A bio-based vanillin epoxy resin and its preparation method
By synthesizing vanillin glycidyl ether from vanillin and epichlorohydrin and reacting it with terminal aminosiloxane, bio-based vanillin epoxy resin was prepared. This solved the problems of difficult recycling and complex synthesis routes of thermosetting epoxy resins, and achieved epoxy resin materials with high reactivity, excellent mechanical properties and good solvent resistance.
Patent Information
- Application Number
- CN202611515106.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing thermosetting epoxy resins are difficult to recycle and have complex synthesis routes. They are also scarce in resources and cause serious environmental pollution, which limits their sustainable development and application potential.
Vanillin glycidyl ether was synthesized using vanillin and epichlorohydrin as raw materials, and then reacted with terminal aminosiloxane to introduce imine bonds. The resulting product was cured with curing agent APBAI in a one-pot process to prepare bio-based vanillin epoxy resin.
The prepared bio-based vanillin epoxy resin has a lower curing activation energy, high reactivity, excellent mechanical properties and reprocessing properties. After three cycles, the tensile strength and elongation at break remain above 93%, and it has good thermal stability and excellent solvent resistance.
Smart Images

Figure CN123107041A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of epoxy resins, specifically relating to a bio-based vanillin epoxy resin and its preparation method. Background Technology
[0002] Thermosetting epoxy resins, due to their permanently cross-linked network structure, exhibit excellent mechanical properties, thermal stability, dimensional stability, and solvent resistance, and have been widely used in composite materials, aerospace, and coatings. However, the sustainable development of this type of material is facing severe challenges. On the one hand, over 90% of thermosetting epoxy resins are cured from petroleum-based bisphenol A type epoxy resins, and this over-reliance on fossil resources is leading to increasingly prominent resource scarcity problems. On the other hand, cured thermosetting epoxy resin waste is difficult to degrade and recycle, causing not only serious environmental pollution but also enormous resource waste.
[0003] To promote the sustainable development of thermosetting epoxy resins, researchers are mainly conducting research in two directions: first, designing and synthesizing thermosetting bio-based epoxy resins to alleviate the shortage of petroleum resources; and second, preparing epoxy-based glass polymers with both ductility and recyclability by introducing dynamic covalent bonds such as ester bonds, imine bonds, disulfide bonds, and siloxane bonds. However, the high-performance bio-based epoxy monomers reported in the literature usually require lengthy and complex synthetic routes, which limits their economic benefits and practical application potential.
[0004] Therefore, how to design and develop epoxy glass polymers that combine reprocessability, recyclability, flame retardancy, and excellent comprehensive properties using inexpensive and readily available renewable raw materials has become a key issue in promoting the sustainable development of thermosetting epoxy resins and expanding their application areas. Summary of the Invention
[0005] The purpose of this invention is to overcome the above-mentioned technical deficiencies and provide a bio-based vanillin epoxy resin and its preparation method, thereby solving the technical problems of the difficulty in recycling or the complexity of the synthesis route of thermosetting epoxy resins prepared in the prior art.
[0006] To achieve the above-mentioned technical objectives, the technical solution provided by this invention is as follows: In a first aspect, the present invention provides a method for preparing a bio-based vanillin epoxy resin, comprising the following steps: S1, using vanillin and epichlorohydrin as raw materials, a synthesis reaction is carried out to obtain vanillin glycidyl ether; S2, the vanillin glycidyl ether is reacted with a terminal aminosiloxane in an organic solvent under reflux to obtain an epoxy resin reaction system with imine bonds; S3, the epoxy resin reaction system with imine bonds is cooled to room temperature, a curing agent is added and mixed evenly, and then subjected to solvent removal treatment and hot pressing curing to obtain a bio-based vanillin epoxy resin.
[0007] Secondly, the present invention provides a bio-based vanillin epoxy resin prepared by the above preparation method.
