A recycled polyethylene resin composition, its preparation method and application

The recycled polyethylene resin composition prepared by specific formulation and purification process solves the problems of poor mechanical properties and appearance defects of recycled polyethylene resin, realizing the production of high-performance geomembranes with good mechanical properties and appearance quality.

CN123107214APending Publication Date: 2026-11-17KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611401439.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing recycled polyethylene resin has poor mechanical properties due to its high impurity content and wide molecular weight distribution, making it unsuitable for direct use in high-performance geomembranes. Furthermore, it has impurity spots and crystal points on its appearance, failing to meet the standard requirements for geomembranes.

Method used

By screening recycled polyethylene resin with specific inorganic solid content and particle size distribution and combining it with virgin high-density polyethylene resin, compatibilizers and toughening agents are added to prepare a recycled polyethylene resin composition. Inorganic solids are used as heterogeneous nucleating agents to improve crystallinity and enhance mechanical properties. The inorganic solids are then purified by a solvent dissolution-three-stage gradient candle filtration process.

Benefits of technology

The prepared geomembrane has excellent tensile properties, puncture resistance and processing performance, and a smooth and uniform appearance, which meets the requirements for the use of geomembranes, reduces production costs, and has environmental and economic value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application belongs to the field of waste polymer material recycling technology, and relates to a recycled polyethylene resin composition, its preparation method and application. The recycled polyethylene resin composition includes a specific amount of recycled polyethylene resin, virgin high-density polyethylene resin, compatibilizer and toughening agent. This application breaks through the traditional understanding that "the less inorganic solids in recycled materials, the better". By limiting the content and particle size distribution of inorganic solids in recycled polyethylene resin, the originally harmful inorganic solids are transformed into beneficial components with heterogeneous nucleation effect, realizing "turning waste into treasure". The final recycled polyethylene resin composition has good tensile properties, puncture resistance and processing properties. The geomembrane prepared with it is smooth and uniform, without crystal points, which can meet the requirements and significantly reduce the raw material cost of geomembrane production, thus having both economic and environmental value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of waste polymer material recycling technology, and relates to a recycled polyethylene resin composition, its preparation method and application. Background Technology

[0002] Geomembranes, as a type of impermeable material, are widely used in engineering projects such as landfills, tailings ponds, and water conservancy dams. Currently, the geomembranes widely used in engineering are mainly polyethylene (PE) geomembranes produced from virgin resin, which have excellent impermeability and mechanical strength.

[0003] However, with the large-scale consumption of plastic products, the recycling and reuse of polyethylene waste materials (such as waste agricultural film, waste packaging film, etc.) has become an urgent need in the field of environmental protection. Due to the complex sources, high impurity content, and wide molecular weight distribution of recycled polyethylene materials on the market, their mechanical properties (such as tensile strength, puncture resistance, etc.) are far lower than those of virgin materials. Direct use in the preparation of geomembranes will result in the following problems: (1) Poor mechanical properties: Geomembranes prepared directly from recycled materials have significantly reduced tensile strength, elongation at break, and puncture resistance, which cannot meet the performance requirements of national standards (such as GB / T 17643-2025) for geomembranes. (2) Appearance defects: Recycled materials often contain a small amount of impurities (such as paper scraps, aluminum scraps, or other polymers). These impurities will not only become stress concentration points, causing the geomembrane to crack prematurely during use, but will also cause multiple crystal points and impurity spots to appear on the surface of the geomembrane, which cannot meet the geomembrane standards.

[0004] Therefore, recycled polyethylene resin in existing technologies is mostly used to manufacture low-end plastic products with low performance requirements, such as garbage bags and shade nets, and cannot be directly used to produce geomembranes with extremely high requirements for mechanical properties and durability. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the purpose of this application is to provide a recycled polyethylene resin composition, its preparation method, and its application. By screening recycled polyethylene resin with specific inorganic solid content and particle size distribution and combining it with virgin high-density polyethylene resin, and supplementing it with functional additives, the resulting recycled polyethylene resin composition has excellent and stable mechanical properties. It can be directly used to produce geomembranes, and the geomembranes produced have a smooth and uniform appearance without crystal points.

