A method for regulating the growth process of polydioxanone molecular chains based on staged energy input

By controlling the polymerization process through staged energy input, the problem of insufficient controllability of the polymerization process under constant energy input was solved, and the molecular weight and molecular weight distribution of poly(p-dioxanone) were controllably adjusted, resulting in high-quality polymer products.

CN123107050APending Publication Date: 2026-11-17PUSEN (SHANDONG) MEDICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611412767.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing ring-opening polymerization methods for polydioxanone, the constant energy input mode cannot provide matching energy conditions at different stages, resulting in insufficient chain growth rate or side reactions such as chain transfer and thermal degradation, which affect the molecular weight and molecular weight distribution of the product.

Method used

A staged energy input control method is adopted, which sets an induction stage, a chain growth stage and a stabilization stage in the polymerization process, and applies different unit mass energy input amounts and durations for each stage. The polymerization kinetics are then regulated by programmed control using microwave irradiation, electromagnetic heating or dielectric heating.

Benefits of technology

This study improved the controllability of the polymerization process, obtaining poly(p-dioxanone) materials with a weight-average molecular weight of 5×10⁴ to 2×10⁵ g/mol, avoiding problems of insufficient chain growth or excess energy, and suppressing thermal degradation and chain transfer side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107050A_ABST
    Figure CN123107050A_ABST
Patent Text Reader

Abstract

This invention discloses a method for regulating the chain growth process of poly(p-dioxanone) based on staged energy input, belonging to the field of biodegradable polyester material preparation technology. The method includes: adding purified p-dioxanone monomer and a catalyst into a polymerization reactor to establish a polymerization system; after the polymerization system temperature reaches 60–130°C, initiating the first stage of energy input at a unit mass energy input rate of 0.01–5 kJ / g for 10–40 min to complete the induction stage; after the induction stage, automatically switching to the second stage of energy input at a unit mass energy input rate of 5–100 kJ / g for 60–240 min to complete the chain growth stage; after the chain growth stage, automatically switching to the third stage of energy input at a unit mass energy input rate of 0.01–20 kJ / g for 20–60 min to complete the stabilization stage; turning off the energy input device and cooling the polymerization system to room temperature to obtain the poly(p-dioxanone) material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention belongs to the field of biodegradable polymer material preparation technology, specifically a method for regulating the growth process of polydioxanone molecular chains based on staged energy input. Background Technology

[0002] Poly(p-dioxanone) is an aliphatic polyester material with good biocompatibility, biodegradability, and excellent flexibility. The unique ether bond structure in the main chain of poly(p-dioxanone) imparts excellent flexibility and bending resistance, making it valuable for clinical applications in absorbable sutures, orthopedic internal fixation devices, tissue engineering scaffolds, and drug delivery. Currently, poly(p-dioxanone) is mainly prepared by ring-opening polymerization of the p-dioxanone monomer under the action of a catalyst. Existing technologies typically employ organometallic catalysts such as stannous octoate for bulk melt ring-opening polymerization at specific temperatures. The polymer properties are adjusted by controlling parameters such as catalyst type, catalyst concentration, reaction temperature, and reaction time.

[0003] However, existing ring-opening polymerization methods for poly(p-dioxanone) have the following drawbacks: traditional polymerization processes typically employ a constant temperature or constant power energy input mode, lacking differentiated control over the monomer activation, chain growth, and chain stabilization stages. Since the activation energy requirements vary at different stages of ring-opening polymerization, a constant energy input cannot provide matching energy conditions for each stage, thus limiting the controllability of the polymerization process. When the energy input is too low, the chain growth rate is insufficient, and the reaction time is prolonged; when the energy input is too high, side reactions such as chain transfer and thermal degradation are prone to occur, affecting the molecular weight and molecular weight distribution of the product. Summary of the Invention

[0004] This invention provides a method for regulating the chain growth process of poly(p-dioxanone) molecular chain based on staged energy input. By setting induction, chain growth and stabilization stages with different energy input characteristics during the ring-opening polymerization of poly(p-dioxanone), the method programmatically adjusts the energy input per unit mass, the duration of energy input and the stage transition nodes, so that different polymerization stages obtain matching energy conditions, thereby regulating the polymerization kinetics and achieving controllable adjustment of the molecular weight and molecular weight distribution of poly(p-dioxanone).