[0008] Compared with the prior art, the beneficial effects of the present invention include: This invention uses vanillin and epichlorohydrin as raw materials to synthesize vanillin glycidyl ether, which is then reacted with a terminal aminosiloxane (BAPT) to introduce imine bonds into the epoxy resin system. The resulting bio-based vanillin epoxy resin is obtained through a one-pot curing process with a curing agent. Compared with traditional E51 epoxy resin and thermosetting materials cured with APBAI curing agent, the bio-based vanillin epoxy resin obtained by this invention has a lower curing activation energy, higher reactivity, and superior mechanical properties. It also exhibits excellent reprocessing performance, with tensile strength and elongation at break remaining above 93% after three cycles; and demonstrates excellent thermal stability. T 5% =302℃, the carbon residue rate is 52.7% at 800℃; it also has good solvent resistance and excellent overall performance. Attached Figure Description
[0009] Figure 1 These are the 1H NMR spectrum (a) and 1C NMR spectrum (b) of VE in Example 1 of this invention. Figure 2 ln(β / T) plotted based on Kissinger equation and Ozawa equation respectively 2 p ) and lnβ with 1 / T p The linear fitting curves are shown, where (a) the first exothermic peak of VEB-APBAI, (b) the first exothermic peak of E51-APBAI, (c) the second exothermic peak of VEB-APBAI, and (d) the second exothermic peak of E51-APBAI. Figure 3 The figures are non-isothermal DSC curves of different samples, with heating rates of 5, 10, 15 and 20 °C / min; where (a) is E51-APBAI and (b) is VEB-APBAI. Figure 4 These are the infrared spectra of the products at each stage; Figure 5 These are the mechanical performance test results, including (a) the stress-strain curve of E51-APBAI, (b) the stress-strain curve of VEB-APBAI, (c) the bending strength and modulus, and (d) the unnotched Izod impact strength. Figure 6 The images are scanning electron microscope images of the impact cross-section morphology, (a) E51-APBAI, (b) VEB-APBAI; Figure 7The results are the analysis results of the dynamic properties of the vitreous body, where (a) is the curve of the normalized relaxation modulus of VEB-APBAI changing with time at different temperatures, and (b) is the fitting result of relaxation time and Arrhenius equation. Figure 8 It involves the physical processing and recycling of VEB-APBAI to produce sample bars; Figure 9 These are the TGA and DTG curves of VEB-APBAI, where (a) is the TGA curve and (b) is the DTG curve; Figure 10 These are the DSC(b) DMA curves of VEB-APBAI, where (a) is the DSC curve and (b) is the DMA curve. Figure 11 VEB-APBAI was soaked in different solvents at room temperature for 0 h and 72 h. Detailed Implementation
[0010] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0011] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.
[0012] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0013] Terminology Abbreviations VAN: Vanillin; ECH: Epichlorohydrin; BAPT: 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane; APBAI: 5-Amino-2-(4-Aminophenyl)benzimidazole; TEBAC: Triethylbenzylammonium chloride.
[0014] To address the shortcomings of currently produced thermosetting epoxy resins, such as difficulty in recycling or complex synthesis routes, this invention provides a bio-based vanillin epoxy resin and its preparation method. Using vanillin (VAN) and epichlorohydrin (ECH) as raw materials, vanillin glycidyl ether (VE) is synthesized. The synthesized VE is reacted with BAPT to obtain an epoxy resin with imine bonds. The resin is then cured with the curing agent APBAI to obtain the bio-based vanillin epoxy resin, which is an imine epoxy resin-like glass polymer that is recyclable and exhibits excellent overall performance.
[0015] In a first aspect, the present invention provides a method for preparing a bio-based vanillin epoxy resin, comprising the following steps: S1, using vanillin (VAN) and epichlorohydrin (ECH) as raw materials, yields vanillin glycidyl ether (VE) through a synthesis reaction. S2, Vanillin glycidyl ether and terminal aminosiloxane are refluxed in an organic solvent to obtain an epoxy resin (VEB) reaction system with imine bonds; S3. The epoxy resin reaction system with imine bonds is cooled to room temperature, a curing agent is added and mixed evenly, and then subjected to solvent removal treatment and hot pressing curing to obtain bio-based vanillin epoxy resin (VEB-APBAI).