[0006] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a recycled polyethylene resin composition, wherein the recycled polyethylene resin composition comprises the following components in parts by weight: 50-70 parts by weight of recycled polyethylene resin; 20-40 parts by weight of virgin high-density polyethylene resin; Compatibilizer 1-8 parts by weight; Toughening agent 2-6 parts by weight; The inorganic solids content in the recycled polyethylene resin is 0.3% to 1% by mass (e.g., 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%, etc.). Based on the total mass of the inorganic solids as 100%, the mass percentage of inorganic solids with a particle size >100 μm is ≤0.01% (e.g., 0.01%, 0.009%, 0.008%, 0.006%, 0.004%, 0.002%, or 0.001%), the mass percentage of inorganic solids with a particle size of 50~100 μm is ≤0.05% (e.g., 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.009%, 0.008%, 0.007%, 0.006%, or 0.005%), and the mass percentage of inorganic solids with a particle size <50 μm is ≥99.94% (e.g., 99.94%, 99.95%, 99.96%, 99.97%, 99.98%, or 99.99%).

[0007] The amount of recycled polyethylene resin used can be 50 parts by weight, 52 parts by weight, 54 parts by weight, 56 parts by weight, 58 parts by weight, 60 parts by weight, 62 parts by weight, 64 parts by weight, 66 parts by weight, 68 parts by weight, or 70 parts by weight, etc.; and based on the total mass of the recycled polyethylene resin composition being 100%, the mass percentage of the recycled polyethylene resin is not less than 50%.

[0008] The amount of virgin high-density polyethylene resin used can be 20 parts by weight, 22 parts by weight, 24 parts by weight, 26 parts by weight, 28 parts by weight, 30 parts by weight, 32 parts by weight, 34 parts by weight, 36 parts by weight, 38 parts by weight, or 40 parts by weight, etc.

[0009] The amount of the compatibilizer can be 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, or 8 parts by weight, etc.

[0010] The amount of the toughening agent can be 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, or 6 parts by weight, etc.

[0011] The recycled polyethylene resin composition provided in this application includes specific amounts of recycled polyethylene resin, virgin high-density polyethylene resin, compatibilizer, and toughening agent. By selecting and combining the above components, and further limiting the mass percentage and particle size distribution of inorganic solids in the recycled polyethylene resin, the inorganic solids contained in the recycled polyethylene resin not only do not have a negative impact on the material properties, but can also act as heterogeneous nucleating agents to help the polyethylene resin crystallize rapidly, thereby effectively improving the crystallinity of the material and accelerating the crystallization rate. The resulting recycled polyethylene resin composition has good tensile properties, puncture resistance, and processing properties. The geomembrane prepared with it is smooth and uniform, without crystal points, and can meet the requirements for geomembrane use, significantly reducing the raw material cost of geomembrane production, and possessing both economic and environmental value.

[0012] In this application, if the content of inorganic solids in the recycled polyethylene resin is less than 0.3%, not only will the purification cost increase significantly, but the beneficial role of inorganic solids as heterogeneous nucleating agents will also be lost. If the content of inorganic solids in the recycled polyethylene resin is greater than 1%, it will cause a series of problems such as a decrease in the mechanical properties of the material, an increase in membrane defects, and frequent clogging of the processing filter.

[0013] In this application, if the particle size distribution of the inorganic solids is not within the specific range mentioned above, firstly, if the content of large inorganic solid particles with a particle size >100 μm is too high (>0.01%), it will cause problems such as frequent filter clogging and excessive melt pressure fluctuations during the extrusion process, thus reducing the continuous production time of the final recycled polyethylene resin composition; secondly, if the content of medium-sized inorganic solid particles with a particle size of 50~100 μm is too high (>0.05%), it will cause problems such as pinholes, defects, and uneven thickness on the surface of the geomembrane after the final recycled polyethylene resin composition is made, and will also lead to a decrease in the impermeability of the geomembrane; finally, limiting the mass percentage content of small inorganic solid particles with a particle size <50 μm to ≥99.94% avoids the large-particle inorganic solids acting as stress concentration sources and damaging the mechanical properties of the material, thereby improving the puncture resistance of the subsequently made geomembrane.

[0014] In this application, the mass percentage of inorganic solids in the recycled polyethylene resin can be obtained by the following method: Take an appropriate amount of recycled polyethylene resin sample, cut or granulate it, accurately weigh the sample mass as m1 (accurate to 0.1 mg), and place it in a crucible that has been pre-ignited to constant weight; place the crucible on an electric furnace or hot plate, and slowly heat it in a fume hood until the sample is carbonized to smokeless. Then transfer it to a muffle furnace and ignite it at 600±25℃ until the residue is completely converted into inorganic solids. Turn off the muffle furnace, and when the temperature drops to about 200℃, remove the crucible with crucible tongs, place it in a desiccator to cool to room temperature, weigh the total mass of the crucible and inorganic solids, and subtract the constant weight of the crucible to obtain the mass of inorganic solids as m2; repeat the ignition (30 min each time), cooling, and weighing until the difference between two consecutive weighings does not exceed 0.5 mg, which is considered constant weight; the final mass percentage of inorganic solids in the recycled polyethylene resin is calculated by the following formula:

[0015] In this application, the mass percentage of inorganic solids with a particle size >100 μm, the mass percentage of inorganic solids with a particle size of 50~100 μm, and the mass percentage of inorganic solids with a particle size <50 μm can be obtained by the following method: Take an appropriate amount of recycled polyethylene resin sample, cut or granulate it, place it in a crucible that has been pre-ignited to constant weight, place the crucible in an electric furnace or hot plate, and slowly heat it in a fume hood to carbonize the sample until no smoke is produced. Then transfer it to a muffle furnace and ignite it at 600±25℃ until the residue is completely converted into inorganic solids. Mix the inorganic solids obtained after ignition evenly and use it as the sample to be tested. Use a laser particle size analyzer to determine the particle size distribution of the sample, and calculate the mass percentage of each particle size using the particle size distribution data. The specific steps are as follows: Add the sample to be tested to a suitable amount of anhydrous ethanol, then add an appropriate amount of 0.1% sodium hexametaphosphate solution, stir, and then sonicate for 1~3 minutes. After min, a uniform suspension is formed, ensuring that the particles are fully dispersed and free of bubbles. The suspension is then placed on a laser particle size analyzer for analysis and testing. The mass percentage of inorganic solids in the following three particle sizes can be read or calculated directly from the particle size distribution chart or the software statistical function.

[0016] It should be noted that this application does not impose any special restrictions on the source of the recycled polyethylene resin, as long as the content of inorganic solids and the particle size distribution thereon meet the requirements of this application.

[0017] For example, the recycled polyethylene resin described in this application is derived from polyethylene agricultural film, and the inorganic solids contained in the recycled polyethylene resin are not intentionally added functional fillers, but process byproducts retained during the recycling of the polyethylene agricultural film. Since the main effective component of the polyethylene agricultural film is polyethylene resin, which itself does not contain too many complex additives, after precise purification processing, the mass percentage of effective polyethylene components in the obtained recycled polyethylene resin can be maintained at 98.5% to 99.5%, containing only a small amount of inorganic solids that meet the above-mentioned specific content and specific particle size distribution by adjusting the recycling process parameters.

[0018] For example, the recycled polyethylene resin can be obtained from polyethylene agricultural film using a solvent dissolution-three-stage gradient candle filtration process. This purification process, by controlling parameters such as dissolution temperature, filtration pressure, filtration flux, and filter replacement cycle, can obtain recycled polyethylene resin with inorganic solid content and particle size distribution within a specific range. It also ensures that the inorganic solids in the obtained recycled polyethylene resin are uniformly dispersed without agglomeration, which is significantly different from the large amount of large-particle impurities (typically >5% with an average particle size >100 μm) commonly found in ordinary physically recycled polyethylene resin. Specifically, the purification process includes: first, completely dissolving the crushed, heavily contaminated agricultural film in a hydrocarbon solvent under heating conditions, and then sequentially passing it through filters with a resolution of 100 μm, 50 μm, and 20 μm. A three-stage candlestick precision filter is used to progressively remove insoluble impurities of different particle sizes, and finally, recycled polyethylene is obtained through devolatilization and granulation. The solvent used in the solvent dissolution-three-stage gradient candlestick filtration process includes one or more of C8-C12 saturated alkanes, xylene, and chlorobenzene. The specific solvent can be flexibly selected according to the dissolution temperature of the polyethylene agricultural film and the subsequent devolatilization energy consumption. It should also be noted that in this process, the polyethylene resin can be completely dissolved to form a homogeneous polymer solution, while the inorganic solids (such as soil, sand, metal oxides, etc.) are insoluble in the solvent and exist in the solution as fine suspended particles. After subsequent filtration and devolatilization, the incompletely filtered inorganic solids are uniformly distributed in the polyethylene resin due to the dispersion effect of the solution. In some specific embodiments, the content of recycled polyethylene resin in the recycled polyethylene resin composition is 55-65 parts by weight.

[0019] In this application, there are no special restrictions on the type of recycled polyethylene resin, as long as the mass percentage of inorganic solids and the particle size distribution therein meet the requirements, including but not limited to recycled low-density polyethylene resin, recycled high-density polyethylene resin, recycled metallocene polyethylene resin, etc.

