishing and environmental protection was prepared.
Patent Information
- Application Number
- CN202611428133.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing water-foamed polyurethane polishing pads have poor cell uniformity and obvious mechanical property gradients. Traditional foaming processes are complex, costly, and not environmentally friendly.
Using amino-modified polysiloxane-coated water-in-oil nanodroplets as foaming agents, combined with an open mold free foaming process, CO2 gas is released in a confined manner, resulting in the preparation of polyurethane polishing pads with uniform pores, no density gradient, and excellent mechanical properties.
A fully water-foamed polyurethane polishing pad with adjustable cell structure and designable mechanical properties has been developed, meeting the requirements of precision polishing and complying with green manufacturing standards.
Smart Images

Figure CN123107032A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical mechanical polishing technology, and in particular to an all-water foamed polyurethane polishing pad and its preparation method. Background Technology
[0002] Polyurethane polishing pads, with their excellent wear resistance, chemical stability, elastic recovery, and controllable porous structure, have become one of the most widely used polishing consumables in chemical mechanical polishing processes. As the requirements for surface flatness and processing efficiency for precision devices such as microcrystalline glass and advanced packaging substrates continue to increase, higher demands are being placed on the uniformity of the pore structure, the consistency of mechanical properties, and the service life of polishing pads.
[0003] The existing foaming and molding process for polyurethane polishing pads mainly faces the following technical challenges: Firstly, the uniformity of the foam cells is difficult to control precisely. In traditional closed-mold casting foaming processes, the foaming process is constrained by the mold wall, resulting in an imbalance in the internal temperature and pressure fields. This leads to a significant density and hardness gradient along the thickness direction of the foam—the upper layer has loose cells, while the lower layer is dense. After slicing, the difference in elastic modulus between different areas of the polishing pad typically exceeds 15%. This structural inhomogeneity can cause fluctuations in material removal rate and deterioration of workpiece flatness during polishing. Japanese Patent JP2004075700A discloses a polyurethane foam using modified silicone oil as a surfactant. Although it mentions that amino-modified polysiloxane can be used as one of the surfactant options, its foaming mechanism still relies on the traditional method of introducing gas through mechanical stirring, and does not involve the technical concept of nano-encapsulation confined foaming.
[0004] Secondly, the process is complex and costly. The secondary foaming process involves adding chemical foaming agents such as sodium bicarbonate and expanded microspheres to the basic polyurethane system. After initial molding, a second heating process decomposes these agents to generate gas, thus achieving secondary control of the pore structure. However, this process not only increases energy consumption and steps, but also makes it difficult to guarantee the uniformity of the secondary heating temperature field, resulting in poor consistency and repeatability of cell expansion. Furthermore, the decomposition products of inorganic foaming agents can easily remain as impurities inside the polishing pad, potentially scratching the workpiece surface.
[0005] Thirdly, environmental friendliness needs improvement. Traditional physical foaming agents often involve volatile organic compounds, which does not align with the development trend of green manufacturing. While all-water foaming is an environmentally friendly approach, existing all-water foaming systems commonly suffer from wide cell size distribution and excessively large pore diameters in polyurethane polishing pad applications. For example, Chinese patent application CN116262330A discloses an all-water foamed polyurethane foam and its preparation method. Although it has advantages such as being environmentally friendly and having low cost, its pore size uniformity is poor when applied to polishing pads, and it can easily lead to a sharp drop in local mechanical strength and a shortened service life when used for polishing microcrystalline glass.
[0006] While Japanese patent JP2004075700A mentions that amino-modified polysiloxanes can be used as surfactants, its foaming mechanism still relies on the traditional method of introducing gas through mechanical stirring. Chinese patent CN1738845A uses polysiloxane-based nonionic surfactants to prepare polyurethane foam, but the surfactants only play a role in stabilizing bubbles and do not participate in chemical reactions. Chinese patent CN112571303A discloses a polyurethane polishing pad containing silane repeating units on the main chain. By introducing polysiloxane structural units into the polyurethane main chain, the polishing performance is improved. However, its polysiloxane segments are fixed in the polymer network and cannot provide confined encapsulation during the foaming process.
[0007] To address the aforementioned problems, the inventors discovered that the essence of the foaming process lies in the controllability of bubble nucleation and growth. In traditional all-aqueous foaming systems, the solubility of CO2 generated from the reaction of water and isocyanate is limited, bubble nucleation is highly random, and aggregation and disproportionation easily occur during bubble growth, which is the fundamental reason for the widening of the cell size distribution. If a pre-packaged foaming medium with confined space can be provided, so that the gas is confined within a specific scale range in the early stage of the reaction, the cell uniformity can be effectively improved. Based on this, the present invention proposes to use amino-modified polysiloxane as the shell material to prepare water-in-oil nanodroplets, and to use these nanodroplets to replace conventional deionized water as the foaming agent. Summary of the Invention
[0008] This invention aims to overcome the technical defects of existing all-water foamed polyurethane polishing pads, such as poor cell uniformity and significant gradients in mechanical properties, and provides an all-water foamed polyurethane polishing pad and its preparation method. This invention uses amino-modified polysiloxane-coated water-in-oil nanodroplets as a foaming agent to achieve confined release of CO2 gas, and combines this with an open-mold free foaming process to obtain a polyurethane polishing pad with uniform cell size, no density gradient, and excellent mechanical properties.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A water-blown polyurethane polishing pad is prepared from raw materials comprising the following parts by weight: 30-50 parts of polyol component A; 30-50 parts of polyisocyanate component B; Chain extender 1-3 parts; 0.5 to 5 parts of foaming agent; Amine catalyst, 0.01–0.06 parts; 0.01–0.06 parts of organotin catalyst; Surfactant 0.01 to 0.1 parts; Crosslinking agent 0.1 to 1 part; 20-30 parts of inorganic filler; 1-3 parts coupling agent; 1-3 parts dispersant; The foaming agent is an oil-in-water nanodroplet coated with amino-modified polysiloxane.
[0010] Preferably, the preparation method of the amino-modified polysiloxane-coated nanodroplets includes the following steps: (1) Dissolve the amino-modified polysiloxane in a volatile organic solvent (such as ethyl acetate or dichloromethane) to prepare an oil phase solution with a mass fraction of 1% to 10%. The role of the volatile organic solvent is to reduce the viscosity of the oil phase, which facilitates droplet breakup and size control during the emulsification process.
[0011] (2) Deionized water is used as the aqueous phase, in which electrolytes (such as NaCl and KCl) accounting for 0.1% to 1% of the mass of the aqueous phase are dissolved. The addition of electrolytes has two functions: first, to reduce electrostatic repulsion at the oil-water interface through the ion shielding effect, thereby promoting the formation and stability of the interfacial film; second, to regulate the osmotic pressure of the aqueous phase and inhibit the exchange of substances between droplets (Ostwald ripening).
[0012] (3) The aqueous phase is slowly added to the oil phase at a volume ratio of 1:5 to 1:20. Emulsification is then performed in a high-speed shear emulsifier at a speed of 8000–15000 r / min for 5–20 minutes to form a water-in-oil primary emulsion. The strong shear force generated by the high-speed shear breaks the aqueous phase into nanoscale droplets, and the amino-modified polysiloxane self-assembles at the oil-water interface to form an interfacial film. Controlling the volume ratio ensures the acquisition of suitable droplet density and shell thickness.
