Low-temperature crack-resistant polyethylene sheath material for optical cables and its preparation method
By forming a dynamic micro-crosslinked phase and adding carbon black in sections in the optical cable sheath material, the problem of easy cracking of the optical cable sheath material at low temperature was solved, a balance between toughness and strength was achieved, the stability of the sheath and the dispersion of carbon black were improved, and the low temperature impact performance was enhanced.
Patent Information
- Application Number
- CN202611436922.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing optical cable sheath materials are prone to cracking at low temperatures, and existing toughening methods cannot effectively balance toughness and strength. The toughening effect diminishes after long-term service, and the carbon black is unevenly dispersed, affecting the stability of the sheath.
By forming a network within a low glass transition temperature block elastomer phase, a dynamic micro-crosslinked phase is formed by reacting hydrogenated C36 dimer fatty acids with epoxy-functionalized ethylene/1-octene block copolymer elastomer. Carbon black is added in sections during extrusion to form β-hydroxy ester crosslinks, which, combined with bimodal medium-density polyethylene and metallocene linear low-density polyethylene matrix, form a submicron dynamic micro-crosslinked phase.
It improves the deformation and energy dissipation capacity of optical cable sheath at low temperatures, maintains the strength and water resistance of the polyethylene continuous phase, reduces the migration of free fatty acids, enhances the extrusion stability of the sheath and the dispersion uniformity of carbon black, and improves ESCR and low-temperature impact performance.
Smart Images

Figure CN123107215A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer sheath materials technology, specifically to a low-temperature crack-resistant polyethylene sheath material for optical cables and its preparation method. Background Technology
[0002] Optical cables used outdoors, in cold regions, and at high altitudes are subjected to repeated bending, impact, and localized stress concentration during laying, coiling, construction traction, and service. Although polyethylene sheaths have advantages such as water resistance, insulation, and low processing costs, the chain segment mobility of its crystalline phase decreases at low temperatures, making scratches, carbon black agglomerates, core protrusions, and residual internal stresses prone to evolving into crack initiation points. Under the combined action of surface-active media or long-term tensile stress, environmental stress cracking may also occur.
[0003] Existing optical cable sheath materials are typically toughened by adjusting the ratio of high-density polyethylene (HDPE) and linear low-density polyethylene (LLDPE) or by directly adding elastomers such as POE, EVA, and olefin block copolymers. While simple blending can lower the embrittlement temperature, insufficient elastomer content leads to inadequate crack passivation, while excessive content reduces tensile strength, increases die expansion, and deteriorates the sheath surface. Furthermore, unconstrained low-molecular-weight plasticizers or fatty acids may migrate and precipitate, resulting in a decrease in toughening effect after long-term service.
[0004] Dynamic covalent crosslinking can regulate the network through bond exchange at processing temperatures, but crosslinking the entire polyethylene matrix significantly increases melt viscosity, which is detrimental to high-speed sheath extrusion. Carbon black also has a high specific surface area; if it coexists with carboxylic acids, metal catalysts, and epoxy functional phases before the reaction, it can easily alter the distribution of reactants among the phases and increase the risk of localized uneven reaction and secondary agglomeration of carbon black. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a low-temperature crack-resistant polyethylene sheath material for optical cables and its preparation method. By selectively forming a network within a low glass transition temperature block elastomer phase, the dispersion domain maintains deformation and energy dissipation capabilities at low temperatures, while the continuous polyethylene phase retains strength, water resistance, and sheath extrusion stability.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing low-temperature crack-resistant polyethylene sheath material for optical cables, comprising the following steps:
[0007] S1. Ethylene / 1-octene block copolymer elastomer, glycidyl methacrylate, free radical initiator and styrene grafting agent are reacted, extruded and devolatilized to obtain epoxy-functionalized ethylene / 1-octene block copolymer elastomer with glycidyl methacrylate grafting rate of 0.6-1.5 wt%.
