A crosslinked copolyamide quaternary ammonium compound, its preparation method and application

Crosslinked copolyamide quaternary ammonium compounds were prepared by copolymerization and crosslinking reactions of caprolactam and functionalized monomers, which solved the shortcomings of nylon 6 polymer in terms of processability and mechanical properties, and realized high-performance materials suitable for plastics and films.

CN123107067APending Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510636137.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing nylon 6 polymers have shortcomings in terms of processability and mechanical properties, especially high water absorption, high crystallinity, low melt strength, and poor flowability, making it difficult to meet the requirements of demanding applications.

Method used

Crosslinked copolyamide quaternary ammonium compounds were prepared by copolymerization of caprolactam and functionalized monomers. The polymerization was carried out under hydrolysis ring-opening conditions without a catalyst, and the crosslinking reaction was carried out by a haloalkane reagent to form copolyamide quaternary ammonium compounds with crosslinked structures.

Benefits of technology

It improves the mechanical properties of copolyamides, makes them easy to mass-produce industrially, and is suitable for the plastics and film industries, exhibiting good mechanical properties and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107067A_ABST
    Figure CN123107067A_ABST
Patent Text Reader

Abstract

This disclosure relates to a crosslinked copolyamide quaternary ammonium compound, its preparation method, and its application. The quaternary ammonium compound is a quaternary ammonium salt containing a crosslinked copolyamide quaternary ammonium cation. The crosslinked copolyamide quaternary ammonium cation includes a first structural unit as shown in formula (1) and a second structural unit as shown in formula (2), where R1 and R2 each independently include substituted or unsubstituted C. 1‑30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3‑12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6‑18 One or more of the aryl groups, or R1 and R2 interconnected with the N group attached thereto, together form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C groups. 1‑30 aliphatic hydrocarbon group, substituted or unsubstituted C 3‑12 alicyclic hydrocarbon group, substituted or unsubstituted C 6‑18 One or more of the arylene groups. The crosslinked copolyamide quaternary ammonium compounds disclosed herein possess good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of polymer technology, specifically to a crosslinked copolyamide quaternary ammonium compound, its preparation method, and its application. Background Technology

[0002] Caprolactam polymers possess excellent properties such as light weight, high strength, wear resistance, and resistance to weak acids, weak alkalis, and some organic solvents, making them widely used in fibers, engineering plastics, and films. However, Nylon 6 contains highly polar amide groups in its molecular chain, which readily form hydrogen bonds with water molecules, causing the product to easily absorb moisture from the environment. Furthermore, Nylon 6 has high crystallinity, low melt strength, and poor flowability, requiring more stringent processability.

[0003] Copolymerization of caprolactam and functionalized monomers is an effective means to improve the properties of caprolactam polymers and expand their application areas. CN104558588A describes a ring-opening polymerization process in the presence of an initiator, where caprolactam containing polymerizable double bonds is polymerized with another caprolactam. The double bonds on the polymer are then further polymerized with other monomers via free radical polymerization to form a multi-branched modified nylon 6 product. CN115707727A describes the preparation of a copolymer of functionalized aminocaprolactam and caprolactam using anionic polymerization. This copolymer, after being dissolved in a solvent, undergoes a quaternization reaction with a haloalkane to obtain a quaternized caprolactam copolymer with antibacterial properties. However, the above methods are complex, and the resulting copolyamides have poor mechanical properties. Summary of the Invention

[0004] The purpose of this disclosure is to provide a crosslinked copolyamide quaternary ammonium compound, its preparation method and application. This crosslinked copolyamide quaternary ammonium compound has good mechanical properties, is easy to mass-produce industrially, and can be used in the fields of plastics and films.

[0005] To achieve the above objectives, the first aspect of this disclosure provides a crosslinked copolyamide quaternary ammonium compound, wherein the quaternary ammonium compound is a quaternary ammonium salt comprising a crosslinked copolyamide quaternary ammonium cation; the crosslinked copolyamide quaternary ammonium cation comprises a first structural unit as shown in formula (1) and a second structural unit as shown in formula (2). Equation (1) Equation (2) R1 and R2 each independently include substituted or unsubstituted C. 1-30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C.1-30 aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups; The substituents of R1, R2, and R3 each independently include C 1~10 alkyl, C 6~10 aryl and C 3~10 One or more of the heteroaryl groups.

[0006] Optionally, R1 and R2 each independently include substituted or unsubstituted C. 1-20 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; preferably, R1 and R2 are the same; R3 includes substituted or unsubstituted C. 1-20 aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups; The substituents of R1, R2, and R3 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, phenyl, and furanyl.

[0007] Optionally, R1 and R2 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl, and nonylphenyl; R3 includes one or more of the following: methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene.

[0008] Optionally, the first structural unit shown in equation (1) includes: .

[0009] Optionally, in the crosslinked copolyamide, the molar content x of the first structural unit is 0.01~0.08, and the molar content y of the second structural unit is 0.92~0.99; wherein, x+y=1.

[0010] Optionally, the crosslinked copolyamide quaternary ammonium cation further includes a third structural unit as shown in formula (3). Equation (3) The molar content z of the third structural unit is 0.01~0.08, and the value of x+z is 0.01~0.08.

[0011] Optionally, the swelling degree of the crosslinked copolyamide quaternary ammonium cation is 19-45.

[0012] Optionally, the anion of the quaternary ammonium salt includes a halide ion, wherein the halide ion includes Cl. - ,Br - and I - One or more of the following, preferably Br - .

[0013] A second aspect of this disclosure provides a method for preparing crosslinked copolyamides, the method comprising the following steps: S1. Caprolactam and caprolactam with nitrogen-containing side groups are polymerized with water to obtain the first copolymer; S2. The first copolymer, the haloalkane reagent, and the solvent are brought into contact to carry out a crosslinking reaction, wherein the molar ratio of the first copolymer to the haloalkane reagent, based on the tertiary amine, is 1:1 to 10. The caprolactam having nitrogen-containing side groups has the structure shown in formula (4), and the haloalkane reagent has the structure shown in formula (5). Equation (4) X1-R3-X2, Equation (5). R1 and R2 each independently include substituted or unsubstituted C. 1-30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C. 1-30 aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic alkylene groups, substituted or unsubstituted C 6-18 One or more aryl groups; X1 and X2 may be the same or different, each being an independent halogen group.

