A polyaromatic polymer and a responsive anion exchange membrane

By designing polyaromatic anion exchange polymers and alkali-resistant responsive ion exchange membranes, the stability problem of anion exchange membranes under high alkalinity and medium-high temperature was solved, achieving high conductivity, antibacterial properties and anti-swelling properties, making them suitable for applications such as alkaline fuel cells and water electrolysis.

CN123107046APending Publication Date: 2026-11-17XINQI TIMES (BEIJING) MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611513468.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing anion exchange membranes are prone to problems such as Hoffmann elimination, SN2 dequaternization, ether bond breakage, mechanical strength decay, ion transport channel collapse, and functional loss under high alkalinity and medium-high temperature conditions, making it difficult to achieve long lifespan and high performance applications.

Method used

A polyaromatic anion exchange polymer is synthesized through acid-catalyzed polyhydroxy alkylation and quaternization reactions. Silver nanoparticles and a responsive polymer layer are loaded onto the surface to form an alkali-resistant responsive ion exchange membrane, avoiding ether bond breakage and Hoffmann elimination. Combined with a SiO2@Ag+ polyphenol antibacterial layer and a responsive brush layer, high conductivity and anti-swelling properties are achieved.

Benefits of technology

It maintains high ion exchange capacity and low swelling rate at 6M KOH and 80°C, prolongs membrane life, and has antibacterial and alkali-resistant properties, making it suitable for applications such as alkaline fuel cells and water electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

This invention discloses a polyaromatic anion exchange polymer and a responsive ion exchange membrane, belonging to the field of polymer and functional membrane materials. The polymer is obtained by copolymerizing N-methyl-4-piperidinone, aromatic hydrocarbons, and cyclohexanone under strong acid catalysis to obtain a tertiary amine-containing polymer, which is then quaternized with alkyl halides. The polymer has no ether bonds in its main chain and has a cyclic quaternary ammonium structure on its side groups, exhibiting excellent alkaline thermal stability. The responsive ion exchange membrane is made of this polymer, with silver nanoparticles loaded on its surface through polyphenol coordination or covalent grafting, and a responsive polymer layer is introduced. It possesses high ionic conductivity, low swelling, long-term stability, antibacterial properties, and stimulation-responsive functions. This membrane is suitable for high-temperature and strong alkaline environments such as alkaline fuel cells and water electrolysis, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer synthesis and membrane application technology, and relates to a polyaromatic polymer and a responsive anion exchange membrane. Background Technology

[0002] In anion exchange membranes / polymers, quaternary ammonium cations are prone to deactivation such as Hoffmann elimination and SN2 dequaternization under strong alkaline (≥1M KOH) and medium-high temperature (60–80°C) conditions. At the same time, the main chain containing aromatic ether bonds (–Ar–O–Ar–) is at risk of ether bond breakage under strong alkaline / high temperature conditions, which leads to problems such as decreased ion exchange capacity (IEC), decreased mechanical strength and reduced conductivity.

[0003] Anion exchange membranes (AEMs) require long-term stable operation under high alkalinity (1–6M KOH) and medium-high temperature (60–80°C) conditions in applications such as alkaline fuel cells, water electrolysis, and electrodialysis. However, current technologies still face multiple challenges. First, primary, secondary, or benzylic substituted quaternary ammonium groups, represented by benzyltrimethylammonium (BTMA), are prone to Hoffmann elimination reactions (forming olefins) and SN2 nucleophilic substitution leading to dequaternization under strong alkaline and high-temperature environments. This results in a sharp decrease in ion exchange capacity (IEC) and ionic conductivity, severely limiting the membrane's lifespan. Relying solely on such traditional functional groups is insufficient to meet the requirements for high alkalinity and long lifespan. Second, the ether bonds or aromatic ether structures in commonly used polyarylether backbone materials (such as PPO and PEEK) are prone to hydrolytic breakage under harsh alkaline conditions, leading to molecular weight decay, mechanical strength degradation, and even ion transport channel collapse, further weakening the overall stability of the membrane. Third, while increasing IEC (interfacial electrochemical conductivity) can enhance ion conductivity, it also significantly increases the membrane's hydrophilicity, leading to severe volume swelling, especially in high-temperature and high-alkali environments. This can easily cause mechanical property degradation or interfacial delamination between the membrane and the electrode layer. Fourth, while traditional crosslinking strategies can effectively suppress swelling, they often sacrifice ion channel connectivity, resulting in increased membrane resistance. Excessive crosslinking density or improper methods can also make the membrane brittle, reducing its mechanical durability. Finally, metal nanoparticles or functional organic polymers introduced to impart additional functions such as antibacterial properties and stimulus responsiveness to AEMs, if directly and extensively doped into the membrane phase, may not only disrupt the continuity of ion channels but also introduce unstable chemical structures susceptible to OH⁻ attack, thus weakening the membrane's chemical and structural stability in alkaline and high-temperature environments. These problems collectively restrict the development and practical application of high-performance, long-life AEMs.

