A card-making adhesive film, its preparation method, and the card-making method thereof.
By introducing thermal latent crosslinking and optical latent crosslinking mechanisms into the adhesive film of card making tape, the contradiction between scratch resistance and hot stamping performance is resolved, achieving a balance between high scratch resistance and hot stamping capability, which is suitable for surface protection of ID cards, bank cards and smart cards.
Patent Information
- Application Number
- CN202611611350.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
The existing card tape adhesive film has insufficient scratch resistance, the coating hardness and hot stamping performance are contradictory, the semi-finished product storage stability is poor, resulting in poor hot stamping and reduced adhesion.
It employs two crosslinking mechanisms, thermal latent crosslinking and optical latent crosslinking, which are activated in the lamination and UV final curing processes of the card manufacturing chain, respectively, to ensure that the crosslinking reaction occurs in stages, achieving high scratch resistance and subsequent hot stamping, and is suitable for long lead times and batch processing.
It achieves a balance between high scratch resistance and post-heat stamping capability, ensuring stable card performance during long-term storage and is suitable for surface protection of ID cards, bank cards, and smart cards.
Smart Images

Figure SMS_9 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional film technology for card making, specifically to an adhesive film for card making, its preparation method, and a card making method. Background Technology
[0002] ID cards, bank cards, and various smart cards generally use PET or PVC adhesive film as the surface protective layer. A typical structure consists of an outer functional coating, a middle thin film substrate layer, and an inner polyurethane hot-melt adhesive layer, which are laminated together with the printed card material at high temperature. To improve the card's scratch resistance, the industry typically adds a UV-cured coating to the film surface. To meet personalized customization needs, post-processing such as hot stamping (gold, silver, laser) is also required on the finished card surface.
[0003] However, existing card tape adhesive films have insufficient scratch resistance, and the surface hardness of conventional card tape adhesive films is relatively low (usually grade B or HB). After using conventional single-stage UV curing to increase hardness, the coating cross-linking density is too high, chemical inertness is enhanced, and surface polar groups are shielded, making it impossible for electroplated aluminum to adhere effectively. If the degree of curing is reduced to retain the hot stamping activity, the coating hardness and wear resistance will decrease significantly. The balance between increasing hardness and retaining hot stamping constitutes an inherent contradiction in existing technologies.
[0004] Meanwhile, the card manufacturing industry currently features long-cycle inventory preparation and batch processing. Furthermore, the production of card adhesive film and card processing are separate processes between the film factory and the card factory. During the storage and transportation of semi-finished products, residual active groups are prone to undergo dark reactions and premature cross-linking, leading to poor hot stamping, reduced adhesion, and unstable batch quality in the later stages. Summary of the Invention
[0005] To overcome the shortcomings of existing card-making adhesive films, such as the mutually exclusive resistance to scratches and the inability to perform subsequent hot stamping, as well as the poor storage stability of semi-finished products, this invention provides an adhesive film for card making, its preparation method, and a card-making method. This invention simultaneously introduces two sets of latent crosslinking mechanisms with non-overlapping activation conditions—thermal latent crosslinking and optical latent crosslinking—into the functional layer. The activation conditions for these two mechanisms are reserved for the two inherent processes in the card-making production chain: lamination and UV final curing. This allows the crosslinking reaction to occur segmentally along the process chain, with the subsequent hot stamping process precisely positioned between the two crosslinking segments. Thus, high scratch resistance and subsequent hot stamping are simultaneously achieved on the same coating system, adapting to the industry needs of film manufacturers requiring long lead times and card manufacturers requiring no equipment modifications.
[0006] One objective of this invention is to provide an adhesive film for card manufacturing, comprising a film substrate layer, a functional layer disposed on one side of the film substrate layer, and an adhesive layer disposed on the other side of the film substrate layer. The functional layer comprises the following raw materials in parts by weight: 45-65 parts of hydroxyl-type polyurethane acrylate resin, 5-15 parts of polycaprolactone diol, 15-28 parts of acrylate active monomer, 3.0-8.0 parts of blocked isocyanate crosslinking agent, 2.0-6.0 parts of nano-scratch-resistant modified powder, 2.5-5.0 parts of UV photoinitiator, 0.5-2.0 parts of functional additives, and 5-15 parts of organic solvent; the unsealing temperature of the blocked isocyanate crosslinking agent is 120-150°C. The dry film thickness of the functional layer is 8~12μm; The functional layer does not contain hydrogen-abstracting UV photoinitiators; The hydroxyl-type polyurethane acrylate resin has a hydroxyl value of 80~102 mgKOH / g, a hydroxyl functionality of 2, and an acrylate optical functionality of 2~4.
[0007] Preferably, the number average molecular weight of the polycaprolactone diol is 1000~3000, for example 1000, 1500, 2000, 2500 or 3000; and / or, the glass transition temperature of the polycaprolactone diol is -70~-60℃, for example -70℃, -65℃ or -60℃.
[0008] Preferably, the UV photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
[0009] Preferably, the mass ratio of the 2-hydroxy-2-methyl-1-phenyl-1-propanone to the phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1:0.4 to 1:1, for example, 1:0.4, 1:0.6, 1:0.8 or 1:1.
[0010] Preferably, the acrylate active monomer includes trimethylolpropane triacrylate and / or pentaerythritol tetraacrylate, such as trimethylolpropane triacrylate, pentaerythritol tetraacrylate, or a combination of trimethylolpropane triacrylate and pentaerythritol tetraacrylate.
[0011] Preferably, the nano-scratch-resistant modified powder comprises silane coupling agent modified nano-silica; and / or, the particle size of the nano-scratch-resistant modified powder is 30~70nm, for example 30nm, 40nm, 50nm, 60nm or 70nm.
[0012] Preferably, the organic solvent includes one or more of ethyl acetate, isopropanol, and butanone, such as ethyl acetate, isopropanol, butanone, a combination of ethyl acetate and isopropanol, a combination of ethyl acetate and butanone, a combination of isopropanol and butanone, or a combination of ethyl acetate, isopropanol, and butanone; and / or, the film substrate layer includes a PET film or a PVC film; and / or, the adhesive layer is made of a thermoplastic waterborne polyurethane adhesive.