[0014] Optionally, R1 and R2 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl and nonylphenyl; preferably one or more of methyl, ethyl, propyl, cyclohexyl, phenyl and benzyl.

[0015] Optionally, the caprolactam having nitrogen-containing side groups comprises one or more of the following structures: .

[0016] Optionally, R3 includes one or more of methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, decylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene; preferably one or more of butylene, hexylene, octylene, and decylene. X1 and X2 each independently include one or more of Cl, Br and I, preferably Br; preferably X1 and X2 are the same. Optionally, the halocarbon reagent includes one or more of 1,4-dibromobutane, 1,6-dibromohexane, 1,8-dibromooctane, and 1,10-dibromodecane.

[0017] Optionally, in step S1, the conditions for the polymerization reaction include: the polymerization temperature is 200~250℃, and the polymerization time is 8~12h; In the polymerization system, the mass fraction of caprolactam is 85-99%, the mass fraction of caprolactam with nitrogen-containing side groups is 1-15%, and the mass of water is 3-10% of the mass of caprolactam.

[0018] Optionally, in step S2, the conditions for the crosslinking reaction include: the temperature of the crosslinking reaction is 50~80℃, and the time of the crosslinking reaction is 8~12h.

[0019] Optionally, in step S2, the molar ratio of the first copolymer (based on tertiary amine) to the haloalkane reagent is 1:4 to 6.

[0020] Optionally, in step S2, the solvent includes a fluorinated organic solvent; the fluorinated organic solvent includes one or more of trifluoroethanol and hexafluoroisopropanol, preferably trifluoroethanol; The mass ratio of the first copolymer to the solvent is 1:5~20, preferably 1:8~12.

[0021] A third aspect of this disclosure provides a crosslinked copolyamide prepared using the method described in the second aspect of this disclosure.

[0022] Optionally, the crosslinked copolyamide has a melting point of 170~213℃, a tensile strength of 55~80MPa, and a zero-shear viscosity of 1900~350000Pa / s at 230℃.

[0023] This fourth aspect of the disclosure provides an application of the crosslinked copolyamide quaternary ammonium compound described in the first and / or third aspects of the disclosure.

[0024] Through the above technical solution, the crosslinked copolyamide quaternary ammonium compound disclosed herein includes a copolyamide quaternary ammonium cation, which has a certain degree of crosslinking, thus improving the mechanical properties of the copolyamide. The method disclosed herein requires no catalyst, the process is easy to control, and it is easy to mass-produce industrially. Furthermore, the resulting copolyamide quaternary ammonium compound exhibits good mechanical properties and can be used in the fields of plastics and films.

[0025] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0026] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings: Figure 1 This is the nuclear magnetic resonance (1H NMR) spectrum of the first copolymer in Example 1 of this disclosure.

[0027] Figure 2 This is a graph showing the changes in storage modulus of the crosslinked copolyamide quaternary ammonium compounds obtained in Examples 1-4 of this disclosure and the products obtained in Comparative Examples 1-2.

[0028] Figure 3 This is a viscosity change curve of the crosslinked copolyamide quaternary ammonium compound obtained in Examples 1-4 of this disclosure and the product obtained in Comparative Examples 1-2. Detailed Implementation

[0029] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.

[0030] The first aspect of this disclosure provides a crosslinked copolyamide quaternary ammonium compound, wherein the quaternary ammonium compound is a quaternary ammonium salt containing a crosslinked copolyamide quaternary ammonium cation; the crosslinked copolyamide quaternary ammonium cation includes a first structural unit as shown in formula (1) and a second structural unit as shown in formula (2). Equation (1) Equation (2) R1 and R2 each independently include substituted or unsubstituted C. 1-30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C. 1-30aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups; The substituents of R1, R2, and R3 each independently include C 1~10 alkyl, C 6~10 aryl and C 3~10 One or more of the heteroaryl groups.

[0031] The crosslinked copolyamide quaternary ammonium compound disclosed herein includes a copolyamide quaternary ammonium cation, which has a certain degree of crosslinking, thereby improving the mechanical properties of the copolyamide.

[0032] The carbon number in this disclosure includes the carbon number of substituents, such as substituted or unsubstituted C146 ... 1~20 The carbon number of the aliphatic hydrocarbon group refers to the number of carbons including the aliphatic hydrocarbon group and the substituents, which ranges from 1 to 20. It represents a chemical bond.

[0033] According to one embodiment of this disclosure, R1 and R2 each independently include substituted or unsubstituted C. 1-20 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups, or R1 and R2 linked together with the N group attached to them, form a 5-7 membered aliphatic ring; the substituents of R1 and R2 each independently include C. 1~8 alkyl, C 6~8 aryl and C 3~8 One or more of the heteroaryl groups; in a further embodiment, R1 and R2 each independently comprise substituted or unsubstituted C. 1-20 Alkanes, substituted or unsubstituted C 3-10 Cycloalkanes, substituted or unsubstituted C 6-15 Phenyl, substituted or unsubstituted C 6-15 One or more of the indole groups; the substituents of R1 and R2 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, phenyl, benzyl, and furanyl. The above embodiments facilitate the formation of a suitable crosslinked copolyamide quaternary ammonium cation, giving the crosslinked copolyamide good mechanical properties.

[0034] In one embodiment, R1 and R2 each independently comprise one or more of the following: methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl, and nonylphenyl; preferably, R1 and R2 are the same. The above embodiments facilitate the formation of a suitable crosslinked copolyamide quaternary ammonium cation, giving the crosslinked copolyamide good mechanical properties; simultaneously, they help reduce production costs.

