A high-hardness hardening film and its preparation method
By combining chemically grafted expanded particles and free radical-cationic hybrid photocurable resin, the problem of warping and deformation of the hardened film when increasing its hardness is solved, resulting in a hardened film with high hardness, low warping and excellent wear resistance, suitable for high-end displays.
Patent Information
- Application Number
- CN202611405098.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing hardened films are prone to warping and deformation when increasing hardness, making it difficult to balance high hardness and warping control. Furthermore, their wear resistance is insufficient, failing to meet the requirements of high-end displays.
By combining chemically grafted expanded particles and free radical-cationic hybrid photocurable resin, a pre-compression stress field and a highly cross-linked network are established through a heat drying and UV light irradiation shaping process, thereby reducing internal stress and improving hardness and wear resistance.
It achieves a hardened film with high hardness and low warpage, with a pencil hardness of 7H-8H, warpage ≤0.9mm, excellent wear resistance, light transmittance ≥90.5%, and strong adhesion, meeting the performance requirements of high-end displays.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyethylene terephthalate (PET) technology, and more specifically to a high-hardness curing film and its preparation method. Background Technology
[0002] With the rapid development of consumer electronics, the performance requirements for screen protectors in mobile phones, tablets, smart wearable devices, and other terminal products are increasing. As the core functional layer of a screen protector, the hardened film's hardness, abrasion resistance, light transmittance, and flatness directly determine the user experience and lifespan of the product.
[0003] Most commonly used hardened films on the market employ UV curing technology, where a UV-curable resin is coated onto a PET substrate to form a hardened layer. However, UV-curable resins generally suffer from volume shrinkage during the polymerization and cross-linking process. As the thickness of the hardened layer increases, the internal stress generated by curing shrinkage can cause severe warping deformation of the film. This warping not only affects the product's surface flatness but also prevents the hardened film from adhering tightly to the screen, severely impacting its performance.
[0004] On the other hand, existing hardened film products have significant shortcomings in terms of hardness and abrasion resistance. The pencil hardness of conventional hardened films typically only reaches 3H-4H, which is insufficient to meet the abrasion and scratch resistance requirements of high-end displays. Although theoretically increasing the crosslinking density or the thickness of the hardened layer can improve hardness, thick coatings exacerbate warping problems, making it difficult for existing products to balance hardness improvement and warping control. This is a long-standing technical challenge in the field that has not yet been effectively resolved.
[0005] Therefore, developing a hardened film that can achieve both high hardness and controllable warpage, and its preparation method, has significant practical importance and market value. Summary of the Invention
[0006] The purpose of this invention is to provide a high-hardness hardening film and its preparation method to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, in one respect, the present invention provides a high-hardness hardening film, comprising: PET substrate, the surface of which has undergone high-energy surface treatment; A hardened layer disposed on at least one surface of the PET substrate; The hardened layer is formed by heat drying and curing of the hardening liquid followed by UV light irradiation for shaping. The hardening liquid includes chemically grafted expanded particles, free radical-cationic hybrid photocurable resin, reactive diluent, photoinitiator, nano-inorganic filler and solvent. The core of the chemically grafted expansion particles is a thermosensitive expansion active material, and the shell is a hyperbranched polymer containing polymerizable reactive groups. The branches of the hyperbranched polymer contain reactive groups that can undergo chemical cross-linking reactions with free radical-cationic hybrid photocurable resin. The photoinitiator includes free radical photoinitiators and cationic photoinitiators.
[0008] During the heat drying stage, the core of the chemically grafted expandable particles undergoes thermal decomposition (azo) or thermally induced phase change expansion (microcapsule type) under thermal stimulation, establishing a pre-compression stress field in the hardened layer. The hyperbranched polymer shell, with its highly branched structure and good compatibility, achieves uniform and stable dispersion with the free radical-cationic hybrid photocurable resin in the system through intermolecular interactions. At this time, permanent chemical cross-linking has not yet formed between the shell and the resin, and the system still maintains sufficient chain segment mobility. During the subsequent UV light irradiation setting stage, UV light excites both free radical photoinitiators and cationic photoinitiators to generate free radicals and protic acids. The reactive groups (acrylate groups) at the shell ends undergo rapid free radical polymerization with the resin matrix under the action of free radicals, while the epoxy ring-opening reaction initiated by cationic polymerization further constructs a cross-linked network. This process firmly anchors the shell to the resin cross-linked network through covalent bonds, achieving an in-situ transformation of the expanded particles from "physical entanglement and dispersion" to "chemical cross-linking and anchoring." During the subsequent UV light irradiation setting stage, UV light excites the free radical photoinitiator and cationic photoinitiator to generate free radicals and protic acids. The reactive groups (acrylate groups) at the shell end undergo rapid free radical polymerization with the resin matrix under the action of free radicals, firmly anchoring the expanding particles to the resin crosslinking network through covalent bonds. At the same time, the free radical-cationic hybrid curing system, due to its cationic polymerization ring-opening mechanism, reduces the overall volume shrinkage rate. The resulting shrinkage tensile stress, combined with the compressive stress pre-established during the heat drying stage, significantly reduces the internal stress level of the hardened layer, thereby effectively suppressing warping. In addition, the high crosslinking density network formed by free radical polymerization, in synergy with the nano-inorganic filler, endows the hardened layer with high hardness and excellent wear resistance.