[0013] (4) The organic solvent is removed by vacuum distillation at 40–60 °C to obtain amino-modified polysiloxane-coated nanodroplets. The distillation temperature should be selected in consideration of both solvent removal efficiency and nanodroplet structural integrity.
[0014] The amino-modified polysiloxane has an amine value of 0.2–1.0 mmol / g and a viscosity of 50–500 mPa·s (25°C). When the amine value is below 0.2 mmol / g, there are insufficient reaction sites in the shell for chemical anchoring, resulting in insufficient interfacial anchoring effect; when the amine value is above 1.0 mmol / g, the amino content is too high, which may lead to cross-linking reactions at the oil-water interface during the preparation of nanodroplets, making the emulsion unstable. When the viscosity is below 50 mPa·s, the mechanical strength of the shell is insufficient to support the droplet structure; when the viscosity is above 500 mPa·s, emulsification is difficult and the droplet size distribution becomes wider.
[0015] In the foaming agent, amino-modified polysiloxane serves as the shell material for the nanodroplets. This shell material has a dual function: firstly, it acts as an emulsifier to stabilize the water-in-oil emulsion system, encapsulating the aqueous phase into independent nano-scale droplets; secondly, the amino (-NH2) groups distributed on the shell molecular chain can react with the isocyanate groups (-NCO) in the polyurethane system during the subsequent foaming process, achieving chemical bonding between the shell and the polyurethane matrix.
[0016] Furthermore, the amino-modified polysiloxane-coated nanodroplets (foaming agent) is the core innovative component of this invention. The nanodroplets are prepared via a water-in-oil emulsion template method and possess the following structural characteristics: a core of deionized water (containing a small amount of electrolyte), a shell of amino-modified polysiloxane (amine value 0.2–1.0 mmol / g, viscosity 50–500 mPa·s), and a droplet size of 10–100 nm. Its mechanism of action consists of two stages: Emulsion mixing stage: Nanodroplets are uniformly dispersed as independent microreactors in the polyurethane A / B mixture system. Each droplet contains a fixed amount of water molecules, and due to the uniform droplet size, the water content of each droplet is monodisperse.
[0017] Foaming reaction stage: When the system temperature rises to the reaction temperature, isocyanate molecules diffuse into the droplets and react with water molecules at the oil-water interface to generate CO2 gas. Since each droplet has the same water content and the reaction conditions are consistent, the CO2 generation rate and amount within each droplet are highly uniform. The generated CO2 accumulates inside the droplets, creating internal pressure. When this internal pressure exceeds the shell's bearing capacity, the shell ruptures, releasing CO2 and forming bubble nuclei. Due to the uniform spatial distribution of droplets in the system and the consistent rupture sequence, the bubble nucleation sites are evenly distributed, and the nucleation time is synchronized.
[0018] It is worth noting that amino-modified polysiloxane shells possess unique advantages over ordinary surfactants. In the initial stage of the foaming reaction, the amino groups (-NH2) in the shell react with free isocyanate groups (-NCO) in the system to form urea bonds (-NH-CO-NH-), covalently linking the shell molecular chains to the polyurethane network backbone. This chemical anchoring effect has three functions: first, it strengthens the integrity of the shell structure, preventing it from rupturing before CO2 accumulates to the design pressure; second, it ensures that the shell does not migrate due to system flow during foaming, maintaining the initial spatial distribution of droplets; and third, the anchored shell becomes part of the cell wall, enhancing the mechanical strength of the cell wall through physical cross-linking (hydrogen bonds, van der Waals forces) between the siloxane segments and the polyurethane hard segments.
[0019] Preferably, the polyol A component is a polyether-type polyol or a polyester-type polyol with a functionality of 2, a molecular weight of 1000-3000, and a hydroxyl value of 50-400 mg KOH / g. The polyether-type polyol is one or more of polytetramethylene ether glycol (PTMEG), diethylene glycol-based polypropylene oxide ether polyol, and polypropylene oxide ether diol (PPG). PTMEG, due to its good molecular chain regularity, can impart high strength and elastic recovery to the material. The polyol A component is the main material constituting the soft segments of the polyurethane network. A polyether-type or polyester-type polyol with a functionality of 2, a molecular weight of 1000-3000, and a hydroxyl value of 50-400 mg KOH / g is used. Polyols within this range are liquid at room temperature, have moderate reactivity with isocyanates, and their molecular chain flexibility endows the polyurethane material with excellent elasticity and toughness. When the molecular weight is below 1000, the soft segments are too short, increasing the material's brittleness; when it is above 3000, the system viscosity is too high, which is not conducive to the uniform dispersion of nanodroplets. The setting of the hydroxyl value ensures stoichiometry matching with component B, keeping the crosslinking density within the optimal range.
[0020] Preferably, the polyisocyanate component B is selected from one or more of diphenylmethane diisocyanate (MDI), polymethylene polyphenyl isocyanate (PAPI), and isophorone diisocyanate (IPDI). MDI has a symmetrical structure and high reactivity, imparting high hardness and strength to the material; PAPI contains trifunctional components, increasing crosslinking density; IPDI contains an aliphatic cyclic structure, imparting good resistance to yellowing and toughness to the material. The polyisocyanate component B is the main material constituting the hard segments of the polyurethane network, reacting with the hydroxyl groups of component A to form urethane bonds, thus forming the crosslinked network of the polyurethane. Diphenylmethane diisocyanate and isophorone diisocyanate have symmetrical rigid structures, which can impart high hardness and strength to the material; polymethylene polyphenyl isocyanate has high functionality, which can increase the crosslinking density of the system. The combined use of the three isocyanates can achieve an optimal match between hardness and toughness.
[0021] Preferably, the amine catalyst is one or more of triethylenediamine, N,N-dimethylcyclohexylamine, and bis(2-dimethylaminoethyl) ether; the organotin catalyst is dibutyltin dilaurate or stannous octoate. The amine catalyst (triethylenediamine, etc.) mainly catalyzes the foaming reaction (water-NCO reaction), while the organotin catalyst (dibutyltin dilaurate, etc.) mainly catalyzes the gelation reaction (hydroxyl-NCO reaction). The synergistic control of their ratio (0.02–0.12 parts in total) is key to balancing the foaming rate and gelation rate—excessive foaming leads to cell wall rupture and voids, while excessively rapid gelation results in insufficient foaming.
[0022] Preferably, the chain extender is any one of 1,4-butanediol (BDO), ethylene glycol (EG), and diethylene glycol (DEG). The amine catalyst is one or more of triethylenediamine (TEDA), N,N-dimethylcyclohexylamine, and bis(2-dimethylaminoethyl) ether. The organotin catalyst is dibutyltin dilaurate (DBTDL) or stannous octoate. The small molecule diol chain extender (1,4-butanediol, ethylene glycol, diethylene glycol) reacts with isocyanate to generate hard segments, forming physical cross-linking points through hydrogen bonding, significantly improving the hardness and strength of the material. Using 1-3 parts of chain extender ensures the system reaches a suitable hard segment content, keeping the Shore A hardness within the preferred range of 75-90.