[0035] According to one embodiment of this disclosure, R3 includes substituted or unsubstituted C. 1-20 aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups; the substituents of R3 include C. 1~8 alkyl, C 6~8 aryl and C 3~8 One or more of the heteroaryl groups. The above embodiments facilitate the formation of crosslinked copolyamide quaternary ammonium cations with suitable structures, giving the crosslinked copolyamide good mechanical properties.

[0036] In one embodiment, R3 comprises one or more of methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene; preferably one or more of butylene, hexylene, octylene, and decylene. The above embodiments facilitate the formation of a suitable crosslinked copolyamide quaternary ammonium cation, giving the crosslinked copolyamide good mechanical properties.

[0037] According to one embodiment of this disclosure, the first structural unit shown in formula (1) includes: The above-described embodiments facilitate the formation of crosslinked copolyamide quaternary ammonium cations with suitable structures, thereby giving the crosslinked copolyamides good mechanical properties.

[0038] According to one embodiment of this disclosure, in the crosslinked copolyamide, the molar content x of the first structural unit is 0.01~0.08, and the molar content y of the second structural unit is 0.92~0.99; wherein x+y=1. This embodiment facilitates the formation of a suitable structure in the crosslinked copolyamide quaternary ammonium cation, resulting in good mechanical properties in the crosslinked copolyamide.

[0039] According to one embodiment of this disclosure, the crosslinked copolyamide quaternary ammonium cation may further include a third structural unit as shown in formula (3). Equation (3) The molar content of the third structural unit is z, and the value of x+z is 0.01~0.08.

[0040] According to one embodiment of this disclosure, the crosslinked copolyamide quaternary ammonium cation may further include a fourth structural unit as shown below. , Wherein, the molar content of the fourth structural unit is m, and the value of x+m is 0.01~0.08; X is a halide ion, for example, Cl. - ,Br - and I - One or more of them.

[0041] According to one embodiment of this disclosure, the swelling degree of the crosslinked copolyamide quaternary ammonium cation is 19-45. In this disclosure, the swelling degree refers to the ratio of the volume increase of the crosslinked copolymer after absorbing solvent molecules in a solvent to reach equilibrium. The swelling degree in this disclosure is tested using a swelling method. The crosslinked copolyamide quaternary ammonium compound of this disclosure exhibits good mechanical properties.

[0042] According to one embodiment of this disclosure, the anion of the quaternary ammonium salt includes a halide ion, wherein the halide ion includes Cl... - ,Br - and I - One or more of the following, preferably Br - .

[0043] A second aspect of this disclosure provides a method for preparing crosslinked copolyamides, the method comprising the following steps: S1. Caprolactam and caprolactam with nitrogen-containing side groups are polymerized with water to obtain the first copolymer; S2. The first copolymer, the haloalkane reagent, and the solvent are brought into contact to carry out a crosslinking reaction, wherein the molar ratio of the first copolymer to the haloalkane reagent, based on the tertiary amine, is 1:1 to 10. The caprolactam having nitrogen-containing side groups has the structure shown in formula (4), and the haloalkane reagent has the structure shown in formula (5). Equation (4) X1-R3-X2, Equation (5). R1 and R2 each independently include substituted or unsubstituted C. 1-30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C.1-30 aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic alkylene groups, substituted or unsubstituted C 6-18 One or more aryl groups; X1 and X2 may be the same or different, each being an independent halogen group.

[0044] The method disclosed herein does not require a catalyst and prepares a first copolyamide under hydrolysis ring-opening conditions. This copolyamide is then crosslinked and polymerized using a haloalkane reagent to obtain a crosslinked copolyamide. The method described herein is easy to control, readily applicable for industrial-scale mass production, and the resulting copolyamide quaternary ammonium compound exhibits excellent mechanical properties, making it suitable for use in the plastics and film industries.

[0045] According to one embodiment of this disclosure, R1 and R2 each independently include substituted or unsubstituted C. 1-20 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups, or R1 and R2 linked together with the N group attached to them, form a 5-7 membered aliphatic ring; the substituents of R1 and R2 each independently include C. 1~8 alkyl, C 6~8 aryl and C 3~8 One or more of the heteroaryl groups; in a further embodiment, R1 and R2 each independently comprise substituted or unsubstituted C. 1-20 Alkanes, substituted or unsubstituted C 3-10 Cycloalkanes, substituted or unsubstituted C 6-15 Phenyl, substituted or unsubstituted C 6-15 One or more of the indole groups; the substituents of R1 and R2 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, phenyl, benzyl, and furanyl. The above embodiments facilitate the formation of a suitable crosslinked copolyamide quaternary ammonium cation, giving the crosslinked copolyamide good mechanical properties.

[0046] In one embodiment, R1 and R2 each independently comprise one or more of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl, and nonylphenyl, preferably R1 and R2 are the same. The above embodiments facilitate the formation of a suitable crosslinked copolyamide quaternary ammonium cation, giving the crosslinked copolyamide good mechanical properties while reducing production costs.

[0047] In one embodiment, the caprolactam having nitrogen-containing side groups comprises one or more of the following structures: The above-described embodiments facilitate the formation of crosslinked copolyamide quaternary ammonium cations with suitable structures, giving the crosslinked copolyamides good mechanical properties while reducing production costs.

[0048] According to one embodiment of this disclosure, R3 includes substituted or unsubstituted C. 1-20 aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups; the substituents of R3 include C. 1~8 alkyl, C 6~8 aryl and C 3~8 One or more of the heteroaryl groups. The above embodiments facilitate the crosslinking reaction of the first copolymer to obtain a crosslinked copolyamide quaternary ammonium compound.

[0049] In one embodiment, R3 comprises one or more of methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene; X1 and X2 each independently comprise one or more of Cl, Br, and I, preferably Br; preferably, X1 and X2 are the same. The above embodiments facilitate the crosslinking reaction of the first copolymer to obtain a crosslinked copolyamide quaternary ammonium compound.