[0009] Preferably, the thermosensitive expandable active material is a microcapsule-type thermoexpansive microsphere.
[0010] The microencapsulated thermally expandable microspheres are microcapsules with polyacrylonitrile or polyvinylidene chloride as the shell material and low-boiling-point alkanes as the core material, with an expansion initiation temperature of 70-100℃. The microencapsulated thermally expandable microspheres are effectively activated in the third stage of thermal drying (80-95℃), resulting in controllable volume expansion. The expansion temperature windows of both types of thermally foamed materials mentioned above are highly matched with the third stage (80-95℃) of the thermal drying process of this invention.
[0011] Preferably, the hyperbranched polymer is grafted from AB2-type self-initiating monomers via surface-initiated atom transfer radical polymerization (SI-ATRP), with a branching degree of 0.5-0.8 and a number-average molecular weight of 2000-8000. The hyperbranched polymer is grafted from AB2-type self-initiating monomer 2-(2-bromoisobutyryloxy)ethyl methacrylate (BiBEM) via SI-ATRP. The core surface is first esterified with 2-bromoisobutyryl bromide to introduce ATRP initiating groups, followed by controlled growth of the hyperbranched shell on the particle surface via SI-ATRP of BiBEM. Specifically, the particle size of the chemically grafted expanded particles is 50-300 nm, much smaller than the visible light wavelength (380-780 nm), effectively avoiding scattering and ensuring a transmittance of ≥90% for the hardened film.
[0012] Preferably, the curing liquid comprises, by weight: 3-6 parts of chemically grafted expanding particles, 30-60 parts of free radical-cationic hybrid photocurable resin, 10-25 parts of reactive diluent, 1.5-3 parts of free radical photoinitiator, 1-3 parts of cationic photoinitiator, 30-50 parts of solvent, 4-15 parts of nano-inorganic filler, 0.1-1 parts of leveling agent, and 0.5-3 parts of anti-graffiti additive.
[0013] Specifically, the free radical photoinitiator can be any one of photoinitiator 184, photoinitiator 1173, and photoinitiator TPO; the cationic photoinitiator can be triarylthionium hexafluorophosphate or diphenyliodonium hexafluorophosphate. When diphenyliodonium hexafluorophosphate is used as the cationic photoinitiator, 0.2-0.8 parts of the sensitizer isopropylthioxanthone (ITX) need to be added to the formulation to improve the utilization efficiency of photons in the 365nm band through energy transfer, so as to ensure the full ring-opening curing of the alicyclic epoxy groups. The reactive diluent can be any one of dipropylene glycol diacrylate (DPGDA), trimethylolpropane triacrylate (TMPTA), and 1,6-hexanediol diacrylate (HDDA). The solvent is ethyl acetate or butanone. The anti-graffiti additive is a fluorinated polyether acrylate type anti-graffiti additive that is compatible with the UV curing system.
[0014] Preferably, the free radical-cationic hybrid photocurable resin is a dual-curing resin containing acrylate double bonds and alicyclic epoxy groups. This resin simultaneously contains free radical-curable acrylate double bonds and cationic-curable alicyclic epoxy groups, enabling UV-based free radical-cationic dual curing. It exhibits rapid curing speed, good curing film flexibility, low volume shrinkage, and strong adhesion. The acrylate double bonds provide rapid free radical curing capability and high crosslinking density to ensure hardness, while the alicyclic epoxy groups provide low shrinkage characteristics and excellent adhesion. The synergistic effect of these two components significantly reduces the overall shrinkage rate of the system.
[0015] Preferably, the nano-inorganic filler is selected from one or more of nano-silica, nano-alumina, and nano-zirconia, with a particle size of 20-80 nm, and its surface is modified with a silane coupling agent. After the surface is modified with the silane coupling agent, it forms a chemical bond with the resin, thereby improving the interfacial bonding strength.
[0016] Preferably, the PET substrate surface is provided with a cross-linked polyester primer coating. This cross-linked polyester primer coating is formed by heat curing a polyester primer liquid containing a melamine-based cross-linking agent (5-15% of the polyester resin mass) at 120-130°C for 2 minutes. This improves the solvent resistance of the primer coating and prevents swelling and damage from solvents in subsequent coatings. After adding the cross-linking agent, the primer coating forms a cross-linked network upon heat curing, exhibiting good solvent resistance (resistant to conventional curing film coating solvents such as ethyl acetate and methyl ethyl ketone), effectively preventing swelling and damage to the primer coating from solvents in subsequent coatings and ensuring interfacial adhesion.
