Nylon acid dye fixing agent and its preparation and fixing treatment methods

By introducing specific groups and modules into the nylon acid dye fixing agent and adopting a segmented preparation process, the problems of poor wet fastness and insufficient chlorine resistance of nylon fabrics have been solved, achieving comprehensive performance of high fastness, low color change, chlorine resistance, and excellent hand feel, which is suitable for dark-colored nylon and spandex blended fabrics.

CN123107097APending Publication Date: 2026-11-17KEKAI CHEMICAL (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611619450.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing acid dyes for nylon have poor wet fastness, and conventional fixing agents suffer from color changes, hard hand feel, and insufficient chlorine resistance, making it difficult to meet environmental regulations. In particular, there is a lack of ideal solutions in the application of dark nylon fabrics and spandex blended fabrics.

Method used

Using a bisphenol-free nylon acid dye fixing agent, a self-emulsifying nano-dispersion is formed by introducing a polydimethylsiloxane backbone, quaternary ammonium salt groups, thioether bonds and short hydrophobic alkyl groups into the molecular structure and using a segmented sequential preparation process. This dispersion is anchored to the fiber by electrostatic interaction and covalent bonds to construct a low surface energy film layer, achieving high fastness, low color change and chlorine resistance.

Benefits of technology

It improves the wet treatment fastness and chlorine resistance of nylon fabrics, maintains a good hand feel, meets environmental protection requirements, and is suitable for high chlorine resistance applications such as dark nylon swimwear and sports fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to a nylon acid dye fixing agent and its preparation and fixing treatment methods. The fixing agent is an aqueous dispersion with a zeta potential ≥ +30mV, a particle size of 20–100nm, and a solid content of 20%–40%. It uses polydimethylsiloxane as its molecular backbone, with side chains containing hydrophilic polyether segments, quaternary ammonium salt groups, C4–C10 short hydrophobic alkyl groups, and chlorine-resistant units containing sulfide bonds. The preparation employs a hydrosilylation and epoxy group-based process, controlled sequentially through "chlorine-resistant grafting – hydrophobic tailing – amination – quaternization" to achieve cationic dyeing, uniform distribution of chlorine-resistant modules, and covalent anchoring of residual epoxy. Testing shows that the treated nylon / spandex fabric exhibits a wash fastness of 4–5, spandex staining of 4, and after immersion in 50ppm available chlorine for 1 hour, spandex strength retention ≥85% and yellowing value ≤2.0. It is suitable for fixing and finishing nylon 6, nylon 66, and their blends with spandex.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organosilicon materials, specifically relating to a nylon acid dye fixing agent and its preparation and fixing treatment methods. Background Technology

[0002] Nylon (also known as polyamide fiber, mainly including nylon 6 and nylon 66) has excellent abrasion resistance, soft hand feel, and good elastic recovery. It is often blended with spandex (polyurethane elastic fiber) to form elastic fabrics, which are widely used in high-end sportswear, yoga pants, swimwear, underwear, and functional compression garments. Nylon fiber molecules contain a large number of terminal amino groups (-NH2). During dyeing, acid dyes or metal complex dyes are typically used, with dyeing occurring through ionic bonds between the sulfonate anions in the dye molecule and the cationized sites of the terminal amino groups on the fiber. However, acid dyes generally have poor wet fastness on nylon. During washing, water molecules can break the ionic and hydrogen bonds between the dye and fiber, causing dye to detach and stain other fibers (especially white or light-colored spandex components), severely affecting the appearance and wearing experience of the fabric.

[0003] To address this issue, the textile industry typically employs color-fixing agents for post-treatment of dyed nylon fabrics. Currently, color-fixing agents for acid dyes in nylon are mainly classified into four categories: cationic polymer type, anionic synthetic tannin type, reactive crosslinking type, and special chlorine-resistant composite type. Among them, cationic polyamine condensates can interact with acid dyes to form insoluble lakes and a protective film on the fiber surface, resulting in a significant improvement in wet fastness and making them the most widely used color-fixing agent in the industry. However, these products generally suffer from drawbacks such as noticeable color changes in the treated fabric, a stiffer hand feel, reduced light fastness, and poor compatibility with anionic textile auxiliaries. Anionic synthetic tannin type color-fixing agents have less interference with fabric color; however, traditional formulations often introduce regulated substances such as bisphenol S and phenol, and their effect on improving wet fastness of dark fabrics is weaker than that of cationic color-fixing agents, often requiring a two-stage treatment process. Reactive crosslinking fixing agents can achieve excellent water wash resistance by relying on covalent bonding, but they have problems such as difficult synthesis process, narrow pH window, and high production cost, making it difficult to promote on a large scale in industry.