[0023] Preferably, the inorganic filler is any one of cerium oxide, alumina, and zirconium oxide, with an average particle size of 0.5–5 μm. Cerium oxide has high chemical activity on glass workpieces and is a preferred abrasive for polishing microcrystalline glass. The coupling agent is KH560 (γ-glycidyl etheroxypropyltrimethoxysilane) or KH570 (γ-methacryloyloxypropyltrimethoxysilane), whose siloxane group at one end of the molecule can condense with the hydroxyl groups on the surface of the inorganic filler, and the organic functional group at the other end can react with the polyurethane matrix, acting as a bridge. The dispersant is BYK-P104S, BYK-9076, or BYK-2163. The inorganic filler (cerium oxide, alumina, zirconium oxide) provides the mechanical grinding action required for polishing. The coupling agent (KH560 / KH570) forms an organic coating layer on the surface of the inorganic filler, improving the interfacial bonding force between the filler and the polyurethane matrix. The dispersant ensures the uniform dispersion of the filler in the system and prevents agglomeration.
[0024] Preferably, the surfactant is polydimethylsiloxane, which acts as an auxiliary surfactant to further reduce the surface tension of the system and promote the uniform dispersion of nanodroplets. The crosslinking agent is preferably trimethylolpropane, a trifunctional crosslinking agent that increases the chemical crosslinking density of the system and improves the elasticity and dimensional stability of the material.
[0025] This invention also provides a method for preparing the aforementioned all-water foamed polyurethane polishing pad, comprising the following steps: (1) Weigh each raw material of component A (polyol, chain extender, foaming agent, catalyst, surfactant, crosslinking agent, coupling agent, dispersant, and inorganic filler) according to the formula weight, and mechanically stir at a high speed of ≥4000r / min for 3 to 5 minutes to ensure that each component is fully mixed and uniform. The purpose of high-speed stirring is to uniformly disperse the nanodroplets and inorganic fillers in the continuous phase of polyol.
[0026] (2) Quickly add component B (polyisocyanate) to component A and mechanically stir at a speed of ≥4000 r / min for 30 to 60 seconds. At this stage, the foaming reaction begins to start, and the stirring time needs to be precisely controlled - too short a time will result in uneven mixing, and too long a time will result in excessive reaction and loss of fluidity, making it impossible to pour.
[0027] (3) Quickly pour the well-stirred mixture into an open mold with an inner anti-stick layer (such as a polytetrafluoroethylene film or a release agent coating), and allow it to foam freely for 1-3 minutes. The open mold design allows the foam to expand freely under unconstrained conditions, avoiding the constraint effect of the mold wall in closed mold foaming. The free foaming time refers to the time from the completion of pouring to the time when the foam volume reaches its maximum (bubble growth stops).
[0028] (4) After foaming, cure at 90-100℃ for 8-12 hours, and then cure at room temperature for 12-24 hours. The curing stage promotes the full cross-linking of the polyurethane network and the complete chemical anchoring reaction of the nano-droplet shell.
[0029] (5) The matured foam is sliced using a slicing machine to obtain a fully water-foamed polyurethane polishing pad of the required thickness.
[0030] The density of the polishing pad is 0.40–0.65 g / cm³. 3 The Shore A hardness is 75-90, the average pore diameter is 50-350μm, and the pore diameter distribution deviation is ≤20%.
[0031] It should be noted that the technical solution of this invention is based on a systematic analysis of the pore-forming mechanism of all-water foamed polyurethane and an innovative application of the confined foaming principle. The following is a detailed explanation from three aspects: theoretical basis, process mechanism, and synergistic effect. 1. In a conventional all-water foaming system, water molecules are uniformly dissolved in the polyurethane A / B mixture in a molecularly dispersed state. When the temperature rises, water reacts with isocyanate groups in the homogeneous system to form unstable carbamic acid, which then decomposes into amines and CO2. R-NCO + H2O → R-NH2 + CO2↑; The reaction occurs simultaneously throughout the system, and the concentration of CO2 molecules gradually increases. When the partial pressure of CO2 exceeds its saturated vapor pressure, the system enters a supersaturated state. According to the classical nucleation theory, bubble nucleation requires the emergence of a germ formed by concentration fluctuations in the system. Only when the radius of this germ exceeds the critical radius r can it spontaneously grow into a stable bubble nucleus. r = 2γ / ΔP; Where γ is the surface tension of the system and ΔP is the supersaturation pressure. Due to the microscopic differences in CO2 concentration, temperature and surface tension in different regions of the system, the critical nucleation conditions are not reached simultaneously in different places, resulting in asynchronous nucleation time and non-uniform nucleation density.
[0032] Once a critical bubble nucleus forms, bubble growth follows a diffusion-controlled mechanism. Small bubbles have high internal pressure (Laplace pressure ΔP = 2γ / r), while large bubbles have low internal pressure. Gas molecules tend to diffuse from small bubbles to large bubbles through the liquid phase (Ostwald ripening). Simultaneously, existing bubbles rise due to density differences, coalescing through collisions during this process. The combined result of these effects is a small number of large-sized bubbles with a wide size distribution.
[0033] In closed-mold foaming, the temperature gradient between the mold wall and the center further exacerbates this problem—the central region has a higher temperature due to the exothermic reaction, resulting in faster and larger cell growth and a significant structural gradient.
[0034] 2. This invention encapsulates water into independent microreactors by using nanodroplets, thereby altering the boundary conditions of the above-mentioned nucleation and growth processes.
[0035] (a) Pre-set nucleation mechanism Nanoparticles divide water into independent units ranging from 10 to 100 nm. The water content of each droplet nucleus is determined by the droplet volume (V0). droplet =4 / 3πr 3 Moisture content ∝ r 3 Because the nanodroplets are prepared through high-speed shear emulsification and size screening, the droplet size is monodisperse (dispersion coefficient <0.2), resulting in highly consistent water content in each droplet.
[0036] During the foaming process, isocyanate molecules must pass through the amino-modified polysiloxane shell from the continuous phase to enter the droplet core and react with water. Due to the mass transfer resistance of the shell, the reaction rate is controlled by shell diffusion rather than chemical reaction, which makes the reaction rate inside each droplet tend to be uniform.
[0037] The reaction inside each droplet can be described using a closed-system model: n(H2O)0-n(H2O) t =∫k·[NCO]·[H2O]dt; Where n(H2O)0 is the initial water volume of the droplet, k is the reaction rate constant, and [NCO] is the isocyanate concentration within the droplet. Since n(H2O)0 is consistent across all droplets, and the droplet sizes are the same, the reaction rate constant k also tends to be consistent across all droplets. Therefore, the amount of CO2 generated by each droplet at any time t is n(CO2). t They are approximately equal.
[0038] When the internal pressure of CO2 accumulates inside the droplet and reaches the critical rupture pressure P_c of the shell, the shell ruptures and releases CO2. Since the P_c values of each droplet vary slightly due to minor differences in shell thickness and cross-linking degree, but statistically follow a normal distribution, the shell rupture sequence is concentrated along the time axis, rather than randomly. This ensures the synchronicity of bubble nucleation time.
[0039] (b) The chemical nature of the interfacial anchoring effect The fundamental difference between amino-modified polysiloxane shells and conventional polysiloxane surfactants lies in their chemical reactivity. In the foaming system, the amino groups (-NH2) in the shell undergo a nucleophilic addition reaction with the excess isocyanate groups (-NCO) present in the polyurethane system: -NH2+OCN-R→-NH-CO-NH-R; The urea bonds generated in this reaction covalently link the polysiloxane molecular chains to the polyurethane network backbone. This chemical anchoring effect plays three key roles in the foaming process: Enhanced shell mechanical integrity: Chemical anchoring enables the shell molecular chains to form covalent cross-links with the polyurethane network, and the mechanical strength of the shell is improved from the level of physical cross-linking (hydrogen bonds, van der Waals forces) to chemical cross-linking, which significantly improves the shell's resistance to breakage and ensures that it can maintain its integrity before the internal pressure of CO2 accumulates to the design threshold.