[0020] In some specific embodiments, the melt index of the recycled polyethylene resin under test conditions of 190°C and 2.16 kg is 2~8 g / 10min, for example 2 g / 10min, 2.5 g / 10min, 3 g / 10min, 3.5 g / 10min, 4 g / 10min, 4.5 g / 10min, 5 g / 10min, 5.5 g / 10min, 6 g / 10min, 6.5 g / 10min, 7 g / 10min, 7.5 g / 10min or 8 g / 10min, etc.

[0021] In some specific embodiments, the melting point of the recycled polyethylene resin is 138~148℃, such as 138℃, 139℃, 140℃, 141℃, 142℃, 143℃, 144℃, 145℃, 146℃, 147℃ or 148℃.

[0022] In this application, the melt index of the recycled polyethylene resin can be obtained by referring to GB / T 3682.1-2018, and the melting point can be obtained by referring to GB / T 19466.3-2004.

[0023] In some specific embodiments, the content of virgin high-density polyethylene resin in the recycled polyethylene resin composition is 25 to 35 parts by weight.

[0024] In some specific embodiments, the melt index of the virgin high-density polyethylene resin under test conditions of 190°C and 2.16 kg is 1~5 g / 10min, such as 1 g / 10min, 1.5 g / 10min, 2 g / 10min, 2.5 g / 10min, 3 g / 10min, 3.5 g / 10min, 4 g / 10min, 4.5 g / 10min or 5 g / 10min, etc.

[0025] In some specific embodiments, the melting point of the virgin high-density polyethylene resin is 148~158℃, such as 148℃, 149℃, 150℃, 151℃, 152℃, 153℃, 154℃, 155℃, 156℃, 157℃ or 158℃.

[0026] In this application, the melt index of the virgin high-density polyethylene resin can be obtained by referring to GB / T 3682.1-2018, and the melting point can be obtained by referring to GB / T 19466.3-2004.

[0027] In some specific embodiments, the compatibilizer content in the recycled polyethylene resin composition is 3 to 5 parts by weight.

[0028] In some specific embodiments, the compatibilizer includes maleic anhydride-grafted polyethylene (PE-g-MAH) and / or maleic anhydride-grafted ethylene-octene copolymer (POE-g-MAH).

[0029] In some specific embodiments, the grafting rates of the maleic anhydride-grafted polyethylene and the maleic anhydride-grafted ethylene-octene copolymer are each independently 0.8% to 1.5%, for example 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, or 1.5%.

[0030] In some specific embodiments, the toughening agent content in the recycled polyethylene resin composition is 3 to 4 parts by weight.

[0031] In some specific embodiments, the toughening agent includes ethylene-vinyl acetate copolymer (EVA) and / or ethylene-octene copolymer (POE).

[0032] In some specific embodiments, the mass percentage of vinyl acetate structure in the ethylene-vinyl acetate copolymer is 15-25%, such as 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, or 25%.

[0033] In some specific embodiments, the recycled polyethylene resin composition further includes any one or a combination of at least two of a light stabilizer, an antioxidant, or a lubricant.

[0034] The light stabilizer and antioxidant work synergistically to inhibit the degradation of recycled polyethylene resin caused by light, heat and oxygen during processing and use, effectively delaying material aging and improving the weather resistance and service life of the obtained recycled polyethylene resin composition in complex outdoor environments. The lubricant effectively reduces the melt viscosity of the recycled polyethylene resin composition during melt extrusion, which can reduce equipment wear, improve processing fluidity, and ensure the molding quality of the parts.

[0035] In some specific embodiments, the content of light stabilizer in the recycled polyethylene resin composition is 0.5 to 3 parts by weight, such as 0.5 parts by weight, 0.7 parts by weight, 0.9 parts by weight, 1.1 parts by weight, 1.3 parts by weight, 1.5 parts by weight, 1.7 parts by weight, 1.9 parts by weight, 2.2 parts by weight, 2.4 parts by weight, 2.6 parts by weight, 2.8 parts by weight, or 3 parts by weight, and more preferably 1 to 2 parts by weight.

[0036] In some specific embodiments, the light stabilizer includes hindered amine light stabilizers (such as light stabilizer 944, light stabilizer 770, etc.) and / or benzotriazole light stabilizers (such as ultraviolet absorber UV-327, ultraviolet absorber UV-329, etc.).

[0037] In some specific embodiments, the antioxidant content in the recycled polyethylene resin composition is 0.2 to 2 parts by weight, such as 0.2 parts by weight, 0.4 parts by weight, 0.6 parts by weight, 0.8 parts by weight, 1 part by weight, 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, 1.8 parts by weight, or 2 parts by weight, and more preferably 0.5 to 1 part by weight.

