Self-healing fluorescent organosilicon materials and their preparation methods

By preparing self-healing fluorescent organosilicon materials, the problems of limited service life and poor mechanical strength of organosilicon materials have been solved, achieving high strength and fluorescence properties, making them suitable for applications in multiple fields.

CN123107091APending Publication Date: 2026-11-17BEIJING UNIV OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510628157.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing organosilicon materials have problems such as limited service life, poor mechanical strength, and environmental pollution. Moreover, most of them are thermosetting materials, which are difficult to achieve self-repair.

Method used

The method for preparing self-healing fluorescent organosilicon materials includes reacting 2-amino-4-hydroxy-6-methylpyrimidine with hexamethylene diisocyanate to generate a monoisocyanate-terminated ureidopyrimidinone (UPy-HDI), and reacting it with linearly side-terminated methylaminoethylaminopropyl polysiloxane, a nitrogen-containing aromatic compound and a metal salt to form a self-healing material with fluorescent effects.

Benefits of technology

While maintaining thermal stability, the mechanical strength of the organosilicon material was significantly improved, and its fluorescent properties were endowed, thus realizing the material's self-healing ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107091A_ABST
    Figure CN123107091A_ABST
Patent Text Reader

Abstract

This invention discloses a self-healing fluorescent organosilicon material and its preparation method. The self-healing fluorescent organosilicon material is obtained by sequentially reacting linear side-terminated methylaminoethylaminopropyl polymethylsiloxane with a nitrogen-containing aromatic compound, a ureidopyrimidinone, and a metal salt, followed by curing. The side-terminated methylaminoethylaminopropyl polymethylsiloxane has a molecular weight range of 1000-100000 g / mol and an ammonia value range of 0.1-0.9. Its specific structure is as follows: the nitrogen-containing aromatic compound includes one or more of imidazole-2-carboxaldehyde, dimethylpyridineacrylamide, pyridine-4-carboxaldehyde, and 4-isocyanate pyridine; the ureidopyrimidinone is end-capped with hexamethylene diisocyanate; the metal salt includes one or more of ZnCl2, ZnSO4, (CH3COO)2Zn, FeCl3, Fe2(SO4)3, La(NO3)3·6H2O, and Eu(NO3)3·6H2O.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organosilicon polymer technology, specifically to self-healing fluorescent organosilicon materials and their preparation methods. Background Technology

[0002] Organosilicon materials are mainly derived from mineral resources, exhibiting relatively low dependence on petrochemical resources and possessing unique and excellent physicochemical properties, such as resistance to high and low temperatures, resistance to UV aging, good biocompatibility, and hydrophobicity. These properties make them important in aerospace, electronics, biotherapy, and daily chemical textiles. However, most organosilicon materials are currently thermosetting, resulting in limited lifespan and environmental pollution after disposal. Furthermore, due to their low cohesive energy, organosilicon materials also suffer from poor mechanical properties. Therefore, developing an organosilicon material with high mechanical properties and the ability to autonomously repair damage under external stimuli is of significant research and practical importance. Organosilicon fluorescent materials are a class of functional materials that combine the excellent properties of organosilicon compounds with their fluorescent characteristics, and have diverse applications: such as displays and lighting: in display technologies such as OLED, QLED, and LED, the high quantum efficiency and thermal stability of organosilicon fluorescent materials can improve the brightness and color purity of devices, while extending their lifespan; imaging and diagnosis, drug tracking and treatment: their excellent biocompatibility and low toxicity make them suitable for in vivo fluorescent labeling and targeted drug delivery, contributing to precision medicine and disease diagnosis and treatment; anti-counterfeiting and information security: their unique optical properties (such as excitation wavelength dependence) can be used for high-security anti-counterfeiting of banknotes and certificates, or for encrypted data storage.

[0003] In recent years, researchers have successfully prepared a series of self-healing organosilicon materials by introducing dynamic interactions such as hydrogen bonds, metal ligand coordination bonds, dynamic disulfide bonds, dynamic imine bonds, and borate ester bonds. In patent CN202410099519.3, Liu Tong et al. simultaneously introduced flexible and rigid monomers capable of forming supramolecular interactions into polydimethylsiloxane, forming a structure with alternating rigid and flexible chain segments, achieving toughening and self-healing effects, but with relatively low overall mechanical strength. In patent CN202410009609.9, Li Mei et al. reacted salicylaldehyde with 2-amino-1,3-propanediol and introduced the product as a chain extender into polydimethylsiloxane. Subsequently, zinc chloride was added for metal coordination to prepare a high-strength organosilicon-modified polyurea coating. Summary of the Invention

[0004] This invention provides a self-healing fluorescent organosilicon material and its preparation method. Compared with the above-mentioned technical solutions, the advantages of this invention are: while retaining thermal stability, it improves the mechanical strength of the organosilicon material, and the material has a fluorescent effect.