[0008] S2. Using 100 parts by weight of polyethylene matrix, 8-16 parts by weight of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer and the polyethylene matrix are added and melt-dispersed through the main feed port of a co-rotating twin-screw extruder. Then, hydrogenated C36 dimer fatty acid and epoxy-carboxyl addition and transesterification catalyst are added through the first side feed port located downstream of the melt dispersion section. The equivalent ratio of the carboxyl group of the hydrogenated C36 dimer fatty acid to the epoxy group in the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.65-0.95. The hydrogenated C36 dimer fatty acid reacts with the epoxy group in the dispersed elastomer phase at 175-195°C to form a dynamic micro-crosslinked phase connected by β-hydroxy ester bonds in situ.
[0009] S3. After the formation of the dynamic micro-crosslinked phase, carbon black masterbatch, antioxidant, acid absorbent, and processing aid are added from the second feed port located downstream of the reaction section, so that the carbon black content is 2.4-2.8 parts by mass, the antioxidant content is 0.25-0.55 parts by mass, the acid absorbent content is 0.05-0.20 parts by mass, and the processing aid content is 0.05-0.30 parts by mass per 100 parts by mass of the polyethylene matrix. After melt mixing, vacuum devolatilization, extrusion, and granulation, the sheath material is obtained.
[0010] Preferably, the polyethylene matrix is composed of 60-75 parts by mass of bimodal medium-density polyethylene and 25-40 parts by mass of metallocene linear low-density polyethylene; the bimodal medium-density polyethylene has a melt flow rate of 0.10-0.60 g / 10 min and a density of 0.938-0.946 g / cm³ at 190°C and 2.16 kg, and the metallocene linear low-density polyethylene has a melt flow rate of 0.50-2.00 g / 10 min and a density of 0.915-0.924 g / cm³ at 190°C and 2.16 kg.
[0011] Preferably, in step S1, based on 100 parts by mass of the ethylene / 1-octene block copolymer elastomer, the amount of glycidyl methacrylate is 1.2 to 2.5 parts by mass, the amount of the styrene grafting agent is styrene and it is 0.4 to 1.2 parts by mass, and the amount of the free radical initiator is 0.03 to 0.08 parts by mass; the temperature of the reactive extrusion is 165 to 190°C, and the gel content of the obtained epoxy-functionalized ethylene / 1-octene block copolymer elastomer, as measured by xylene extraction at 140°C, is less than 3 wt%.
[0012] Preferably, the hydrogenated C36 dimer fatty acid contains not less than 95 wt% C36 dimer acid, has an acid value of 185-200 mg KOH / g, and an iodine value of not more than 10 g I2 / 100 g; the catalyst is zinc acetylacetonate and / or zinc acetate, and its amount is 0.03-0.20 wt% of the mass of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer, and the equivalent ratio of the carboxyl group to the epoxy group is 0.72-0.88.
[0013] Preferably, the reaction temperature in step S2 is 180–190°C, and the average residence time of the material from the addition of the hydrogenated C36 dimer fatty acid to the addition of the carbon black masterbatch is 35–70 s. After the obtained sheath material is extracted with xylene at 140°C for 24 h, the mass of insoluble matter is reduced by the mass of carbon black, acid absorbent, and catalyst added, and the gel content is calculated based on the sum of the masses of the added epoxy-functionalized ethylene / 1-octene block copolymer elastomer and hydrogenated C36 dimer fatty acid, which is 25–55 wt%.
[0014] Preferably, the co-rotating twin-screw extruder has a length-to-diameter ratio of 44 to 56 and a screw speed of 250 to 500 r / min; with the effective screw length as 100%, the first side feed port is located at 30% to 45%, the second side feed port is located at 65% to 80%, a distribution mixing element and a kneading element are sequentially arranged between the first side feed port and the second side feed port, and a devolatilization port with a vacuum degree of -0.06 to -0.095 MPa is arranged downstream of the second side feed port.
[0015] Preferably, the carbon black masterbatch uses bimodal medium-density polyethylene as a carrier and contains 35-50 wt% furnace black, wherein the primary particle size of the furnace black is 15-25 nm and the dibutyl phthalate oil absorption value is 90-130 mL / 100 g; the antioxidant includes hindered phenolic antioxidant, phosphite antioxidant and thiodipropionate antioxidant; the acid absorbent is hydrotalcite; and the processing aid is a fluoropolymer processing aid.