[0004] Current nylon color-fixing technologies still face several common technical bottlenecks: incomplete removal of loose dye from the fabric surface easily induces color-fixing spots; color-fixing agents are prone to decomposition under high-temperature setting conditions (>160℃), causing yellowing of the fabric; and there is a contradiction between environmental regulations such as REACH and blue sign and high performance indicators such as chlorine resistance, low color change, and high lightfastness. Especially in high-chlorine-resistant applications such as dark-colored nylon swimwear and sports fabrics, conventional nonionic chlorine-resistant auxiliaries have limited effect on improving wash fastness. In particular, when nylon / spandex blended fabrics are used in swimming pools and similar settings, the poor chlorine resistance of conventional color-fixing agents remains unresolved. Furthermore, existing bio-based and nanocomposite modified color-fixing agents suffer from insufficient high-temperature stability and poor uniformity of water dispersion systems. Therefore, the industry urgently needs to develop a comprehensive nylon acid dye color-fixing agent that combines excellent wet fastness, low color change, chlorine and lightfastness, and meets environmental control requirements. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a bisphenol-free nylon acid dye fixing agent and its preparation and fixing methods. Starting with the molecular structure design of the fixing agent, specific groups and modules are introduced into its structure, using a small amount of residual epoxy in the fixing agent as an anchor point. This simultaneously imparts the functions of high-density dyeing with side-chain quaternary ammonium salts, chlorine-resistant module grafting, short hydrophobic chain external sliding, and self-emulsification of the polyether segment. A segmented sequential preparation process is employed, first chlorine-resistant grafting followed by quaternization, resulting in a novel bisphenol-free nylon acid dye fixing agent with new structure and properties. This effectively improves upon the aforementioned shortcomings of existing technologies and is particularly suitable for fixing acid dyes in chlorine-resistant nylon / spandex elastic fabrics.

[0006] The bisphenol-free nylon acid dye fixing agent provided by the present invention is an aqueous dispersion with a zeta potential ≥ +30mV, a particle size of 20–100nm, and a solid content of 20%–40%. The base material of the fixing agent comprises the following structural units: (a) It has a polydimethylsiloxane molecular backbone with polyether hydrophilic segments on the chain; (b) Contains a quaternary ammonium salt group, which is formed by a ring-opening reaction of a side chain epoxy group with a monofunctional compound containing a tertiary amino group and then by treatment with a quaternizing agent; (c) Contains short hydrophobic alkyl groups of C4-C10, which are linked to the siloxane skeleton via ether bonds; (d) Contains chlorine-resistant and antioxidant structural units, which are structural units containing sulfide bonds.

[0007] In this invention, the hydrophilic polyether segment endows the product with self-emulsifying ability, enabling the product to spontaneously form a uniform nano-dispersion in water; the quaternary ammonium salt group is formed by the ring-opening reaction of the side chain epoxy group and the monofunctional compound containing tertiary amino group, followed by quaternization treatment, which can efficiently capture the sulfonate anions of acid dyes through electrostatic interaction; the C4-C10 short hydrophobic alkyl group is linked to the siloxane backbone through ether bonds, and together with polydimethylsiloxane, it constitutes a low surface energy component, giving the fabric a hydrophobic and smooth feel; the chlorine-resistant and antioxidant structural unit containing sulfide bonds can preferentially react with active chlorine in chlorinated water environments, consume oxidizing substances, and protect spandex fibers from chlorine damage.

[0008] Preferably, the hydrophilic segment of the polyether is introduced by an allyl polyether epoxy compound, wherein the allyl polyether epoxy compound is an allyl polyoxyethylene ether glycidyl ether with 6 to 12 ethylene oxide units.

[0009] Preferably, the monofunctional compound containing a tertiary amino group is at least one of N-methylpiperazine, N-(3-dimethylaminopropyl)-methylamine, and N-(12-dimethylaminododecyl)-methylamine; the quaternizing agent is selected from at least one of dimethyl sulfate, chloromethane, and diethyl sulfate.

[0010] Preferably, the thioether-containing structural unit is introduced by a ring-opening reaction between a thiol-containing compound and an epoxy group on a silane chain, wherein the thiol-containing compound is at least one of mercaptoethanol and mercaptoacetic acid; the C4-C10 short hydrophobic alkyl group is introduced by a ring-opening reaction between a C4-C10 alkanol and a residual epoxy group in a silicon chain, wherein the C4-C10 alkanol is at least one of C4-C10 straight-chain alkanols.