[0016] In step S2 of this invention, there is no need to wash, dry or perform other post-treatment on the epoxy resin (VEB) with imine bonds obtained from the reflux reaction. Instead, the curing agent is added directly after cooling to prepare the target product. Therefore, this invention uses vanillin glycidyl ether as raw material to achieve one-pot preparation of the target product VEB-APBAI.
[0017] In some embodiments, in step S1, the molar ratio of vanillin to epichlorohydrin is 1:(8-12).
[0018] In some embodiments, in step S1, vanillin and epichlorohydrin are synthesized in the presence of triethylbenzylammonium chloride and an alkaline solution. Specifically, vanillin, triethylbenzylammonium chloride A, and epichlorohydrin are mixed and heated at 70–90°C for 1–2 h. Afterward, the mixture is cooled to room temperature, and triethylbenzylammonium chloride B and an alkaline solution are added dropwise. The mixture is then reacted at 20–30°C for 20–40 min, and then post-treated to obtain vanillin glycidyl ether.
[0019] Furthermore, the molar ratio of vanillin, triethylbenzylammonium chloride A, and triethylbenzylammonium chloride B is 1:(0.09-0.12):(0.08-0.11).
[0020] Furthermore, the alkaline solution comprises a 4–6 mol / L sodium hydroxide solution; the mass ratio of vanillin to the alkaline solution is (7–8):4.
[0021] Further post-treatment includes dissolving in ethyl acetate, washing with distilled water, drying with anhydrous Na2SO4, solvent removal, and drying.
[0022] In some embodiments, in step S2, the molar ratio of vanillin glycidyl ether to terminal aminosiloxane is 1:(0.4-0.6); the terminal aminosiloxane is 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.
[0023] In some embodiments, in step S2, the organic solvent includes 1,4-dioxane.
[0024] In some embodiments, in step S2, the reflux reaction is carried out at 105–115°C for 8–12 hours.
[0025] In some embodiments, in step S3, the curing agent includes 5-amino-2-(4-aminophenyl)benzimidazole.
[0026] In some embodiments, in step S3, the amount of curing agent used is 20-50% of the mass of vanillin glycidyl ether, more preferably 20-30%.
[0027] In some embodiments, in step S3, the solvent removal treatment is performed by vacuum drying at 15–25°C.
[0028] In some embodiments, step S3, hot-press curing includes four stages: maintaining at 75-85°C for 1.5-2.5 hours; maintaining at 95-105°C for 1.5-2.5 hours; maintaining at 135-145°C for 1.5-2.5 hours; and applying pressure to 10-20 MPa at 145-155°C and maintaining for 8-12 hours.
[0029] Secondly, the present invention provides a bio-based vanillin epoxy resin prepared by the above preparation method.
[0030] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0031] The E-51 epoxy resin was purchased from Guangzhou Jinyonggu New Materials Co., Ltd., and is of industrial grade.
[0032] Example 1 The synthesis route in this embodiment is as follows:
[0033]
[0034] A method for preparing a bio-based vanillin epoxy resin includes the following steps: S1, VE Synthesis: Vanillin glycidyl ether (VE) was synthesized from vanillin (VAN) and epichlorohydrin (ECH). The synthesis steps are as follows: 7.61 g (0.05 mol) of vanillin was added to a 250 mL double-necked round-bottom flask. 1.20 g (0.0053 mol) of TEBAC and 46.26 g (0.5 mol) of epichlorohydrin were added to the flask. The mixture was heated at 80 °C for 2 h. The mixture was cooled to room temperature. 1.14 g (0.005 mol) of TEBAC and 4 g of 5 mol / L NaOH solution were added dropwise to the mixture. The reaction was continued at 30 °C for 30 min. The mixture was dissolved in ethyl acetate. The organic layer was washed three times with distilled water. The organic layer was dried with anhydrous Na₂SO₄, and excess solvent was removed using a rotary evaporator. The product was dried in an oven overnight to obtain vanillin glycidyl ether (VE).
[0035] S2, Preparation of VEB: 5.2 g (0.025 mol) of synthesized VE and 3.1 g (0.0125 mol) of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane (BAPT) were refluxed in 1,4-dioxane (Diox) at 110 °C for 10 h to obtain an epoxy resin (VEB) reaction system with imine bonds.