[0013] A second objective of this invention is to provide a method for preparing a card-making adhesive film as described in any of the above embodiments, characterized by comprising the following steps: S1. Perform surface pretreatment on the thin film substrate layer; S2. Apply a functional layer coating to one side of the thin film substrate layer, and control the dry film thickness to be 8~12μm; S3. Pre-dry the coated layer at 40~60℃ and cool it to 20~30℃. S4. Apply an adhesive layer to the other side of the film substrate layer and dry and set it. S5. After curing, roll up the package, seal it in a light-proof container, and store it in a light-proof warehouse at 10~30℃.
[0014] Preferably, the preparation method satisfies at least one of the following features: in step S3, the pre-drying time is 30~120s, for example, 30s, 60s, 90s or 120s; in step S4, the drying and shaping temperature is 50~60℃, for example, 50℃, 55℃ or 60℃; in step S5, the ripening time is 1~3h, for example, 1h, 2h or 3h, and the light-proof storage period is not less than 180 days; and in step S1, the surface pretreatment is corona treatment.
[0015] The third objective of this invention is to provide a card manufacturing method, characterized by using an adhesive film for card manufacturing as described in any of the above embodiments, comprising the following steps: laminating the adhesive film with a printed card material at 120~150℃ and 5~15MPa, and punching it into individual cards; performing hot stamping on the surface of the individual cards at a temperature of 100~140℃ and a contact time of 0.3~1.5s; and subjecting the hot-stamped individual cards to UV final curing at a curing energy of 50~300mJ / cm².
[0016] The beneficial effects of this invention are: This invention employs a thermal latent crosslinking system composed of hydroxyl-type polyurethane acrylate resin and a blocked isocyanate crosslinking agent in the functional layer, and a photolatent crosslinking system composed of acrylate active monomers and a UV photoinitiator. The activation conditions of the two crosslinking mechanisms do not overlap and are activated separately by the card lamination process and the UV final curing process after hot stamping, allowing the crosslinking reaction to occur segmentally along the card manufacturing process chain. Thus, the semi-finished product is already shaped and uncrosslinked in its factory state, avoiding batch quality fluctuations caused by the dark reaction of residual active groups, achieving stable long-term light-protected storage for over 180 days, and adapting to the long-term stock preparation and batch processing production mode of the card manufacturing industry. In the lamination process, the blocked isocyanate crosslinking agent is deblocked at 120~150℃ and undergoes thermal crosslinking with the resin hydroxyl groups, giving the coating cohesive strength and interlayer bonding. Since the thermal crosslinking is activated during the lamination process, film manufacturers do not need to add a thermal curing section, and card manufacturers do not need to modify equipment. The UV final curing after hot stamping activates the photocrosslinking, giving the coating high hardness and high scratch resistance. Because thermal crosslinking and photocrosslinking are placed on opposite sides of the hot stamping process, the same coating can successively perform two mutually exclusive functions: hot stamping capability and high hardness, solving the problem of the incompatibility between scratch resistance and subsequent hot stamping performance. Furthermore, polycaprolactone diol, as a reactive toughening component, participates in the crosslinking network, improving the crack resistance and dimensional stability of the high-crosslinking density coating, and reducing final curing volume shrinkage to suppress card warping. Nano-anti-scratch modified powder is dispersed in the coating, further enhancing surface hardness and abrasion resistance. The dry film thickness of the functional layer is controlled at 8~12μm, balancing scratch resistance margin, flexibility, and hot stamping heat transfer. The hydroxyl-type polyurethane acrylate resin has a hydroxyl value of 80~102mgKOH / g, a hydroxyl functionality of 2, and an acrylate photofunctionality of 2~4, providing sufficient hydroxyl sites for thermal crosslinking. The adhesive film is laminated with the printed card material through an adhesive layer, resulting in a simple overall structure that is easy to promote on existing production lines. Verification by examples shows that the hot stamping adhesion of cards using the technical solution of the present invention can reach level 0, the pencil hardness after final curing is above 2H, there is no cracking after more than 2000 bends, and all performances remain stable after long-term light-proof storage. Detailed Implementation
[0017] The present application will be further described in detail below with reference to embodiments. In the following description, certain specific details are included to provide a comprehensive understanding of the various disclosed embodiments. However, those skilled in the art will recognize that the present invention can be practiced without employing one or more of these specific details, but using other methods, components, materials, etc.
[0018] According to a first aspect of the present invention, a card-making adhesive film is provided, comprising a film substrate layer, a functional layer disposed on one side of the film substrate layer, and an adhesive layer disposed on the other side of the film substrate layer, wherein the functional layer comprises the following raw materials in parts by weight: 45-65 parts of hydroxyl-type polyurethane acrylate resin, 5-15 parts of polycaprolactone diol, 15-28 parts of acrylate active monomer, 3.0-8.0 parts of blocked isocyanate crosslinking agent, 2.0-6.0 parts of nano-scratch-resistant modified powder, 2.5-5.0 parts of UV photoinitiator, 0.5-2.0 parts of functional additives, and 5-15 parts of organic solvent; The unblocking temperature of the blocked isocyanate crosslinking agent is 120~150℃; The dry film thickness of the functional layer is 8~12μm; The functional layer does not contain hydrogen-abstracting UV photoinitiators; The hydroxyl-type polyurethane acrylate resin has a hydroxyl value of 80~102 mgKOH / g, a hydroxyl functionality of 2, and an acrylate optical functionality of 2~4.
[0019] In this invention, the unsealing temperature refers to the starting temperature at which the blocked isocyanate crosslinking agent begins to unseale and release isocyanate groups. 120~150℃ indicates that the crosslinking agent begins to unseale at 120℃, and the higher the temperature, the more complete the unsealing.
[0020] In this invention, the hydroxyl-type polyurethane acrylate resin is a polyurethane acrylate oligomer containing hydroxyl groups. The functional layer of the adhesive film used in card making simultaneously possesses two sets of latent crosslinking mechanisms with non-overlapping activation conditions: The first is a thermal latent mechanism, where the hydroxyl groups of the hydroxyl-type polyurethane acrylate resin interact with the blocked isocyanate crosslinking agent. The activation condition is reaching the unsealing temperature of 120-150°C, which is first met by the lamination process in the entire production chain. Although the temperature range of the hot stamping process partially overlaps with the unsealing temperature, its stamping contact time is only 0.3-1.5 seconds, the coating heating time is extremely short, and the thermal crosslinking has already been completed during the lamination stage when hot stamping occurs, so it has no substantial impact. The second is a light latent mechanism, where the acrylate double bonds interact with the UV photoinitiator. The activation condition is receiving ultraviolet light irradiation, which is only met by the UV final curing process. These two mechanisms are independently controlled and activated sequentially, allowing the crosslinking reaction to occur segmentally along the card making process chain.