[0005] The technical solution of the present invention is as follows: a method for preparing self-healing fluorescent organosilicon materials, comprising the following steps:

[0006] (1) 2-Amino-4-hydroxy-6-methylpyrimidine is reacted with hexamethylene diisocyanate to obtain a monoisocyanate-terminated ureidopyrimidinone, abbreviated as UPy-HDI.

[0007] (2) Weigh 2g of linear methylaminoethylaminopropyl polysiloxane and 0.02-0.50g of nitrogen-containing aromatic compound, dissolve them and add them to a three-necked flask equipped with a spherical condenser and a magnetic stirrer. Purge with nitrogen and stir continuously.

[0008] (3) Weigh 0.10-0.50g of UPy-HDI, dissolve it in chloroform and add it to a three-necked flask, stirring continuously.

[0009] (4) Weigh 0.02-0.20g of metal salt, dissolve it and add it to a three-necked flask. Stir continuously to react, then evaporate the solvent and solidify to obtain a self-healing fluorescent organosilicon material.

[0010] In step (2), the solvent includes tetrahydrofuran or chloroform, the reaction temperature is 60-120℃, and the reaction time is 4-24h.

[0011] In step (3), the reaction temperature is 60-100℃ and the reaction time is 3-6h.

[0012] In step (4), the solvent includes anhydrous methanol or anhydrous ethanol, and the metal salt concentration is 0.001-0.05 g / mL; the reaction temperature is 25-120℃, and the reaction time is 1-12 h; the solvent is evaporated at room temperature for 6-24 h, or more specifically 10-18 h; the curing temperature is 60-100℃, and the curing time is 8-24 h, or more specifically 12-16 h. Attached Figure Description

[0013] Figure 1 This is a tensile curve of the self-healing fluorescent organosilicon material prepared in Example 2 of the present invention, with a tensile strength and elongation at break of 3.80 MPa and 199%, respectively.

[0014] Figure 2 The figure shows the TGA curve of the self-healing fluorescent organosilicon material prepared in Example 3 of this invention. The data in the figure show that the temperature at which the mass loss is 10% is 380.6℃, and the residual weight at 800℃ is 10.61%.

[0015] Figure 3 This is the fluorescence spectrum of the self-healing fluorescent organosilicon material prepared in Example 4 of the present invention at an excitation wavelength of 365 nm.

[0016] Figure 4This is a self-healing fluorescent organosilicon material prepared in Example 5 of the present invention under a 365nm ultraviolet lamp. The material prepared in Example 5 was cut with a blade and placed at 80°C for 24 hours to repair itself. Detailed Implementation

[0017] The present invention will be further described below with reference to specific embodiments and accompanying drawings. It should be noted that the specific embodiments described are only for illustrating the present invention and are not intended to limit the scope of the present invention.

[0018] Example 1

[0019] (1) Weigh 2.50 g of 2-amino-4-hydroxy-6-methylpyrimidine and 22.50 mL of hexamethylene diisocyanate into a 100 mL three-necked flask, add 6 mL of pyridine, purge with high-purity nitrogen, and stir continuously at 100 °C for 16 h; pour the liquid obtained from the reaction into 250 mL of n-hexane for reverse precipitation and filter under reduced pressure, and dry under vacuum to obtain UPy-HDI.

[0020] (2) Take 2g of methylaminoethylaminopropyl polysiloxane (molecular weight 1000g / mol, ammonia value 0.8) and dissolve it completely in 10mL of tetrahydrofuran, and add 0.04g of imidazole-2-carboxaldehyde (dissolved in 5mL of tetrahydrofuran) to it, and react at 60℃ for 24h.

[0021] (3) Weigh 0.12g of UPy-HDI and dissolve it completely in 5mL of chloroform and add it to a three-necked flask. React at 80℃ for 4h.

[0022] (4) Weigh 0.02g of zinc chloride and dissolve it completely in 3mL of anhydrous methanol and add it to a three-necked flask. React at 60℃, transfer it to a mold and evaporate the solvent at room temperature in a fume hood. Then transfer it to an 80℃ oven and cure for 12h to obtain the target product.

[0023] Example 2

[0024] (1) Weigh 2.50 g of 2-amino-4-hydroxy-6-methylpyrimidine and 22.50 mL of hexamethylene diisocyanate into a 100 mL three-necked flask, add 6 mL of pyridine, purge with high-purity nitrogen, and stir continuously at 100 °C for 16 h; pour the liquid obtained from the reaction into 250 mL of n-hexane for reverse precipitation and filter under reduced pressure, and dry under vacuum to obtain UPy-HDI.