[0005] To achieve the above objectives, the present invention provides the following technical solution: A method for regulating the growth process of poly(p-dioxanone) molecular chains based on staged energy input, characterized by comprising the following steps: S1. The purified p-dioxanone monomer and catalyst are added to the polymerization reactor. Under the protection of inert gas, the temperature of the polymerization system is raised to 60-130°C at a heating rate of 2-5°C / min, so that the solid p-dioxanone monomer is completely melted into liquid and the catalyst is evenly dispersed in the liquid molten monomer to form a homogeneous polymerization system. S2. Start the energy input device to apply the first stage of energy input to the polymerization system. The energy input per unit mass is 0.01 to 5 kJ / g, and the duration is 10 to 40 min to complete the induction stage. S3. After the induction stage is completed, keep the energy input device in the start state, adjust the unit mass energy input to 5-100kJ / g, apply the second stage energy input to the polymerization system for 60-240min, and complete the chain growth stage. S4. After the chain growth stage is completed, keep the energy input device in the start state, adjust the unit mass energy input to 0.01-20 kJ / g, apply the third stage energy input to the polymerization system for 20-60 min, and complete the stabilization stage. S5. After the stabilization phase is completed, the energy input device is turned off, and the polymerization system is cooled to room temperature under inert gas protection to obtain solid polydioxanone material. S6. The transition between the induction phase, chain growth phase and stabilization phase is automatically completed by the program controller, which switches phases according to the preset duration of each phase.

[0006] Furthermore, the energy input method is one of microwave irradiation, electromagnetic heating, dielectric heating, or radio frequency heating.

[0007] Furthermore, the energy input method is microwave irradiation, and the microwave frequency is 2.45 GHz.

[0008] Furthermore, the catalyst is selected from one of stannous octoate, zinc acetate, triethylaluminum, or n-butyllithium.

[0009] Furthermore, the amount of catalyst added is 0.005% to 0.05% of the mass of the dioxane monomer.

[0010] Furthermore, the polymerization temperature is 80–120°C.

[0011] Furthermore, a weight-average molecular weight of 5 × 10⁻⁶ is obtained through the staged energy input. 4 ~2×10 5 g / mol of poly(p-dioxanone) material.

[0012] Furthermore, the inert gas is nitrogen or argon.

[0013] Furthermore, the duration of the induction phase is 10–40 min, the duration of the chain growth phase is 60–240 min, and the duration of the stabilization phase is 20–60 min.

[0014] This invention provides a method for regulating the growth process of poly(p-dioxanone) molecular chains based on staged energy input, which has the following beneficial effects: This invention employs three stages with different energy input characteristics—an induction stage, a chain growth stage, and a stabilization stage—to programmatically control the polymerization process, rather than using a constant energy input mode. This achieves differentiated energy supply for different polymerization stages, avoiding the problems of insufficient energy in the chain growth stage or excessive energy in the stabilization stage under constant energy input.

[0015] This invention regulates polymerization kinetics by adjusting the unit mass energy input, duration, and stage transition nodes at different stages, thus improving the adjustability of the polymerization process. It enables the production of poly(p-dioxanone) materials with different molecular weights by changing the energy input program within a single polymerization system.

[0016] This invention uses microwave and other energy input methods to directly act on the polymerization system without the need to add additional microwave absorbing agents or energy transfer media. Therefore, it does not change the chemical composition of polydioxanone material and avoids the impact of external additives on the biocompatibility of the material.

[0017] This invention achieves effective control of chain growth rate through staged energy input, thus enabling the production of a weight-average molecular weight of 5 × 10⁻⁶ under conditions that avoid thermal degradation and chain transfer side reactions. 4 ~2×10 5 Polydioxanone materials in the g / mol range. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the process of regulating the growth of the polydioxanone molecular chain by staged energy input according to the present invention. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Example