[0021] In this invention, the segmented activation places the subsequent hot stamping process between two crosslinking stages: during storage, it remains non-crosslinked and stable; during lamination, thermal crosslinking imparts cohesive strength and interlayer bonding to the coating; during hot stamping, the coating is not yet photocured, retaining polar groups and unreacted double bonds on the surface, allowing for good adhesion of electroplated aluminum; after hot stamping, UV final curing allows the double bonds to fully polymerize, achieving the final hardness. The order of thermal crosslinking and photocrosslinking is not interchangeable. If photocuring is performed before hot stamping, the surface becomes inert and cannot be hot stamped; if photocuring is not performed, the hardness will not meet the requirements. Thus, the same coating system successively undertakes the two mutually exclusive functions of hot stamping capability and high hardness, resolving the inherent contradiction that scratch resistance and subsequent hot stamping cannot be simultaneously achieved.
[0022] In this invention, the functional layer utilizes hydroxyl-type polyurethane acrylate resin to provide thermal crosslinking sites and photocrosslinking network density. Polycaprolactone diol, as a reactive toughening component, is grafted into the crosslinking network during the lamination stage, improving toughness while reducing final curing volume shrinkage to suppress card warping. Nano-sized anti-scratch modified powder is dispersed to enhance surface hardness and wear resistance. A UV photoinitiator eliminates the type II hydrogen abstraction system to avoid dark reactions during storage. The synergistic effect of these components and two latent mechanisms enables the adhesive film to possess high scratch resistance, allow for personalized hot stamping, and provide stable storage over a long period.
[0023] In this invention, the dry film thickness of the functional layer is 8~12μm, for example, 8μm, 9μm, 10μm, 11μm or 12μm. The dry film thickness of the functional layer of 8~12μm balances scratch resistance, flexibility and heat transfer during hot stamping: if it is too thin, the scratch resistance and abrasion resistance are insufficient; if it is too thick, the flexibility and lamination adhesion decrease, and the heat from hot stamping is more difficult to penetrate. This thickness matches the overall thickness of the card-making film and is suitable for surface protection of ID cards, bank cards and smart cards.
[0024] In this invention, the hydroxyl-type polyurethane acrylate resin has a hydroxyl value of 80-102 mgKOH / g, a hydroxyl functionality of 2, and an acrylate optical functionality of 2-4. If the hydroxyl value is too low, there will be insufficient hydroxyl sites for thermal crosslinking, and the blocked isocyanate crosslinking agent will not react sufficiently after deblocking during the lamination stage, resulting in insufficient cohesive strength and interlayer bonding in the coating. If the hydroxyl value is too high, the resin will be too polar, the system viscosity will be too high, the coating leveling properties will decrease, and the coating brittleness will increase. Within the above-mentioned hydroxyl value range, the resin can provide sufficient hydroxyl sites for thermal crosslinking while maintaining good coatability and flexibility. A hydroxyl functionality of 2 provides bifunctional crosslinking sites while avoiding premature gelation during storage due to excessive functionality. An acrylate optical functionality of 2-4 ensures the density of the photocured network and the final hardness, while avoiding over-crosslinking that causes brittleness.
[0025] In a preferred embodiment of the present invention, the hydroxyl-type polyurethane acrylate resin includes Sartamomer CN9062 or U-CURE 93726; preferably, the hydroxyl value of Sartamomer CN9062 is 85 mg KOH / g, the hydroxyl value of U-CURE 93726 is 96 mg KOH / g, and the hydroxyl functionality of both is 2.
[0026] In a preferred embodiment of the present invention, the number average molecular weight of the polycaprolactone diol is 1000~3000, for example 1000, 1500, 2000, 2500 or 3000; and / or, the glass transition temperature of the polycaprolactone diol is -70~-60℃, for example -70℃, -65℃ or -60℃.
[0027] In this preferred embodiment, the number-average molecular weight of polycaprolactone diol (1000~3000) and its glass transition temperature (-70~-60℃) jointly determine its reactive toughening and final curing shrinkage control effects: if the molecular weight is too small, the toughening segments are too short and the toughness improvement is limited; if the molecular weight is too large, the viscosity increases and coating becomes difficult. The lower the glass transition temperature, the easier it is for the flexible segments to dissipate energy through deformation at the card's operating temperature, thus suppressing the brittle cracking of the high cross-linking density coating. At the same time, its low melting point and softening and melting at the hot stamping temperature are beneficial for inter-fusion and anchoring with the electroplated aluminum hot melt adhesive layer.
[0028] In a preferred embodiment of the present invention, the polycaprolactone diol comprises Perstorp Capa 2100A or Perstorp Capa 2302A.
[0029] In a preferred embodiment of the present invention, the blocked isocyanate crosslinking agent includes TrixeneBI7982.
[0030] In a preferred embodiment of the present invention, the UV photoinitiator comprises 2-hydroxy-2-methyl-1-phenyl-1-propanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, wherein the mass ratio of the 2-hydroxy-2-methyl-1-phenyl-1-propanone to the phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1:0.4 to 1:1, for example, 1:0.4, 1:0.6, 1:0.8 or 1:1.
[0031] In this preferred embodiment, 2-hydroxy-2-methyl-1-phenyl-1-propanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide are both Norrish type I UV photoinitiators, such as BASF Irgacure 1173 and BASFIrgacure 819, which generate active free radicals only under the action of ultraviolet photons and do not initiate in the absence of light; the mass ratio of the two is 1:0.4 to 1:1 to ensure sufficient initiation and deep curing at the main wavelength of UV-LED (365~420nm); the functional layer does not contain type II hydrogen-abstracting UV photoinitiators and their amine co-initiators, which can avoid dark reactions caused by charge transfer complexes during storage, and is an important guarantee for long-term stable storage.