[0050] According to one embodiment of this disclosure, the halocarbon reagent includes one or more of 1,4-dibromobutane, 1,6-dibromohexane, 1,8-dibromooctane, and 1,10-dibromodecane. The above embodiment facilitates the crosslinking reaction of the first copolymer to obtain a crosslinked copolyamide quaternary ammonium compound.

[0051] According to one embodiment of this disclosure, in step S1, the conditions of the polymerization reaction include: a polymerization temperature of 200~250°C, for example, any value within the range of 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or any combination thereof; and a polymerization time of 8~12 hours, for example, any value within the range of 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, or any combination thereof. This embodiment facilitates better copolymerization of caprolactam and caprolactam with nitrogen-containing side groups, forming a copolyamide with a suitable structure.

[0052] According to one embodiment of this disclosure, in step S1, the polymerization reaction includes pre-reacting the first copolymer, the haloalkane reagent, and the solvent by contacting them, followed by heating to carry out the polymerization reaction. The pre-reaction temperature is 170~250℃, the pressure is 0.5~1.3MPa, and the time is 3.5~5.5h. This embodiment facilitates the hydrolytic ring-opening of caprolactam and caprolactam with nitrogen-containing side groups, leading to better copolymerization and the formation of a copolyamide with a suitable structure.

[0053] According to one embodiment of this disclosure, step S1 further includes: after the polymerization reaction, depressurizing the reaction system to allow it to continue reacting under a second pressure; the second pressure is -0.8 to -0.1 MPa, preferably -0.8 to -0.5 MPa, the temperature is 240 to 260°C, and the reaction time is 0.5 to 2 h, preferably 1 to 1.5 h. This embodiment facilitates better copolymerization of caprolactam and caprolactam with nitrogen-containing side groups, forming a copolyamide with a suitable structure.

[0054] According to one embodiment of this disclosure, in step S1, the mass fraction of caprolactam in the polymerization reaction system is 85-99%, and the mass fraction of caprolactam having nitrogen-containing side groups is 1-15%; the mass of water is 3-10% of the mass of caprolactam. This embodiment facilitates the preparation of copolyamides under hydrolysis ring-opening conditions without the need for additional catalysts, thereby reducing production costs and further facilitating the acquisition of well-structured crosslinked copolyamide quaternary ammonium compounds.

[0055] According to one embodiment of this disclosure, in step S2, the conditions for the crosslinking reaction include: a crosslinking reaction temperature of 50-80°C, for example, any value within the range of 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or any combination thereof; and a crosslinking reaction time of 8-12 hours, for example, any value within the range of 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, or any combination thereof. This embodiment facilitates a better crosslinking reaction of the first copolymer, resulting in a well-structured crosslinked copolyamide quaternary ammonium compound.

[0056] According to one embodiment of this disclosure, in step S2, the molar ratio of the first copolymer to the haloalkane reagent is 1:4 to 6, for example, it can be any value within the range of 1:4.1, 1:4.2, 1:4.3, 1:4.5, 1:4.7, 1:4.9, 1:5, 1:5.1, 1:5.3, 1:5.5, 1:5.7, 1:5.9, 1:6, or any combination thereof. This embodiment facilitates better crosslinking of the first copolymer, resulting in a well-structured crosslinked copolyamide quaternary ammonium compound.

[0057] According to one embodiment of this disclosure, in step S2, the solvent includes a fluorinated organic solvent, which includes one or more of trifluoroethanol and hexafluoroisopropanol. This embodiment facilitates better dissolution of the first copolymer, further enabling better crosslinking of the first copolymer to obtain a well-structured crosslinked copolyamide quaternary ammonium compound.

[0058] According to one embodiment of this disclosure, the mass ratio of the first copolymer to the solvent is 1:5 to 20, preferably 1:8 to 12. This embodiment facilitates better crosslinking of the first copolymer, resulting in a well-structured crosslinked copolyamide quaternary ammonium compound.

[0059] A third aspect of this disclosure provides a crosslinked copolyamide prepared using the method described in the second aspect of this disclosure.

[0060] According to one embodiment of this disclosure, the crosslinked copolyamide has a melting point of 170~213℃, a tensile strength of 55~80MPa, and a zero-shear viscosity of 1900~350000Pa / s at 230℃.

[0061] This fourth aspect of the disclosure provides an application of the crosslinked copolyamide quaternary ammonium compound described in the first and / or third aspects of the disclosure.

[0062] In one embodiment, the crosslinked copolyamide quaternary ammonium compound can be used in the fields of plastics and films.

[0063] The present disclosure is further described in detail below through examples, but is not intended to limit the present disclosure.

[0064] The test method for the obtained crosslinked copolyamide quaternary ammonium compound in this disclosure is as follows: The structure of the first copolymer, caprolactam copolymer, was determined by nuclear magnetic resonance (NMR) at 25°C using a Burker AV-300 liquid superconducting NMR spectrometer with deuterated trifluoroacetic acid as the solvent.

[0065] The relative viscosity (η) of the first copolymer rThe test was conducted using a fully automated Ubbelohde viscometer (ZVISCO-IV2000), and the test methods included: First, the first copolymer was dissolved in 96% sulfuric acid to prepare a test solution (solute:solvent = 1g:100mL). The eluent times of the solvent and polymer test solution at 25°C were measured using an Ubbelohde viscometer and recorded as t0 and t, respectively. Both t0 and t were measured three times consecutively, and the average value was taken. η r It can be calculated using the following formula.

[0066] , The method for testing the melting point of cross-linked copolyamide quaternary ammonium compounds includes: using a differential scanning calorimeter (model DSC3) from Mettler Toledo; the specific method is as follows: (1) Weigh 5 mg of the sample and place it in the sample cell of the DSC3 differential scanning calorimeter. In a nitrogen flow of 50 mL / min, heat from 25℃ to 250℃ at a heating rate of 10℃ / min and hold at that temperature for 5 min; (2) Then lower the temperature to 25℃ at a rate of 10℃ / min; (3) Then heat the temperature to 250℃ at a rate of 10℃ / min to detect the melting point of the sample.