[0011] The method for preparing the bisphenol-free nylon acid dye fixing agent provided by the present invention comprises the following steps: Preparation of dual-terminal and side-chain hydrogen-containing silicone oil by S1: Tetramethyldihydrodisiloxane, octamethylcyclotetrasiloxane, and tetramethylcyclotetrasiloxane are added to a reactor and stirred under nitrogen protection. Dry acidic clay solid catalyst, accounting for 1.5% to 5.0% of the total mass of raw materials, is added. Ring-opening polymerization is carried out at a controlled temperature of 50 to 60°C for 6 to 8 hours. After the reaction is completed, the mixture is cooled to room temperature and neutralized to neutral by dry method with sodium bicarbonate. Acidic clay and trace impurities are removed by filtration. Then, low-boiling substances are removed at 140 to 150°C under reduced pressure for 2 to 3 hours to obtain dual-terminal and side-chain hydrogen-containing silicone oil with complete SiH activity. The mass ratio of tetramethyldihydrodisiloxane, octamethylcyclotetrasiloxane, and tetramethylcyclotetrasiloxane is 1:10 to 20:3 to 8. S2 Preparation of Side-Chain / Terminal Group Epoxy Polyether Silicone Oil: The hydrogen-containing silicone oil with dual ends and side chains obtained in step S1 is subjected to a hydrosilylation reaction with a mixture of allyl glycidyl ether and allyl polyether epoxy compound in the presence of a platinum catalyst. The reaction temperature is 60-120℃ and the reaction time is 2-8h. The mass fraction of platinum metal based on the mass of the hydrogen-containing silicone oil is 4-20ppm. Epoxy polyether silicone oil with polyether segments in the side chains and epoxy groups in both the side chains and end groups is obtained. The molar ratio of allyl glycidyl ether to allyl polyether epoxy compound is 2-6:1. The total molar ratio of double bonds in the mixture to the SiH molar ratio of the hydrogen-containing silicone oil with dual ends and side chains obtained in step S1 is 0.90-1:1. The allyl polyether epoxy compound is allyl polyoxyethylene ether glycidyl ether with 6-12 ethylene oxide units. S3 Introducing chlorine-resistant and antioxidant structural units: Adding a mercapto-containing compound to the product obtained in step S2, and reacting with some epoxy groups to undergo a mercapto-epoxy ring-opening reaction, with a reaction temperature of 60-80℃ and a reaction time of 3-6h, to introduce structural units containing thioether bonds. S4 Introduction of short hydrophobic alkyl side chains: C4-C10 alkanols and catalysts are added to the product obtained in step S3 to undergo a ring-opening reaction with some residual epoxy groups. The reaction temperature is 90-110℃ and the reaction time is 4-6h. The C4-C10 short hydrophobic alkyl groups are grafted onto the siloxane side chains in the form of ether bonds. S5 Epoxy Ring-Opening Amination: The product obtained in step S4 is reacted with a monofunctional compound containing a tertiary amino group at a reaction temperature of 30–50 °C for 4–8 h, so that the residual epoxy group is ring-opened to introduce the tertiary amino group, while retaining a small amount of residual epoxy group. S6 Quaternization: The product obtained in step S5 is reacted with a quaternization reagent at a temperature of 50-85°C for 3-8 hours to convert the side chain tertiary amino group into a quaternary ammonium salt group. S7 Self-emulsifying water dispersion: The bulk product obtained in step S6 is dispersed in deionized water under stirring or high-speed shearing conditions at 40-70°C to obtain a bisphenol-free nylon acid dye fixing agent with a solid content of 20%-40%.

[0012] Preferably, the mercapto-containing compound in step S3 is at least one of mercaptoethanol and mercaptoacetic acid, and the molar amount is 8% to 24% of the total molar amount of epoxy groups on the silane chain obtained after the reaction in step S2.

[0013] Preferably, the C4-C10 alkanol in step S4 is a straight-chain alcohol, and the molar amount is 10% to 30% of the total number of epoxy groups on the silane chain. The catalyst is at least one of tetrabutylammonium bromide or aluminum acetylacetonate, and the amount of catalyst is 0.005% to 2% of the total mass of the reactants.

[0014] Preferably, the molar ratio of the monofunctional compound containing a tertiary amino group to the total epoxy group of the silane chain in step S5 is 0.4 to 0.8:1, and the monofunctional compound containing a tertiary amino group is at least one of N-methylpiperazine, N-(3-dimethylaminopropyl)-methylamine, and N-(12-dimethylaminododecyl)-methylamine.

[0015] Preferably, the quaternizing agent in step S6 is at least one of dimethyl sulfate, diethyl sulfate, or chloromethane; the high-speed shearing speed in step S7 is 2000-5000 rpm, and the dispersion time is 20-40 min.

[0016] The present invention provides a method for fixing acid dyes on nylon fabrics, using the aforementioned bisphenol-free nylon acid dye fixing agent, comprising the following steps: preparing an aqueous dispersion of the fixing agent into a working solution with a concentration of 1-10 g / L, adjusting the pH value to 4-6, padding or impregnating the dyed fabric, and then drying it at 80-110°C for 1-5 min; wherein the fabric is nylon 6, nylon 66, or an elastic fabric blended with spandex.

[0017] In this application, the color-fixing agent on the polysiloxane molecule, through controlled preparation process, can achieve a better spatially ordered arrangement of functional groups. This allows each functional module to spontaneously perform its specific function when the color-fixing agent forms a film on the surface of nylon fabrics, especially nylon / spandex fabrics: anchoring, center gripping, side protection, and outer sliding. A small amount of unreacted epoxy groups remain in the color-fixing agent structure. The epoxy three-membered ring has significant ring strain; under drying conditions (80–110°C), its electron-deficient carbon atoms are easily attacked by the nucleophilic group of the nylon terminal amino group (-NH2), undergoing a ring-opening addition reaction and anchoring to the fiber through covalent bonds. This contributes to providing excellent wash fastness. Starting with bi-terminal and side-chain hydrogen-containing silicone oil, epoxy groups are simultaneously introduced into the side chains and terminal groups through hydrosilylation. Subsequently, a monofunctional compound containing a tertiary amino group is used to react with... After the ring-opening reaction of the side-chain epoxy, the tertiary amino group is retained in the molecule. This is then converted to a quaternary ammonium salt by a quaternizing agent. This salt can efficiently form an insoluble lake with the sulfonate anions of acid dyes, while simultaneously generating strong electrostatic attraction with the anionic sites on the fiber surface. Before quaternization, the fixing agent grafts sulfide bonds onto the silicone oil backbone. Sulfide bonds are classic free radical scavengers; the sulfide groups are preferentially oxidized by active chlorine, thus consuming oxidizing substances and protecting the urea and ether bonds in the spandex fiber from oxidative degradation. Simultaneously, introducing a chlorine-resistant module before quaternization avoids oxidative damage to the sulfide bonds by the quaternizing agent, maximizing chlorine resistance efficiency. Finally, the fixing agent grafts C4-C10 short hydrophobic alkyl groups onto the siloxane side chain through the residual epoxy groups of the alkanoic acid ring-opening portion. These, together with the polydimethylsiloxane molecular backbone, constitute a low surface energy component. During film formation, thermodynamically driven migration towards the air interface contributes to a smooth feel and a certain degree of hydrophobic and stain-resistant properties in the fabric.