[0032] In a preferred embodiment of the present invention, the acrylate active monomer comprises trimethylolpropane triacrylate and / or pentaerythritol tetraacrylate, such as trimethylolpropane triacrylate, pentaerythritol tetraacrylate, or a combination of trimethylolpropane triacrylate and pentaerythritol tetraacrylate; preferably, the trimethylolpropane triacrylate comprises Sartomer SR351, and the pentaerythritol tetraacrylate comprises Sartomer SR295; In a preferred embodiment of the present invention, the nano-scratch-resistant modified powder comprises silane coupling agent modified nano-silica, and the particle size of the nano-scratch-resistant modified powder is 30~70nm, for example, 30nm, 40nm, 50nm, 60nm or 70nm.
[0033] The preparation method of the silane coupling agent modified nano-silica is as follows: the nano-silica is dried at 120℃ for 4 hours; the dried nano-silica and KH-570 are added to an ethanol / water mixture with a volume ratio of 11:1, the amount of KH-570 being 3% of the mass of the nano-silica; the pH is adjusted to 4-5 with acetic acid; the reaction is refluxed at 80℃ for 2 hours; the reaction solution is centrifuged, washed with acetone, and then dried at 120℃ for 48 hours to obtain the final product.
[0034] In this preferred embodiment, the acrylate active monomer is trimethylolpropane triacrylate and / or pentaerythritol tetraacrylate, which provides multiple double bond sites for photocrosslinking to construct a high crosslinking density network and improve the final hardness; the nano-scratch-resistant modified powder is made of silane coupling agent modified nano-silica with a particle size of 30~70nm. The nanoparticles are dispersed in the coating to improve surface hardness and wear resistance. The coupling agent improves the interfacial bonding between the nanoparticles and the resin. If the particle size is too small, it is easy to agglomerate; if it is too large, the surface is rough and the light transmittance is reduced.
[0035] In a preferred embodiment of the present invention, the functional additives include one or more of leveling agents, defoamers, and coupling agents; the leveling agent is, for example, BYK-350, the defoamer is, for example, BYK-055, and the silane coupling agent is, for example, KH-570.
[0036] In a preferred embodiment of the present invention, the organic solvent includes one or more of ethyl acetate, isopropanol, and butanone, such as ethyl acetate, isopropanol, butanone, a combination of ethyl acetate and isopropanol, a combination of ethyl acetate and butanone, a combination of isopropanol and butanone, or a combination of ethyl acetate, isopropanol, and butanone; and / or, the film substrate layer includes a PET film or a PVC film; and / or, the adhesive layer is made of a thermoplastic waterborne polyurethane adhesive.
[0037] In this preferred embodiment, the organic solvent is one or more of ethyl acetate, isopropanol, and methyl ethyl ketone, used to adjust the coating viscosity and evaporation gradient and ensure surface drying and setting during the pre-drying stage; the film substrate layer is made of PET or PVC card film, and the adhesive layer is made of thermoplastic waterborne polyurethane adhesive, both of which are mature systems in the card manufacturing industry and are easy to promote on existing production lines.
[0038] According to a second aspect of the present invention, a method for preparing a card-making adhesive film as described above is provided, characterized by comprising the following steps: S1, performing surface pretreatment on the film substrate layer; S2, coating a functional layer coating on one side of the film substrate layer, controlling the dry film thickness to be 8~12μm; S3, pre-drying the coated layer at 40~60℃, and cooling it to 20~30℃; S4, coating an adhesive layer on the other side of the film substrate layer and drying and shaping it; S5, after curing, winding it up, sealing it in a light-proof package, and storing it in a light-proof warehouse at 10~30℃.
[0039] In this invention, the preparation method involves pre-drying at 40-60°C and then cooling to 20-30°C, allowing the functional layer to surface dry and set while the blocked isocyanate remains unopened and the double bonds are fully preserved, resulting in a set but uncrosslinked semi-finished product. The adhesive layer is dried and set at 50-60°C, below the unopening temperature, to avoid interference with the thermal crosslinking of the functional layer. After curing and winding, the semi-finished product is stored in a light-proof warehouse at 10-30°C, allowing for long-term stable storage and batch processing. This preparation method reserves the activation of thermal crosslinking for subsequent lamination processes, eliminating the need for film manufacturers to add a thermal curing section.
[0040] In a preferred embodiment of the present invention, the preparation method satisfies at least one of the following features: in step S3, the pre-drying time is 30~120s; in step S4, the drying and shaping temperature is 50~60℃, and is lower than the unsealing initiation temperature of the blocked isocyanate crosslinking agent; in step S5, the curing time is 1~3h, and the light-proof storage period is not less than 180 days; and in step S1, the surface pretreatment is corona treatment.
[0041] In this preferred embodiment, step S3, with a pre-drying time of 30-120 seconds, ensures that the coating is surface-dry and set, and that the solvent is basically removed, without unsealing the closed isocyanate; step S4, with the adhesive layer dried at 50-60°C, below the unsealing initiation temperature, does not trigger thermal cross-linking of the functional layer; step S5, with a curing time of 1-3 hours, allows the adhesive layer to be initially set, and the light-proof storage for no less than 180 days is suitable for long-cycle inventory preparation in the card manufacturing industry; step S1, with corona treatment, ensures that the surface wetting tension of the substrate is no less than 48 mN / m, thereby improving the bonding force between the functional layer and the substrate.
[0042] According to a third aspect of the present invention, a card manufacturing method is provided, using the card-making adhesive film as described above, comprising the following steps: S1, laminating the adhesive film with a printed card material at 120~150℃ and 5~15MPa, thereby desealing the blocked isocyanate crosslinking agent and thermally crosslinking it with the hydroxyl groups in the functional layer, and punching it into individual cards; S2, performing hot stamping on the surface of the individual cards, with a hot stamping temperature of 100~140℃ and an stamping contact time of 0.3~1.5s; S3, subjecting the hot-stamped individual cards to ultraviolet final curing with a curing energy of 50~300mJ / cm².
[0043] The card manufacturing method involves laminating the adhesive film and printed card material at 120-150℃ and 5-15MPa. This process simultaneously de-encapsulates the closed isocyanate and completes the thermal cross-linking of the functional layers, imparting cohesive strength and interlayer bonding to the coating. Subsequently, during hot stamping (100-140℃, 0.3-1.5s), the coating surface retains active groups and unreacted double bonds, allowing for good adhesion of electroplated aluminum. Finally, UV curing (50-300mJ / cm²) fully polymerizes the double bonds, increasing the hardness to above 2H. This three-stage process, with thermal cross-linking, hot stamping, and photocross-linking sequentially, allows the same coating to achieve both high scratch resistance and the ability to be hot stamped later. The lamination temperature of 120~150℃ and the unsealing temperature of 120~150℃ are matched. The actual lamination temperature is not lower than the unsealing start temperature of the crosslinking agent so that the crosslinking agent can be unsealed and thermally crosslinked with the hydroxyl group. The higher the lamination temperature, the higher the degree of thermal crosslinking. For example, the gel content is 68% when laminating at 120℃ in Example 2 and 91% when laminating at 150℃ in Example 3, both of which meet the requirements for use.