[0036] S2, VEB-APBAI: The epoxy resin (VEB) reaction system with imine bonds was cooled to room temperature, and 1.4 g of 5-amino-2-(4-aminophenyl)benzimidazole (APBAI) was added and stirred for 5 min. The solvent was then removed in a vacuum drying oven at 20 °C. The mixture was then subjected to a gradient heating process: 80 °C / 2 h, 100 °C / 2 h, 140 °C / 2 h, 150 °C, and pressurized to 15 MPa / 10 h, and obtained by hot pressing to obtain VEB-APBAI epoxy glass polymer material.
[0037] Comparative Example 1 The synthetic route for this comparative example is as follows:
[0038] A method for preparing E51-APBAI epoxy resin includes the following steps: 10 g (epoxy equivalent 0.051 mol) of E-51 epoxy resin was placed in a beaker and heated to 50℃. 2.24 g (active hydrogen equivalent 0.05 mol) of APBAI was added to the epoxy resin, and the mixture was stirred for 5 min using a vacuum degassing mixer at 1800 r / min. The mixture was then placed in a polytetrafluoroethylene mold for curing, with a gradient heating process: 100℃ / 1 h, 140℃ / 1 h, and 160℃ / 1 h, to obtain the thermosetting epoxy resin material E51-APBAI.
[0039] Comparative Example 2 Compared to Example 1, the APBAI curing step was removed, while the other steps and conditions were the same as in Example 1.
[0040] Performance testing (1) Nuclear magnetic resonance hydrogen and carbon spectrum analysis To verify the successful synthesis of vanillin glycidyl ether (VE), its proton and carbon NMR spectra were analyzed, and the results are as follows: Figure 1 As shown.
[0041] Depend on Figure 1 It can be seen that δ 9.86 ppm is the proton peak at position 1 on the aldehyde group, δ 7.45 ppm is the proton peak at position 2 on the benzene ring, δ 7.43 ppm is the proton peak at position 3 on the benzene ring, δ 7.04 ppm is the proton peak at position 4 on the benzene ring, δ 4.39 and 4.10 ppm are the proton peaks at position 5 on the methylene group, δ 3.94 ppm is the proton peak at position 6 on the methoxy group, δ 3.42 ppm is the proton peak at position 7 on the epoxy group, and δ 2.93 and 2.79 ppm are the proton peaks at position 8 on the epoxy methylene group. Where C1 corresponds to the carbon on the aldehyde group, C2 is the carbon on the benzene ring connected to the oxygen, C3 is the carbon on the benzene ring connected to the methoxy group, C4 is the carbon on the benzene ring connected to the aldehyde group, C5, C6, and C7 are the three carbons on the benzene ring, C8 is the carbon on the methylene group, C9 is the methyl carbon, C10 is the carbon connecting the methylene group and the epoxy group, and C11 is the carbon on the epoxy methylene group.
[0042] (2) Non-isothermal DSC analysis In the ring-opening addition reaction of epoxy groups, the stoichiometric reaction between epoxides and amines is a typical reaction achieved through a stepwise polymerization process. The non-isothermal curing behavior of VEB and APBAI is as follows: Figure 2 As shown.
[0043] Depend on Figure 2It can be seen that the thermosetting processes of VEB and APBAI are consistent with those of E51-APBAI, both exhibiting exothermic bimodal growth. Since APBAI contains both primary and secondary amine hydrogens, the curing process is divided into two stages. The hydrogens on the primary amine are more reactive and can participate in the reaction at lower temperatures. As the temperature increases, the hydrogens on the secondary amine also begin to participate in the reaction and act as catalysts. Compared to the exothermic peak temperature of E51-APBAI at a heating rate of 10℃ / min (145.2℃), the peak temperature of VEB-APBAI is lower (130.1℃), indicating that this material has higher curing activity.