[0025] (2) Take 2g of methylaminoethylaminopropyl polysiloxane (molecular weight 1000g / mol, ammonia value 0.8) and dissolve it completely in 10mL of tetrahydrofuran, and add 0.08g of imidazole-2-carboxaldehyde (dissolved in 10mL of tetrahydrofuran) to it, and react at 60℃ for 24h.

[0026] (3) Weigh 0.23g of UPy-HDI, dissolve it completely in 15mL of chloroform, and add it to a three-necked flask. React at 80℃ for 4h.

[0027] (4) Weigh 0.03g of zinc chloride and dissolve it completely in 3mL of anhydrous methanol and add it to a three-necked flask. React at 60℃, transfer it to a mold and evaporate the solvent at room temperature in a fume hood. Then transfer it to an 80℃ oven and cure for 12h to obtain the target product.

[0028] Example 3

[0029] (1) Weigh 2.50 g of 2-amino-4-hydroxy-6-methylpyrimidine and 22.50 mL of hexamethylene diisocyanate into a 100 mL three-necked flask, add 6 mL of pyridine, purge with high-purity nitrogen, and stir continuously at 100 °C for 16 h; pour the liquid obtained from the reaction into 250 mL of n-hexane for reverse precipitation and filter under reduced pressure, and dry under vacuum to obtain UPy-HDI.

[0030] (2) Take 2g of methylaminoethylaminopropyl polysiloxane (molecular weight 1000g / mol, ammonia value 0.8) and dissolve it completely in 10mL of tetrahydrofuran, and add 0.12g of imidazole-2-carboxaldehyde (dissolved in 10mL of tetrahydrofuran) to it, and react at 60℃ for 24h.

[0031] (3) Weigh 0.12g of UPy-HDI and dissolve it completely in 5mL of chloroform and add it to a three-necked flask. React at 80℃ for 4h.

[0032] (4) Weigh 0.04g of zinc chloride and dissolve it completely in 3mL of anhydrous methanol and add it to a three-necked flask. React at 60℃, transfer to a mold and evaporate the solvent at room temperature in a fume hood. Transfer to an 80℃ oven and cure for 12h to obtain the target product.

[0033] Example 4

[0034] (1) Weigh 3.00 g of dimethylpyridinium amine and dissolve it in 30 mL of anhydrous chloroform. Add 1.83 g of ultra-dry triethylamine and 1.64 g of acryloyl chloride to it and react at room temperature for 16 h. Then wash thoroughly with deionized water and separate the liquid. Collect the oil phase, dry it with anhydrous sodium sulfate, and then rotary evaporate it at 45 °C to obtain dimethylpyridinium acrylamide.

[0035] (2) Weigh 2.50 g of 2-amino-4-hydroxy-6-methylpyrimidine and 22.50 mL of hexamethylene diisocyanate into a 100 mL three-necked flask, add 6 mL of pyridine, purge with high-purity nitrogen, and stir continuously at 100 °C for 16 h; pour the liquid obtained from the reaction into 250 mL of n-hexane for reverse precipitation and filter under reduced pressure, and dry under vacuum to obtain UPy-HDI.

[0036] (3) Take 2g of methylaminoethylaminopropyl polysiloxane (molecular weight 1000g / mol, ammonia value 0.8) and dissolve it completely in 10mL of chloroform, and add 0.40g of dimethylpyridineacrylamide (dissolved in 5mL of chloroform) to it, and react at 60℃ for 24h.

[0037] (4) Weigh 0.12g of UPy-HDI and dissolve it completely in 5mL of chloroform and add it to a three-necked flask. React at 80℃ for 4h.

[0038] (4) Weigh 0.11g of zinc chloride and dissolve it completely in 5mL of anhydrous ethanol and add it to a three-necked flask. React at 60℃, transfer it to a mold and evaporate the solvent at room temperature in a fume hood. Then transfer it to an 80℃ oven and cure for 12h to obtain the target product.

[0039] Example 5

[0040] (1) Weigh 3.00 g of dimethylpyridinium amine and dissolve it in 30 mL of anhydrous chloroform. Add 1.83 g of ultra-dry triethylamine and 1.64 g of acryloyl chloride to it and react at room temperature for 16 h. Then wash thoroughly with deionized water and separate the liquid. Collect the oil phase, dry it with anhydrous sodium sulfate, and then rotary evaporate it at 45 °C to obtain dimethylpyridinium acrylamide.

[0041] (2) Weigh 2.50 g of 2-amino-4-hydroxy-6-methylpyrimidine and 22.50 mL of hexamethylene diisocyanate into a 100 mL three-necked flask, add 6 mL of pyridine, purge with high-purity nitrogen, and stir continuously at 100 °C for 16 h; pour the liquid obtained from the reaction into 250 mL of n-hexane for reverse precipitation and filter under reduced pressure, and dry under vacuum to obtain UPy-HDI.