[0040] Suppressing shell migration: In systems stabilized by conventional surfactants, surfactant molecules redistribute during foaming due to interfacial energy, disrupting the initially stable emulsion structure. Chemical anchoring fixes the shell molecular chains at their nucleation sites, suppressing migration.
[0041] Cell wall reinforcement: After the shell breaks down, the polysiloxane segments anchored to the polyurethane network remain in the cell wall. Strong hydrogen bonding (Si-O...HN) exists between the polysiloxane segments and the hard segments of the polyurethane, forming physical cross-linking points that enhance the mechanical properties of the cell wall.
[0042] (c) Mechanisms for eliminating Ostwald ripening The driving force for Ostwald ripening originates from the Laplace pressure difference between bubbles of different sizes. In this invention, due to the highly uniform droplet size and synchronized nucleation time, the initial bubble nuclei are nearly uniform in size, resulting in a minimal Laplace pressure difference and a significantly reduced driving force for Ostwald ripening. Furthermore, the polysiloxane segments anchored in the bubble walls form a dense interfacial film, reducing the permeability of gas molecules between the bubbles and further inhibiting gas diffusion.
[0043] (d) Mechanism without density gradient Open-mold free foaming combined with confined foaming is key to eliminating density gradients. In conventional foaming, the density gradient originates from the buoyancy and coalescence of bubbles—small bubbles rise and coalesce into larger bubbles, resulting in large pores and low density in the upper layer, and small pores and high density in the lower layer. In this invention, the nucleation sites for bubbles are predetermined by the spatial distribution of droplets, and the distribution of droplets in the system is determined by the uniform mixing of high-speed stirring, and does not change during the foaming process. Therefore, the distribution of bubbles in three-dimensional space is uniform, there is no bubble buoyancy and coalescence, and the density gradient is naturally eliminated.
[0044] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses amino-modified polysiloxane-coated water-in-oil nanodroplets to replace conventional deionized water as the blowing agent in the all-water foaming system. Combined with the confinement encapsulation technology in the nanodroplet preparation process and the chemical anchoring reaction mechanism between the shell amino and isocyanate groups during the foaming process, this invention solves the technical problems of wide cell size distribution and density and hardness gradients along the thickness direction in existing all-water foamed polyurethane polishing pads. This invention enables the preparation of all-water foamed polyurethane polishing pads with controllable cell structure and designable mechanical properties.
[0045] 2. This invention encapsulates water into independent microreactors using nanodroplets, transforming the random distribution of CO2 gas release sites into pre-defined nucleation sites, fundamentally solving the problem of uneven nucleation in all-water foaming. Experimental results show that the polishing pad prepared using this invention's confined foaming technology allows for adjustable pore sizes in its L1, L2, and L3 layers within a wide range from 230–310 μm (Example 1) to 110–140 μm (Example 2), with layer hardness ranging from 87 / 88 / 86A to 78 / 72 / 65A and density of 0.58 / 0.59 / 0.57 g / cm³. 3 Up to 0.41 / 0.49 / 0.43 g / cm³ 3 It can be designed to meet the specific needs of different polishing scenarios.
[0046] 3. This invention utilizes the chemical bonding reaction between the active amino groups of the amino-modified polysiloxane shell and the isocyanate groups to anchor the nanodroplet shell within the polyurethane network framework via urea bonds. This ensures the structural integrity of the shell during foaming and enhances the mechanical strength of the cell walls. Experimental results show that, under sufficient crosslinking density, the polishing pad using this invention exhibits a significant cell wall enhancement effect—that is, it maintains high hardness (87A) even with a large cell size (310 μm), breaking the inherent rule in conventional foaming that "large bubbles inevitably have low hardness."
[0047] 4. This invention utilizes an open-mold free-foaming process, avoiding the anisotropic structure caused by mold constraints in closed-mold foaming. This results in a polishing pad with no density or hardness gradient along its thickness direction, and a density deviation of ≤0.02g / cm³ between the upper, middle, and lower layers. 3 The Shore A hardness deviation is ≤2, and the TTV reaches 1.2μm, which meets the requirements for precision polishing.
[0048] 5. This invention ensures that the polishing pad has a uniform pore structure and consistent mechanical properties in three dimensions through the synergistic effect of three mechanisms: the monodisperse distribution of nanodroplet size, the inhibition of Ostwald curing by shell chemical anchoring, and the elimination of bubble buoyancy and aggregation by free foaming process.
[0049] 6. When used for polishing microcrystalline glass, this invention achieves a total thickness variation (TTV) ≤ 1.5 μm, a scratch count ≤ 2 scratches / piece, and a material removal rate consistently between 0.52 and 0.78 μm / min, meeting the requirements for precision polishing. 3M's Trizact™ series of polishing pads claims performance indicators including low total thickness variation (TTV) and high removal rate; the TTV and removal rate of this invention are at the same level as industrial-grade products.
[0050] 7. This invention uses an all-water foaming system, which does not contain organic foaming agents or chemical foaming agent decomposition residues, and has no VOC emissions, meeting the requirements of green manufacturing. Attached Figure Description
[0051] Figure 1 The image shows the microstructure of the all-water foamed polyurethane polishing pad prepared in Example 1 of this invention. Figure 2 The image shows the microstructure of the foamed polyurethane polishing pad prepared in Example 2 of this invention. Figure 3 Microscopic morphology of the all-water foamed polyurethane polishing pad prepared for Comparative Example 1. Figure 4 This is a comparison diagram of the Shore A hardness distribution along the thickness direction of Examples 1 and 2 and Comparative Example 1; Figure 5 This is a comparison diagram of the density distribution along the thickness direction of Examples 1 and 2 and Comparative Example 1. Detailed Implementation
[0052] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0053] The raw materials used in the following experiments of this invention are all known products, obtained by purchasing commercially available products. Among them: Diethylene glycol-based polyoxypropylene ether polyol: industrial grade, hydroxyl value 56 mgKOH / g, number average molecular weight approximately 2000, functionality 2; Poly(propylene oxide) ether diol: industrial grade, hydroxyl value 112 mgKOH / g, number average molecular weight approximately 1000, functionality 2; Polytetramethylene ether glycol: industrial grade, hydroxyl value 56 mgKOH / g, number average molecular weight approximately 2000, functionality 2; Isophorone diisocyanate (IPDI): Industrial grade, purity ≥99.5%, NCO content ≥37.5%; Polymethylene polyphenyl isocyanate (PAPI): Industrial grade, NCO content 30.5-32.0%, average functionality 2.7; Diphenylmethane diisocyanate (MDI): Industrial grade, purity ≥99.5%, NCO content ≥33.5%; Amino-modified polysiloxane: industrial grade, amine value 0.5 mmol / g, viscosity 200 mPa·s (25℃), aminopropyl side chain modified; 1,4-Butanediol (BDO): Analytical grade, purity ≥99.5%; Ethylene glycol (EG): analytical grade, purity ≥99.5%; Diethylene glycol (DEG): analytical grade, purity ≥99.0%; Triethylenediamine (TEDA): Industrial grade, purity ≥99%; N,N-Dimethylcyclohexylamine: Industrial grade, purity ≥98%; Dibutyltin dilaurate (DBTDL): Industrial grade, tin content 17-19%; Stannous octoate: Industrial grade, tin content ≥28%; Polydimethylsiloxane: Industrial grade, viscosity 350 mPa·s (25℃); Trimethylolpropane (TMP): Industrial grade, purity ≥98%; Triethanolamine: Industrial grade, purity ≥98%; KH560: γ-glycidyl etheroxypropyltrimethoxysilane, industrial grade, purity ≥97%; KH570: γ-Methacryloxypropyltrimethoxysilane, industrial grade, purity ≥97%; BYK-P104S: Polymer dispersant, BYK Corporation; BYK-9076: Polymer dispersant, BYK Corporation; BYK-2163: Polymer dispersant, BYK Corporation; Cerium oxide: average particle size 1.5 μm, purity ≥99.9%; Alumina: average particle size 2.0 μm, purity ≥99.5%; Zirconia: average particle size 1.0 μm, purity ≥99.5%; Silicone oil DC193: a non-reactive polysiloxane surfactant with a viscosity of approximately 500 mPa·s (25°C). Polypropylene triol (N-330): Industrial grade, hydroxyl value 56 mgKOH / g, number average molecular weight approximately 3000, functionality 3; In addition, the preparation process of amino-modified polysiloxane-coated nanodroplets: Amino-modified polysiloxane (amine value 0.5 mmol / g, viscosity 200 mPa·s) was dissolved in ethyl acetate to prepare a 5% (w / w) oil phase solution. Deionized water and NaCl were mixed at a mass ratio of 100:0.5 to form the aqueous phase. The aqueous phase was slowly added dropwise to the oil phase at a volume ratio of 1:10 using a high-speed shear emulsifier with stirring at 12000 r / min. After the addition was complete, emulsification continued for 10 minutes. The resulting emulsion was transferred to a rotary evaporator, and ethyl acetate was removed by vacuum distillation at 50°C, yielding amino-modified polysiloxane-coated nanodroplets with a solid content of approximately 10% and an average particle size of approximately 80 nm. This invention first needs to verify the feasibility of using water-in-silicone nanodroplets as a novel foaming agent instead of water; therefore, only one preparation process was established.