[0067] Storage modulus and zero-shear viscosity of crosslinked copolyamide quaternary ammonium compounds: tested using a rotational rheometer (HAAKE MARSP25CSL). Before testing, samples were injection molded into circular samples with a diameter of 20 min and a thickness of 1 min. The dynamic viscoelastic properties of the samples were tested by frequency scanning in an oscillation mode at a temperature of 230℃, a strain of 1%, and a frequency range of 0.1-500 rad / s.

[0068] Mechanical properties of crosslinked copolyamide quaternary ammonium compounds: tested according to ASTM D638 standard using a universal tensile testing machine (MTS / SANS CMT2000) at a strain rate of 10 mm / min.

[0069] The swelling degree test method includes: the swelling test is carried out at 20°C, and the test sample is immersed in trifluoroethanol for 12 h to swell. Q TFE The degree of swelling, used to characterize the swelling equilibrium of cross-linked copolymers in trifluoroethanol solution, is calculated using the following formula: Swelling Degree Q TFE The volume V of the cross-linked polymer after swelling can be used to determine its cross-linking properties. f Volume V of the initial crosslinked polymer i The ratio is used to represent this, and further expressed as the weight fraction m of the cross-linked network in the initial gel. i The weight fraction m of the cross-linked network in the final gel f And the density ρ of trifluoroethanol TFE(= 1.39 g / mL) and the density ρ of PA6 PA6 It is expressed as (= 1.14 g / mL).

[0070] , Where: V f V is the volume of the cross-linked polymer after swelling; i It is the volume of the initial crosslinked polymer; m f It is the weight fraction of the cross-linked network in the final gel; m i Weight fraction of cross-linked network in the initial gel; ρ PA6 This is the density of PA6 (1.14 g / mL); ρ TFE This is the density of trifluoroethanol (1.39 g / mL).

[0071] Preparation Example 1 (a) Weigh 546 g (3 mol) of L-lysine hydrochloride and 1.5 L of methanol into a 2 L three-necked flask. Add 176 mL (3.3 mol) of concentrated sulfuric acid (98%) dropwise using a constant pressure dropping funnel while mechanically stirring. After the concentrated sulfuric acid is added, the solution becomes clear. Transfer the solution to a 2 L single-necked flask and reflux for 8 h to obtain methylated lysine. Transfer the methylated lysine to a 50 L reactor, add 28.5 L of methanol and continue mechanical stirring. Add a methanol solution of sodium hydroxide (480 g sodium hydroxide solution + 2 L methanol) dropwise and react at room temperature for 10–12 h. After concentration and recrystallization, aminocaprolactam is obtained with a yield of 80% and a purity of 90% according to 1H NMR spectroscopy.

[0072] (b) Weigh 30 g (234 mmol) of the aminocaprolactam prepared in step (a) and dissolve it in 500 ml of methanol. Add 42 g (514 mmol) of formaldehyde solution (37% by mass) and 3 g of 10% palladium on carbon. React under a hydrogen atmosphere for 24 h. After filtration, concentration, and recrystallization, dimethyl-protected aminocaprolactam is obtained. The yield of α-dimethylamino-ε-caprolactam is 92%, and its purity is 98% according to 1H NMR spectroscopy.

[0073] Example 1 S1. 0.4 g of α-dimethylamino-ε-caprolactam obtained in Preparation Example 1, 20 g of caprolactam, and 2 g of water were added to a 50 mL high-pressure reactor. The reaction system was purged with nitrogen at room temperature and a ring-opening polymerization reaction was carried out under a nitrogen atmosphere. The stirring speed was 120 rpm, and the reaction was maintained at 180 °C and 1.1 MPa for 3 h (aqueous phase ring-opening stage). The temperature was then increased to 220 °C and 1.8 MPa and maintained for 2 h (high-pressure polymerization stage). After that, the pressure was reduced to -0.7 MPa and 200 °C and the reaction was continued for 1 h (low-pressure polymerization stage). In the polymerization reaction system, the mass fraction of caprolactam was 98%, the mass fraction of α-dimethylamino-ε-caprolactam was 2%, and the mass of water was 10% of the mass of caprolactam, resulting in a first copolymer (relative viscosity 2.405). The first copolymer included a first repeating unit as shown in formula (6) and a second repeating unit as shown in formula (7). Equation (6) Equation (7) Nuclear magnetic resonance (NMR) test 1 HNMR) such as Figure 1 As shown, the yield was 90%, and the molar content x of the first repeating unit was 0.01 and the molar content y of the second repeating unit was 0.99, as determined by NMR. The melting point was 216 °C.

[0074] S2. Dissolve 10g of the first copolymer from step S1 in 100g of trifluoroethanol and 0.94g of 1,4-dibromobutane, mix in a 250mL three-necked flask, and react at 65°C for 24h. The molar ratio of the first copolymer (based on tertiary amine) to 1,4-dibromobutane is 1:5, and the mass ratio of the first copolymer to trifluoroethanol is 1:10. The reaction product is subjected to rotary evaporation. The evaporated solid is washed with ethanol to obtain a crosslinked copolyamide quaternary ammonium compound, which includes the structure shown in formula (1-1). Equation (1-1), where R3 is butylene.