[0038] In some specific embodiments, the antioxidants include hindered phenolic antioxidants (such as antioxidant 1010, antioxidant 1076, etc.) and / or phosphite antioxidants (such as antioxidant 168, antioxidant 626, etc.).

[0039] In some specific embodiments, the antioxidant includes a combination of hindered phenolic antioxidants and phosphite antioxidants, with a mass ratio of 1:(1~2), such as 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, etc.

[0040] In some specific embodiments, the content of lubricant in the recycled polyethylene resin composition is 0.1 to 1 part by weight, such as 0.1 part by weight, 0.2 part by weight, 0.3 part by weight, 0.4 part by weight, 0.5 part by weight, 0.6 part by weight, 0.7 part by weight, 0.8 part by weight, 0.9 part by weight or 1 part by weight, and more preferably 0.3 to 0.6 parts by weight.

[0041] In some embodiments, the lubricant includes any one or a combination of at least two of zinc stearate, calcium stearate, or polyethylene wax.

[0042] In some specific embodiments, the number average molecular weight of the polyethylene wax is 1000~5000, such as 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500 or 5000.

[0043] In this application, the number-average molecular weight of the polyethylene wax can be obtained by testing in accordance with GB / T 36214.4-2018.

[0044] Secondly, this application provides a method for preparing the recycled polyethylene resin composition as described in the first aspect, the method comprising: mixing the various components and extruding and granulating them to obtain the recycled polyethylene resin composition.

[0045] In some specific embodiments, the step of drying the recycled polyethylene resin is included before mixing.

[0046] In some specific embodiments, the drying temperature is 60~80℃, such as 60℃, 62℃, 64℃, 66℃, 68℃, 70℃, 72℃, 74℃, 76℃, 78℃ or 80℃.

[0047] In some specific embodiments, the drying time is 2 to 4 hours, such as 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours, or 4 hours.

[0048] In some specific embodiments, the mass percentage of moisture in the dried recycled polyethylene resin is ≤0.1%, for example, 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, or 0.03%.

[0049] In some specific embodiments, the mixing is carried out in a high-speed mixer.

[0050] In some specific embodiments, the mixing speed is 300~500 rpm, such as 300 rpm, 320 rpm, 340 rpm, 360 rpm, 380 rpm, 400 rpm, 420 rpm, 440 rpm, 460 rpm, 480 rpm or 500 rpm.

[0051] In some specific embodiments, the mixing time is 8 to 15 minutes, such as 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes, 10 minutes, 10.5 minutes, 11 minutes, 11.5 minutes, 12 minutes, 12.5 minutes, 13 minutes, 13.5 minutes, 14 minutes, 14.5 minutes, or 15 minutes.

[0052] In some specific embodiments, the extrusion granulation is carried out in a twin-screw extruder.

[0053] In some specific embodiments, the screw speed of the twin-screw extruder is 200~300 rpm, such as 200 rpm, 210 rpm, 220 rpm, 230 rpm, 240 rpm, 250 rpm, 260 rpm, 270 rpm, 280 rpm, 290 rpm or 300 rpm.

[0054] In some specific embodiments, the screw temperatures of the twin-screw extruder from the feed port to the die head are as follows: Zone 1 temperature is 70~90℃ (e.g., 70℃, 72℃, 74℃, 76℃, 78℃, 80℃, 82℃, 84℃, 86℃, 88℃, or 90℃, etc.); Zones 2 to 4 temperatures are each independently 140~160℃ (e.g., 140℃, 142℃, 144℃, 146℃, 148℃, 150℃, 152℃, 154℃, 1...). The temperatures in zones five through seven are independent, ranging from 160 to 180°C (e.g., 160°C, 162°C, 164°C, 166°C, 168°C, 170°C, 172°C, 174°C, 176°C, 178°C, or 180°C), while the temperature at the machine head is 170 to 185°C (e.g., 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, or 185°C).

[0055] In some specific embodiments, the screw length-to-diameter ratio of the twin-screw extruder is (36~48):1, such as 36:1, 37:1, 38:1, 39:1, 40:1, 42:1, 44:1, 46:1 or 48:1, etc.

[0056] Thirdly, this application provides a film article comprising the recycled polyethylene resin composition as described in the first aspect.

[0057] In some specific embodiments, the film component includes a geomembrane.

[0058] In some specific embodiments, the geomembrane includes any one of impermeable geomembrane, composite geomembrane, or drainage geomembrane.