[0044] Combination Figure 2 The activation energies (Ea) of the first exothermic peak, calculated using the Kissinger and Ozawa methods, are 72.58 kJ / mol and 79.07 kJ / mol, respectively, while those of the second exothermic peak are 53.13 kJ / mol and 60.03 kJ / mol, respectively. These values are consistent with the reported values for the epoxide amine system (approximately 55 kJ / mol). Under the same evaluation conditions, the Ea values of the first exothermic peak of E51-APBAI were measured to be 74.49 kJ / mol and 80.31 kJ / mol, respectively, and the Ea values of the second exothermic peak were measured to be 94.11 kJ / mol and 101.18 kJ / mol, respectively. The relatively low Ea values of the VEB-APBAI system further confirm its high reactivity.
[0045] like Figure 3 As shown, when the heating rate changed from 5℃ / min to 20℃ / min, the exothermic peak temperature gradually increased from 114.9℃ to 146.1℃. The VEB-APBAI reaction curing conditions were preliminarily obtained using non-isothermal DSC curves: 80℃ / 2 h, 100℃ / 2 h, 140℃ / 2 h, and 150℃ / 10 h. To verify complete curing, qualitative analysis was performed using infrared spectroscopy.
[0046] (3) Infrared spectroscopy analysis FTIR analysis was performed on the products of each step in the synthesis and preparation process. Figure 4 These are the infrared spectra of the products at each stage.
[0047] from Figure 4 The image shows that VE is present at 1682 cm. -1 There is a distinct infrared characteristic peak at 910 cm⁻¹, which is the characteristic peak of -C=O. -1 The presence of a distinct characteristic peak of epoxide-COC- at 1682 cm⁻¹, combined with the proton and carbon spectra, indicates the successful synthesis of VE. The infrared spectrum shows a peak at 1682 cm⁻¹ for VEB. -1 There are still aldehyde residues at the location, and at 1644 cm-1 A new infrared characteristic peak, -C=N, appeared. This indicates that the condensation reaction between the aldehyde and amino groups was incomplete, and the unreacted primary amine can significantly accelerate the imine exchange reaction through a concerted mechanism. Therefore, this invention uses a one-pot method to directly prepare epoxy imine glass. VEB-APBAI can be observed at 1682 cm⁻¹ in the infrared spectrum. -1 The characteristic peak has completely disappeared, 1644 cm⁻¹ -1 The -C=N characteristic peak still exists at 910 cm⁻¹. -1 The disappearance of the epoxy characteristic peak at 910 cm⁻¹ indicates that the material has been completely cured, further confirming the feasibility of the curing conditions. Similarly, E51-APBAI at 910 cm⁻¹... -1 The disappearance of the epoxy characteristic peak at the point indicates that the material has been completely cured.
[0048] (4) Mechanical performance analysis Figure 5 The mechanical properties of VEB-APBAI and the baseline network E51-APBAI are compared. Specific data on strength, modulus and elongation at break are shown in Table 1.
[0049] Table 1. Strength, modulus, and elongation at break data of VEB-APBAI and the baseline network E51-APBAI
[0050] Depend on Figure 5 As shown in Table 1, VEB-APBAI exhibits excellent tensile and flexural properties comparable to the benchmark sample E51-APBAI. Of particular note is its significantly higher flexural modulus than the benchmark sample, a result that is in excellent agreement with the dynamic mechanical analysis (DMA) data described below. The high mechanical rigidity of the VEB-APBAI glass-transformed polymer is mainly attributed to its aromatic Schiff base structure and the intermolecular hydrogen bond network formed by imine bonds.
[0051] In particular, VEB-APBAI exhibits excellent toughness properties, which are first demonstrated in tensile and bending tests. VEB-APBAI displays a completely different yield fracture behavior from E51-APBAI, with a maximum elongation at break of 14.7%, such as... Figure 5 (b); In the bending test, the specimen neither yielded nor fractured before reaching the specified maximum deflection (1.5 times the specimen thickness). Its toughness was further verified by unnotched Izod impact testing; detailed data can be found in [link to relevant data]. Figure 5(d) and Table 1. The impact strength of VEB-APBAI reached 63.7 kJ / m², exhibiting superior toughness that is 368% higher than that of the traditional BPA epoxy resin system (12.4 ± 1.2 kJ / m²). The study speculates that this is related to the low crosslinking density of the long-chain flexible siloxane spacer groups and the epoxy glass (EV) in the material. VEB-APBAI does not exhibit the brittle defects of the flexible siloxane segments, nor does it expose the brittleness problem of the rigid conjugated aromatic rings, but rather achieves a perfect complementarity and synergistic effect between the two.