[0044] The preparation method of silane coupling agent modified nano-silica is as follows: Nano-silica was dried at 120℃ for 4 hours. The dried nano-silica and KH-570 were added to an ethanol / water mixture with a volume ratio of 11:1, with KH-570 accounting for 3% of the nano-silica mass. The pH was adjusted to 4-5 with acetic acid. The mixture was refluxed at 80℃ for 2 hours. After centrifugation and washing with acetone, the reaction solution was dried at 120℃ for 48 hours to obtain silane coupling agent (KH-570) modified nano-silica, hereinafter referred to as silane coupling agent modified nano-silica. All modified nano-silica used in the examples was prepared by this method, and raw material particle sizes of 30nm, 40nm, 50nm, 60nm, or 70nm were selected according to the requirements of the examples.
[0045] Example 1 A 50 μm thick PET film was used as the film substrate layer and subjected to corona treatment to achieve a surface wetting tension of over 48 mN / m. 55 parts of hydroxyl-type polyurethane acrylate resin U-CURE 93726 and 10 parts of polycaprolactone diol Perstorp Capa2200A (number average molecular weight 2000, glass transition temperature...) were used. The following ingredients were mixed uniformly at 20-30°C in the dark to obtain the functional layer coating: 13 parts of acrylate reactive monomer trimethylolpropane triacrylate Sartomer SR351 and 9 parts of pentaerythritol tetraacrylate Sartomer SR295, 5.0 parts of blocked isocyanate crosslinking agent Trixene BI7982, 4.0 parts of silane coupling agent modified nano silica (particle size 50nm), 1.88 parts of Irgacure 1173 and 1.32 parts of Irgacure 819 (mass ratio 1:0.7), 0.5 parts of BYK-350, 0.4 parts of BYK-055 and 0.3 parts of KH-570, 6 parts of organic solvent ethyl acetate and 4 parts of butanone.
[0046] The functional layer coating is applied to one side of the PET film after corona treatment, and the dry film thickness is controlled to be 10 μm. It is pre-dried at 50℃ for 75s, with a residual solvent content of 5%, and then cooled to 20~30℃. A thermoplastic waterborne polyurethane adhesive is applied to the other side of the PET film and dried and shaped at 55℃. After curing for 2 hours, it is rolled up, sealed in a light-proof package, and stored in a light-proof warehouse at 10~30℃ for 180 days to obtain the adhesive film for card making.
[0047] Card making: The obtained adhesive film and printed card material are laminated together at 135℃ and 10MPa to deseal the blocked isocyanate crosslinking agent and thermally crosslink with the hydroxyl groups in the functional layer. The card is then punched into individual cards. Hot stamping is performed on the surface of the individual cards at a temperature of 120℃ and a contact time of 0.9s. The hot-stamped individual cards are then subjected to UV final curing at a curing energy of 175mJ / cm².
[0048] Example 2 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 45 parts of hydroxyl-type polyurethane acrylate resin U-CURE 93726; and 15 parts of polycaprolactone diol Perstorp Capa 2302A (number average molecular weight 3000, glass transition temperature...). (61℃); the active monomer of acrylate is 28 parts of pentaerythritol tetraacrylate Sartomer SR2952; the blocked isocyanate crosslinking agent Trixene BI7982 is 3.0 parts; the silane coupling agent modified nano-silica (particle size 30nm) is 2.0 parts; the UV photoinitiator is 2.5 parts of Irgacure 1173 and 2.5 parts of Irgacure 819 (mass ratio 1:1); the functional additives are 0.8 parts of BYK-350, 0.7 parts of BYK-055 and KH-570. 0.5 parts; organic solvent: ethyl acetate 5 parts; film substrate: PVC film; dry film thickness: 12 μm; pre-drying: 45℃ for 60 s; residual solvent content in coating: 4%; drying and setting temperature of thermoplastic waterborne polyurethane adhesive layer: 50℃; curing time: 1.5 h; card making lamination conditions: 120℃, 5 MPa; hot stamping conditions: 100℃, 0.3 s; UV final curing energy: 50 mJ / cm².
[0049] Example 3 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 65 parts of hydroxyl-type polyurethane acrylate resin (Sartomer CN9062); and 5 parts of polycaprolactone diol (Perstorp Capa 2100A, number average molecular weight 1000, glass transition temperature...). (68℃); the active monomer of acrylate is 15 parts of trimethylolpropane triacrylate Sartomer SR351; the blocked isocyanate crosslinking agent Trixene BI7982 is 8.0 parts; the silane coupling agent modified nano silica (particle size 70nm) is 6.0 parts; the UV photoinitiator is 1.79 parts of Irgacure 1173 and 0.71 parts of Irgacure 819 (mass ratio 1:0.4); the functional additives are 0.2 parts of BYK-350, 0.2 parts of BYK-055 and KH-570. 0.1 parts; organic solvents: 8 parts ethyl acetate and 7 parts methyl ethyl ketone; dry film thickness: 8 μm; pre-drying at 55℃ for 90 s, residual solvent content in coating: 6%; drying and setting temperature of thermoplastic waterborne polyurethane adhesive layer: 60℃; curing time: 2.5 h; card making lamination conditions: 150℃, 15 MPa; hot stamping conditions: 140℃, 1.5 s; UV final curing energy: 300 mJ / cm².