[0054] Example 1. Preparation of all-water foamed polyurethane polishing pad: Raw material formula: 200g of diethylene glycol-based polypropylene oxide polyol, 200g of polypropylene oxide diol, 10g of 1,4-butanediol, 2g of amino-modified polysiloxane-coated nanodroplets (10% solid content), 0.5g of 33% triethylenediamine + 67% dipropylene glycol, 0.3g of dibutyltin dilaurate, 0.5g of polydimethylsiloxane, 5g of trimethylolpropane, 10g of KH560, 20g of BYK-P104S, 200g of cerium oxide, 200g of isophorone diisocyanate, and 100g of polymethylene polyphenyl isocyanate.
[0055] Preparation method: Weigh out all raw materials of component A (polyol, chain extender, foaming agent, catalyst, surfactant, crosslinking agent, coupling agent, dispersant, and inorganic filler) according to the formula, and stir in a dispersion tank at 4500 r / min for 3 minutes until uniform; quickly add component B (isophorone diisocyanate and polymethylene polyphenyl isocyanate), and stir at 4500 r / min for 40 seconds; quickly pour into an open stainless steel mold (300mm×300mm×100mm) lined with polytetrafluoroethylene film, and allow it to foam freely for about 2 minutes; place it in a 95℃ oven to cure for 10 hours, and then let it mature at room temperature for 18 hours; use a slicing machine to slice the foam into sheets with a thickness of 2.0mm.
[0056] The performance characteristics of the polishing pad prepared in this embodiment are as follows: Reference Figure 1 Regarding the cell size, the average cell diameter of the L1 layer (upper layer) is 310 μm, that of the L2 layer (middle layer) is 260 μm, and that of the L3 layer (lower layer) is 230 μm. The cell size of the three layers decreases from top to bottom, but the overall distribution deviation is 16%, indicating that the cell size is relatively concentrated in a statistical sense.
[0057] Reference Figure 4 In terms of hardness, the Shore A hardness of layer L1 is 87, layer L2 is 88, and layer L3 is 86, with the three layers having almost identical hardness (deviation ≤2). In terms of density, layer L1 has a density of 0.58 g / cm³. 3 The L2 layer has a concentration of 0.59 g / cm³. 3 The L3 layer has a concentration of 0.57 g / cm³. 3 The three layers have almost identical densities (deviation ≤ 0.02 g / cm³). 3 ).
[0058] Reference Figure 5 In terms of mechanical properties, the tensile strength is 15.8 MPa, the compressive strength is 4.5 MPa, and the wear loss is 16.5 mg. In terms of polishing performance, the TTV is 1.5 μm, the number of scratches is 1 per piece, and the material removal rate (RR) is 0.52 μm / min.
[0059] In this embodiment, although the cell size of the L1 layer reaches 310 μm, the hardness is as high as 87A. This seemingly anomalous phenomenon precisely verifies the effectiveness of the core mechanism of this invention. In conventional polyurethane foaming, cell size and hardness are usually negatively correlated—the larger the cell size, the less polymer backbone per unit volume, and the lower the hardness. However, this embodiment uses amino-modified polysiloxane nanodroplet confined foaming technology. During the foaming process, the amino groups (-NH2) of the nanodroplet shell react with the isocyanate groups (-NCO) to form urea bonds, covalently anchoring the polysiloxane segments to the polyurethane network backbone. These polysiloxane segments form nanoscale reinforcing phases within the cell walls, forming physical crosslinking points through Si-O...HN hydrogen bonding, which significantly improves the intrinsic strength of the cell walls. Therefore, despite the large cell size, the load-bearing capacity of the cell walls is sufficient to compensate for the strength loss caused by the increased cell size, resulting in an increase in hardness instead of a decrease.
[0060] The three layers exhibit a high degree of density uniformity (0.58 / 0.59 / 0.57 g / cm³). 3This indicates that the confined foaming of nanodroplets pre-fixes the CO2 release sites, and the pores are uniformly distributed in the system, eliminating the density gradient caused by bubble buoyancy and aggregation in conventional foaming. Literature reports that conventional all-water foamed polishing pads often have a lower density in the upper layer than in the lower layer due to the bubble buoyancy effect (e.g., 0.35 for the upper layer and 0.55 for the lower layer in Comparative Example 1). This embodiment effectively suppresses this phenomenon through the confined foaming mechanism.
[0061] Example 2. Preparation of all-water foamed polyurethane polishing pad: Raw material formula: 200g diethylene glycol-based polypropylene oxide ether polyol, 250g polypropylene oxide ether diol, 10g 1,4-butanediol, 3g amino-modified polysiloxane-coated nanodroplets (10% solid content), 0.5g 33% triethylenediamine + 67% dipropylene glycol, 0.3g dibutyltin dilaurate, 0.5g polydimethylsiloxane, 5g trimethylolpropane, 10g KH560, 20g BYK-P104S, 200g cerium oxide, 200g isophorone diisocyanate, 150g polymethylene polyphenyl isocyanate.
[0062] The preparation method is the same as in Example 1.
[0063] The performance characteristics of the polishing pad prepared in this embodiment are as follows: Reference Figure 2 Regarding cell size, the average cell diameter of L1 layer is 110μm, L2 layer is 130μm, and L3 layer is 140μm. The cell size of the three layers increases from top to bottom, with a distribution deviation of 18%.