[0075] The storage modulus of this quaternary ammonium compound is as follows: Figure 2 As shown, the energy storage modulus exhibits a clear plateau at low frequencies; the viscosity variation of this quaternary ammonium compound is as follows. Figure 3 As shown, the crosslinked copolyamide quaternary ammonium compound exhibits high viscosity. The viscosity decreases with increasing frequency, further demonstrating that a crosslinked copolyamide quaternary ammonium compound was prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0076] Example 2 S1. 1.1 g of α-dimethylamino-ε-caprolactam, 20 g of caprolactam, and 2 g of water were added to a 50 mL high-pressure reactor. The reaction system was purged with nitrogen at room temperature and a ring-opening polymerization reaction was carried out under a nitrogen atmosphere. The stirring speed was 120 rpm, and the reaction was maintained at 180°C and 1.1 MPa for 3 h. Then the temperature was increased to 220°C and 1.8 MPa and maintained for 2 h (high-pressure polymerization stage). After that, the pressure was reduced to -0.7 MPa and 200°C and the reaction was continued for 1 h (low-pressure polymerization stage). In the polymerization reaction system, the mass fraction of caprolactam was 95%, the mass fraction of α-dimethylamino-ε-caprolactam was 5%, and the mass of water was 10% of the mass of caprolactam. The first copolymer (relative viscosity 2.401) was obtained. The first copolymer included a first repeating unit as shown in formula (6) and a second repeating unit as shown in formula (7). Equation (6) Equation (7) The molar content x of the first repeating unit is 0.03, the molar content y of the second repeating unit is 0.97, and the melting point is 211°C.

[0077] S2. Dissolve 10 g of the first copolymer from S1 in 100 g of trifluoroethanol and 2.84 g of 1,4-dibromobutane, add the mixture to a 250 mL three-necked flask, and react at 65°C for 24 h. The molar ratio of the first copolymer (based on tertiary amine) to 1,4-dibromobutane is 1:5, and the mass ratio of the first copolymer to trifluoroethanol is 1:10. The reaction product is subjected to rotary evaporation, and the evaporated solid is washed with ethanol to obtain a crosslinked copolyamide quaternary ammonium compound. The quaternary ammonium compound comprises the structure shown in formula (1-1); Equation (1-1), where R3 is butylene.

[0078] The storage modulus of this quaternary ammonium compound is as follows: Figure 2 As shown, the energy storage modulus exhibits a clear plateau at low frequencies; the viscosity variation of this quaternary ammonium compound is as follows. Figure 3 As shown, the crosslinked copolyamide quaternary ammonium compound exhibits high viscosity. The viscosity decreases with increasing frequency, further demonstrating that a crosslinked copolyamide quaternary ammonium compound was prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0079] Example 3 S1. 2.2 g of α-dimethylamino-ε-caprolactam, 20 g of caprolactam, and 2 g of water were added to a 50 mL high-pressure reactor. The reaction system was purged with nitrogen at room temperature and a ring-opening polymerization reaction was carried out under a nitrogen atmosphere. The stirring speed was 120 rpm, and the reaction was maintained at 180°C and 1.1 MPa for 3 h. Then the temperature was increased to 220°C and 1.8 MPa and maintained for 2 h (high-pressure polymerization stage). After that, the pressure was reduced to -0.7 MPa and 200°C and the reaction was continued for 1 h (low-pressure polymerization stage). In the polymerization reaction system, the mass fraction of caprolactam was 90%, the mass fraction of α-dimethylamino-ε-caprolactam was 10%, and the mass of water was 10% of the mass of caprolactam. The first copolymer (relative viscosity 2.398) was obtained. The first copolymer included a first repeating unit as shown in formula (6) and a second repeating unit as shown in formula (7). Equation (6) Equation (7) The molar content x of the first repeating unit is 0.05, the molar content y of the second repeating unit is 0.95, and the melting point is 203°C.

[0080] S2. Dissolve 10 g of the first copolymer from S1 in 100 g of trifluoroethanol and 4.73 g of 1,4-dibromobutane, add to a 250 mL three-necked flask and mix. React at 65 °C for 24 h. The molar ratio of the first copolymer (based on tertiary amine) to 1,4-dibromobutane is 1:5, and the mass ratio of the first copolymer to trifluoroethanol is 1:10. The reaction product is subjected to rotary evaporation, and the solid after evaporation is washed with ethanol to obtain a crosslinked copolyamide quaternary ammonium compound, which includes the structure shown in formula (1-1). Equation (1-1), where R3 is butylene.

[0081] The storage modulus of this quaternary ammonium compound is as follows: Figure 2 As shown, the energy storage modulus exhibits a clear plateau at low frequencies; the viscosity variation of this quaternary ammonium compound is as follows. Figure 3 As shown, the crosslinked copolyamide quaternary ammonium compound exhibits high viscosity. The viscosity decreases with increasing frequency, further demonstrating that a crosslinked copolyamide quaternary ammonium compound was prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0082] Example 4 S1. Add 3.5g of α-dimethylamino-ε-caprolactam, 20g of caprolactam, and 2g of water to a 50mL high-pressure reactor. At room temperature, the reaction system is purged with nitrogen and a ring-opening polymerization reaction is carried out under a nitrogen atmosphere. The stirring speed is 120 rpm, and the reaction is maintained at 180°C and 1.1MPa for 3h. Then, the temperature is raised to 220°C and 1.8MPa and maintained for 2h (high-pressure polymerization stage). After that, the pressure is reduced to -0.7MPa and 200°C and the reaction continues for 1h (low-pressure polymerization stage). In the polymerization reaction system, the mass fraction of caprolactam is 85%, the mass fraction of α-dimethylamino-ε-caprolactam is 15%, and the mass of water is 10% of the mass of caprolactam. The first copolymer (relative viscosity 2.380) is obtained as shown below. The first copolymer includes a first repeating unit as shown in formula (6) and a second repeating unit as shown in formula (7). Equation (6) Equation (7) The molar content x of the first repeating unit is 0.08, the molar content y of the second repeating unit is 0.92, and the melting point is 190°C.

[0083] S2. Dissolve 10g of the first copolymer from S1 in 100g of trifluoroethanol and 7.57g of 1,4-dibromobutane, add to a 250mL three-necked flask and mix. React at 65°C for 24h. The molar ratio of the first copolymer (based on tertiary amine) to 1,4-dibromobutane is 1:5, and the mass ratio of the first copolymer to trifluoroethanol is 1:10. The reaction product is subjected to rotary evaporation, and the evaporated solid is washed with ethanol to obtain a crosslinked copolyamide quaternary ammonium compound. This quaternary ammonium compound has the structure shown in formula (1-1). Equation (1-1), where R3 is butylene.