[0017] On the other hand, the present invention also discloses a method for preparing the above-mentioned high-hardness hardening film, comprising the following steps: (1) Preparation of hardening solution: Mix the raw materials of hardening solution, stir evenly, filter, and obtain hardening solution; (2) Substrate pretreatment: Surface treatment of PET substrate; (3) Coating: The curing liquid prepared in step (1) is coated onto the surface of the PET substrate after pretreatment in step (2) to form a wet film; (4) Heat drying and curing: The coated PET substrate is heated and dried to allow the solvent to fully evaporate and activate the chemically grafted expansion particles, thus establishing pre-compression stress in the hardened layer; (5) UV light irradiation for curing: Under nitrogen protection, the film is cured by UV irradiation. The reactive groups at the end of the shell layer and the free radical-cation hybrid photocurable resin undergo chemical cross-linking and anchoring during the UV irradiation stage to obtain a high-hardness hardened film.
[0018] Preferably, the temperature for heat drying and curing in step (4) is 40-95℃, and the time is 17-30 min. Specifically, the specific method for heat drying and curing is as follows: First stage: Heat and dry at 40-50℃ for 10-15 minutes; slowly evaporate the solvent at low temperature to avoid concentrated vaporization of the solvent and the generation of micropore defects, while allowing the coating system to slowly thicken and form a stable gel network skeleton.
[0019] Second stage: Heat and dry at 60-80℃ for 5-10 minutes; medium temperature further removes residual solvent, so that the hardened layer is initially shaped, making room for the subsequent activation of expanding particles and maintaining the integrity of the coating structure.
[0020] The third stage: heating and drying at 80-95℃ for 2-5 minutes. The high temperature fully activates the chemically grafted expandable particles, causing them to expand in volume and establish pre-compression stress inside the hardened layer, laying the foundation for offsetting the shrinkage tensile stress of subsequent UV curing.
[0021] Preferably, the ultraviolet light irradiation energy in step (5) is 400-800 mJ / cm². 2 During the UV irradiation stage, the methacrylate double bonds (from the residual polymeric ends of BiBEM) contained at the ends of the hyperbranched polymer shell are copolymerized and crosslinked with the acrylate groups in the system under the initiation of free radicals generated by the free radical photoinitiator. This achieves covalent bond anchoring between the expanded particle shell and the resin crosslinking network, thereby firmly locking the expanded particles in the hardened layer during the heat drying stage and ensuring the long-term maintenance of compressive stress.
[0022] The beneficial effects of this invention are as follows: (1) Chemically grafted expansion particles have a core-shell structure. The core thermosensitive expansion active material (microcapsule-type thermal expansion microspheres or azo thermal foaming agent) is activated in the third stage of thermal drying (80-95℃) to generate controllable volume expansion and establish a uniform nanoscale pre-compression stress field in the hardened layer. The hyperbranched polymer shell achieves dispersion stability in the thermal drying stage through intermolecular interactions (such as van der Waals forces, hydrogen bonds, etc.) and is anchored to the resin network through covalent bonds formed by terminal reactive groups in the UV curing stage, avoiding the problem of uneven dispersion and shedding of traditional simple physical mixing expansion additives.
[0023] (2) The acrylate double bonds in the free radical-cationic hybrid photocurable resin undergo rapid free radical polymerization under the action of free radical photoinitiator to form a high cross-linking density network, ensuring the high hardness of the hardened layer; the alicyclic epoxy groups undergo ring-opening cationic polymerization under the action of cationic photoinitiator to form an interpenetrating network structure. Its inherent low volume shrinkage rate significantly reduces the overall curing shrinkage. The pre-compression stress established by the expanding particles works synergistically to significantly reduce the curing internal stress, thereby effectively suppressing warping.
[0024] (3) The segmented hot drying process achieves the decoupling of solvent evaporation and particle expansion in time through a three-stage process: low-temperature slow desolventizing in the first stage, medium-temperature shaping in the second stage, and high-temperature precise activation of expanded particles in the third stage. This avoids the formation of micropore defects in the coating when the two occur simultaneously, and ensures that the hardened film has a high light transmittance of ≥90%. Detailed Implementation
[0025] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0026] It should be noted that all reagents and raw materials used in this invention are commercially available, and the reagents are of analytical grade.
[0027] PET substrate was purchased from Dongguan Lingmei New Materials Co., Ltd., model TORAY Lumirror T60. Microencapsulated thermally expandable microspheres were purchased from Guangzhou Daixun Trading Co., Ltd., model Expancel 031 DU 40. Free radical-cationic hybrid photocurable resin was purchased from Shenzhen Youyang Technology Co., Ltd., model U-9100A. Nano-silica was purchased from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., model XFI04, which underwent KH570 treatment. Leveling agent was from BYK Additives (Shanghai) Co., Ltd., model BYK-307. Anti-graffiti additive was purchased from Guangdong Lancolu New Materials Co., Ltd., model Lencolo 3007F. Polyester resin was purchased from Shenzhen Junhua Technology Co., Ltd., model VYLON 200#. Melamine crosslinking agent was from Zhanxin Resin (Shanghai) Co., Ltd., model Cymel. ® 325.