[0004] In view of the shortcomings of the prior art, the present invention aims to provide an anion exchange polymer system that is stable for a long time under strong alkali and high temperature.

[0005] This invention aims to simultaneously address two types of failures while also ensuring simple synthesis, readily available raw materials, and scalable processes, achieving long-term stable conductivity and structural integrity at 1–6M KOH and 60–80°C. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a polyaromatic anion exchange polymer and a responsive ion exchange membrane.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] A polyaromatic anion exchange polymer, the synthesis method of which includes the following steps:

[0009] S1, Polymerization reaction, acid-catalyzed polyhydroxyalkylation:

[0010] The polymer containing tertiary amine groups was obtained by copolymerizing N-methyl-4-piperidinone with aromatic and alkane monomers in a strong acid.

[0011] S2, Quaternization reaction:

[0012] The polymer containing tertiary amine groups obtained in S1 is reacted with an alkyl halide and quaternized under neutral conditions to obtain the polymer.

[0013] The aromatic hydrocarbon is one of diphenylmethane or diphenylethane;

[0014] The ketone monomer is cyclohexanone;

[0015] The strong acid is at least one of trifluoroacetic acid or trifluoromethanesulfonic acid;

[0016] The alkyl halide is bromomethane;

[0017] Specifically, the reaction equation is as follows:

[0018] .

[0019] Preferably, in the reactants of the S1 polymerization reaction, the ratio of aromatic hydrocarbon to N-methyl-4-piperidinone is 1:1 in molar amounts.

[0020] Preferably, in the reactants of the S2 quaternization reaction, the ratio of polymer structural unit containing tertiary amine to alkyl halide is 1:1–1.5 in molar terms.

[0021] Preferably, in the reactants, the ratio of aromatic hydrocarbon to cyclohexanone is 1:(0.3–0.7) in molar amounts.

[0022] Preferably, the reaction conditions are 0-5℃ and the reaction time is 12-24h.

[0023] The present invention also provides a responsive ion exchange membrane, wherein the ion exchange membrane is composed of a polyaromatic anion exchange polymer, and at least one side of the surface of the polymer contains silver nanoparticles supported by polyphenol coordination or covalent grafting or nanoparticles coated with silver nanoparticles, wherein the polyphenol is tannic acid or tea polyphenol, and the ion exchange membrane is further grafted with a responsive polymer layer or groups on the surface.

[0024] Preferably, the responsive ion exchange membrane is prepared by the following steps:

[0025] 1) Dissolve the polyaromatic anion exchange polymer in a polar organic solvent, add 0.5–2.0 mol% of a crosslinking agent with relative functional groups, cast a film on a substrate, and obtain a polymer film with a thickness of 20–80 μm by solvent evaporation and heat treatment;

[0026] 2) The polymer membrane is reacted with a quaternizing agent to convert the side-chain tertiary amine into a quaternary ammonium cation, and then converted into a hydroxide ion type through ion exchange to obtain an anion primary ion exchange membrane;

[0027] 3) Introduce silver nanoparticles and polyphenolic compounds into the surface or interface layer of the exchange membrane in step 2), and use in-situ reduction or coating methods to make the content of silver nanoparticles 0.05–1.0 wt% of the membrane mass, and form coordination or coating layers with polyphenols.

[0028] 4) A responsive polymer layer is introduced onto the membrane surface by grafting or coating to obtain a responsive ion exchange membrane.

[0029] Preferably, the quaternizing agent is methyl iodide or bromomethane, and the molar ratio of tertiary amine to alkyl halide is 1:1.2–1.5.

[0030] Preferably, the thickness of the response layer is 2-3 μm.