[0052] To investigate the relationship between the material's high toughness and structure, scanning electron microscopy (SEM) was used to further analyze the impact cross-sectional morphology. SEM images revealed that VEB-APBAI exhibited significant ductile fracture characteristics, which contrasted sharply with the smooth fracture surface of the conventional epoxy (E51-APBAI) in Comparative Example 1. Figure 6 The fracture surface exhibits a rough and irregular morphology, with a significant increase in the number of ripples and the density of folds. The rigid-flexible composite structure formed by the Schiff base aromatic skeleton and long-chain siloxane spacer groups can effectively induce crack bifurcation or deflection, thereby consuming energy and passivating the crack to prevent its propagation, such as... Figure 6 As shown in (b). In addition, the "radial" cracks and fiber fragments work together to reduce stress concentration and promote energy dissipation through multi-directional stress dispersion.
[0053] Overall, the long flexible spacer group of this invention not only reduces the crosslinking density but also increases the crosslinking molecular weight of VEB-APBAI. Therefore, it enhances the flexibility of the network and the fluidity of the inter-crosslinking segments, and also improves the plastic deformation capacity of the matrix.
[0054] (5) Analysis of the dynamic properties of the vitreous body In the presence of imine groups, the exchange of imine bonds can occur efficiently via a dynamic pathway. Furthermore, glassy polymers release stress and flow through a dynamic mechanism, and their bond count remains constant over time, which is consistent with… T v and T g The topological freezing is related. Overall, the assumptions of imine-containing dynamic covalent networks obtained through Maxwell's relations are... T v The value is significantly lower than its T g Value. When T v < T < T g While the likelihood of bond exchange reactions increases, the actual bond exchange reaction cannot proceed because the cross-linked structure is frozen due to restricted chain segment movement. Therefore, T gIt is a key factor determining the relaxation temperature. Dynamic mechanical analysis (DMA) technology was used to monitor the change in modulus of samples over time at different temperatures under constant tensile strain conditions, and to characterize the internal dynamic bond exchange rate. For example... Figure 7 As shown in (a), the relaxation modulus G / G of VEB-APBAI increases with increasing temperature. (0) As the temperature gradually decreases, the stress relaxation time shortens significantly. Specifically, the relaxation time is 116.4 s at 90℃, but drops sharply to 28.5 s when the temperature rises to 120℃, indicating that the material exhibits rapid thermal stress relaxation characteristics at lower temperatures. At 90℃ and 100℃, the relaxation modulus did not reach equilibrium within 300 s. When the temperature is further increased to 110℃ and 120℃, the plateau value measured after 300 s is less than 2%, and the stress is almost completely released. Specific data are shown in Table 2.
[0055] Table 2. Time required for stress relaxation of VEB-APBAI to decrease to 1 / e of its initial value at different temperatures.
[0056] The stress relaxation activation energy calculated using the Arrhenius equation is only 56.37 kJ / mol, significantly lower than other EVs containing Schiff bases (90-103 kJ / mol). This superior stress relaxation performance is primarily attributed to the material's chemical structure. The presence of imine bonds in the flexible siloxane chains significantly reduces inter-segment internal friction, and the average molecular weight at the two crosslinking points in the VEB-APBAI glass matrix (…) M c With the increase in crosslinking density and the decrease in crosslinking intensity, the fluidity of the network segments is significantly enhanced. Therefore, the rapid relaxation and low activation energy of the VEB-APBAI glass transition polymer at low temperatures not only reduce energy consumption but also significantly improve the recyclability of the material.
[0057] (6) Recyclability and reprocessability Given the excellent ductility of VEB-APBAI, this invention systematically examines its performance from the perspective of multiple recycling cycles. Figure 8 ).
[0058] Through a physical reprocessing technique, the sample was cut into small pieces and hot-pressed at 15 MPa for 30 minutes. The finished product after three reprocessing steps into small pieces is shown below. Figure 8 As shown in (c); the tensile properties after multiple reprocessing were also studied in detail. Figure 5 (b) shows the stress-strain curves after three reprocessing steps. For details, see Table 3.