[0028] The preparation method of chemically grafted expanded particles is as follows: (1) Introducing atom transfer radical polymerization (ATRP) initiating groups on the surface of the nucleus: Add 30g of microcapsule-type thermally expandable microspheres to a three-necked flask, then add 100mL of anhydrous tetrahydrofuran (THF), and disperse the microspheres under nitrogen protection with ultrasonic assistance (power 200W, frequency 40kHz, ultrasonic 30s / stop 10s, cycle 5 times) to form a uniform suspension; under nitrogen protection, add 32g of 2-Bromoisobutyryl bromide and 20 g of anhydrous triethylamine were dissolved in 30 mL of anhydrous THF to obtain a dropping solution, which was transferred to a constant pressure dropping funnel and sealed. A three-necked flask was placed in an ice-water bath at 0 °C, and the dropping solution was added dropwise at a rate of 1 drop / second under stirring (350 rpm). After the addition was completed, the ice bath was removed, and the mixture was allowed to rise naturally to room temperature. The mixture was stirred and reacted for 12 h. Then, the mixture was heated to 40 ± 2 °C in an oil bath and the reaction was continued for 4 h. After the reaction was completed, the mixture was filtered while hot to remove the triethylamine salt. The filter cake was washed twice with 20 mL of cold THF (about 0 °C), and the filtrates were combined. The filtrate was slowly added dropwise to 500 mL of petroleum ether, stirred thoroughly, and allowed to stand to precipitate. The lower solid was washed twice with a mixture of petroleum ether / diethyl ether (volume ratio 1:1) and once with anhydrous diethyl ether. The solid was collected by filtration and dried in a vacuum drying oven at 40 °C for 12 h to obtain the ATRP macromolecular initiator. (2) Surface-initiated ATRP construction of hyperbranched polymer shell: In a nitrogen glove box (water and oxygen content <1ppm), 15g of the above-mentioned ATRP macromolecular initiator (solid particles), 12g of 2-(2-bromoisobutyryloxy)ethyl methacrylate (BiBEM), 0.25g of purified cuprous bromide (CuBr), and 0.35mL of N,N,N',N'',N''-pentamethyldiethylenetriamine were added sequentially to a Shrek tube, followed by 40mL of anhydrous THF, and sealed. After purging with high-purity nitrogen (purity 99.999%) for 30min to remove oxygen, the tube was placed in an oil bath at 60±1℃ and stirred (400rpm) for 10h. After the reaction was completed, the tube was naturally cooled to room temperature, and air was introduced and stirred for 15min to terminate the polymerization, yielding the reaction solution. (3) Purification: The reaction solution was centrifuged at 8000×g and 10℃ for 15min and the supernatant was discarded. 20mL of anhydrous THF was added to the precipitate and ultrasonically dispersed (power 200 W, frequency 40 kHz, ultrasonic for 30s, stop for 10s, cycled 3 times). The mixture was then centrifuged at 8000×g and 10℃ for 15min and washed three times with anhydrous THF. The product was then washed twice with 0.5wt% EDTA disodium aqueous solution and twice with deionized water. Each time, the product was centrifuged at 8000×g and 10℃ for 10min. The final product was dried in a vacuum drying oven at 40℃ for 24h. After preliminary crushing, the product was transferred to an agate mortar and ground for 15min. The powder was then passed through a 100-mesh sieve and collected to obtain chemically grafted expanded particles.
[0029] Example 1 This embodiment provides a method for preparing a high-hardness hardening film, including the following steps: (1) Preparation of hardening solution Weigh the following components by weight: 5 parts chemically grafted expanded particles, 45 parts free radical-cationic hybrid photocurable resin, 15 parts reactive diluent DPGDA, 1.5 parts free radical photoinitiator 184, 1.5 parts cationic photoinitiator diphenyliodonium hexafluorophosphate, 0.5 parts sensitizer 2-isopropylthioxanthraquinone, 35 parts ethyl acetate / butanone (mass ratio 1:1) mixed solvent, 6 parts nano silica, 0.2 parts leveling agent, and 1 part anti-graffiti additive; Add the above components to a stainless steel container in the following order: first add the solvent and reactive diluent, then add the free radical photoinitiator and cationic photoinitiator, and stir to dissolve; then add the free radical-cationic hybrid photocurable resin and stir evenly; then add the chemically grafted expanding particles and nano-silica, and stir to disperse; finally add the leveling agent and anti-graffiti additive, and mechanically stir at 1000 rpm for 1.5 h to obtain a uniformly dispersed hardened liquid, which is then filtered using a 5 μm polypropylene filter cartridge for later use.