[0050] Example 4 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 50 parts of hydroxyl-type polyurethane acrylate resin (Sartomer CN9062); and 8 parts of polycaprolactone diol (Perstorp Capa 2200A, number average molecular weight 2000, glass transition temperature...). (65℃); the active monomer of acrylate is 18 parts of trimethylolpropane triacrylate Sartomer SR351; the blocked isocyanate crosslinking agent Trixene BI7982 is 4.0 parts; the silane coupling agent modified nano silica (particle size 40nm) is 3.0 parts; the UV photoinitiator is 1.75 parts of Irgacure 1173 and 1.05 parts of Irgacure 819 (mass ratio 1:0.6); the functional additives are 0.35 parts of BYK-350, 0.3 parts of BYK-055 and KH-570. 0.15 parts; 8 parts isopropanol as organic solvent; PVC film as substrate layer; 9 μm dry film thickness; pre-drying at 50℃ for 60 s, with a residual solvent content of 5% in the coating; drying and setting temperature of the thermoplastic waterborne polyurethane adhesive layer at 55℃; card lamination conditions at 125℃ and 8 MPa; hot stamping conditions at 110℃ and 0.6 s; UV final curing energy at 120 mJ / cm².
[0051] Example 5 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 60 parts of hydroxyl-type polyurethane acrylate resin U-CURE 93726; and 12 parts of polycaprolactone diol Perstorp Capa 2200A (number average molecular weight 2000, glass transition temperature...). (65℃); the active monomers of acrylate are 15 parts of trimethylolpropane triacrylate Sartomer SR351 and 10 parts of pentaerythritol tetraacrylate Sartomer SR295; the blocked isocyanate crosslinking agent Trixene BI7982 is 6.5 parts; the silane coupling agent modified nano-silica (particle size 60nm) is 5.0 parts; the UV photoinitiator is 2.22 parts of Irgacure 1173 and 1.78 parts of Irgacure 819 (mass ratio 1:0.8); the functional additives are 0.65 parts of BYK-350, 0.55 parts of BYK-055 and KH-570. 0.4 parts; organic solvents: 6 parts ethyl acetate, 3 parts isopropanol, and 3 parts butanone; dry film thickness: 11 μm; pre-drying at 50℃ for 90 s; residual solvent content in the coating: 4%; drying and setting temperature of the thermoplastic waterborne polyurethane adhesive layer: 58℃; card lamination conditions: 145℃, 12MPa; hot stamping conditions: 130℃, 1.2 s; UV final curing energy: 250 mJ / cm².
[0052] Example 6 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the following differences: 52 parts of hydroxyl-type polyurethane acrylate resin (Sartomer CN9062); 12 parts of trimethylolpropane triacrylate (Sartomer SR351) and 8 parts of pentaerythritol tetraacrylate (Sartomer SR295); 5.5 parts of blocked isocyanate crosslinking agent (Trixene BI7982); 4.5 parts of silane coupling agent-modified nano-silica (50nm particle size); 2.06 parts of UV photoinitiator (Irgacure 1173) and 1.44 parts of Irgacure 819 (mass ratio 1:0.7); and 0.4 parts of functional additives (BYK-350, BYK-055, and KH-570). 0.25 parts; pre-drying at 40℃ for 30s, residual solvent content in coating is 3%; drying and setting temperature of thermoplastic waterborne polyurethane adhesive layer is 52℃; curing time is 1h; card making lamination conditions are 130℃ and 10MPa.
[0053] Example 7 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 58 parts of hydroxyl-type polyurethane acrylate resin (Sartomer CN9062); and 10 parts of polycaprolactone diol (Perstorp Capa 2100A) (number average molecular weight 1000, glass transition temperature...). The composition of the coating is as follows: 68℃); the active monomers of the acrylate are 14 parts of trimethylolpropane triacrylate Sartomer SR351 and 10 parts of pentaerythritol tetraacrylate Sartomer SR295; the blocked isocyanate crosslinking agent Trixene BI7982 is 6.0 parts; the silane coupling agent modified nano-silica (particle size 50nm) is 3.5 parts; the UV photoinitiator is 2.14 parts of Irgacure 1173 and 0.86 parts of Irgacure 819 (mass ratio 1:0.4); the functional additives are 0.6 parts of BYK-350, 0.5 parts of BYK-055 and 0.3 parts of KH-570; pre-drying is carried out at 60℃ for 120s, and the residual solvent content of the coating is 8%; the drying and setting temperature of the thermoplastic waterborne polyurethane adhesive layer is 56℃; the curing time is 3h; the card making lamination conditions are 130℃ and 10MPa.
[0054] Example 8 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: 54 parts of hydroxyl-type polyurethane acrylate resin U-CURE 93726; and 5 parts of polycaprolactone diol, a compound of 5 parts of Perstorp Capa 2100A and 5 parts of Perstorp Capa 2302A (number average molecular weight 2000, glass transition temperature...). (65℃); the active monomer of acrylate is 21 parts of pentaerythritol tetraacrylate Sartomer SR295; the UV photoinitiator is 2.29 parts of Irgacure 1173 and 0.91 parts of Irgacure 819 (mass ratio 1:0.4).
[0055] Example 9 The adhesive film for card making was prepared and cards were made according to the method of Example 1, with the difference being: the hydroxyl-type polyurethane acrylate resin was 56 parts of U-CURE 93726; the polycaprolactone diol was a compound of 4.8 parts of Perstorp Capa 2200A and 7.2 parts of Perstorp Capa 2302A (number average molecular weight 2600, glass transition temperature...). The acrylate active monomer is 20 parts of trimethylolpropane triacrylate Sartomer SR351; the UV photoinitiator is 1.8 parts of Irgacure 1173 and 1.8 parts of Irgacure 819 (mass ratio 1:1); the dry film thickness is 12 μm.
[0056] Example 10 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that the light-proof storage period was 240 days.
[0057] The following comparative examples are all based on the formula and process of Example 1, with only one technical feature changed, and the other conditions are the same as in Example 1, in order to illustrate the contribution of each technical feature to high scratch resistance, subsequent hot stamping performance and long-term storage stability.
[0058] Comparative Example 1 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that the blocked isocyanate crosslinking agent Trixene BI7982 was not added.
[0059] Comparative Example 2 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that 0.3 parts of an organic bismuth catalyst were added to reduce the desealing initiation temperature of the blocked isocyanate to 65°C.
[0060] Comparative Example 3 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that the amount of the blocked isocyanate crosslinking agent Trixene BI7982 was 1.5 parts.
[0061] Comparative Example 4 The adhesive film for card making was prepared and cards were made according to the method of Example 1, except that polycaprolactone diol Perstorp Capa 2200A was not added.
[0062] Comparative Example 5 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that the amount of polycaprolactone diol Perstorp Capa 2200A used was 20 parts.