[0018] This application presents a bisphenol-free nylon acid dye fixing agent prepared through a segmented sequential method involving seven steps: preparation of bipolar and side-chain hydrogen-containing silicone oil, preparation of side-chain / terminal epoxy polyether silicone oil, introduction of chlorine-resistant and antioxidant structural units, introduction of short hydrophobic alkyl side chains, epoxy ring-opening amination, quaternization, and self-emulsifying aqueous dispersion. This process ensures that the chemical integrity of each functional group is not interfered with by subsequent steps, and the final product is a linear, slightly branched, or slightly network-like organosilicon chain molecule, which is beneficial for spreading on the fiber surface. Furthermore, the prepared product exhibits uniform particle size and storage stability after self-emulsifying dispersion.

[0019] After this bisphenol-free nylon acid dye fixing agent is applied to the fabric, the fixing agent substrate will fuse into a continuous film as the moisture evaporates. During this process, thermodynamically driven self-assembly orientation occurs: (1) Low surface energy components move outward: The surface energy of the polydimethylsiloxane molecular skeleton and C4-C10 short hydrophobic alkyl groups is much lower than that of the quaternary ammonium salt and the fiber surface. When the film is formed, it spontaneously migrates and accumulates towards the air interface, forming a smooth outer layer with low surface energy; (2) Cationic segments move inward: The side chain quaternary ammonium salt has a strong electrostatic attraction with the acid dye anions and fiber anion sites, tending to be distributed towards the fiber surface, forming an inner layer that "grabs the dye"; (3) Residual epoxy anchors downward: A small amount of residual end-side group epoxy undergoes a ring-opening reaction with the nylon end amino groups at the drying temperature, covalently fixing the entire film layer to the fiber surface; (4) Chlorine-resistant modules are evenly distributed: Chlorine-resistant structural units are randomly distributed in various parts of the silicone oil skeleton, forming a uniform anti-chlorine protection network in the film layer.

[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. By using the ring-opening amination modification method of epoxy groups, multiple quaternary ammonium salt groups can be grafted onto a single siloxane molecular backbone. The high cationic charge density is beneficial to improving the complexation efficiency and color-fixing performance of acid dyes.

[0021] 2. The lack of chlorine resistance in the design of color-fixing agents for nylon / spandex fabrics has become a pain point in the industry, making it difficult to meet the requirements for high chlorine resistance. This application combines a chlorine-resistant and antioxidant sulfide structure with an organosilicon quaternary ammonium salt color-fixing system in a synergistic manner. By introducing a chlorine-resistant module first and then quaternizing it, the process design helps to ensure chlorine resistance and anti-yellowing effect.

[0022] 3. This invention uses a small amount of residual epoxy groups to anchor the fibers, which helps to improve wash fastness, make the finishing effect more durable, and at the same time helps to maintain a good hand feel.

[0023] 4. This invention relies on the synergistic effect of the siloxane molecular skeleton and C4-C10 short hydrophobic alkyl groups to make the fixing agent uniformly migrate to the surface of the fiber membrane. The treated fabric has a good hand feel, which helps to improve the problem of dryness and roughness of the fabric after fixing with traditional fixing agents, and gives the fabric a smooth hand feel.

[0024] 5. This invention employs a segmented polymerization process, precisely constructing each functional structural unit step by step. This helps avoid the problems of disordered functional group distribution and uncontrollable product performance inherent in traditional random copolymerization. The product can self-emulsify to form a uniform nano-aqueous dispersion with a particle size of 20–100 nm, exhibiting excellent storage stability and directly adaptable to various industrial color-fixing processes such as padding and impregnation. Detailed Implementation

[0025] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0026] The terms “first,” “second,” “third,” “fourth,” etc. (if present) in the specification and claims of this invention are used to distinguish similar objects and are not necessarily used to describe a particular order or sequence. It should be understood that such data can be interchanged where appropriate so that embodiments of the invention described herein can be implemented, for example, in orders other than those described herein. Furthermore, the terms “comprising” and “having,” and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0027] This application relates to a bisphenol-free nylon acid dye fixing agent suitable for nylon fabrics, especially nylon / spandex elastic fabrics. It uses polydimethylsiloxane as a flexible molecular backbone, and through stepwise precise modification, controllably grafts hydrophilic polyether segments, high-density quaternary ammonium salts, sulfide chlorine-resistant units, and C4-C10 short hydrophobic alkyl groups onto the side chains. The polyether structure endows the product with excellent self-emulsifying properties, forming a uniform 20-100nm nano-dispersion. The high-density quaternary ammonium salts on the side chains efficiently capture acid dyes through electrostatic interactions, improving wet fastness. The sulfide bonds preferentially react with active chlorine to undergo oxidation, protecting spandex fibers from chlorine damage and inhibiting yellowing. The short hydrophobic alkyl groups migrate directionally on the fiber surface, constructing a smooth hydrophobic film layer and optimizing the fabric feel. Residual epoxy groups in the system form covalent bonds with the nylon terminal amino groups during drying, achieving strong anchoring. The synergistic effect of these functional units gives the product a comprehensive advantage of high fastness, low color change, chlorine and light resistance, excellent feel, and environmental friendliness (bisphenol-free).