[0030] (2) Substrate pretreatment Take a PET substrate with a thickness of 50μm, place the PET substrate in a plasma treatment instrument, treat it for 50s in an oxygen atmosphere with a power of 200W, and the surface tension after treatment is 55dynes / cm. Then, use a wire rod to coat the plasma-treated surface with a cross-linked polyester primer (by mass percentage: polyester resin 28%, melamine cross-linking agent 3.5%, ethyl acetate 34%, and methyl ethyl ketone balance), dry at 120℃ for 2min, and heat-cur to form a cross-linked primer coating with a dry film thickness of about 0.5μm. (3) Coating The pretreated PET substrate is fixed on the coating machine, and the curing liquid is evenly coated on the surface of the base coating using a wire bar. The wet film thickness is controlled so that the final dry film thickness is 60μm. (4) Heat drying and curing The coated PET substrate is placed in a forced-air drying oven for segmented heat drying and curing: First stage: Heat and dry at 45℃ for 12 minutes; Second stage: Heat and dry at 75℃ for 8 minutes; Third stage: Heat and dry at 90℃ for 3 minutes; (5) UV light irradiation for shaping The heat-dried film is then placed in a UV curing machine (equipped with a high-pressure mercury lamp) and cured under nitrogen protection at a temperature of 500 mJ / cm². 2 The film is cured by irradiation with ultraviolet light energy to obtain a high-hardness hardened film.
[0031] Example 2 This embodiment provides a method for preparing a high-hardness hardening film, including the following steps: (0) Modification of nano-zirconia KH570:water:ethanol was mixed in a volume ratio of 1:1:4, and the pH was adjusted to 4.5 with acetic acid. The mixture was stirred at room temperature for 30 min to obtain a KH570 hydrolysate. Nano-zirconia (average particle size 30 nm) was dispersed in ethanol (10% solid content) and ultrasonically dispersed for 15 min to obtain a dispersion. The KH570 hydrolysate was added to the dispersion, with the amount of KH570 being 5% of the mass of the nano-zirconia. The mixture was stirred at 70 °C for 3 h. After the reaction, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 12 h to obtain modified nano-zirconia.
[0032] (1) Preparation of hardening solution Weigh the following components by weight: 6 parts of chemically grafted expanded particles, 60 parts of free radical-cationic hybrid photocurable resin, 25 parts of reactive diluent TMPTA, 2 parts of free radical photoinitiator 1173, 1 part of cationic photoinitiator triarylthionium hexafluorophosphate, 30 parts of ethyl acetate / butanone (mass ratio 1:1) mixed solvent, 25 parts of modified nano-zirconia, 0.1 parts of leveling agent, and 0.5 parts of anti-graffiti additive; the mixing, stirring, and filtration methods are the same as in Example 1.
[0033] (2) Substrate pretreatment A PET substrate with a thickness of 50 μm was subjected to corona treatment in a corona treatment machine at a power of 2.5 kW and a speed of 20 m / min. The surface tension after treatment was 52 dynes / cm. Then, a cross-linked polyester primer (with the same composition as in Example 1) was applied to the corona-treated surface using a wire rod. The primer was dried at 120 °C for 2 min to obtain a cross-linked primer with a dry film thickness of about 0.5 μm. (3) Coating The pretreated PET substrate is fixed on the coating machine, and the curing liquid is evenly coated on the surface of the base coating using a wire bar. The wet film thickness is controlled so that the final dry film thickness is 40μm. (4) Heat drying and curing The coated PET substrate is placed in a forced-air drying oven for segmented heat drying and curing: First stage: Heat and dry at 50℃ for 15 minutes; Second stage: Heat and dry at 70℃ for 10 minutes; Third stage: Heat and dry at 85℃ for 5 minutes; (5) UV light irradiation for shaping The heat-dried film is then placed in a UV curing machine (equipped with a high-pressure mercury lamp) and cured under nitrogen protection at a temperature of 400 mJ / cm². 2 The film is cured by irradiation with ultraviolet light energy to obtain a high-hardness hardened film.
[0034] Example 3 This embodiment provides a method for preparing a high-hardness hardening film, including the following steps: (0) Modification of nano-alumina KH570:water:ethanol was mixed in a volume ratio of 1:1:4, and the pH was adjusted to 4.5 with acetic acid. The mixture was stirred at room temperature for 30 min to obtain a KH570 hydrolysate. Nano-alumina (average particle size 60 nm) was dispersed in ethanol (10% solid content) and ultrasonically dispersed for 15 min to obtain a dispersion. The KH570 hydrolysate was added to the dispersion, with KH570 accounting for 5% of the mass of the nano-alumina. The mixture was stirred at 70 °C for 3 h. After the reaction, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 12 h to obtain modified nano-alumina.
[0035] (1) Preparation of hardening solution Weigh the following components by weight: 3 parts of chemically grafted expanded particles, 30 parts of free radical-cationic hybrid photocurable resin, 10 parts of reactive diluent TMPTA, 3 parts of free radical photoinitiator 184, 3 parts of cationic photoinitiator triarylthionium hexafluorophosphate, 50 parts of ethyl acetate / butanone (mass ratio 1:1) mixed solvent, 4 parts of modified nano alumina, 1 part of leveling agent, and 3 parts of anti-graffiti additive; the mixing, stirring, and filtration methods are the same as in Example 1.