[0059] Compared with the prior art, this application has the following advantages: The recycled polyethylene resin composition provided in this application breaks through the traditional understanding that "the fewer impurities in recycled materials, the better." By limiting the content and particle size distribution of inorganic solids in the recycled polyethylene resin, inorganic solids that were originally considered harmful are transformed into beneficial components with heterogeneous nucleation effects, thus realizing "turning waste into treasure." The recycled polyethylene resin composition provided in this application has good mechanical properties, weather resistance, and processing performance. The geomembrane prepared with it can meet the various index requirements of engineering construction, while significantly reducing the raw material cost of geomembrane production, thus possessing both economic and environmental value. Detailed Implementation

[0060] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0061] The detailed information of some of the raw materials involved in the following specific implementation methods is shown below: (1) Recycled polyethylene resin R1: The inorganic solids have a mass percentage content of 0.4% and a melt index of 3 g / 10min (190℃ / 2.16 kg). The inorganic solids have a mass percentage content of 0.01% for particles >100 μm, a mass percentage content of 0.04% for particles 50~100 μm, and a mass percentage content of 99.95% for particles <50 μm. R1 is obtained by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it through multiple stages, extruding and devolatilizing it, and then granulating it. R2: The inorganic solids content is 0.3% by mass, the melt index is 5 g / 10min (190℃ / 2.16 kg), the inorganic solids with a particle size >100 μm have a mass percentage of 0.01%, the inorganic solids with a particle size of 50~100 μm have a mass percentage of 0.05%, and the inorganic solids with a particle size <50 μm have a mass percentage of 99.94%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R3: The inorganic solids content is 0.5% by mass, the melt index is 7 g / 10min (190℃ / 2.16 kg), the inorganic solids with a particle size >100 μm have a mass percentage of 0.01%, the inorganic solids with a particle size of 50~100 μm have a mass percentage of 0.02%, and the inorganic solids with a particle size <50 μm have a mass percentage of 99.97%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R4: The inorganic solids content is 0.1% by mass, the melt index is 3 g / 10min (190℃ / 2.16 kg), the inorganic solids with a particle size >100 μm have a mass percentage of 0.01%, the inorganic solids with a particle size of 50~100 μm have a mass percentage of 0.01%, and the inorganic solids with a particle size <50 μm have a mass percentage of 99.99%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R5: Inorganic solids content is 1.2%, melt index is 3 g / 10min (190℃ / 2.16 kg), and the mass percentage of inorganic solids with particle size >100 μm is 0.01%, the mass percentage of inorganic solids with particle size 50~100 μm is 0.05%, and the mass percentage of inorganic solids with particle size <50 μm is 99.94%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R6: The inorganic solids content is 0.4% by mass, the melt index is 3 g / 10min (190℃ / 2.16 kg), the inorganic solids with a particle size >100 μm have a mass percentage of 0.05%, the inorganic solids with a particle size of 50~100 μm have a mass percentage of 0.05%, and the inorganic solids with a particle size <50 μm have a mass percentage of 99.9%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R7: The inorganic solids content is 0.4% by mass, the melt index is 3 g / 10min (190℃ / 2.16 kg), the inorganic solids with a particle size >100 μm have a mass percentage of 0.01%, the inorganic solids with a particle size of 50~100 μm have a mass percentage of 0.1%, and the inorganic solids with a particle size <50 μm have a mass percentage of 99.89%. Its preparation method includes: obtaining it by crushing and sorting polyethylene agricultural film, dissolving it in solvent, filtering it in multiple stages, extruding and devolatilizing it, and then granulating it. R8: The mass percentage of inorganic solids is 0.5%, and the D of inorganic solids is... 50 The particle size is 120 μm, and its preparation method includes: crushing and cleaning polyethylene polluted agricultural film using ordinary machinery; R9: Add 0.02% of 100-mesh quartz sand (simulating large particles) based on the total mass of R1 during the extrusion devolatilization process in the R1 preparation method.

[0062] (2) Virgin high-density polyethylene resin HDPE-1: Melt index is 2 g / 10min (190℃ / 2.16 kg), melting point is 150℃, manufactured by PetroChina Daqing Petrochemical. HDPE-2: Melt index is 4 g / 10min (190℃ / 2.16 kg), melting point is 155℃, manufactured by PetroChina Daqing Petrochemical. HDPE-3: Melt index is 1 g / 10min (190℃ / 2.16 kg), melting point is 158℃, CNOOC Shell.

[0063] (3) Compatibilizer PE-g-MAH: Grafting rate 1%, Shanghai SECCO; POE-g-MAH: Grafting rate 1.2%, Dow Chemical.