[0031] Preferably, the responsive polymer layer is poly(N-isopropylacrylamide), polyacrylic acid, chitosan, polyvinyl alcohol, or copolymers thereof.

[0032] The beneficial effects of this invention are:

[0033] 1) Higher stability due to alkali-thermal synergy, no ether bonds in the main chain, and no benign cyclic quaternary ammonium inhibition and elimination in the side groups and SN2;

[0034] 2) Balanced electrical conductivity and mechanical properties, with cross-linking achieving both high IEC and low swelling;

[0035] 3) The process is short, the conditions are mild, the equipment is versatile, and it can be completed in an atmospheric pressure glass reactor;

[0036] 4) It is scalable and cost-controllable, with mature monomer and catalyst supply, high process tolerance, and easy to scale up from kilogram to ton scale;

[0037] In summary, compared with existing membranes represented by BTMA / aryl ether backbones, the polymer and membrane described in this invention exhibit higher IEC retention rate, lower swelling rate, and longer lifetime under 6MKOH and 80℃ conditions. Simultaneously, through the surface-confined SiO2@Ag+ polyphenol antibacterial layer and alkali-resistant responsive brush layer, a composite function of "high conductivity + antibacterial + anti-swelling + responsiveness" is achieved without introducing easily OH- resistant membranes. – The chemical sites attacked. Detailed Implementation

[0038] The present invention will be further described below through specific embodiments. To make the inventive objectives, technical solutions, and beneficial technical effects of the present invention clearer, the present invention will be further described in detail below with reference to the embodiments. It should be understood that the embodiments described in this specification are merely for explaining the present invention and are not intended to limit the present invention.

[0039] Unless otherwise stated, all instruments and reagents used in the examples are commercially available or synthesized using conventional methods and can be used directly without further processing, and all instruments used in the examples are commercially available.

[0040] Example 1:

[0041] Raw materials include the aromatic monomer diphenylmethane, the cyclic ketone monomer N-methyl-4-piperidinone, cyclohexanone as a comonomer to adjust the rigidity of the main chain, trifluoromethanesulfonic acid as an acid catalyst, divinylbenzene as a low-content crosslinking agent, dichloromethane or dichloroethane as the solvent, bromomethane as the quaternizing agent, and potassium hydroxide solution and deionized water as the displacement and cleaning agents.

[0042] preparation:

[0043] 1) Dissolution and preparation: Dichloromethane was added to a 250mL three-necked flask to dissolve diphenylmethane and cyclohexanone. After cooling to 0 to 5°C, N-methyl-4-piperidinone was slowly added at a molar ratio of aromatic hydrocarbon:piperidinone = 1:1. Then, TfOH was added as a catalyst at a molar ratio of TfOH:N-methyl-4-piperidinone = 10:1. The mixture was added dropwise to an ice bath and stirred for 12–24 hours. The temperature was then controlled at 0–25°C.

[0044] 2) Product processing: After the reaction is completed, the product is neutralized with alkali and washed by phase separation. The solvent is recovered, and the crude polymer is dissolved in DMF or NMP. The solid content is adjusted by filtration for casting.

[0045] 3) Casting and drying: After filtering the solution, coat it onto the treated glass or polyester substrate. Control the wet film thickness so that the dry film is about 20–80 μm. First, allow the solvent to evaporate naturally at 40–60°C for 1–2 hours, and then vacuum dry at 80°C for 2 hours to remove the solvent.

[0046] 4) Thermal crosslinking: If a crosslinking agent is used, the dry film is heated at 120°C for 1 hour in a nitrogen atmosphere to complete free radical crosslinking. The amount of the crosslinking agent, divinylbenzene, is 0.5–2.0 mol of relative functional groups.

[0047] 5) Quaternization: Cut the dry film into small pieces and place them in DMSO or DMF. Add methyl bromide at a ratio of 1:1.2–1.5 of the tertiary amine molars. React at 5°C for 12–24 hours to complete the conversion of the tertiary amine to the quaternary ammonium.

[0048] 6) Ion replacement and washing: Wash away residual reagents with plenty of deionized water and ethanol, then soak in 1M KOH solution for 24 hours with multiple solution changes to replace halogens with OH. – .