[0036] (2) Substrate pretreatment A PET substrate with a thickness of 50 μm was subjected to corona treatment in a corona treatment machine at a power of 2.5 kW and a speed of 20 m / min. The surface tension after treatment was 52 dynes / cm. Then, a cross-linked polyester primer (with the same composition as in Example 1) was applied to the corona-treated surface using a wire rod. The primer was dried at 120 °C for 2 min to obtain a cross-linked primer with a dry film thickness of about 0.5 μm. (3) Coating The pretreated PET substrate is fixed on the coating machine, and the curing liquid is evenly coated on the surface of the base coating using a wire bar. The wet film thickness is controlled so that the final dry film thickness is 100μm. (4) Heat drying and curing The coated PET substrate is placed in a forced-air drying oven for segmented heat drying and curing: First stage: Heat and dry at 40℃ for 10 minutes; Second stage: Heat and dry at 85℃ for 5 minutes; Third stage: Heat and dry at 95℃ for 2 minutes; (5) UV light irradiation for shaping The heat-dried film is then placed in a UV curing machine (equipped with a high-pressure mercury lamp) and cured under nitrogen protection at a temperature of 800 mJ / cm². 2 The film is cured by irradiation with ultraviolet light energy to obtain a high-hardness hardened film.
[0037] Example 4 This embodiment provides a method for preparing a high-hardness hardening film, including the following steps: (1) Preparation of hardening solution Weigh the following components by weight: 4 parts of chemically grafted expanded particles, 45 parts of free radical-cationic hybrid photocurable resin, 15 parts of reactive diluent DPGDA, 1.5 parts of free radical photoinitiator 184, 1.5 parts of cationic photoinitiator diphenyliodonium hexafluorophosphate, 0.5 parts of sensitizer 2-isopropylthioxanthraquinone, 35 parts of ethyl acetate / butanone (mass ratio 1:1) mixed solvent, 15 parts of nano silica (Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., model XFI03, unmodified by KH570), 0.2 parts of leveling agent, and 1 part of anti-graffiti additive; the mixing, stirring, and filtration methods are the same as in Example 1.
[0038] (2) Substrate pretreatment A PET substrate with a thickness of 50 μm was subjected to corona treatment in a corona treatment machine at a power of 2.5 kW and a speed of 20 m / min. The surface tension after treatment was 52 dynes / cm. Then, a solvent-based polyester base coating (solvent-based polyester (by mass percentage): 30% polyester resin, 35% ethyl acetate, 35% methyl ethyl ketone) was applied to the corona-treated surface using a wire rod. The coating was dried at 120 °C for 1 min, and the dry film thickness was approximately 0.5 μm. (3) Coating The pretreated PET substrate is fixed on the coating machine, and the curing liquid is evenly coated on the surface of the base coating using a wire bar. The wet film thickness is controlled so that the final dry film thickness is 80μm. (4) Heat drying and curing The coated PET substrate is placed in a forced-air drying oven for segmented heat drying and curing: First stage: 48℃, heat and dry for 14 minutes; Second stage: Heat and dry at 75℃ for 7 minutes; Third stage: Heat and dry at 92℃ for 3 minutes; (5) UV light irradiation for shaping The heat-dried film is then placed in a UV curing machine (equipped with a high-pressure mercury lamp) and cured under nitrogen protection at a temperature of 600 mJ / cm². 2 The film is cured by irradiation with ultraviolet light energy to obtain a high-hardness hardened film.
[0039] Comparative Example 1 The difference from Example 1 is that the hardening solution in step (1) does not contain chemically grafted expanded particles. The remaining components and steps are the same as in Example 1.
[0040] Comparative Example 2 Compared with Example 1, the difference is that in step (1), 8 parts by weight of microcapsule-type thermally expandable microspheres (unmodified Expansionl 031 DU 40 raw material, i.e., bare core, without hyperbranched polymer shell) were used instead of chemically grafted expandable particles in the hardening solution. The remaining components and steps are the same as in Example 1.
[0041] Comparative Example 3 Compared with Example 1, the difference is that step (4) is omitted, and the UV light irradiation shaping step is performed directly after coating. The remaining components and steps are the same as in Example 1.
[0042] Comparative Example 4 Compared with Example 1, the difference is that in step (1), an equal amount of bifunctional polyurethane acrylate (EBECRYL® 284, containing only free radical curing groups) was used to replace the free radical-cationic hybrid photocurable resin in the curing solution, and no cationic photoinitiator was included. The remaining components and steps are the same as in Example 1.
[0043] Comparative Example 5 The difference from Example 1 is that step (4) involves drying directly at 90°C for 15 minutes. The remaining components and steps are the same as in Example 1.
[0044] The hardened films prepared in Examples 1-4 and Comparative Examples 1-5 were subjected to relevant performance tests. The test indicators and methods are as follows: 1. Pencil Hardness: According to GB / T 6739-2022 "Determination of Hardness of Paints and Varnishes by Pencil Method", a pencil hardness tester was used with a load of 500g. The pencil hardness ranged from 6B to 9H. The lowest hardness that could scratch the paint film was taken as the test result. Five different locations were tested for each sample, and the consistent values were taken.
[0045] 2. Abrasion Resistance (Steel Wool Friction): An abrasion testing machine was used. The friction head was made of #0000 steel wool (particle size approximately 5μm). The load was 1000g, the friction stroke was 40mm, the speed was 40 times / minute, and 1000 reciprocating friction cycles were performed. After the test, the scratches on the sample surface were visually observed under a standard light source. Evaluation criteria: No scratches (Excellent), slight scratches (Good, scratch length <5mm and number ≤3), obvious scratches (Poor, scratch length ≥5mm or number >3).