[0064] Reference Figure 4 In terms of hardness, the Shore A hardness of layer L1 is 78, layer L2 is 72, and layer L3 is 65, showing a decreasing trend from top to bottom (deviation 13). In terms of density, layer L1 has a density of 0.41 g / cm³. 3 The L2 layer has a concentration of 0.49 g / cm³. 3 The L3 layer has a concentration of 0.43 g / cm³. 3 The middle layer is the highest, and the upper and lower layers are the lowest.
[0065] Reference Figure 5 In terms of mechanical properties, the tensile strength is 12.5 MPa, the compressive strength is 3.0 MPa, and the wear loss is 9.8 mg. In terms of polishing performance, the TTV is 1.2 μm, the number of scratches is 2 per piece, and the material removal rate (RR) is 0.78 μm / min.
[0066] Example 3. Preparation of all-water foamed polyurethane polishing pad: Raw material formula: 250g polytetramethylene ether glycol (Mn≈2000), 150g diethylene glycol-based polypropylene oxide ether polyol, 12g ethylene glycol, 4g amino-modified polysiloxane-coated nanodroplets (10% solid content), 0.4g N,N-dimethylcyclohexylamine, 0.3g stannous octoate, 0.6g polydimethylsiloxane, 4g triethanolamine, 12g KH570, 18g BYK-9076, 220g alumina (average particle size 2μm), 180g diphenylmethane diisocyanate, and 120g polymethylene polyphenyl isocyanate.
[0067] The preparation method is the same as in Example 1.
[0068] Example 4. Preparation of all-water-foamed polyurethane polishing pad: Raw material formula: 300g of polyoxypropylene ether diol (Mn≈1000), 100g of diethylene glycol-based polyoxypropylene ether polyol, 15g of diethylene glycol, 1.5g of amino-modified polysiloxane-coated nanodroplets (10% solid content), 0.3g of bis(2-dimethylaminoethyl) ether, 0.4g of dibutyltin dilaurate, 0.8g of polydimethylsiloxane, 6g of trimethylolpropane, 15g of KH560, 20g of BYK-2163, 250g of zirconium oxide (average particle size 1μm), 250g of isophorone diisocyanate, and 80g of polymethylene polyphenyl isocyanate.
[0069] The preparation method is the same as in Example 1.
[0070] Comparative Example 1 (Conventional all-water foaming, without the use of nano-droplets): Raw material formula: Polypropylene triol (N-330, Mn≈3000) 300g, ethylene glycol 12g, deionized water 6g, 33% triethylenediamine + 67% dipropylene glycol 6g, dibutyltin dilaurate 0.75g, silicone oil DC193 9g, triethanolamine 6g, cerium oxide 69g, diphenylmethane diisocyanate 240g.
[0071] The preparation method is the same as in Example 1, but deionized water is used directly as the foaming agent instead of nanodroplets.
[0072] The performance characteristics of the polishing pad prepared in this comparative example are as follows: Reference Figure 1 Regarding the cell size, the average cell diameter of the L1 layer is 1520μm, that of the L2 layer is 270μm, and that of the L3 layer is 110μm, showing an extreme gradient that decreases sharply from top to bottom, with a distribution deviation of several times.
[0073] Reference Figure 4In terms of hardness, the Shore A hardness of layer L1 is 35, layer L2 is 45, and layer L3 is 87, showing an extreme gradient with a sharp increase from top to bottom (deviation 52). In terms of density, layer L1 has a density of 0.35 g / cm³. 3 The L2 layer has a concentration of 0.42 g / cm³. 3 The L3 layer has a concentration of 0.55 g / cm³. 3 It exhibits a significant gradient increasing from top to bottom (deviation 0.20 g / cm). 3 ).
[0074] Reference Figure 5 In terms of mechanical properties, the tensile strength is 2.1 MPa, the compressive strength is 0.5 MPa, and the wear loss is 83.2 mg. In terms of polishing performance, the TTV is 5.8 μm, the number of scratches is 11 per piece, and the material removal rate (RR) is 0.09 μm / min.
[0075] This comparative example employs a conventional all-water foaming process, where water molecules are uniformly dissolved in the polyurethane system in a molecular-level dispersion state. During the foaming process, the CO2 generated from the reaction of water and isocyanate undergoes homogeneous nucleation within the system. Due to microscopic differences in CO2 concentration, temperature, and surface tension across different regions of the system, the critical nucleation conditions are not reached simultaneously, resulting in asynchronous nucleation times and non-uniform nucleation densities. Driven by density differences, the nucleated bubbles rise upwards, merging through collisions during this process, with smaller bubbles coalescing into larger ones. Simultaneously, the Ostwald ripening effect causes gas molecules from smaller bubbles to diffuse through the liquid phase into larger bubbles, further exacerbating the widening of the pore size distribution. Therefore, conventional all-water foaming inevitably produces significant gradients in pore size, hardness, and density.
[0076] Comparative Example 2 (Nanodroplet shell using non-reactive polysiloxane): The raw material formulation is the same as in Example 1, but the amino-modified polysiloxane is replaced with an equal amount of non-reactive polydimethylsiloxane (amino-free, viscosity 200 mPa·s) to prepare nanodroplets.
[0077] The preparation method is the same as in Example 1.
[0078] Comparative Example 3 (Nanodroplet dosage below the lower limit: 0.5 parts): The raw material formula is the same as in Example 1, but the amount of nanodroplets is adjusted to 0.2g.
[0079] The preparation method is the same as in Example 1.
[0080] Comparative Example 4 (Nanodroplet dosage exceeds the upper limit: 5 parts): The raw material formula is the same as in Example 1, but the amount of nanodroplets is adjusted to 8g.
[0081] The preparation method is the same as in Example 1.
[0082] Comparative Example 5 (Amount of Component A below the lower limit: 30 parts): The total amount of polyol in component A of the raw material formula was adjusted to 20g (i.e., 10g of diethylene glycol-based polypropylene oxide ether polyol and 10g of polypropylene oxide ether diol), and the rest was the same as in Example 1.
[0083] The preparation method is the same as in Example 1.
[0084] Comparative Example 6 (Component B dosage was less than the lower limit of 30 parts): The total amount of isocyanate in component B of the raw material formula was adjusted to 25g (i.e., 15g of isophorone diisocyanate and 10g of polymethylene polyphenyl isocyanate), and the rest was the same as in Example 1.
[0085] The preparation method is the same as in Example 1.
[0086] The products from Examples 1-4 and Comparative Examples 1-6 were subjected to the following tests: Cell morphology observation: The cell morphology of each group of samples was observed using an optical microscope (Olympus BX51, Japan) at a magnification of 100×. The average cell diameter and distribution deviation were statistically analyzed using Image-Pro Plus image analysis software, with no fewer than 200 cells counted for each sample.
[0087] Hardness test: Refer to GB / T 531.1-2008, use LX-A type Shore hardness tester to test the Shore A hardness of the upper, middle and lower layers of the sample, and take 5 test points for each layer and take the average value.
[0088] Density test: Referring to GB / T 533-2008, the density of the upper, middle and lower layers of the sample was tested using the water displacement method. Three parallel samples were tested in each group and the average value was taken.
[0089] Tensile strength test: Refer to GB / T 528-2009, use a universal testing machine (Instron 5967), the specimen is dumbbell-shaped (length 25mm), the tensile rate is 50mm / min, and the average value of 5 parallel samples in each group is taken.
[0090] Compressive strength test: Refer to GB / T 8813-2008, use a universal testing machine, sample size 20mm×20mm×10mm, compression rate is 3mm / min, the stress when compressed to 50% deformation is recorded as compressive strength, and the average value of 5 parallel samples in each group of tests is taken.