[0059] Table 3. Mechanical properties and three-cycle mechanical properties of VEB-APBAI
[0060] After 1-3 reprocessing cycles, the retention rates of tensile strength and elongation at break both exceeded 93%. Consistent with the results of material plasticity testing, the high fluidity of the polymer segments significantly increased the probability of imine bond exchange reactions. Simultaneously, with increasing cycle number, the tensile strength and elongation at break of the reprocessed samples showed a decreasing trend, attributed to the recombination of unsaturated C=N bonds during reprocessing, forming a network structure with a high energy barrier. Similarly, repeated hot-pressing and plasticizing oxidized the material, altering its topology and reducing the original topological structure.
[0061] (7) Thermal performance analysis The thermal stability of the cured material was determined by thermogravimetric analysis (TGA) under N2 atmosphere. The relevant curves are shown in the figure. Figure 9 .
[0062] VEB-APBAI material at 5% weight loss temperature ( T 5% The temperature reached 302℃, indicating good thermal stability. Typically, due to the low binding energy of imine bonds, these materials are prone to dissociation at high temperatures. Literature reports on EPs containing Schiff base groups... T 5% Most of them are in the 270-290℃ range. It is worth noting that VEB-APBAI still retains 52.7% of its residue at 800℃, and the decomposition process is slow. This is due to the conversion of the inherent siloxane and imidazole aromatic Schiff base groups into carbon residue at high temperatures.
[0063] The glass transition temperature of VEB-APBAI was measured using differential scanning calorimetry (DSC). T g .Depend on Figure 10 (a) It can be known that VEB-APBAI's T g The temperature was 84.9℃. T g Mainly influenced by the molecular chain structure, the BAPT main chain contains flexible groups -Si-O-, which are prone to internal rotation, increasing the mobility of polymer chain segments and lowering the glass transition temperature.
[0064] Based on the Dynamic Mechanical Analysis (DMA) test results, as follows Figure 10 (b) The storage modulus of VEB-APBAI shows that it undergoes only a single transition from the glassy state to the viscoelastic state, without a second obvious transition plateau, and the tan δ of the material exhibits only a single peak, indicating that the material is homogeneous overall. DMA measurements...T g The temperature is 110℃. The storage modulus and loss modulus are 3020 MPa and 148 MPa, respectively. Its high rigidity is attributed to the intermolecular hydrogen bonds provided by the strong conjugated benzene ring and imine bond.
[0065] (8) Solvent resistance test To obtain the solvent resistance properties of VEB-APBAI, long strips were prepared and immersed in seven common organic solvents at room temperature for 72 h.
[0066] Figure 11 The results showed that the sample exhibited almost no change in methanol (MeOH), ethanol (EtOH), acetone (Acetone), water, and ethyl acetate (EtOAc) solvents. Slight swelling occurred in N,N-dimethylformamide (DMF), and only significant swelling, resulting in loss of mechanical properties, was observed in dichloromethane (DCM). This is because of the strong interaction between the solvent molecules and the permanent dipole moments of the imine groups in the copolymer. This polar matching effect is stronger than a simple strong polar interaction, and the small size of dichloromethane molecules allows for easier penetration into the cross-linked network, improving dissolution efficiency.
[0067] All of these demonstrate that VEB-APBAI exhibits excellent solvent resistance in non-polar solvents, alcohol solvents, and highly polar DMF. In practical applications, this ensures the long-term reliability of the material under harsh chemical environments, extends its service life, and reduces the risk of performance degradation due to solvent erosion, resulting in excellent physical and chemical properties.
[0068] Comparing Example 1 and Comparative Example 2, it can be seen that the APBAI curing agent introduced in this invention results in a higher glass transition temperature (Tg) for VEB-APBAI (reaching 84.9℃, an increase of approximately 15℃ compared to Comparative Example 2), significantly improved tensile strength (approximately 15 MPa higher than Comparative Example 2), and also improved elongation at break and impact strength. This is mainly because the curing agent introduced in this invention contains a specific imidazole ring structure, which can produce a glass-like polymer material with a higher degree of crosslinking, thereby exhibiting better mechanical properties while maintaining high flexibility.