[0049] Example 2:

[0050] Raw materials: The anion exchange membrane obtained in Example 1 was used as the substrate. The raw materials used for surface functionalization included tannic acid or tea polyphenols as polyphenol adsorbents and reducers, silver nitrate as Ag precursor, tetraethoxysilane for SiO2 coating, ammonia for sol-gel catalysis, ethanol and deionized water as reaction dispersion solvents, POEGMA monomer for temperature-responsive grafting, acetophenone as photoinitiator, and PVA as an interfacial binder.

[0051] Process:

[0052] 1) Polyphenol adsorption: Immerse the dry film in a tannic acid / ethanol mixed solution for 30 min to allow polyphenols to adsorb onto the film surface and form a thin layer. Remove the film and lightly spin dry.

[0053] 2) In-situ reduction of silver ions: The polyphenol-modified membrane is immersed in AgNO3 solution (0.5–1.0 mM) for 30–60 min, during which the polyphenols slowly reduce the Ag ions. + Dispersed AgNPs are formed on the membrane surface, and unreacted ions are then washed away with an ethanol / water mixture.

[0054] 3) SiO2 coating: The membrane and suspension were placed in an ethanol / water 1:1 system, and 0.1–0.5 mL of TEOS and 0.1–0.3 mL of NH4OH were added. The mixture was stirred at room temperature for 30–60 min to form a thin SiO2 shell on the AgNP surface. The membrane was then washed and dried at 40–60°C.

[0055] 4) Surface activation: Plasma treatment or ozone treatment of the film surface for 2–5 min is used to introduce hydroxyl sites, or short-term acid / alkali treatment is used to generate hydrophilic sites.

[0056] 5) Photo-initiated grafting: Immerse the membrane in a solution containing 0.4 g POEGMA monomer, 10 mL ethanol, and 0.02 g acetophenone for 5 min to allow the monomer to adsorb onto the surface. Then, perform surface grafting polymerization by irradiation with 365 nm UV for 15–30 min under nitrogen protection. Wash and dry at 40°C. The target brush layer should have a dry weight of approximately 0.5–2 wt% and a dry thickness not exceeding 1 μm. A pH response is required; add 1–5 mol% acrylic acid to the grafting solution as a copolymer component.

[0057] 6) Post-treatment: Immerse in 1M KOH for 24h to replace ions and heat treat at 60°C for 1h to promote interlayer adhesion. Finally, determine the Ag content in the membrane by ICP-OES and control it within 0.05–0.3wt%.

[0058] Example 3:

[0059] Raw materials: The anion exchange membrane obtained in Example 1 was used as the substrate, pre-fabricated SiO2@Ag nanoparticles were used as the antibacterial carrier, 3-aminopropyltriethoxysilane APTES was used to introduce amine groups on the membrane surface, EDC / NHS was used to activate carboxyl groups to achieve covalent coupling, and the total Ag loading of the target encapsulated type was controlled at 0.2–1.0 wt%.

[0060] Process:

[0061] 1) Surface hydroxylation and amination: Plasma treatment is performed on the membrane surface for 2–5 min to generate hydroxyl sites, followed by APTES solution or gas phase treatment to introduce amino groups into the membrane surface. After reacting for 30–60 min, the membrane is washed and dried.

[0062] 2) Particle preparation or purchase: Prepare or purchase a suspension of SiO2@Ag nanoparticles with carboxyl groups on the surface and adjust the particle size and dispersion state to facilitate grafting.

[0063] 3) EDC / NHS activation and coupling: Activate the carboxyl groups on the surface of SiO2@Ag particles in a buffer solution containing EDC / NHS, then add the membrane sample and stir at room temperature for 1-2 hours to achieve covalent coupling, wash and dry.

[0064] 4) Ion replacement and heat treatment: Immersion in 1M KOH to replace the OH form and short-term heat treatment at 80℃ to enhance interface stability. The target Ag content of 0.2-1.0 wt% is achieved by adjusting the feed amount.

[0065] Example 4:

[0066] Raw materials: The anion exchange membrane obtained in Example 1 is used as the matrix. The monomers of the response layer include POEGMA for temperature response, a small amount of acrylic acid for pH response, and a low content of ferrogen-derived monomers for introducing redox response centers. The molar fraction of functional units is controlled at 0.5–2 mol% of the total monomers in the functional layer. The outer protection can be SiO2 or an inert polymer shell.