[0091] Wear test: Take a sample with a diameter of 110mm and a thickness of 3.0mm and test the wear using a Taber abrasion tester (Taber 5135). Use an H-18 ceramic grinding wheel with a load of 1kg and rotate it 3000 times at 40rpm. Weigh the sample and the mass loss is the wear amount.
[0092] TTV Test: The microcrystalline glass was polished using a double-sided polishing machine (Hunan Mowang). Polishing conditions were: cerium oxide polishing solution (particle size 1.1μm, density 1.8g / mL, pH 7.3), lower plate rotation speed 35rpm, upper plate rotation speed 15rpm, polishing solution flow rate 1200mL / min, and polishing time 30min. After polishing and cleaning the glass cover, the thickness was measured using a dial indicator (Mitutoyo, accuracy 1μm). TTV = T max -T min .
[0093] Scratch test: After polishing, the sample is placed in a standard light source box (NHKU HL-DFL-F280CH, Japan) and observed from multiple angles at a distance of 30-40cm from the product. Bright lines longer than 2cm are judged as scratches, and the number of scratches for each piece is recorded.
[0094] RR (Material Removal Rate): RR = (H0 - H1) / T, where H0 is the initial thickness of the polished workpiece (μm), H1 is the thickness of the workpiece after polishing (μm), and T is the polishing time (min).
[0095] Table 1. Structural characteristics of each group of all-water-foamed polyurethane polishing pads
[0096] Note: In Comparative Example 5, due to a severe deficiency of component A, the crosslinking density of the system was too high, severely limiting cell growth and preventing the formation of an effective porous structure. Most areas were in a dense state, so the cell diameter could not be accurately measured.
[0097] Table 2. Performance test results of each group of all-water foamed polyurethane polishing pads
[0098] Data Analysis: 1. The effect of confined foaming of nanodroplets on cell uniformity: Comparing Examples 1-4 (distribution deviation 16%-19%) with Comparative Example 1 (distribution deviation several times greater), confined foaming significantly improves the uniformity of cell structure. The mechanism can be understood from classical nucleation theory.
[0099] In conventional all-water foaming (Comparative Example 1), the bubble nucleation rate J is controlled by the following formula: J=A·exp(-16πγ 3 / (3kT·ΔP2 )); Where γ is the surface tension of the system, and ΔP is the CO2 supersaturation pressure. Due to the microscopic differences in CO2 concentration, temperature, and surface tension in different regions of the system, ΔP is non-uniformly distributed in space and time. Small fluctuations in ΔP cause J to change exponentially, resulting in nucleation rates that differ by several orders of magnitude. After nucleation, the bubbles rise under the drive of density difference, and the rising velocity v is determined by Stokes' law: v=(ρ matrix -ρ gas )·g·r 2 / (18η); The larger the bubble radius r, the faster it rises. During the rising process, larger bubbles continuously engulf smaller bubbles, forming a positive feedback loop of pursuit-coalescence. Ultimately, this causes the L1 layer bubbles to expand rapidly to 1520 μm, while the L3 layer is only 110 μm.
[0100] In this invention, nanodroplets separate water into independent microreactors, and the water content of each droplet (∝r) 3 The high degree of uniformity in isocyanate molecule diffusion across the shell ensures a consistent reaction rate within each droplet, resulting in a high degree of overlap in CO2 generation curves across the droplets on the time axis. Nucleation sites are predetermined by the spatial distribution of the droplets. The number of pores N and the concentration of nanodroplets C are related. droplet Directly related: N≈C droplet ·V system ·η nucleation ; Where η nucleation The nucleation efficiency is approximately 1, meaning each droplet forms one bubble. Each bubble is uniformly anchored in three-dimensional space, with no buoyancy, and the density gradient is eliminated at the source.
[0101] 2. The effect of chemical anchoring on mechanical properties: Comparing Example 1 (tensile strength 15.8 MPa, compressive strength 4.5 MPa) with Comparative Example 2 (tensile strength 3.8 MPa, compressive strength 0.9 MPa), the contribution of amino chemical reactivity to mechanical properties can be quantified: tensile strength increased by 315% and compressive strength increased by 400%.
[0102] Its mechanism can be understood from the interfacial shear strength τ: τ=σ f ·(d / 4l); Where σ fThe term represents the segment fracture strength of the polysiloxane, where d is the segment diameter and l is the interface length. In Example 1, the amino group reacts with the isocyanate to form a urea bond (-NH-CO-NH-), and the interface length l is equal to the chemical bond length (on the order of ~0.15 nm), allowing for efficient load transfer through covalent bonds. In Comparative Example 2, the non-reactive polysiloxane is adsorbed onto the matrix solely by van der Waals forces, with an interface length l equal to the thickness of the physical adsorption layer (on the order of ~1 nm), resulting in an interfacial shear strength that is more than an order of magnitude lower. This difference in load transfer efficiency directly determines the failure mode of the cell walls under stress—Example 1 shows ductile fracture within the polyurethane matrix, while Comparative Example 2 shows brittle fracture due to interfacial debonding.
[0103] 3. Control of bubble size by formulation parameters: The cell sizes of Example 1 (cell size 310 / 260 / 230μm) and Example 2 (cell size 110 / 130 / 140μm) differ by about 2 to 3 times. The main reason for this is the difference in the NCO / OH equivalent ratio.
[0104] Calculated based on the formula: Example 1: The total amount of hydroxyl groups in component A = 200g / 2000×2 + 200g / 1000×2 = 0.2 + 0.4 = 0.6 mol. In component B, the amount of NCO in IPDI = 200 / 222.3×2 ≈ 1.80 mol (222.3 is the molecular weight of IPDI), and the amount of NCO in PAPI = 100 / approximately 340×2.7 ≈ 0.79 mol (340 is the average molecular weight of PAPI, and 2.7 is the average functionality). The total amount of NCO in component B ≈ 2.59 mol. NCO / OH = 2.59 / 0.6 ≈ 4.32.
[0105] Example 2: The total amount of hydroxyl groups in component A = 200 / 2000 × 2 + 250 / 1000 × 2 = 0.2 + 0.5 = 0.7 mol. In component B, the amount of NCO in IPDI = 200 / 222.3 × 2 ≈ 1.80 mol, and the amount of NCO in PAPI = 150 / 340 × 2.7 ≈ 1.19 mol. The total amount of NCO in component B ≈ 2.99 mol. NCO / OH = 2.99 / 0.7 ≈ 4.27.
[0106] The NCO / OH equivalent ratios of the two embodiments were almost identical (4.32 vs 4.27), so the large difference in cell size could not be attributed to the NCO / OH equivalent ratio.
[0107] Therefore, the core reason for the difference in pore size lies in the difference in the amount of total hydroxyl content, which determines the theoretical CO2 production. The reaction between water and isocyanate is: R-NCO + H2O → R-NH2 + CO2↑. Each mole of water produces 1 mole of CO2 gas. The water content of the nanodroplets in Examples 1 and 2 is different: the amount of nanodroplets used in Example 1 is 2g (solid content 10%, water content 1.8g = 0.1mol), and in Example 2 it is 3g (water content 2.7g = 0.15mol).
[0108] Theoretical CO2 production: Example 1: 0.1 mol × 22.4 L / mol ≈ 2.24 L; Example 2: 0.15 mol × 22.4 L / mol ≈ 3.36 L. The production differs by 50%. With a comparable number of nucleation sites (nanodroplet amounts of 2 g and 3 g respectively, a 50% difference), the amount of CO2 distributed per unit nucleation site determines the final pore size.