[0028] The following detailed description, in conjunction with specific embodiments, illustrates a nylon acid dye fixing agent and its preparation and fixing methods as proposed in this application. All raw materials used are commercially available industrial products. The evaluation methods / standards involved are: epoxy value titration using the hydrochloric acid-acetone method according to GB / T1677-2023; analysis of cationic charge density using colloidal titration (PVSK standard solution, with the test object being an aqueous dispersion); and analysis using Malvern Zetasizer Nano... The particle size and ζ-potential were determined by ZS dynamic light scattering method; the color fastness to washing was evaluated according to condition A (40℃, 30min) in GB / T3921-2008 standard; the staining rating of spandex was evaluated according to GB / T251-2008 staining grey scale; the tensile recovery rate was evaluated according to GB / T3923.1-2013; the chlorine resistance test was conducted according to the method in GB / T8433-2013 color fastness to chlorinated water, with soaking at 25℃ for 1h in 50ppm available chlorine (NaClO, pH7.0); the spandex strength retention rate and yellowing value (Δb*) were determined (ISO105-E03); the water contact angle was measured using the seat drop method (5μL deionized water, reading 10s after contact); the hand feel rating of the fabric before and after finishing was conducted by 5 blind judges, with grades 1-5 (grade 5 being the smoothest).

[0029] Example 1

[0030] Step S1: Preparation of dual-terminal and side-chain hydrogen-containing silicone oil 2.8 g of tetramethyldihydrodisiloxane, 45.4 g of octamethylcyclotetrasiloxane, and 14.2 g of tetramethylcyclotetrasiloxane were mixed, and 1.30 g of pretreated acidic clay (vacuum dried at 105℃ for 4 h) was added. The mixture was stirred at 55℃ for 7 h under nitrogen protection. After the reaction was completed, the mixture was cooled to room temperature, and solid sodium bicarbonate was added for dry neutralization. After thorough stirring, a sample was taken and filtered. The pH of the filtrate was tested and adjusted to 6-7. The acidic clay and solid salt impurities were removed by filtration. The resulting filtrate was subjected to reduced pressure at 145℃ and a pressure <1 kPa for 2.5 h to remove low-boiling substances, yielding a dual-terminal and side-chain hydrogen-containing silicone oil.

[0031] Step S2: Preparation of side-chain / terminal group epoxy polyether silicone oil Take 30g of the above-mentioned hydrogen-containing silicone oil, add 11.7g of allyl glycidyl ether, 14.4g of allyl polyoxyethylene ether glycidyl ether (EO number 9), and 75μL of isopropanol chloroplatinate solution (Pt 3000ppm), and react under nitrogen protection at 82℃. Take samples every 1 hour for FT-IR monitoring. When 2160cm⁻¹… -1 Heating was stopped when the Si-H characteristic peaks became relatively stable, with only trace amounts of inert Si-H absorption remaining (approximately 4.5 hours). This yielded an epoxy polyether silicone oil with polyether segments in the side chains and epoxy groups in both the side chains and end groups.

[0032] Step S3: Introduce the sulfide chlorine-resistant module 1.53 g of mercaptoethanol was added to the above product, and the reaction was carried out at 75 °C for 4 h. The -SH group of mercaptoethanol underwent a ring-opening reaction with the epoxides on the silane chain (mainly side-chain epoxides, with a small amount of terminal epoxides also involved), introducing a structural unit containing a thioether bond. FT-IR: 2570 cm⁻¹ -1 The thiol peak disappeared.

[0033] Step S4: Introduce short hydrophobic chains (alkanol-epoxy ring opening) 2.56 g of 1-octanol and 0.5 g of tetrabutylammonium bromide (TBAB) were added to the above product, and the reaction was carried out at 100 °C for 5 h. Under the phase transfer catalysis of TBAB, the hydroxyl group of 1-octanol underwent an alcohol-epoxy ring-opening reaction with the residual epoxy, and the C8 alkyl group was grafted onto the siloxane side chain via an ether bond. FT-IR: at 1050-1150 cm⁻¹ -1 The appearance of a new CO-C stretching vibration peak proves that the C8 alkoxy grafting was successful.

[0034] Step S5: Epoxy ring-opening amination 7.46 g of N-methylpiperazine was added to the above-mentioned epoxy polyether silicone oil, and the reaction was carried out at 35 °C for 5 h. N-methylpiperazine, as a monofunctional compound containing a tertiary amino group, randomly undergoes ring-opening reactions with both side-chain and terminal-group epoxides. Since the number of side-chain epoxides is much greater than that of terminal-group epoxides (2 per molecule), statistically, most of the N-methylpiperazine reaction occurs on the side chains, with a small portion occurring on the terminal groups. FT-IR: 910 cm⁻¹ -1 The epoxy peak was significantly weakened. A small amount of unreacted residual epoxy (from end groups and side chain sites) remained in the final product. This epoxy could further react with the nylon terminal amino groups during subsequent drying to form multi-point covalent anchoring.

[0035] Step S6: Quaternization Add 4.7 g of dimethyl sulfate and react at 70 °C for 5 h. This converts the introduced side chain and terminal tertiary amine groups into quaternary ammonium salt groups. Since the tertiary amines in the side chain are the majority, the quaternary ammonium salt groups are mainly distributed in the side chain, with a small amount of quaternary ammonium salt also present in the terminal groups.