[0064] (4) Toughening agent EVA: The VA content is 20% by mass, produced by Beijing Organic Chemical Plant; POE: ExxonMobil.

[0065] (5) Light stabilizers Light stabilizer 944: Commercially available; UV-327: Commercially available.

[0066] (6) Antioxidants Antioxidant 1010: Commercially available; Antioxidant 168: Regularly available in the market.

[0067] (7) Lubricant Polyethylene wax: Number average molecular weight 3000, commercially available.

[0068] (8) Virgin polyethylene Virgin LLDPE: melt index 3 g / 10min (190℃ / 2.16 kg), purchased from Dow Chemical, grade GM8480.21.

[0069] Examples 1-10 and Comparative Examples 1-10 Examples 1-10 and Comparative Examples 1-10 each provide a recycled polyethylene resin composition, the components and amounts of which are shown in Table 1 and Table 2. In Table 1 and Table 2, the amount of each component is in "parts by weight". Table 1 Table 2 The preparation methods of the recycled polyethylene resin compositions provided in Examples 1-10 and Comparative Examples 1-10 include the following steps: (1) Place the recycled polyethylene resin in a drying oven and dry it at 70°C for 3 hours until the moisture content is ≤0.1%. HDPE and each additive are dried and cleaned separately for later use. (2) Weigh each component according to the ratio, add them to a high-speed mixer, and mix for 10 min at a speed of 400 r / min to obtain a uniform mixture. (3) The mixture is added to a twin-screw extruder for melt blending and extrusion. The screw length-to-diameter ratio of the twin-screw extruder is 40:1. The extrusion temperature is set in the following sections: 80℃ in zone 1, 150℃ in zones 2-4, 170℃ in zones 5-7, 180℃ at the die head, and the screw speed is 250 r / min. The extrudate is cooled by water and pelletized to obtain a recycled polyethylene resin composition.

[0070] Comparative Example 11 A polyethylene resin composition, the preparation method of which includes the following steps: (1) Virgin LLDPE and 0.4% by mass of quartz sand were melt-blended at 180°C to obtain an intermediate component; the quartz sand contained in the intermediate component had a particle size >100 μm of 0.01% by mass, a particle size of 50~100 μm of 0.04% by mass, and a particle size <50 μm of 99.95% by mass. (2) Place the intermediate component obtained in step (1) in a drying oven and dry it at 70°C for 3 h until the moisture content is ≤0.1%. HDPE and each additive are dried and purified separately for later use. (3) Add 55 parts by weight of dried intermediate component, 35 parts by weight of HDPE-1, 3 parts by weight of PE-g-MAH, 3 parts by weight of EVA, 1 part by weight of light stabilizer 944, 0.25 parts by weight of antioxidant 1010, 0.25 parts by weight of antioxidant 168 and 0.3 parts by weight of polyethylene wax into a high-speed mixer and mix for 10 min at a speed of 400 r / min to obtain a uniform mixture. (4) The mixture is added to a twin-screw extruder for melt blending and extrusion. The screw length-to-diameter ratio of the twin-screw extruder is 40:1. The extrusion temperature is set in the following sections: 80°C in zone 1, 150°C in zones 2-4, 170°C in zones 5-7, 180°C at the die head, and the screw speed is 250 r / min. The extrudate is cooled by water and pelletized to obtain the polyethylene resin composition.

[0071] Performance testing (1) Tensile properties: The recycled polyethylene resin composition was prepared into standard tensile specimens by injection molding machine. The injection temperature was 180℃ and the mold temperature was 40℃. The test was carried out in accordance with GB / T 1040.2-2006 standard for testing tensile properties of plastics. The test environment was room temperature (23±2℃), relative humidity was 50±5% RH, and the tensile rate was 50 mm / min. Five parallel specimens were tested for each example, and the average value was taken as the final test result. The test indexes were tensile strength (MPa) and elongation at break (%).

[0072] (2) Puncture resistance: Tested according to GB / T 17643-2011.

[0073] (3) Appearance: The recycled polyethylene composition is dried, mixed, melt-plasticized and calendered. The roller temperature is controlled at 180°C and the roller gap is precisely adjusted according to the target geomembrane thickness of 1.0 mm. The error is controlled within ±0.02 mm. The calendered membrane is cooled and solidified by air cooling to obtain the geomembrane. The appearance of the obtained geomembrane is then observed.