[0016] The present invention also provides a low-temperature crack-resistant polyethylene sheath material for optical cables, comprising, by weight: 100 parts of polyethylene matrix, 8-16 parts of epoxy-functionalized ethylene / 1-octene block copolymer elastomer, 0.002-0.032 parts of hydrogenated C36 dimer fatty acid, 0.002-0.032 parts of epoxy-carboxyl addition and transesterification catalyst, 2.4-2.8 parts of carbon black, 0.25-0.55 parts of antioxidant, 0.05-0.20 parts of acid absorbent, and 0.05-0.30 parts of processing aid;
[0017] The glycidyl methacrylate grafting rate of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.6–1.5 wt%, and the equivalent ratio of the carboxyl group of the hydrogenated C36 dimer fatty acid to the epoxy group in the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.65–0.95. The epoxy-functionalized ethylene / 1-octene block copolymer elastomer forms a dynamic micro-crosslinked phase containing β-hydroxy ester bonds through the reaction of its epoxy groups with the hydrogenated C36 dimer fatty acid. The dynamic micro-crosslinked phase exists as dispersed domains in the polyethylene matrix, and the number-average equivalent diameter of the dispersed domains is 0.20–1.20 μm and the D90 is not greater than 2.50 μm.
[0018] Preferably, the polyethylene sheath material has a melt flow rate of 0.20-0.65 g / 10 min and a density of 0.932-0.946 g / cm³ at 190°C and 2.16 kg; an environmental stress cracking time F50 of not less than 1000 h; a tensile strength of not less than 18 MPa; and an elongation at break of not less than 450%.
[0019] Compared with existing technologies, this invention provides a low-temperature crack-resistant polyethylene sheath material for optical cables and its preparation method, which has the following beneficial effects: By selectively forming a network within a low glass transition temperature block elastomer phase, the dispersion domain maintains deformation and energy dissipation capacity at low temperatures, while the continuous polyethylene phase retains strength, water resistance, and sheath extrusion stability. Hydrogenated C36 dimer fatty acids are covalently fixed as β-hydroxy ester crosslinking bridges, reducing free fatty acid migration, precipitation, and long-term toughening effect attenuation. Partitioned feeding, with network formation followed by carbon black addition, decouples the reaction and carbon black dispersion, improving dimer acid conversion rate, gel controllability, and carbon black dispersion uniformity. The bimodal medium-density polyethylene / metallocene linear low-density polyethylene matrix and the submicron dynamic micro-crosslinked phase jointly improve ESCR, low-temperature impact, and elongation at break. The β-hydroxy ester network can undergo limited topological rearrangement at extrusion temperatures, providing a wider reprocessing window than a permanently crosslinked network and reducing the likelihood of incomplete melting or severe network clogging. Attached Figure Description
[0020] Figure 1 This is an atomic force microscopy quantitative nanomechanical elastic modulus distribution diagram of the radially frozen ultrathin cross section of the simulated outer sheath of the optical cable in Embodiment 3 of the present invention;
[0021] Figure 2 This is a transmission electron microscope image of the dispersion morphology of carbon black aggregates in the radially frozen ultrathin cross-section of the simulated outer sheath of the optical cable in Embodiment 3 of the present invention.
[0022] Figure 3 This is a field emission scanning electron microscope image of the fracture surface of the simulated outer sheath of the optical cable in Embodiment 3 of the present invention after being subjected to a low-temperature impact of −50°C.
[0023] Figure 4 This is a field emission scanning electron microscope image of the notch tip region after an environmental stress cracking test of the sheath material in Embodiment 3 of the present invention. Detailed Implementation
[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0025] Please see Figures 1-4 This invention provides a technical solution for a low-temperature crack-resistant polyethylene sheath material for optical cables and its preparation method:
[0026] The following examples are used to illustrate the present invention, but should not be construed as limiting the scope of protection. Unless otherwise specified, parts by weight and percentage content are all by mass; the equipment in the examples is limited only to type and key process capabilities, not to brand and model. All examples provide complete steps for grafting, selective reactive blending, downstream carbon black addition, and sample preparation.
[0027] Bimodal medium-density polyethylene: density 0.938~0.946g / cm³, MFR 0.10~0.60g / 10min under 190℃ / 2.16kg conditions, containing high molecular weight slow crack growth resistance components and low molecular weight processing components.