[0069] Meanwhile, the amount of curing agent also affects the performance of the resulting product. The present invention preferably uses 20-50% of the mass of vanillin glycidyl ether to balance mechanical properties and flexibility.
[0070] In summary, this invention introduces imine bonds into the epoxy resin system, reacts epoxy imide with APBAI curing agent to obtain epoxy imide-based glass materials, and systematically studies the various properties of epoxy imide-based glass materials by comparing them with traditional thermosetting materials cured with E51 epoxy resin and APBAI curing agent. (1) VEB-APBAI has a lower activation energy for curing reaction. The activation energies of both stages of curing reaction of VEB-APBAI are lower than those of E51-APBAI, indicating that VEB-APBAI has higher reactivity.
[0071] (2) Regarding mechanical properties, VEB-APBAI has higher tensile strength, elongation at break, flexural modulus and notched impact strength than E51-APBAI. Considering the mechanical properties of the two, VEB-APBAI has superior mechanical properties.
[0072] (3) VEB-APBAI exhibits excellent reprocessing performance, with tensile strength and elongation at break remaining above 93% after three cycles; it also demonstrates excellent thermal stability. T 5% =302℃, the carbon residue rate is 52.7% at 800℃; it also has good solvent resistance.
[0073] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a bio-based vanillin epoxy resin, characterized in that, Includes the following steps: S1, using vanillin and epichlorohydrin as raw materials, is synthesized to obtain vanillin glycidyl ether through a reaction; S2, Vanillin glycidyl ether and terminal aminosiloxane are refluxed in an organic solvent to obtain an epoxy resin reaction system with imine bonds. S3, the epoxy resin reaction system with imine bonds is cooled to room temperature, a curing agent is added and mixed evenly, and then subjected to solvent removal treatment and hot pressing curing to obtain bio-based vanillin epoxy resin.
2. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S1, the molar ratio of vanillin to epichlorohydrin is 1:(8-12).
3. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S1, vanillin and epichlorohydrin are synthesized in the presence of triethylbenzylammonium chloride and alkaline solution. Specifically, vanillin, triethylbenzylammonium chloride A and epichlorohydrin are mixed and heated at 70-90°C for 1-2 hours. After cooling to room temperature, triethylbenzylammonium chloride B and alkaline solution are added dropwise, and the reaction is continued at 20-30°C for 20-40 minutes. Vanillin glycidyl ether is then obtained after post-treatment.
4. The method for preparing the bio-based vanillin epoxy resin according to claim 3, characterized in that, The molar ratio of vanillin, triethylbenzylammonium chloride A, and triethylbenzylammonium chloride B is 1:(0.09-0.12):(0.08-0.11). The alkaline solution comprises a 4-6 mol / L sodium hydroxide solution; the mass ratio of vanillin to the alkaline solution is (7-8):4; The post-treatment includes dissolving in ethyl acetate, washing with distilled water, drying with anhydrous Na2SO4, solvent removal, and drying.
5. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S2, the molar ratio of vanillin glycidyl ether to terminal aminosiloxane is 1:(0.4-0.6); the terminal aminosiloxane is 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.
6. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S2, the organic solvent includes 1,4-dioxane.
7. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S2, the reflux reaction is carried out at 105–115°C for 8–12 hours.
8. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S3, the curing agent includes 5-amino-2-(4-aminophenyl)benzimidazole; The amount of curing agent used is 20-50% of the mass of vanillin glycidyl ether.
9. The method for preparing bio-based vanillin epoxy resin according to claim 1, characterized in that, In step S3, the solvent removal process is performed by vacuum drying at 15–25°C. Hot pressing curing includes four stages: maintaining at 75-85℃ for 1.5-2.5 hours; maintaining at 95-105℃ for 1.5-2.5 hours; maintaining at 135-145℃ for 1.5-2.5 hours; and applying pressure to 10-20 MPa at 145-155℃ and maintaining for 8-12 hours.
10. The bio-based vanillin epoxy resin prepared by the preparation method according to any one of claims 1-9.