[0067] Process:

[0068] 1) Surface activation: Ozone or plasma treatment is used to introduce active sites on the film surface.

[0069] 2) Preparation of grafting solution: Prepare a mixed solution of POEGMA, acrylic acid and ferrogen monomer in ethanol / water solvent, wherein POEGMA accounts for 95–98 mol, acrylic acid accounts for 1–5 mol, and ferrogen monomer accounts for 0.5–2 mol.

[0070] 3) Photoinitiated grafting: The membrane is immersed in a grafting solution and grafted under nitrogen atmosphere by photoinitiated UV irradiation with acetophenone for 20–30 min to form a copolymer response layer with a thickness of 3 μm.

[0071] 4) Protective coating (optional): To protect the stability of the redox center in a strongly alkaline or seawater environment, an extremely thin SiO2 or inert polymer shell with a thickness of 10–50 nm can be coated on the outer layer of the response layer.

[0072] 5) Ion replacement and heat treatment: Replace with 1M KOH and perform heat treatment to stabilize the interface.

[0073] Example 5:

[0074] Raw materials: The AEM obtained in Example 2 was used as the anion layer, and the cation layer was a commercial CEM such as sulfonated polyaromatic hydrocarbon or Nafion. The interfacial catalyst layer material was TiO2 nanoparticles dispersed in a PVA matrix, and PVA solution was used as an interfacial binder. The dry thickness of the interfacial catalyst layer was controlled at 0.5–3 μm.

[0075] Process:

[0076] 1) Preparation of interfacial adhesive layer: A 1 wt% PVA solution was coated on the AEM surface and semi-dried to form a buffer adhesive layer.

[0077] 2) Catalytic layer coating: A PVA slurry with 3–7 wt% TiO2 dispersed on the PVA layer is coated and dried at room temperature to a semi-cured state.

[0078] 3) Lamination and hot pressing: The treated AEM and the prefabricated CEM are aligned and stacked, and then hot-pressed in a hot press at 80–120°C for 1–3 minutes to achieve interpenetration and firm bonding between the layers.

[0079] 4) Ion replacement and cleaning: AEL and CEL were treated with 1M KOH and 1M H2SO4 respectively, and finally rinsed with deionized water until neutral and preliminary electrochemical tests were performed.

[0080] Comparative Example 1: Traditional BTMA and ether-containing backbone

[0081] A precursor monomer containing benzyltrimethylammonium side groups and a PPO-type polymer containing aryl ether bonds were used to prepare a film using a conventional quaternization method. The IEC and thickness were comparable to those in Example 1, and were used to directly compare the alkaline thermal stability and mechanical properties.

[0082] Comparative Example 2: A large amount of uncoated AgNP was incorporated into the main phase.

[0083] In Example 1, uncoated AgNP was directly incorporated into the bulk phase up to 0.5 wt% and quaternization and replacement were completed without SiO2 coating or encapsulation treatment, in order to compare metal release and conductivity loss.

[0084] Examples 1-5 and Comparative Examples 1-2 were compared in terms of the performance and characterization of the resulting membranes under tests of IEC, conductivity, swelling, antibacterial properties, Ag release, 500 / 1000h alkaline heat aging, IEC retention rate, mechanical strength, and responsiveness. The results are shown in the table below:

[0085]

[0086] The data comparison in the table shows that Example 1 is used to disclose and verify the basic preparation method and performance baseline of the combination of the aromatic ether-free poly(aromatic-methylene) main chain and cyclic quaternary ammonium side groups described in this invention, highlighting the stability of the main chain and side group design under alkaline and thermal conditions and the possibility of achieving high IEC. Example 2 is used to demonstrate that by controlling the crosslinking dosage and the ratio of cyclohexanone comonomer, the film swelling can be significantly reduced and the mechanical durability improved while ensuring IEC and conductivity, thereby overcoming the technical problem of uncontrolled swelling caused by high IEC. Example 3 is used to demonstrate the surface-confined polyphenol-Ag antibacterial module, which achieves stable loading of silver nanoparticles through polyphenol coordination and in-situ reduction and provides significant antibacterial performance without damaging the host ion channels, proposing a solution to the shortcomings of existing technologies in balancing functionality and alkali resistance. Example 4 is used to further demonstrate that the integration of the SiO2 coating strategy and the alkali-resistant temperature-responsive brush layer can balance anti-Ag loss in seawater scenarios, responsive functionality, and long-term conductivity maintenance, thereby gaining technical advantages in application expansion. Example 5 elevates the above materials and processes to the device level. Through the assembly of bipolar membranes, it is demonstrated that the materials of the present invention can be extended to device-level applications such as water electrolysis for hydrogen production and seawater desalination. Furthermore, the design of the interface catalytic layer optimizes the water splitting overpotential and interface stability, thus distinguishing it from existing technologies that are limited to single-layer membranes.