[0028] Metallocene linear low-density polyethylene: density 0.915~0.924g / cm³, MFR 0.50~2.00g / 10min at 190℃ / 2.16kg, comonomer is 1-hexene or 1-octene.
[0029] Ethylene / 1-octene block copolymer elastomer: density 0.866~0.887g / cm³, hard segment mass fraction 15~35%, soft segment glass transition temperature not higher than -58℃.
[0030] Carbon black masterbatch: using bimodal medium-density polyethylene as a carrier, containing 35-50 wt% furnace black; the carrier of the masterbatch is included in 100 parts of the total polyethylene matrix to avoid double counting.
[0031] The carboxyl / epoxy equivalent ratio is converted into carboxyl equivalent based on the dimer fatty acid acid value, and into epoxy equivalent based on the GMA grafting rate and the relative molecular mass of GMA 142.15.
[0032] GMA grafting rate: Unreacted monomers were removed by Soxhlet extraction with acetone for 8 hours. An infrared spectrum of 1730 cm⁻¹ was established using a calibrated sample with a known grafting rate. -1Carbonyl absorption peak / 720cm -1 The working curve of the internal standard peak of polyethylene was tested in parallel three times.
[0033] Dimeric fatty acid conversion rate: Material is sampled at the sampling port between the first and second side feed ports and rapidly cooled; free acid is extracted and titrated after swelling with hot xylene, and the conversion rate is calculated based on the added acid equivalent and the residual acid equivalent.
[0034] Gel content: The final sheath material was extracted in xylene at 140℃ for 24 hours. The mass of insoluble matter was reduced by the theoretical mass of carbon black, hydrotalcite and catalyst, and the total mass of epoxy functionalized elastomer and dimer fatty acid was used as the basis for calculation.
[0035] Dispersion domain particle size: The extruded sheath was frozen at -100℃ and ultrathin sections were prepared. The 5μm×5μm region was scanned using atomic force microscopy in quantitative nanomechanical mode. The elastomer phase was segmented according to the modulus difference. Five fields of view were randomly selected for each sample, and no less than 500 dispersion domains were counted. The numerical mean of the equivalent circle diameter and D90 were calculated.
[0036] Example 1
[0037] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 60 kg is bimodal medium-density polyethylene with a density of 0.938 g / cm³ and an MFR of 0.10 g / 10 min under 190℃ / 2.16 kg conditions; and 40 kg is metallocene linear low-density polyethylene with a density of 0.915 g / cm³ and an MFR of 0.50 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0038] S1. Preparation of epoxy-functionalized block elastomers. Based on 100 parts by mass of ethylene / 1-octene block copolymer elastomer, 1.2 parts by mass of glycidyl methacrylate, 0.4 parts by mass of styrene, and 0.03 parts by mass of dicumyl peroxide were mixed to prepare a liquid grafting solution. The elastomer was added through the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 165℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 0.60 wt%, and the pre-gel content was measured to be 0.6 wt% after extraction with xylene at 140℃.
[0039] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 44 was used, with the screw speed set at 250 r / min and the total output set at 120 kg / h. 55.543 kg of bimodal medium-density polyethylene, 40 kg of metallocene linear low-density polyethylene, and 8 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 30% of the effective screw length, 0.067 kg of hydrogenated C36 dimer fatty acid and 0.0024 kg of zinc acetylacetonate were added via a metering pump kept at 80°C. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 185 mg KOH / g, an iodine value of 10 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.65. The reaction zone temperature between the first and second feed ports is 175℃, and the average material residence time is controlled to 35s by adjusting the output and screw configuration. Subsequently, 6.857 kg of carbon black masterbatch is added at 65% of the effective screw length. This masterbatch contains 35.0 wt% furnace black and 65.0 wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.40 kg of carbon black and 4.457 kg of MPE. The furnace black has a native particle size of 25 nm and a DBP oil absorption value of 90 mL / 100g. Simultaneously, 0.08 kg of antioxidant 1010, 0.08 kg of antioxidant 168, 0.09 kg of distearate thiodipropionate, 0.05 kg of hydrotalcite, and 0.05 kg of fluoropolymer processing aids are added along with the masterbatch. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.060MPa. The die head temperature is 175℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0040] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 1.20mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0041] Example 2
[0042] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 75 kg is bimodal medium-density polyethylene with a density of 0.946 g / cm³ and an MFR of 0.60 g / 10 min under 190℃ / 2.16 kg conditions; and 25 kg is metallocene linear low-density polyethylene with a density of 0.924 g / cm³ and an MFR of 2.00 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0043] S1. Preparation of epoxy-functionalized block elastomers. Based on 100 parts by mass of ethylene / 1-octene block copolymer elastomer, 2.5 parts by mass of glycidyl methacrylate, 1.2 parts by mass of styrene, and 0.08 parts by mass of dicumyl peroxide were mixed to form a liquid grafting solution. The elastomer was added through the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 190℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 1.50 wt%, and the pre-gel content was measured to be 2.8 wt% after extraction with xylene at 140℃.