[0084] The storage modulus of this quaternary ammonium compound is as follows: Figure 2 As shown, the energy storage modulus exhibits a clear plateau at low frequencies; the viscosity variation of this quaternary ammonium compound is as follows. Figure 3 As shown, the crosslinked copolyamide quaternary ammonium compound exhibits high viscosity. The viscosity decreases with increasing frequency, further demonstrating that a crosslinked copolyamide quaternary ammonium compound was prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0085] Example 5 The method in this embodiment is the same as in Example 4, except that the crosslinking reaction temperature in S2 is 95°C and the time is 13 hours. Testing showed that the quaternary ammonium compound exhibited a significant plateau in its storage modulus at low frequencies; furthermore, the viscosity of this quaternary ammonium compound was lower than that in Example 4, indicating that a crosslinked copolyamide quaternary ammonium compound was successfully prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0086] Example 6 The method in this embodiment is the same as in Example 4, except that: the amount of 1,4-dibromobutane used in S2 is 4.54 g, and the molar ratio of tertiary amine to 1,4-dibromobutane in the first copolymer is 1:3. Testing showed that the storage modulus of this quaternary ammonium compound exhibited a clear plateau at low frequencies, and the viscosity of this quaternary ammonium compound was lower than that in Example 4, indicating that a crosslinked copolyamide quaternary ammonium compound was successfully prepared in this embodiment. Melting point, tensile strength, zero-shear viscosity, and degree of crosslinking are shown in Table 1.

[0087] Comparative Example 1 S1. 3.5 g of α-dimethylamino-ε-caprolactam, 20 g of caprolactam, and 2 g of water were added to a 50 mL high-pressure reactor. The reaction system was purged with nitrogen at room temperature, and ring-opening polymerization was carried out under a nitrogen atmosphere. The stirring speed was 120 rpm, and the reaction was maintained at 180°C and 1.1 MPa for 3 h. Then, the temperature was increased to 220°C and 1.8 MPa and maintained for 2 h (high-pressure polymerization stage). Afterward, the pressure was reduced to -0.7 MPa and the reaction was continued at 200°C for 1 h. In the polymerization system, the mass fraction of caprolactam was 85%, the mass fraction of α-dimethylamino-ε-caprolactam was 15%, and the mass of water was 10% of the mass of caprolactam, resulting in the first copolymer shown below (relative viscosity 2.380). The first copolymer includes a first repeating unit as shown in formula (6) and a second repeating unit as shown in formula (7). Equation (6) Equation (7) The molar content x of the first repeating unit is 0.08, the molar content y of the second repeating unit is 0.92, and the melting point is 190°C.

[0088] S2. Dissolve 10g of the first copolymer from S1 in 100g of trifluoroethanol and 1.1g of 1,4-dibromobutane, and add the mixture to a 250mL three-necked flask. React at 65°C for 24h. The molar ratio of the tertiary amine to 1,4-dibromobutane in the first copolymer is 1:0.7, and the mass ratio of the first copolymer to trifluoroethanol is 1:10. The reaction product is rotary evaporated, and the solid after evaporation is washed with ethanol to obtain a copolymer of dimethylaminocaprolactam and caprolactam. The storage modulus of this copolymer is as follows: Figure 2 As shown, there is no plateau in the storage modulus at low frequencies; the viscosity of the copolymer changes as follows. Figure 3 As shown, the viscosity is low, and the viscosity of the copolymer does not change significantly with increasing frequency, further indicating that the copolyamide quaternary ammonium compound without cross-linking structure was not obtained in this comparative example. The copolymer obtained in this comparative example has a melting point of 215℃ and a tensile strength of 49MPa.

[0089] Comparative Example 2 20 g of caprolactam and 2 g of water were added to a 50 mL high-pressure reactor. The reaction system was purged with nitrogen at room temperature, and ring-opening polymerization was carried out under a nitrogen atmosphere. The stirring speed was 120 rpm, and the reaction was maintained at 180°C and 1.1 MPa for 3 h. Then, the temperature was increased to 220°C and maintained at 1.8 MPa for 2 h (high-pressure polymerization stage). Afterward, the pressure was reduced to -0.7 MPa and the reaction was continued at 200°C for 1 h (low-pressure polymerization stage), yielding nylon 6 (PA6) with a yield of 93% and a melting point of 218°C. The storage modulus of nylon 6 is as follows: Figure 2 As shown, there is no plateau in the energy storage modulus at low frequencies; viscosity changes as follows: Figure 3 As shown, the viscosity is low, and the viscosity of the copolymer does not change significantly with increasing frequency, indicating that no cross-linked structure has been formed.

[0090] Table 1

[0091] Based on the examples, comparative examples, and the data in Table 1, it can be seen that the method disclosed herein does not require a catalyst, the process is easy to control, and it is easy to mass-produce industrially. Compared with comparative examples 1-2, the copolyamide quaternary ammonium compound disclosed herein has a higher degree of swelling and zero-shear viscosity, an increased degree of crosslinking of the polymer, and the copolymer has better mechanical properties.

[0092] A comparison of Examples 4 and 5 shows that, within the preferred crosslinking reaction conditions of this disclosure, the obtained crosslinked copolyamide quaternary ammonium compound has superior mechanical properties.

[0093] A comparison of Examples 4 and 6 shows that, within the preferred molar ratio range of the first copolymer to the halogenated hydrocarbon reagent in this disclosure, the obtained crosslinked copolyamide quaternary ammonium compound exhibits superior mechanical properties.