[0046] 3. Warpage: Refer to the flatness determination method in GB / T 13542.2-2021 "Films for Electrical Insulation - Part 2: Test Methods". Cut the sample into 100mm×100mm pieces, place them on a marble platform (flatness 0.01mm), and use a digital feeler gauge to measure the maximum height difference (mm) between the four corners and the platform. Take the average value of 3 samples.
[0047] 4. Transmittance: In accordance with GB / T 2410-2008 "Determination of transmittance and haze of transparent plastics", a transmittance haze meter was used with a wavelength range of 400~700nm. Each sample was tested 5 times and the average value was taken.
[0048] 5. Adhesion: According to GB / T 9286-2021 "Cross-cut Test for Paints and Varnishes", a cross-cut tester (11 teeth, 1mm spacing) is used to score the surface. After scoring, 3M 600 tape is applied and quickly peeled off at a 60° angle. The extent of coating peeling is observed. Rating standards: Grade 0 (completely smooth cut edges, no peeling); Grade 1 (minor peeling at the intersection of cuts, peeling area <5%); Grade 2 (peeling at the intersection of cuts and / or along the cut edges, peeling area 5%~15%); Grade 3 (partial or complete peeling of large squares, peeling area 15%~35%); Grade 4 (complete peeling of large squares or partial peeling of small squares, peeling area 35%~65%); Grade 5 (peeling area >65%).
[0049] The test results are shown in Table 1.
[0050] Table 1 Performance Test Results
[0051] As can be seen from the table above, the performance of the embodiments is superior to that of the comparative examples. The specific reasons are as follows: Comparative Example 1 (without expanding particles): Compared to Example 1, the hardening solution of Comparative Example 1 did not contain any chemically grafted expanding particles, resulting in a warpage of up to 2.52 mm (approximately 6 times that of Example 1), a pencil hardness of only 4H, and an abrasion resistance rating of "obvious scratches (poor)". This is because the lack of compressive stress established by expanding particles during the heat drying stage means that the low shrinkage characteristics of the free radical-cationic hybrid curing system alone cannot effectively offset all the internal stress generated by UV curing. After the coating is cured, residual tensile stress is concentrated, leading to severe warpage.
[0052] Comparative Example 2 (Conventional Expanded Monomer): Compared to Example 1, Comparative Example 2 used an equal mass of unmodified microcapsule-type thermally expandable microspheres to replace the chemically grafted expanded particles. The results showed a warpage of 2.16 mm (approximately 5.3 times that of Example 1), a hardness of only 5H, and abrasion resistance still classified as "significant scratches (poor)." Light transmittance decreased to 89.3%. This is because the bare core lacks the steric stabilization and chemical anchoring effects provided by the hyperbranched polymer shell, resulting in uneven dispersion and uncontrollable expansion behavior in the resin system, making it difficult to establish a uniform and stable compressive stress field. Furthermore, some aggregated microspheres expand to form large scattering centers, leading to a decrease in light transmittance. This comparative example fully demonstrates the indispensability of the chemically grafted hyperbranched polymer shell.
[0053] Comparative Example 3 (eliminating segmented heat drying, direct UV curing): Compared to Example 1, Comparative Example 3 eliminated the heat drying process and directly subjected the coating to UV light irradiation for shaping. The warpage was 1.15 mm (approximately 2.8 times that of Example 1), the hardness was 6H, the abrasion resistance was "slight scratches (good)", and the light transmittance was 90.6%. Although the light transmittance was acceptable, the warpage was significantly increased. The fundamental reason is that the expanding particles were not activated by heat drying, and the compressive stress was not effectively established; at the same time, the solvent was not removed in advance, and solvent evaporation and curing occurred simultaneously during the UV curing process, resulting in a small number of micropores inside the coating, and the hardness and abrasion resistance were also lower than those of Example 1.
[0054] Comparative Example 4 (pure free radical cured resin, without bifunctional hybrid system): Compared to Example 1, Comparative Example 4 used a bifunctional polyurethane acrylate (containing only free radical curing groups) to replace the free radical-cationic hybrid photocurable resin, and did not add a cationic photoinitiator. The resulting warpage was 0.93 mm (lower than Comparative Examples 1-3, but at the cost of hardness, only 3H), abrasion resistance was "obvious scratches (poor)", light transmittance was 90.4%, and adhesion was grade 0. The typical volume shrinkage rate of a pure free radical cured system is 6%~15%, and although the expanding particles provide compressive stress, the warpage is still difficult to reduce to below 0.5 mm; at the same time, the lack of a cationic polymeric interpenetrating network results in a significant decrease in hardness. This comparative example demonstrates the necessity of a free radical-cationic hybrid curing system.