[0036] Step S7: Self-emulsifying water dispersion Take 30g of the above bulk product, preheat to 55℃, and slowly drop it dropwise into 70g of deionized water under high-speed shearing at 3000rpm. Continue stirring for 30min to obtain a blue transparent self-emulsifying aqueous dispersion with a solid content of 30% (product number F1). Measurements show that this bisphenol-free nylon acid dye fixing agent has a zeta potential of +35mV, a particle size of 50nm, and a cationic charge density of 3.0mmol / g.

[0037] Example 2

[0038] Steps S1-S4: Same as in Example 1.

[0039] Step S5: Add 7.62 g of N-(3-dimethylaminopropyl)-methylamine to the product obtained in step S4 and react at 50 °C for 5 h.

[0040] Step S6: Add chloromethane gas and react in a closed reactor at 60°C and 0.2 MPa pressure for 6 hours.

[0041] Step S7: Same as in Example 1.

[0042] The product number F2 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +34mV, the particle size was 55nm, and the cationic charge density was 2.9mmol / g.

[0043] Example 3

[0044] Steps S1-S2: Same as in Example 1.

[0045] Step S3: Add 1.7 g of mercaptoethanol to the product obtained in step S2 and react at 75 °C for 4 h.

[0046] Steps S4-S7: Same as in Example 1.

[0047] The product number F3 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +36mV, the particle size was 48nm, and the cationic charge density was 3.1mmol / g.

[0048] Example 4

[0049] Steps S1-S3: Same as in Example 1.

[0050] Step S4: Add 2.01 g of 1-hexanol and 0.5 g of TBAB to the product obtained in step S3, and react at 100 °C for 5 h.

[0051] Steps S5-S7: Same as in Example 1.

[0052] The product number F4 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +35mV, the particle size was 52nm, and the cationic charge density was 3.0mmol / g.

[0053] Example 5

[0054] Steps S1-S5: Same as in Example 1.

[0055] Step S6: Add 5.75 g of diethyl sulfate to the product obtained in step S5 and react at 70 °C for 5 h.

[0056] Step S7: Same as in Example 1.

[0057] The product number F5 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +33mV, the particle size was 58nm, and the cationic charge density was 2.8mmol / g.

[0058] Example 6

[0059] Steps S1-S4: Same as in Example 1.

[0060] Step S5: Add 19.13 g of N-(12-dimethylaminododecyl)-methylamine to the product obtained in step S4 and react at 30°C for 8 h.

[0061] Steps S6-S7: Same as in Example 1.

[0062] The product number F6 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +31mV, the particle size was 65nm, and the cationic charge density was 2.6mmol / g.

[0063] Example 7

[0064] Steps S1-S3: Same as in Example 1.

[0065] Step S4: Add 3.11 g of 1-decyl alcohol and 0.5 g of TBAB to the product obtained in step S3, and react at 110 °C for 6 h.

[0066] Steps S5-S7: Same as in Example 1.

[0067] The product number F7 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +32mV, the particle size was 62nm, and the cationic charge density was 2.8mmol / g.

[0068] Example 8

[0069] Steps S1-S2: Same as in Example 1.

[0070] Step S3: Add 1.95 g of mercaptoacetic acid to the product obtained in step S2 and react at 75 °C for 4 h.

[0071] Steps S4-S7: Same as in Example 1.

[0072] The product number F8 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +37mV, the particle size was 45nm, and the cationic charge density was 3.2mmol / g.

[0073] Example 9

[0074] Steps S1-S4: Same as in Example 1.

[0075] Step S5: Add 6.22 g of N-methylpiperazine to the product obtained in step S4 and react at 35 °C for 5 h.

[0076] Steps S6-S7: Same as in Example 1.

[0077] The product number F9 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +33mV, the particle size was 60nm, and the cationic charge density was 2.5mmol / g.

[0078] Example 10

[0079] Steps S1-S4: Same as in Example 1.

[0080] Step S5: Add 8.75 g of N-methylpiperazine to the product obtained in step S4 and react at 30°C for 8 h.

[0081] Steps S6-S7: Same as in Example 1.

[0082] The product number F10 fixing agent was obtained. It was determined that the zeta potential of this bisphenol-free nylon acid dye fixing agent was +38mV, the particle size was 42nm, and the cationic charge density was 3.5mmol / g.

[0083] Comparative Example 1 Skip step S3, the remaining steps are the same as in Example 1. A color-fixing agent with product number C1 is obtained.

[0084] Comparative Example 2 In the preparation process, steps S6 and S3 are interchanged, and the rest is the same as in Example 1. A color-fixing agent with product number C2 is obtained.

[0085] Comparative Example 3 Skip step S4, the rest is the same as in Example 1. A color-fixing agent with product number C3 is obtained.

[0086] Comparative Example 4 In step S2, only allyl glycidyl ether is used (without allyl polyoxyethylene ether glycidyl ether), and the rest is the same as in Example 1. In step S7, the product cannot self-emulsify and requires the addition of emulsifier AEO-3 (15% of product mass) for forced emulsification. This yields a color-fixing agent with product number C4.

[0087] Each sample was prepared into a working solution with a mass concentration of 10% (pH 5.0) for use on nylon 66 / spandex (80 / 20) woven elastic fabric (190 g / m²). 2 The samples (dyed with CIAcidRed266) underwent two dips and two nips (80% pick-up) and were dried at 100℃ for 2 minutes. The performance test results of each sample and the finished fabric are shown in Table 1 below.

[0088] Table 1. Performance test results of each sample after finishing.