[0020] S1. Under nitrogen protection, 100g of solid purified p-dioxanone monomer was added to the polymerization reactor; 0.01g of liquid stannous octoate catalyst was added to the polymerization reactor, the amount of stannous octoate added being 0.01% of the mass of p-dioxanone monomer; The heating device was started, and the temperature of the polymerization system was raised to 100℃ at a heating rate of 3℃ / min, so that the solid p-dioxanone monomer was completely melted into a liquid state. The liquid stannous octoate catalyst was evenly dispersed in the liquid molten monomer by stirring. The stirring speed was 60 rpm. When the temperature of the polymerization system stabilized at 100℃±1℃ and the catalyst was evenly dispersed; S2. Start the microwave generator with a microwave frequency of 2.45 GHz to apply the first stage microwave energy input to the polymerization system; the microwave power is 200 W and the duration is 20 min; the energy input per unit mass in the first stage is 2.4 kJ / g; during the first stage energy input process, the temperature of the polymerization system is maintained at 100℃±2℃; when the duration of the first stage reaches 20 min; S3. Keep the microwave generator in the start state, adjust the microwave power to 600W, and apply the second stage microwave energy input to the polymerization system for a duration of 120min; the energy input per unit mass in the second stage is 43.2kJ / g; during the second stage energy input process, the temperature of the polymerization system rises to 118-122℃; when the duration of the second stage reaches 120min; S4. Keep the microwave generator in the start state, adjust the microwave power to 200W, and apply the third stage microwave energy input to the polymerization system for 30 minutes; the energy input per unit mass of the third stage is 3.6kJ / g; during the third stage energy input process, the temperature of the polymerization system drops from 118-122℃ to 95-100℃; when the duration of the third stage reaches 30 minutes; S5. Turn off the microwave generator and allow the polymerization system to cool naturally to room temperature under nitrogen protection to obtain solid polydioxanone material. Example

[0021] S1. Under nitrogen protection, 100g of solid purified p-dioxanone monomer was added to the polymerization reactor; 0.01g of liquid stannous octoate catalyst was added to the polymerization reactor, the amount of stannous octoate added being 0.01% of the mass of p-dioxanone monomer; the heating device was started, and the temperature of the polymerization system was raised to 100℃ at a heating rate of 3℃ / min, so that the solid p-dioxanone monomer was completely melted into a liquid state, and the liquid stannous octoate catalyst was evenly dispersed in the liquid molten monomer by stirring; the stirring speed was 60 rpm; when the temperature of the polymerization system stabilized at 100℃±1℃ and the catalyst was evenly dispersed; S2. Start the microwave generator with a microwave frequency of 2.45 GHz to apply the first stage microwave energy input to the polymerization system; the microwave power is 200 W and the duration is 20 min; the energy input per unit mass in the first stage is 2.4 kJ / g; during the first stage energy input process, the temperature of the polymerization system is maintained at 100℃±2℃; when the duration of the first stage reaches 20 min; S3. Keep the microwave generator in the start state, adjust the microwave power to 800W, and apply the second stage microwave energy input to the polymerization system for a duration of 180min; the energy input per unit mass in the second stage is 86.4kJ / g; during the second stage energy input process, the temperature of the polymerization system rises to 120-125℃; when the duration of the second stage reaches 180min; S4. Keep the microwave generator in the start state, adjust the microwave power to 200W, and apply the third stage microwave energy input to the polymerization system for 30 minutes; the energy input per unit mass of the third stage is 3.6kJ / g; during the third stage energy input process, the temperature of the polymerization system drops from 120-125℃ to 95-100℃; when the duration of the third stage reaches 30 minutes; S5. Turn off the microwave generator and allow the polymerization system to cool naturally to room temperature under nitrogen protection to obtain solid polydioxanone material. Example

[0022] S1. Under nitrogen protection, 100g of solid purified p-dioxanone monomer was added to the polymerization reactor; 0.03g of solid zinc acetate catalyst was added to the polymerization reactor, the amount of zinc acetate added being 0.03% of the mass of p-dioxanone monomer; the heating device was started, and the temperature of the polymerization system was raised to 110℃ at a heating rate of 3℃ / min, so that the solid p-dioxanone monomer and solid zinc acetate catalyst were completely melted, and the zinc acetate was evenly dispersed in the liquid molten monomer by stirring; the stirring speed was 60 rpm; when the temperature of the polymerization system stabilized at 110℃±1℃ and the zinc acetate catalyst was evenly dispersed; S2. Start the microwave generator with a microwave frequency of 2.45 GHz to apply the first stage microwave energy input to the polymerization system; the microwave power is 300 W and the duration is 30 min; the energy input per unit mass in the first stage is 5.4 kJ / g; during the first stage energy input process, the temperature of the polymerization system is maintained at 110℃±2℃; when the duration of the first stage reaches 30 min; S3. Keep the microwave generator in the start state, adjust the microwave power to 700W, and apply the second stage microwave energy input to the polymerization system for a duration of 120min; the energy input per unit mass in the second stage is 50.4kJ / g; during the second stage energy input process, the temperature of the polymerization system rises to 118-122℃; when the duration of the second stage reaches 120min; S4. Keep the microwave generator in the start state, adjust the microwave power to 200W, and apply the third stage microwave energy input to the polymerization system for 40 minutes; the energy input per unit mass of the third stage is 4.8kJ / g; during the third stage energy input process, the temperature of the polymerization system drops from 118-122℃ to 95-100℃; when the duration of the third stage reaches 40 minutes; S5. Turn off the microwave generator and allow the polymerization system to cool naturally to room temperature under nitrogen protection to obtain solid polydioxanone material.