[0063] Comparative Example 6 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that 2.0 parts of benzophenone and 1.2 parts of triethanolamine were used to replace Irgacure 1173 and Irgacure 819.
[0064] Comparative Example 7 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that: the film was first cured with ultraviolet light at an energy of 175 mJ / cm², and then hot stamping was performed.
[0065] Comparative Example 8 The adhesive film for card making was prepared and the cards were made according to the method of Example 1, except that the dry film thickness of the functional layer was 20 μm.
[0066] Performance testing methods The following performance tests were performed on the obtained card-making adhesive film and the cards made from it.
[0067] T1 pencil hardness: According to GB / T 6739-2022, after UV final curing, it is placed at 20~30℃ for 24h and tested with a 750g load.
[0068] T2 hot stamping adhesion: According to GB / T 9286-2021, the hot stamping area is divided into grids with a 1mm interval. After peeling with 3M 600 tape, it is rated from 0 to 5, with 0 being the best.
[0069] T3 Scratch Resistance: 0000# steel wool is wrapped and fixed to a cylindrical pressure head with a bottom diameter of 1cm. The coated surface is rubbed back and forth 20 times with a load of 750g (the friction stroke is about 5cm). The surface scratches are visually inspected and rated from 0 to 5. 0 indicates no visible scratches and 5 indicates severe scratches.
[0070] T4 flexural strength: Card bending test according to ISO / IEC 10373-1:2020, record the number of bends when visible cracks appear, with an upper limit of 3000 times.
[0071] T5 Card Warping: Place the card freely on the platform and measure the maximum height of the four corners from the surface.
[0072] T6 thermal crosslinking degree: The laminated coating was extracted with methyl ethyl ketone (MEK) by Soxhlet extraction for 8 hours, and the percentage of insoluble dry weight to the original dry weight was used as the gel content.
[0073] T7 surface roughness Ra: measured according to ISO 21920-2:2021 using a stylus-type surface roughness tester, with a sampling length of 0.8 mm, and the average value of 5 points is taken.
[0074] T8 Storage Stability: After storage at 10~30℃ in the dark for 180 days or 240 days, the viscosity change rate of the coating is determined by the Forte 4 cup according to GB / T 1723-1993, and T1 and T2 are retested to determine the stability of the UV curing system during storage and the complete retention of active groups, ensuring normal hot stamping and UV final curing.
[0075] T9 Hot Stamping Pattern Integrity: Visually inspect the edges of the hot stamping pattern for jagged edges and missing areas under 10x magnification. ○ indicates good condition, △ indicates minor defects, and × indicates obvious defects.
[0076] Table 1 Performance test results of Examples 1-10
[0077] Table 2 Performance test results after long-term light-proof storage
[0078] Table 3 Performance test results of Comparative Examples 1-8
[0079] Comparing Example 1 with Comparative Examples 1 and 7, it can be seen that the gel content after lamination in Example 1 reaches 82%, indicating that the blocked isocyanate is fully unblocked and thermally crosslinked within the lamination window, while the hot stamping adhesion remains at grade 0 and the pencil hardness reaches 3H after final curing. Comparative Example 1, without the addition of blocked isocyanate, has a gel content of only 21%. This 21% gel originates from the partial thermally initiated polymerization of acrylate double bonds in the resin and multifunctional monomers within the functional layer at high lamination temperatures. Its network does not contain urethane crosslinks and its density is much lower than that of Example 1, thus lacking cohesive strength. The hot stamping adhesion drops to grade 2, and obvious scratches (grade 2) appear in the steel wool scratch resistance test. In Comparative Example 7, the UV final curing is advanced to before hot stamping, resulting in fully polymerized double bonds on the coating surface and shielded polar groups. The hot stamping adhesion drops to grade 4, and obvious missed hot stamping patterns appear. It is evident that thermal crosslinking and photocrosslinking must be placed on opposite sides of the hot stamping process, activated in stages according to the order of lamination, hot stamping, and UV final curing; the order of the two cannot be interchanged.
[0080] Comparing Example 1 with Comparative Examples 2 and 3, it can be seen that in Comparative Example 2, after adding an organic bismuth catalyst to lower the desealing initiation temperature to 65°C, the coating underwent a dark reaction during the drying of the adhesive layer and storage at 10-30°C. After 180 days of storage, the coating viscosity increased by 46%, the hot stamping adhesion dropped to level 3, and obvious defects appeared in the hot stamping pattern. This indicates that the thermal latency mechanism loses its unique orientation in the production chain when the desealing temperature is below 120°C. In Comparative Example 3, when the amount of crosslinking agent was reduced to 1.5 parts, the gel content was only 55%. The thermal crosslinking network formed during the lamination stage was insufficient to support the hot stamping and scratch resistance requirements, the hardness dropped to H, and visible scratches (level 1) appeared in the steel wool scratch resistance test. In Example 2, at a lamination temperature of 120°C, and in Example 3, at a lamination temperature of 150°C, the gel contents were 68% and 91%, respectively, both within the usable range. This indicates that the desealing temperature window of 120-150°C matches the card lamination process window.
[0081] As can be seen from the comparison between Example 1 and Comparative Examples 4 and 5, when no polycaprolactone diol was added to Comparative Example 4, although the coating could reach a hardness of 3H and the hot stamping adhesion was grade 0, it cracked after only 700 flexing cycles and the card warped by 1.8 mm. This indicates that when the reactive toughening component is missing, the high cross-linking density coating is brittle and the final curing volume shrinkage cannot be suppressed. In Comparative Example 5, the amount of polycaprolactone diol was increased to 20 parts, resulting in excessive flexibility of the coating. The pencil hardness dropped to HB, and the steel wool scratch resistance test showed obvious scratches (grade 2) and the surface became sticky. A comparison of Examples 8 and 9 shows that, within the range of 10-12 parts of total polycaprolactone diol, the number-average molecular weight of the compound was increased from 2000 to 2600, the number of flexural cycles was increased from 2800 to over 3000, while the hardness remained at 2H-3H. This indicates that polycaprolactone diol, by being grafted into the crosslinking network in a reactive manner, can improve crack resistance and suppress card warping without sacrificing hardness.