[0089] Note: Color fastness and staining rating: 1 is the worst, 5 is the best; the higher the tensile recovery rate and strength retention rate, the better; the lower the yellowing value, the better.

[0090] As shown in the table above, in all embodiments, the final product retains a very small amount of unreacted epoxy (mainly from end groups and a small number of side chain sites). Under drying conditions (100°C, 2 min), it undergoes a ring-opening reaction with the nylon terminal amino groups to form CN covalent bonds. Simultaneously, the high-density quaternary ammonium salts on the side chains capture the dye through electrostatic interaction, and the two work synergistically to achieve excellent wash fastness (4-5 grade). The above data are based on nylon 66 / spandex (80 / 20) woven elastic fabric, CIAcidRed 266 dyeing, two-dip two-nip process, and the test conditions listed in the table. They are not extrapolated to other fabric specifications, dye types, or processing techniques.

[0091] As can be seen from the table above, comparing each example with Comparative Example C1, the former has a chlorine strength retention rate of 86-90%, while the latter is 65%; the former has a yellowing value of 1.6-2.0, while the latter is 4.8, indicating that the sulfide preferentially consumes active chlorine through oxidation, which is beneficial for protecting the spandex. Comparing Example 1 with Comparative Example 2, it can be seen that quaternization followed by the introduction of the chlorine-resistant module severely inhibits the thiol-epoxy ring-opening reaction, resulting in a significant decrease in chlorine resistance (88% in the former, 68% in the latter), indicating that the process order of "chlorine resistance first, then quaternization" cannot be reversed. Comparing Example 1 with Comparative Example 4, it can be seen that without the polyether segment, self-emulsification is impossible, requiring the addition of an emulsifier, leading to increased particle size and a color fastness of only 3-4 grades, indicating that the introduction of polyether in S2 is a prerequisite for achieving self-emulsification and high performance. Comparing Example 1 with Comparative Example 3, it can be seen that without the C8 chain, the contact angle is only 83°, resulting in poor slippage and a hand feel rating of 3.0, indicating that short hydrophobic chains play a crucial role in surface properties.

[0092] The table above also shows that all examples exhibit excellent overall performance. Example 6 has a slightly lower charge density (2.6 mmol / g), possibly due to the steric hindrance of the long-chain alkyl group. Examples 1 (mercaptoethanol) and 8 (mercaptoacetic acid) effectively introduce chlorine-resistant modules and have comparable performance. Example 8 has a slightly higher charge density (3.2 mmol / g), possibly attributed to the additional electronegativity of the carboxyl group in the mercaptoacetic acid molecule, which is beneficial for improving colloidal stability. Example 4 (1-hexanol, C6) has similar performance to Example 1 (1-octanol, C8). Example 7 (1-decanol, C10) exhibits a higher contact angle (112°) and good feel; the longer alkyl chain helps improve hydrophobic slip properties. Example 9 has the lowest charge density (2.5 mmol / g), but still meets the requirements. Example 10 has the highest charge density (3.5 mmol / g) and excellent overall performance.

[0093] The EO number of the allyl polyether epoxy compound used in the above embodiments can be adjusted within the range of 6-12; N-(3-dimethylaminopropyl)-methylamine can be replaced with N-methylpiperazine or N-(12-dimethylaminododecyl)-methylamine; mercaptoethanol can be replaced with mercaptoacetic acid; 1-octanol can be replaced with 1-hexanol or 1-decanol; the hydrosilylation temperature can be selected within the range of 60-120°C; and commercially available products can be directly used for the dual-end and side-chain hydrogen-containing silicone oils. These substitutions are all conventional equivalent transformations of this application.

[0094] The various embodiments described in this specification are presented in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

[0095] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A nylon acid dye fixing agent, characterized in that, The base material of the fixing agent comprises the following structural units: (a) It has a polydimethylsiloxane molecular backbone with polyether hydrophilic segments on the chain; (b) Contains a quaternary ammonium salt group, which is formed by a ring-opening reaction of a side chain epoxy group with a monofunctional compound containing a tertiary amino group and then by treatment with a quaternizing agent; (c) Contains short hydrophobic alkyl groups of C4-C10, which are linked to the siloxane skeleton via ether bonds; (d) Contains chlorine-resistant and antioxidant structural units, which are structural units containing sulfide bonds.

2. The nylon acid dye fixing agent according to claim 1, characterized in that, The hydrophilic segment of the polyether is introduced by an allyl polyether epoxy compound, which is an allyl polyoxyethylene ether glycidyl ether with 6 to 12 ethylene oxide units.

3. The nylon acid dye fixing agent according to claim 1, characterized in that, The monofunctional compound containing a tertiary amino group is at least one of N-methylpiperazine, N-(3-dimethylaminopropyl)-methylamine, and N-(12-dimethylaminododecyl)-methylamine; The quaternizing agent is selected from at least one of dimethyl sulfate, chloromethane, and diethyl sulfate.

4. The nylon acid dye fixing agent according to claim 1, characterized in that, The thioether bond-containing structural unit is introduced by a ring-opening reaction between a thiol-containing compound and an epoxy group on a silane chain, wherein the thiol-containing compound is at least one of mercaptoethanol and mercaptoacetic acid; The C4-C10 short hydrophobic alkyl group is introduced through a ring-opening reaction between a C4-C10 alkanol and a residual epoxy group in the silicon chain, wherein the C4-C10 alkanol is at least one of the C4-C10 straight-chain alkanols.