[0042] (3) Take 2g of methylaminoethylaminopropyl polysiloxane (molecular weight 1000g / mol, ammonia value 0.8) and dissolve it completely in 10mL of chloroform, and add 0.40g of dimethylpyridineacrylamide (dissolved in 5mL of chloroform) to it, and react at 60℃ for 24h.

[0043] (4) Weigh 0.47g of UPy-HDI, dissolve it completely in 20mL of chloroform, and add it to a three-necked flask. React at 80℃ for 4h.

[0044] (4) Weigh 0.11g of zinc chloride and dissolve it completely in 5mL of anhydrous ethanol and add it to a three-necked flask. React at 60℃, transfer it to a mold and evaporate the solvent at room temperature in a fume hood. Then transfer it to an 80℃ oven and cure for 12h to obtain the target product.

[0045] Appendix Explanation

Claims

1. A self-healing fluorescent organosilicon material, characterized in that, A linear side-chain methylaminoethylaminopropyl polysiloxane is grafted with a nitrogen-containing aromatic compound and a monoisocyanate-terminated ureidopyrimidinone, and a metal salt is introduced. Metal ligand coordination bonds and hydrogen bonds between the side chains act as physical crosslinking points, forming a dynamic double-crosslinked network structure. The side-chain methylaminoethylaminopropyl polysiloxane has a molecular weight range of 1000-100000 g / mol and an ammonia value range of 0.1-0.

9. The specific structure is shown below: The nitrogen-containing aromatic compounds include one or more of imidazole-2-carboxaldehyde, dimethylpyridineacrylamide, pyridine-4-carboxaldehyde, and 4-isocyanate pyridine; the metal salts include one or more of ZnCl2, ZnSO4, (CH3COO)2Zn, FeCl3, Fe2(SO4)3, La(NO3)3·6H2O, and Eu(NO3)3·6H2O.

2. The molecular weight of the methylaminoethylaminopropyl polysiloxane according to claim 1 is in the range of 1000-100000 g / mol, and the ammonia value is in the range of 0.1-0.9, preferably 0.6-0.

8.

3. The self-healing fluorescent organosilicon material according to claim 1, characterized in that, Nitrogen-containing aromatic compounds are grafted onto linear side-terminated methylaminoethylaminopropyl polysiloxane chains using amino-aldehyde Schiff base reaction, amino-double bond Michael addition reaction, or amino-isocyanate group addition reaction.

4. The self-healing fluorescent organosilicon material according to claim 1, characterized in that... A monoisocyanate-terminated ureidopyrimidinone was grafted onto a linearly side-terminated methylaminoethylaminopropyl polysiloxane chain using an amino-isocyanate group addition reaction.

5. The self-healing fluorescent organosilicon material according to claim 1, characterized in that, In nitrogen-containing aromatic compounds, nitrogen atoms form metal ligand coordination bonds with metal ions.

6. The self-healing fluorescent organosilicon material according to claim 1, characterized in that, Ureidinones form quadruple hydrogen bonds with each other.

7. The self-healing fluorescent organosilicon material according to claim 1, characterized in that, Includes the following steps: (1) 2-amino-4-hydroxy-6-methylpyrimidine was reacted with hexamethylene diisocyanate to obtain a monoisocyanate-terminated ureidopyrimidinone; (2) In the first solution, the side-methylaminoethylaminopropylpolysiloxane reacts with a nitrogen-containing aromatic compound to obtain polymer 1; (3) In the second solution, polymer 1 reacts with a monoisocyanate-terminated ureidopyrimidinone to obtain polymer 2; (4) In the third solution, polymer 2 reacts with the metal salt, and then the solvent is removed and the mixture is cured to obtain a self-healing fluorescent organosilicon material.

8. The preparation method according to claim 7, characterized in that, In step (2), the solvent includes tetrahydrofuran or chloroform, the reaction temperature is 60-120℃, and the reaction time is 4-24h.

9. The preparation method according to claim 7, characterized in that, In step (3), the solvent includes chloroform, the reaction temperature is 60-100℃, and the reaction time is 3-6h.

10. The preparation method according to claim 7, characterized in that, In step (4), the concentration of the metal salt is 0.001-0.05 g / mL; the solvent includes chloroform and anhydrous methanol or chloroform and anhydrous ethanol; the reaction temperature is 25-120℃; the reaction time is 1-12 h; the solvent is evaporated at room temperature for 6-24 h, or more specifically 10-18 h; the curing temperature is 60-100℃; the curing time is 8-24 h, or more specifically 12-16 h.

Citation Information

Patent Citations

  • Preparation method of Zn < 2 + > coordination-containing high-strength organic silicon modified polyurea marine antifouling coating

    CN117986984A

  • Toughening and self-repairing organic silicon elastomer based on supramolecular action and preparation method thereof

    CN118108945A