[0055] Comparative Example 5 (One-Step Hot Drying): Compared to Example 1, Comparative Example 5 eliminated the segmented design and directly heated and dried at 90°C for 15 minutes. The warpage was 1.29 mm (approximately 3 times that of Example 1), the hardness was 6H, the abrasion resistance was "slight scratches (good)", the light transmittance was only 87.1%, and the adhesion was grade 1. The key difference is that: one-step high-temperature drying causes the activation of expanding particles and the concentrated and rapid evaporation of solvent to occur simultaneously. The microcapsules expand under heat in the coating that has not yet fully solidified, resulting in excessive local expansion and the formation of uneven micron-sized bubbles (scattering centers), which damages the optical uniformity of the coating and causes the light transmittance to drop significantly to 87.1% (below the basic requirement of ≥90% in the screen protector industry); and the adhesion of the base coating drops to grade 1 (when the cross-linking of the base coating is insufficient, one-step high temperature will also cause excessive stress at the interface between the base coating and the substrate). In Example 1, the segmented thermal drying process fully removes the solvent in the first stage (45°C, 12 min) to set the coating, and then precisely activates the expanding particles in the third stage (90°C, 3 min). This time-sequence decoupling effectively avoids the above-mentioned defects.
[0056] Examples 1-3 exhibited excellent performance in five dimensions: pencil hardness (7H-8H), abrasion resistance (excellent), warpage (≤0.9mm), light transmittance (≥90.5%), and adhesion (grade 0), achieving a synergy between high hardness and low warpage. Example 4, using unmodified nano-silica, showed slightly lower abrasion resistance (minor scratches), indicating that surface modification of the nanofiller helps improve the interfacial bonding strength with the resin.
[0057] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, and these simple modifications all fall within the protection scope of the present invention. Furthermore, it should be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe the various possible combinations.
[0058] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A high-hardness curing film, characterized in that, include: PET substrate, the surface of which has undergone high-energy surface treatment; A hardened layer disposed on at least one surface of the PET substrate; The hardened layer is formed by heat drying and curing of the hardening liquid followed by UV light irradiation for shaping. The hardening liquid includes chemically grafted expanded particles, free radical-cationic hybrid photocurable resin, reactive diluent, photoinitiator, nano-inorganic filler and solvent. The core of the chemically grafted expansion particles is a thermosensitive expansion active material, and the shell is a hyperbranched polymer containing polymerizable reactive groups. The branches of the hyperbranched polymer contain reactive groups that can undergo chemical cross-linking reactions with free radical-cationic hybrid photocurable resin. The photoinitiator includes free radical photoinitiators and cationic photoinitiators.
2. The high-hardness hardening film according to claim 1, characterized in that, The thermosensitive expansion active material is a microcapsule-type thermal expansion microsphere, which is a microcapsule with an acrylonitrile-based copolymer as the shell material and a low-boiling-point alkane as the core material.
3. The high-hardness hardening film according to claim 2, characterized in that, The hyperbranched polymer is grafted from AB2 type self-initiated monomers via surface-initiated atom transfer radical polymerization. The degree of branching of the hyperbranched polymer is 0.5-0.8, and the number average molecular weight is 2000-8000.
4. The high-hardness hardening film according to claim 1, characterized in that, The curing liquid comprises, by weight: 3-6 parts of chemically grafted expanding particles, 30-60 parts of free radical-cationic hybrid photocurable resin, 10-25 parts of reactive diluent, 1.5-3 parts of free radical photoinitiator, 1-3 parts of cationic photoinitiator, 30-50 parts of solvent, 4-15 parts of nano-inorganic filler, 0.1-1 parts of leveling agent, and 0.5-3 parts of anti-graffiti additive.
5. The high-hardness hardening film according to claim 4, characterized in that, The free radical-cationic hybrid photocurable resin is a dual-curing resin containing acrylate double bonds and alicyclic epoxy groups.
6. The high-hardness hardening film according to claim 4, characterized in that, The nano-inorganic filler is selected from one or more of nano-silica, nano-alumina, and nano-zirconia, with a particle size of 20-80 nm, and its surface is modified by a silane coupling agent.
7. The high-hardness hardening film according to claim 1, characterized in that, The PET substrate surface is provided with a cross-linked polyester base coating, which is formed by heat curing a polyester base coating liquid containing melamine cross-linking agent at 120-130℃.
8. A method for preparing a high-hardness hardening film as described in any one of claims 1-7, characterized in that, Includes the following steps: (1) Preparation of hardening solution: Mix the raw materials of hardening solution, stir evenly, filter, and obtain hardening solution; (2) Substrate pretreatment: Surface treatment of PET substrate; (3) Coating: The curing liquid prepared in step (1) is coated onto the surface of the PET substrate after pretreatment in step (2) to form a wet film; (4) Heat drying and curing: The coated PET substrate is heated and dried; (5) UV light curing: Under nitrogen protection, the film is cured by UV light to obtain a high-hardness hardened film.
9. The method for preparing a high-hardness hardening film according to claim 8, characterized in that, In step (4), the temperature for heat drying and curing is 40-95℃ and the time is 17-30min.
10. The method for preparing a high-hardness hardening film according to claim 8, characterized in that, The ultraviolet light irradiation energy in step (5) is 400-800 mJ / cm. 2 .