5. A method for preparing the nylon acid dye fixing agent according to claim 1, characterized in that, Prepare according to the following steps: Preparation of dual-terminal and side-chain hydrogen-containing silicone oil by S1: Tetramethyldihydrodisiloxane, octamethylcyclotetrasiloxane, and tetramethylcyclotetrasiloxane are added to a reactor and stirred under nitrogen protection. Dry acidic clay solid catalyst, accounting for 1.5% to 5.0% of the total mass of raw materials, is added. Ring-opening polymerization is carried out at a controlled temperature of 50 to 60°C for 6 to 8 hours. After the reaction is completed, the mixture is cooled to room temperature and neutralized to neutral by dry method with sodium bicarbonate. Acidic clay and trace impurities are removed by filtration. Then, low-boiling substances are removed at 140 to 150°C under reduced pressure for 2 to 3 hours to obtain dual-terminal and side-chain hydrogen-containing silicone oil with complete SiH activity. The mass ratio of tetramethyldihydrodisiloxane, octamethylcyclotetrasiloxane, and tetramethylcyclotetrasiloxane is 1:10 to 20:3 to 8. S2 Preparation of Side-Chain / Terminal Group Epoxy Polyether Silicone Oil: The aforementioned dual-terminal and side-chain hydrogen-containing silicone oil is subjected to a hydrosilylation reaction with a mixture of allyl glycidyl ether and allyl polyether epoxy compound in the presence of a platinum catalyst. The reaction temperature is 60-120℃, the reaction time is 2-8h, and the mass fraction of platinum metal based on the mass of the hydrogen-containing silicone oil is 4-20ppm. This yields an epoxy polyether silicone oil with polyether segments in the side chains and epoxy groups in both the side chains and end groups. The molar ratio of allyl glycidyl ether to allyl polyether epoxy compound is 2-6:1, and the total molar ratio of double bonds in the mixture to the SiH molar ratio of the dual-terminal and side-chain hydrogen-containing silicone oil obtained in step S1 is 0.90-1:

1. The allyl polyether epoxy compound is allyl polyoxyethylene ether glycidyl ether with 6-12 ethylene oxide units. S3 Introducing chlorine-resistant and antioxidant structural units: Adding a mercapto-containing compound to the product obtained in step S2, and reacting with some epoxy groups to undergo a mercapto-epoxy ring-opening reaction, with a reaction temperature of 60-80℃ and a reaction time of 3-6h, to introduce structural units containing thioether bonds. S4 Introduction of short hydrophobic alkyl side chains: C4-C10 alkanols and catalysts are added to the product obtained in step S3 to undergo a ring-opening reaction with some residual epoxy groups. The reaction temperature is 90-110℃ and the reaction time is 4-6h. The C4-C10 short hydrophobic alkyl groups are grafted onto the siloxane side chains in the form of ether bonds. S5 Epoxy Ring-Opening Amination: The product obtained in step S4 is reacted with a monofunctional compound containing a tertiary amino group at a reaction temperature of 30–50 °C for 4–8 h, so that the residual epoxy group is ring-opened to introduce the tertiary amino group, while retaining a small amount of residual epoxy group. S6 Quaternization: The product obtained in step S5 is reacted with a quaternization reagent at a temperature of 50-85°C for 3-8 hours to convert the side chain tertiary amino group into a quaternary ammonium salt group. S7 Self-emulsifying water dispersion: The bulk product obtained in step S6 is dispersed in deionized water under stirring or high-speed shearing conditions at 40-70°C to obtain a nylon acid dye fixing agent with a solid content of 20%-40%.

6. The method for preparing the nylon acid dye fixing agent according to claim 5, characterized in that, The mercapto-containing compound in step S3 is at least one of mercaptoethanol and mercaptoacetic acid, and the molar amount is 8% to 24% of the total molar amount of epoxy groups on the silane chain obtained after the reaction in step S2.

7. The method for preparing the nylon acid dye fixing agent according to claim 5, characterized in that, In step S4, the C4-C10 alkanol is a straight-chain alcohol, and the molar amount is 10% to 30% of the total number of epoxy groups on the silane chain. The catalyst is at least one of tetrabutylammonium bromide or aluminum acetylacetonate, and the amount of catalyst is 0.005% to 2% of the total mass of the reactants.

8. The method for preparing the nylon acid dye fixing agent according to claim 5, characterized in that, In step S5, the molar ratio of the monofunctional compound containing a tertiary amino group to the total epoxy group of the silane chain is 0.4 to 0.8:1, and the monofunctional compound containing a tertiary amino group is at least one of N-methylpiperazine, N-(3-dimethylaminopropyl)-methylamine, and N-(12-dimethylaminododecyl)-methylamine.

9. The method for preparing the nylon acid dye fixing agent according to claim 5, characterized in that, The quaternizing agent mentioned in step S6 is at least one of dimethyl sulfate, diethyl sulfate, or chloromethane; the high-speed shearing speed in step S7 is 2000-5000 rpm, and the dispersion time is 20-40 min.

10. A method for fixing acid dyes on nylon fabrics, characterized in that, Using the nylon acid dye fixing agent according to claim 1 includes the following steps: The fixing agent aqueous dispersion is prepared into a working solution with a concentration of 1-10 g / L, the pH value is adjusted to 4-6, and the dyed fabric is subjected to padding or impregnation treatment, and then dried at 80-110℃ for 1-5 min; the fabric is nylon 6, nylon 66 and elastic fabrics blended with spandex.