[0082] A comparison of Example 1 and Comparative Example 6 shows that in Comparative Example 6, after replacing the compounded Type I initiator with a Type II hydrogen-abstraction system composed of benzophenone and triethanolamine, the coating viscosity increased by 62% after 180 days of storage in the dark at 10-30°C, the hot stamping adhesion dropped to level 3, and obvious defects appeared in the hot stamping pattern. This indicates that the hydrogen-abstraction system undergoes a dark reaction through charge transfer complexation during storage, prematurely consuming the surface active groups. This is the reason why the functional layer does not contain a hydrogen-abstraction UV photoinitiator. Furthermore, in Examples 3 and 8, when the mass ratio of Irgacure 1173 to Irgacure 819 was 1:0.4, and curing energies of 300 mJ / cm² and 175 mJ / cm² were used respectively, a 2H hardness could still be achieved. This indicates that the combination of these two substances with a curing energy window of 50-300 mJ / cm² can achieve sufficient curing over a relatively wide energy range.
[0083] Meanwhile, Examples 2, 1, and 3 used powders with wavelengths of 30nm, 50nm, and 70nm, respectively, with surface roughnesses of 0.06μm, 0.07μm, and 0.13μm, and hot stamping adhesion grades of 0, 0, and 1, respectively, all within the usable range. As can be seen from Comparative Example 8, when the dry film thickness increased to 20μm, the film cracked after 900 bends, the card warped by 1.1mm, and the hot stamping heat could not penetrate to the interface between the coating and the electroplated aluminum, resulting in a hot stamping adhesion grade of 2. However, Example 2, at 12μm, and Example 3, at 8μm, still achieved hardnesses of 2H and 4H, respectively, indicating that a dry film thickness window of 8~12μm simultaneously considered scratch resistance margin, flexibility, and hot stamping heat transfer.
[0084] As shown in Table 2, after 180 days of storage in the dark at 10-30℃, the viscosity change rates of the coatings in Examples 1, 6, and 7 were +3%, +2%, and +7%, respectively. The hardness and hot stamping adhesion were consistent with those before storage, and the hot stamping pattern remained intact. In Example 10, after 240 days of storage, the viscosity change rate was +5%, the hardness remained 3H, and the hot stamping adhesion remained at grade 0. Among these, Example 7, with a pre-drying temperature of 60℃ and a residual solvent content of 8%, exhibited a relatively high viscosity change rate after storage, indicating that the pre-drying temperature and residual solvent content should be controlled within the middle range of 40-60℃ and 3-8%, respectively. These results demonstrate that the blocked isocyanate does not dissociate under storage conditions, the type I photoinitiator does not decompose under light-protected conditions, and both the thermal latency system and the photocuring system remain stable. The semi-finished product can still undergo normal UV final curing and hot stamping after storage, and can be stably stored for more than 180 days, making it suitable for the long-cycle inventory preparation and batch processing production model of the card manufacturing industry.
[0085] The applicant declares that the present invention is illustrated by the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A film for card manufacturing, comprising a film base layer, a functional layer provided on one side of the film base layer, and an adhesive layer provided on the other side of the film base layer, characterized in that, The functional layer comprises the following raw materials in parts by weight: 45-65 parts of hydroxyl-type polyurethane acrylate resin; 5-15 parts of polycaprolactone diol; 15-28 parts of acrylate reactive monomer; 3.0~8.0 parts of blocked isocyanate crosslinking agent; 2.0~6.0 parts of nano-scratch-resistant modified powder; 2.5~5.0 parts of UV photoinitiator; Functional additives 0.5-2.0 parts; and, 5-15 parts organic solvent; The unblocking temperature of the blocked isocyanate crosslinking agent is 120~150℃; The dry film thickness of the functional layer is 8~12μm; The functional layer does not contain hydrogen-abstracting UV photoinitiators; The hydroxyl-type polyurethane acrylate resin has a hydroxyl value of 80~102 mgKOH / g, a hydroxyl functionality of 2, and an acrylate optical functionality of 2~4.
2. The film according to claim 1, wherein The number-average molecular weight of the polycaprolactone diol is 1000-3000; and / or, The glass transition temperature of the polycaprolactone diol is -70 to -60°C.
3. The film according to claim 1, wherein the film is a film for card manufacturing. The UV photoinitiator includes 2-hydroxy-2-methyl-1-phenyl-1-propanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.
4. The film according to claim 3, wherein the film is a film for card manufacturing. The mass ratio of the 2-hydroxy-2-methyl-1-phenyl-1-propanone to the phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide is 1:0.4 to 1:
1.
5. The film according to claim 1, wherein the film is a film for card manufacturing. The acrylate active monomers include trimethylolpropane triacrylate and / or pentaerythritol tetraacrylate.
6. The film according to claim 1, wherein The nano-scratch-resistant modified powder comprises silane coupling agent modified nano-silica; and / or, The particle size of the nano-scratch-resistant modified powder is 30~70nm.
7. The film according to claim 1, wherein the film is a film for card manufacturing. The organic solvent includes one or more of ethyl acetate, isopropanol, and butanone; and / or, The film substrate layer includes a PET film or a PVC film; and / or, The adhesive layer is made from thermoplastic waterborne polyurethane adhesive.
8. A method for preparing a card-making adhesive film as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Perform surface pretreatment on the thin film substrate layer; S2. Apply a functional layer coating to one side of the thin film substrate layer, and control the dry film thickness to be 8~12μm; S3. Pre-dry the coated layer at 40~60℃ and cool it to 20~30℃. S4. Apply an adhesive layer to the other side of the film substrate layer and dry and set it. S5. After curing, roll up the package, seal it in a light-proof container, and store it in a light-proof warehouse at 10~30℃.
9. The preparation method according to claim 8, characterized in that, Satisfy at least one of the following characteristics: (a) In step S3, the pre-drying time is 30~120s; (b) In step S4, the drying and shaping temperature is 50~60℃; (c) In step S5, the ripening time is 1-3 hours, and the light-proof storage period is no less than 180 days; and, (d) In step S1, the surface pretreatment is corona treatment.
10. A card manufacturing method, characterized in that, Using the adhesive film for card making as described in any one of claims 1 to 7, the method includes the following steps: S1. The adhesive film and the printed card material are laminated together at 120~150℃ and 5~15MPa, and then punched into single cards. S2. Perform hot stamping on the surface of the single card. The hot stamping temperature is 100~140℃ and the stamping contact time is 0.3~1.5s. S3, ultraviolet final curing for the single card which has been hot stamped, curing energy is 50~300mJ / cm 2 .