[0094] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0095] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0096] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A crosslinked copolyamide quaternary ammonium compound, characterized in that, The quaternary ammonium compound is a quaternary ammonium salt containing a crosslinked copolyamide quaternary ammonium cation; the crosslinked copolyamide quaternary ammonium cation includes a first structural unit as shown in formula (1) and a second structural unit as shown in formula (2). Equation (1) Equation (2) wherein R1, R2each independently includes a substituted or unsubstituted C 1-30 aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 aliphatic hydrocarbon group, substituted or unsubstituted C 6-18 one or more of aryl groups, or R1, R2are connected to each other and the N to which they are connected together form a 5-7 membered aliphatic ring; R3comprises one or more of substituted or unsubstituted C 1-30 substituted or unsubstituted C 3-12 substituted or unsubstituted C 6-18 substituted or unsubstituted C R1, R2, R3substituents each independently include one or more of C 1~10 alkyl, C 6~10 aryl, and C 3~10 heteroaryl.

2. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, R1 and R2 each independently include substituted or unsubstituted C. 1-20 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; preferably, R1 and R2 are the same; R3 includes substituted or unsubstituted C. 1-20 aliphatic hydrocarbon group, substituted or unsubstituted C 3-10 alicyclic hydrocarbon group, substituted or unsubstituted C 6-15 One or more of the aryl groups; The substituents of R1, R2, and R3 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, phenyl, and furanyl.

3. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, R1 and R2 each independently include one or more of the following: methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl, and nonylphenyl; R3 includes one or more of the following: methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene.

4. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, The first structural unit shown in equation (1) includes: 。 5. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, In the crosslinked copolyamide, the molar content x of the first structural unit is 0.01~0.08, and the molar content y of the second structural unit is 0.92~0.99; wherein, x+y=1.

6. The crosslinked copolyamide quaternary ammonium compound according to claim 5, wherein, The crosslinked copolyamide quaternary ammonium cation also includes a third structural unit as shown in formula (3). Equation (3) The molar content z of the third structural unit is 0.01~0.08, and the value of x+z is 0.01~0.

08.

7. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, The swelling degree of the cross-linked copolyamide quaternary ammonium cation is 19~45.

8. The crosslinked copolyamide quaternary ammonium compound according to claim 1, wherein, The anion of the quaternary ammonium salt includes a halide ion, which includes Cl-. - ,Br - and I - One or more of the following, preferably Br - .

9. A method for preparing crosslinked copolyamide quaternary ammonium compounds, characterized in that, The method includes the following steps: S1. Caprolactam and caprolactam with nitrogen-containing side groups are polymerized with water to obtain the first copolymer; S2. The first copolymer, the haloalkane reagent, and the solvent are brought into contact to carry out a crosslinking reaction, wherein the molar ratio of the first copolymer to the haloalkane reagent, based on the tertiary amine, is 1:1 to 10. The caprolactam having nitrogen-containing side groups has the structure shown in formula (4), and the haloalkane reagent has the structure shown in formula (5). Equation (4) X1-R3-X2, Equation (5). R1 and R2 each independently include substituted or unsubstituted C. 1-30 Aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 Alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more of the aryl groups, or R1 and R2 connected to each other and together with the N connected to them, form a 5-7 membered aliphatic ring; R3 includes substituted or unsubstituted C. 1-30 aliphatic hydrocarbon group, substituted or unsubstituted C 3-12 alicyclic hydrocarbon group, substituted or unsubstituted C 6-18 One or more aryl groups; X1 and X2 may be the same or different, each being an independent halogen group.

10. The method according to claim 9, wherein, R1 and R2 each independently include one or more of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, nonyl, undecyl, cyclopropyl, cyclopentyl, cyclohexyl, phenyl, benzyl, heptylphenyl, octylphenyl and nonylphenyl; preferably one or more of methyl, ethyl, propyl, cyclohexyl, phenyl and benzyl.

11. The method according to claim 9, wherein, The caprolactam having nitrogen-containing side groups includes one or more of the following structures: 。 12. The method according to claim 9, wherein, R3 includes one or more of methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, decylene, nonylene, undecylene, cyclopropylene, cyclopentylene, cyclohexylene, phenylene, benzylene, heptylphenylene, octylphenylene, and nonylphenylene; preferably one or more of butylene, hexylene, octylene, and decylene. X1 and X2 each independently include one or more of Cl, Br and I, preferably Br; preferably X1 and X2 are the same. Optionally, the halocarbon reagent includes one or more of 1,4-dibromobutane, 1,6-dibromohexane, 1,8-dibromooctane, and 1,10-dibromodecane.

13. The method according to claim 9, wherein, In step S1, the conditions for the polymerization reaction include: the polymerization temperature is 200~250℃, and the polymerization time is 8~12h; In the polymerization system, the mass fraction of caprolactam is 85-99%, the mass fraction of caprolactam with nitrogen-containing side groups is 1-15%, and the mass of water is 3-10% of the mass of caprolactam.

14. The method according to claim 9, wherein, In step S2, the conditions for the crosslinking reaction include: the temperature of the crosslinking reaction is 50~80℃, and the time of the crosslinking reaction is 8~12h.

15. The method according to claim 9, wherein, In step S2, the molar ratio of the first copolymer (based on tertiary amine) to the haloalkane reagent is 1:4~6.

16. The method according to claim 9, wherein, In step S2, the solvent includes a fluorinated organic solvent; the fluorinated organic solvent includes one or more of trifluoroethanol and hexafluoroisopropanol, preferably trifluoroethanol; The mass ratio of the first copolymer to the solvent is 1:5~20, preferably 1:8~12.

17. The crosslinked copolyamide prepared by the method according to any one of claims 9 to 16.

18. The crosslinked copolyamide according to claim 17, wherein, The crosslinked copolyamide has a melting point of 170~213℃, a tensile strength of 55~80MPa, and a zero-shear viscosity of 1900~350000Pa / s at 230℃.

19. Use of the crosslinked copolyamide quaternary ammonium compound according to any one of claims 1-8 and 17-18.

Citation Information

Patent Citations

  • Nylon polymer and preparation method thereof

    CN104558588A

  • Antibacterial nylon 6 material as well as preparation method and application thereof

    CN115707727A