[0023] Comparative Example 1 Using constant energy input: Under nitrogen protection, 100g of solid purified p-dioxanone monomer was added to the polymerization reactor; 0.01g of liquid stannous octoate catalyst was added to the polymerization reactor, the amount of stannous octoate added being 0.01% of the mass of p-dioxanone monomer. The heating device was started, and the temperature of the polymerization system was raised to 100℃ at a heating rate of 3℃ / min, so that the solid p-dioxanone monomer was completely melted into a liquid state. The liquid stannous octoate catalyst was evenly dispersed in the liquid molten monomer by stirring. The stirring speed was 60 rpm. When the temperature of the polymerization system stabilized at 100℃±1℃ and the catalyst was evenly dispersed, the microwave generator was started and continuously input with a constant microwave power of 800W for 180min. After stopping the microwave input, the polymerization system was naturally cooled to room temperature under nitrogen protection to obtain solid polydioxanone material; the molecular weight, molecular weight distribution, residual polydioxanone monomer content and intrinsic viscosity of the sample obtained in Comparative Example 1 were compared with those of the samples obtained in Examples 1 to 3.

[0024] Comparative Example 2 Using a constant low-power energy input method: Under nitrogen protection, 100g of solid purified p-dioxanone monomer was added to the polymerization reactor; 0.01g of liquid stannous octoate catalyst was added to the polymerization reactor, the amount of stannous octoate added being 0.01% of the mass of p-dioxanone monomer. The heating device was started, and the temperature of the polymerization system was raised to 100℃ at a heating rate of 3℃ / min, so that the solid p-dioxanone monomer was completely melted into a liquid state. The liquid stannous octoate catalyst was evenly dispersed in the liquid molten monomer by stirring. The stirring speed was 60 rpm. When the temperature of the polymerization system stabilized at 100℃±1℃ and the catalyst was evenly dispersed, the microwave generator was started and continuously input with a constant microwave power of 200W for 180min. After stopping the microwave input, the polymerization system was naturally cooled to room temperature under nitrogen protection to obtain solid polydioxanone material; the molecular weight, molecular weight distribution, residual polydioxanone monomer content and intrinsic viscosity of the sample obtained in Comparative Example 2 were compared with those of Examples 1-3 and Comparative Example 1.

[0025] Comparison of results between the examples and the comparative examples The polydioxanone samples obtained in Examples 1-3 and Comparative Examples 1-2 were tested for molecular weight, molecular weight distribution, residual polydioxanone monomer content and intrinsic viscosity, respectively. The test results are shown in Table 1.

[0026] Table 1 Comparison of performance parameters of PPDO samples obtained in Examples 1-3 and Comparative Examples 1-2 serial number Energy Input Mode <![CDATA[Weight average molecular weight (×10 4 g / mol)]]> Molecular weight distribution (PDI) Residual PDO monomer content (%) Intrinsic viscosity (dL / g) Example 1 Phased approach (200W→600W→200W) 12.8 1.52 0.6 1.85 Example 2 Phased approach (200W→800W→200W) 18.6 1.48 0.4 2.41 Example 3 Phased approach (300W→700W→200W) 14.2 1.55 0.5 2.03 Comparative Example 1 Constant high power (800W) 8.4 2.31 0.3 1.36 Comparative Example 2 Constant low power (200W) 3.6 1.96 18.5 0.72 In the above tests, the weight-average molecular weight was determined by gel permeation chromatography with hexafluoroisopropanol as the mobile phase, a column temperature of 40℃, and a flow rate of 1.0 mL / min. Narrowly distributed polymethyl methacrylate was used as the standard for calibration. The molecular weight distribution (PDI) was calculated by the ratio of the weight-average molecular weight to the number-average molecular weight. The residual p-dioxanone monomer content was determined by gas chromatography with dichloromethane as the solvent and quantified using the internal standard method. The intrinsic viscosity was measured using an Ubbelohde viscometer in hexafluoroisopropanol solvent under a constant temperature water bath at 25℃±0.1℃. Five sample solutions of different concentrations were prepared, and the elution time at each concentration was measured. The intrinsic viscosity value was calculated by extrapolation.