[0109] However, it should be noted that larger or smaller bubble size is not necessarily better; rather, it depends on performance requirements. Example 1: High gas production → Large bubble size (approximately 300μm) → High density (0.58g / cm³). 3 High hardness (87A) → Suitable for polishing applications requiring high hardness. Example 2: Low gas production → Small pore size (approximately 100μm) → Low density (0.41g / cm³). 3 → Moderate hardness (78A) → Suitable for polishing scenarios that require high softness and fit.
[0110] 4. Effect of nanodroplet dosage on pore structure: Comparative Example 1 (2g nanodroplets, pore size 310 / 260 / 230μm) with Comparative Example 3 (0.2g, pore size 430 / 380 / 320μm) and Comparative Example 4 (8g, pore size 75 / 65 / 55μm): The amount of nanodroplets used determines the nucleation site density N∝C droplet When the total CO2 production V CO2 At a given time, the average bubble volume V cell =V CO2 / N. In Comparative Example 3, N is too small, V cell If the pore size is too large (pore size > 400 μm) and the droplet spacing is too large (> 500 μm), a uniform array cannot be formed. In Comparative Example 4, N is too large, and V... cell The size was too small (pore size <100μm), but the excessive polysiloxane shell produced a plasticizing effect, the pore wall became thinner, and the wear amount increased from 16.5mg in Example 1 to 32.5mg.
[0111] 5. Effect of components A / B on mechanical properties: Comparative Example 5 (A=20g) showed an NCO / OH ratio of approximately 12.96 (significantly greater than 1), indicating a severe excess of isocyanate. After all hydroxyl groups reacted, the remaining NCO groups reacted with water to generate a large number of urea groups and biuret crosslinks, resulting in an excessively high crosslinking density (hardness 92A). Cell growth was limited by the excessive rigidity of the cell walls, preventing them from fully extending.
[0112] Comparative Example 6 (B=25g) showed an NCO / OH ratio of approximately 0.43 (far less than 1), indicating a severe excess of hydroxyl groups. The polyurethane chains terminated at the hydroxyl groups, resulting in extremely low crosslinking density (hardness 38–45A). The foaming reaction was incomplete, leaving a large amount of unreacted hydroxyl groups.
[0113] The TTV values of the two ratios reached 4.8 μm and 6.8 μm, respectively, neither of which met the requirements for precision polishing. This indicates that the ratio of components A / B must be within a reasonable range (30-50 parts in this invention) to obtain the optimal balance between crosslinking density and foaming behavior.
[0114] 6. Overall structure-property relationship of polishing performance: The TTV is determined by the isotropic compressive modulus of the polishing pad. In Example 1, the three layers with hardness of 87 / 88 / 86A are almost identical, the compressive modulus of each region is uniform, the contact pressure is evenly distributed, and the TTV is only 1.5μm.
[0115] The compression modulus (RR) is determined by the Preston equation RR = Kp·P·V. In Comparative Example 1, the compressive modulus is too low and unstable, resulting in drastic fluctuations in contact conditions and an RR of only 0.09 μm / min. In Examples 1–4, the RR is stable between 0.52 and 0.78 μm / min.
[0116] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A fully water-foamed polyurethane polishing pad, characterized in that, It is prepared from raw materials comprising the following parts by weight: 30-50 parts of polyol component A; 30-50 parts of polyisocyanate component B; Chain extender 1-3 parts; 0.5 to 5 parts of foaming agent; Amine catalyst, 0.01–0.06 parts; Organotin catalyst, 0.01–0.06 parts; Surfactant 0.01 to 0.1 parts; Crosslinking agent 0.1 to 1 part; 20-30 parts of inorganic filler; 1-3 parts coupling agent; 1-3 parts dispersant; The foaming agent is an oil-in-water nanodroplet coated with amino-modified polysiloxane.
2. The all-water foamed polyurethane polishing pad according to claim 1, characterized in that, The preparation process of the amino-modified polysiloxane-coated nanodroplets includes the following steps: (1) Dissolve the amino-modified polysiloxane in a volatile organic solvent to prepare an oil phase solution with a mass fraction of 1% to 10%; (2) Deionized water is used as the aqueous phase, in which electrolytes accounting for 0.1% to 1% of the mass of the aqueous phase are dissolved; (3) Slowly add the aqueous phase to the oil phase, with a volume ratio of 1:5 to 1:20 between the aqueous and oil phases, and emulsify in a high-speed shear emulsifier at a speed of 8000 to 15000 r / min for 5 to 20 minutes to form a water-in-oil type primary emulsion. (4) Remove the organic solvent by vacuum distillation at 40-60℃ to obtain amino-modified polysiloxane-coated nanodroplets; The amino-modified polysiloxane has an amine value of 0.2–1.0 mmol / g and a viscosity of 50–500 mPa·s at 25°C.
3. The all-water foamed polyurethane polishing pad according to claim 1, characterized in that, The polyol component A is a polyether-type polyol or a polyester-type polyol with a functionality of 2, a molecular weight of 1000-3000, and a hydroxyl value of 50-400 mg KOH / g; the polyether-type polyol is one or more of polytetramethylene ether diol, diethylene glycol-based polyoxypropylene ether polyol, and polyoxypropylene ether diol.
4. The all-water foamed polyurethane polishing pad according to claim 1, characterized in that, The polyisocyanate component B is selected from one or more of diphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, and isophorone diisocyanate.
5. The all-water foamed polyurethane polishing pad according to claim 1, characterized in that, The chain extender is any one of 1,4-butanediol, ethylene glycol, and diethylene glycol; the amine catalyst is one or more of triethylenediamine, N,N-dimethylcyclohexylamine, and bis(2-dimethylaminoethyl) ether; and the organotin catalyst is dibutyltin dilaurate or stannous octoate.
6. The all-water foamed polyurethane polishing pad according to claim 1, characterized in that, The inorganic filler is any one of cerium oxide, alumina, and zirconium oxide, with an average particle size of 0.5–5 μm; the coupling agent is KH560 or KH570; and the dispersant is BYK-P104S, BYK-9076, or BYK-2163.
7. The method for preparing the all-water foamed polyurethane polishing pad according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Weigh each raw material of component A according to the formula weight, mix them and then mechanically stir at a speed of ≥4000r / min for 3 to 5 minutes; (2) Quickly add component B to component A and mechanically stir at a speed of ≥4000 r / min for 30 to 60 seconds; (3) Pour the well-stirred mixture into an open mold with an anti-stick layer on the inside, and allow it to foam freely for 1 to 3 minutes; (4) After foaming, cure at 90-100℃ for 8-12 hours, and then cure at room temperature for 12-24 hours; (5) The matured foam is sliced using a slicing machine to obtain the all-water foamed polyurethane polishing pad.
8. The preparation method according to claim 7, characterized in that, The density of the obtained all-water-blown polyurethane polishing pad is 0.40–0.65 g / cm³. 3 The Shore A hardness is 75-90, the average pore diameter is 50-350, and the pore diameter distribution deviation is ≤20%.
Citation Information
Patent Citations
Polishing pad, method for manufacturing same, and polishing method using same
CN112571303A
Classification equipment and polishing pad
CN116262330A
Method of fabricating polyurethane foam with micro pores and polishing pad therefrom
CN1738845A
Polyurethane foam for polishing sheet and method for producing the same, polishing sheet for polishing pad, and polishing pad