[0074] The recycled polyethylene resin compositions provided in Examples 1-10 and Comparative Examples 1-11 were tested according to the above test methods, and the test results are shown in Table 3. Table 3 According to the data in Table 3: The recycled polyethylene resin compositions provided in Examples 1-10 have a tensile strength of not less than 19.4 MPa, an elongation at break of not less than 546%, and a puncture resistance of not less than 90%. The resulting geomembranes have a smooth and uniform appearance, are free of crystalline points, and exhibit excellent overall performance.

[0075] Compared with Example 1, in the comparative examples, the content of inorganic solids in the recycled polyethylene resin composition was too low (Comparative Example 1), too high (Comparative Example 2), the particle size distribution of inorganic solids was not compliant (Comparative Examples 3, 4, 6), or ordinary recycled materials were used (Comparative Example 5), all of which led to a decrease in mechanical properties and defects such as impurity spots and pinholes on the film surface. The lack of compatibilizer or toughening agent in the recycled polyethylene resin composition (Comparative Examples 9, 10) also significantly reduced the elongation at break and puncture resistance. In addition, the polyethylene resin composition made by using virgin LLDPE with inorganic solids in Comparative Example 11 also had a decrease in mechanical properties and defects such as impurity spots and pinholes on the film surface.

[0076] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A recycled polyethylene resin composition, characterized in that, The recycled polyethylene resin composition comprises the following components in parts by weight: 50-70 parts by weight of recycled polyethylene resin; 20-40 parts by weight of virgin high-density polyethylene resin; Compatibilizer 1-8 parts by weight; Toughening agent 2-6 parts by weight; The inorganic solids content in the recycled polyethylene resin is 0.3% to 1% by mass. Based on the total mass of the inorganic solids as 100%, the mass percentage of inorganic solids with a particle size > 100 μm is ≤ 0.01%, the mass percentage of inorganic solids with a particle size of 50~100 μm is ≤ 0.05%, and the mass percentage of inorganic solids with a particle size < 50 μm is ≥ 99.94%.

2. The recycled polyethylene resin composition according to claim 1, characterized in that, The recycled polyethylene resin composition contains 55-65 parts by weight of recycled polyethylene resin. And / or, the melt index of the recycled polyethylene resin under test conditions of 190°C and 2.16 kg is 2~8 g / 10min.

3. The recycled polyethylene resin composition according to claim 1, characterized in that, The content of virgin high-density polyethylene resin in the recycled polyethylene resin composition is 25-35 parts by weight. And / or, the melt index of the virgin high-density polyethylene resin under test conditions of 190°C and 2.16 kg is 1~5 g / 10min.

4. The recycled polyethylene resin composition according to claim 1, characterized in that, The compatibilizer content in the recycled polyethylene resin composition is 3-5 parts by weight; And / or, the compatibilizer comprises maleic anhydride-grafted polyethylene and / or maleic anhydride-grafted ethylene-octene copolymer.

5. The recycled polyethylene resin composition according to claim 1, characterized in that, The toughening agent content in the recycled polyethylene resin composition is 3-4 parts by weight; And / or, the toughening agent includes ethylene-vinyl acetate copolymer and / or ethylene-octene copolymer.

6. The recycled polyethylene resin composition according to claim 1, characterized in that, The recycled polyethylene resin composition further includes any one or a combination of at least two of light stabilizers, antioxidants, or lubricants. Preferably, the content of light stabilizer in the recycled polyethylene resin composition is 0.5 to 3 parts by weight; Preferably, the light stabilizer includes hindered amine light stabilizers and / or benzotriazole light stabilizers; Preferably, the antioxidant content in the recycled polyethylene resin composition is 0.2 to 2 parts by weight; Preferably, the antioxidant includes hindered phenolic antioxidants and / or phosphate ester antioxidants; Preferably, the content of lubricant in the recycled polyethylene resin composition is 0.1 to 1 part by weight; Preferably, the lubricant comprises any one or a combination of at least two of zinc stearate, calcium stearate, or polyethylene wax.

7. A method for preparing the recycled polyethylene resin composition according to any one of claims 1 to 6, characterized in that, The preparation method includes: mixing the various components and extruding and granulating them to obtain the recycled polyethylene resin composition.

8. The preparation method according to claim 7, characterized in that, The mixing is carried out in a high-speed mixer; And / or, the mixing speed is 300~500 rpm; And / or, the mixing time is 8 to 15 minutes; And / or, the extrusion granulation is carried out in a twin-screw extruder.

9. A thin film component, characterized in that, The film component comprises any one of the recycled polyethylene resin compositions described in 1 to 6.

10. The thin film article according to claim 9, characterized in that, The thin film component includes a geomembrane.