[0027] As can be seen from the data in Table 1: Poly(p-dioxanone) obtained through a staged energy input method in Examples 1-3 has a weight-average molecular weight of 12.8 × 10⁻⁶. 4 ~18.6×10 4 The molecular weight distribution (PDI) is adjustable within the g / mol range, ranging from 1.48 to 1.55, and the residual p-dioxanone monomer content ranges from 0.4% to 0.6%. Comparative Example 1, using a constant high-power (800W) input method, experienced chain transfer and thermal degradation side reactions due to excessive energy input during polymerization, resulting in a poly-p-dioxanone with a weight-average molecular weight of only 8.4 × 10⁻⁶. 4 g / mol, with a molecular weight distribution PDI as broad as 2.31; Comparative Example 2 used a constant low-power (200W) input method. Due to insufficient energy input to drive the efficient chain growth stage, a large amount of p-dioxanone monomer failed to participate in the polymerization, resulting in a residual monomer content as high as 18.5%. The weight-average molecular weight of the obtained poly-p-dioxanone was only 3.6 × 10⁻⁶. 4 g / mol.

[0028] Comparing Example 2 with Comparative Example 1, both have a total energy input of 86.4 kJ / g. However, Example 2 employs a phased energy input mode: a low power input of 200 W during the induction phase, a high power input of 800 W during the chain growth phase, and a low power input of 200 W during the stabilization phase. Compared to the constant power input of 800 W in Comparative Example 1, the weight-average molecular weight of Example 2 is 8.4 × 10⁻⁶ kJ / g. 4 g / mol increased to 18.6 × 10 4 g / mol, the molecular weight distribution PDI narrowed from 2.31 to 1.48.

[0029] The comparison results show that, under the same total energy input conditions, the staged energy input method can more effectively promote the orderly growth of polydioxanone molecular chains compared to the constant power input method, while inhibiting the occurrence of chain transfer and thermal degradation side reactions under high power conditions.

[0030] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for regulating the growth process of poly(p-dioxanone) molecular chains based on staged energy input, characterized in that, Includes the following steps: S1. The purified p-dioxanone monomer and catalyst are added to the polymerization reactor. Under the protection of inert gas, the temperature of the polymerization system is raised to 60-130°C at a heating rate of 2-5°C / min, so that the solid p-dioxanone monomer is completely melted into liquid and the catalyst is evenly dispersed in the liquid molten monomer to form a homogeneous polymerization system. S2. Start the energy input device to apply the first stage energy input to the polymerization system. The energy input per unit mass is 0.01 to 5 kJ / g, and the duration is 10 to 40 min to complete the induction stage. S3. After the induction stage is completed, keep the energy input device in the start state, adjust the unit mass energy input to 5-100kJ / g, apply the second stage energy input to the polymerization system for 60-240min, and complete the chain growth stage. S4. After the chain growth stage is completed, keep the energy input device in the start state, adjust the unit mass energy input to 0.01-20 kJ / g, apply the third stage energy input to the polymerization system for 20-60 min, and complete the stabilization stage. S5. After the stabilization phase is completed, the energy input device is turned off, and the polymerization system is cooled to room temperature under inert gas protection to obtain solid polydioxanone material. S6. The transition between the induction phase, chain growth phase and stabilization phase is automatically completed by the program controller, which switches phases according to the preset duration of each phase.

2. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The energy input method is one of microwave irradiation, electromagnetic heating, dielectric heating, or radio frequency heating.

3. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 2, characterized in that, The energy input method is microwave irradiation, and the microwave frequency is 2.45 GHz.

4. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The catalyst is selected from one of stannous octoate, zinc acetate, triethylaluminum, or n-butyllithium.

5. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The amount of catalyst added is 0.005% to 0.05% of the mass of dioxanehexanone monomer.

6. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The polymerization temperature is 80–120°C.

7. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, A weight-average molecular weight of 5 × 10⁻⁶ was obtained through the staged energy input. 4 ~2×10 5 g / mol of poly(p-dioxanone) material.

8. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The inert gas is nitrogen or argon.

9. The method for regulating the growth process of polydioxanone molecular chains based on staged energy input according to claim 1, characterized in that, The duration of the induction phase is 10–40 min, the duration of the chain growth phase is 60–240 min, and the duration of the stabilization phase is 20–60 min.

10. The polydioxanone material prepared by the method according to any one of claims 1 to 9 based on the staged energy input regulation of the polydioxanone molecular chain growth process.