[0087] In summary, the present invention provides a responsive ion exchange membrane that combines the advantages of "high conductivity + antibacterial + anti-swelling + responsiveness".

[0088] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A polyaromatic anion exchange polymer, characterized in that, The method for synthesizing the polymer includes the following steps: S1, Polymerization reaction, acid-catalyzed polyhydroxyalkylation: The polymer containing tertiary amine groups was obtained by copolymerizing N-methyl-4-piperidinone with aromatic and alkane monomers in a strong acid. S2, Quaternization reaction: The polymer containing tertiary amine groups obtained in S1 is reacted with an alkyl halide and quaternized under neutral conditions to obtain the polymer. The aromatic hydrocarbon is one of diphenylmethane or diphenylethane; The ketone monomer is cyclohexanone; The strong acid is at least one of trifluoroacetic acid or trifluoromethanesulfonic acid; The alkyl halide is bromomethane; Specifically, the reaction equation is as follows: 。 2. The polyaromatic anion exchange polymer according to claim 1, characterized in that, In the S1 polymerization reaction, the ratio of aromatic hydrocarbon to N-methyl-4-piperidinone is 1:1 in molar amounts.

3. The polyaromatic anion exchange polymer according to claim 1, characterized in that, In the reactants of the S2 quaternization reaction, the ratio of polymer structural units containing tertiary amines to alkyl halides is 1:1–1.5 in molar terms.

4. The polyaromatic anion exchange polymer according to claim 1, characterized in that, In the reactants, the ratio of aromatic hydrocarbons to cyclohexanone is 1:(0.3–0.7) in molar amounts.

5. The polyaromatic anion exchange polymer according to claim 1, characterized in that, The reaction conditions are 0-5℃ and the reaction time is 12-24h.

6. A responsive anion exchange membrane, characterized in that, The ion exchange membrane is composed of a polyaromatic anion exchange polymer, and at least one side of the polymer surface further contains silver nanoparticles loaded by polyphenol coordination or covalent grafting, or nanoparticles coated with silver nanoparticles. The polyphenols are tannic acid or tea polyphenols, and the ion exchange membrane is further grafted with a responsive polymer layer or responsive groups on its surface.

7. The responsive anion exchange membrane according to claim 6, characterized in that, It is prepared by the following steps: 1) Dissolve the polyaromatic anion exchange polymer in a polar organic solvent, add 0.5–2.0 mol% of a crosslinking agent with relative functional groups, cast a film on a substrate, and obtain a polymer film with a thickness of 20–80 μm by solvent evaporation and heat treatment; 2) The polymer membrane is reacted with a quaternizing agent to convert the side-chain tertiary amine into a quaternary ammonium cation, and then converted into a hydroxide ion type through ion exchange to obtain a primary anion exchange membrane; 3) Introduce silver nanoparticles and polyphenolic compounds into the surface or interface layer of the exchange membrane in step 2), and use in-situ reduction or coating methods to make the content of silver nanoparticles 0.05–1.0 wt% of the membrane mass, and form coordination or coating layers with polyphenols to obtain a modified anion exchange membrane. 4) A responsive polymer layer is introduced onto the membrane surface by grafting or coating to obtain a responsive ion exchange membrane.

8. The responsive anion exchange membrane according to claim 7, characterized in that, The quaternizing agent is methyl iodide or bromomethane, and the molar ratio of tertiary amine to alkyl halide is 1:1.2–1.

5.

9. The responsive anion exchange membrane according to claim 7, characterized in that, The thickness of the responsive polymer layer is 2-3 μm.

10. The responsive anion exchange membrane according to claim 7, characterized in that, The responsive polymer layer is poly(N-isopropylacrylamide), polyacrylic acid, chitosan, polyvinyl alcohol, or copolymers thereof.