[0044] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 56 was used, with the screw speed set at 500 r / min and the total output set at 60 kg / h. 72.2 kg of bimodal medium-density polyethylene, 25 kg of metallocene linear low-density polyethylene, and 16 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 45% of the effective screw length, 0.45 kg of hydrogenated C36 dimer fatty acid and 0.032 kg of zinc acetate were added via a metering pump kept at 80°C. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 200 mg KOH / g, an iodine value of 2 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.95. The reaction zone temperature between the first and second feed ports is 195℃, and the average material residence time is controlled to 70s by adjusting the output and screw configuration. Subsequently, 5.6kg of carbon black masterbatch is added at 80% of the effective screw length. This masterbatch contains 50.0wt% furnace black and 50.0wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.80kg of carbon black and 2.8kg of MPE. The furnace black has a native particle size of 15nm and a DBP oil absorption value of 130mL / 100g. Simultaneously added with the masterbatch are 0.15kg of antioxidant 1010, 0.20kg of antioxidant 168, 0.20kg of distearate thiodipropionate, 0.20kg of hydrotalcite, and 0.30kg of fluoropolymer processing aids. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.095MPa. The die head temperature is 190℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0045] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 3.00mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0046] Example 3
[0047] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 67.5 kg is bimodal medium-density polyethylene with a density of 0.942 g / cm³ and an MFR of 0.35 g / 10 min under 190℃ / 2.16 kg conditions; and 32.5 kg is metallocene linear low-density polyethylene with a density of 0.920 g / cm³ and an MFR of 1.20 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0048] S1. Preparation of epoxy-functionalized block elastomers. Based on 100 parts by weight of ethylene / 1-octene block copolymer elastomer, 1.85 parts by weight of glycidyl methacrylate, 0.8 parts by weight of styrene, and 0.055 parts by weight of dicumyl peroxide were mixed to form a liquid grafting solution. The elastomer was added through the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 178℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 1.05 wt%, and the pre-gel content was measured to be 1.4 wt% after extraction with xylene at 140℃.
[0049] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 50 was used, with the screw speed set at 375 r / min and the total output set at 90 kg / h. 63.982 kg of bimodal medium-density polyethylene, 32.5 kg of metallocene linear low-density polyethylene, and 12 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 37.5% of the effective screw length, 0.207 kg of hydrogenated C36 dimer fatty acid and 0.012 kg of zinc acetylacetonate were added via a metering pump kept at 80°C. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 192 mg KOH / g, an iodine value of 5 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.80. The temperature of the reaction zone between the first and second feed ports is 185℃, and the average residence time of the material is controlled to 52s by adjusting the output and screw configuration. Subsequently, 6.118 kg of carbon black masterbatch is added at 72.5% of the effective screw length. This masterbatch contains 42.5 wt% furnace black and 57.5 wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.60 kg of carbon black and 3.518 kg of MPE. The furnace black has a native particle size of 20 nm and a DBP oil absorption value of 110 mL / 100g. Simultaneously, 0.12 kg of antioxidant 1010, 0.14 kg of antioxidant 168, 0.14 kg of distearate thiodipropionate, 0.12 kg of hydrotalcite, and 0.15 kg of fluoropolymer processing aids are added along with the masterbatch. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.080MPa. The die head temperature is 185℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0050] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 2.10mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0051] Example 4
[0052] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 62.5 kg is bimodal medium-density polyethylene with a density of 0.940 g / cm³ and an MFR of 0.20 g / 10 min under 190℃ / 2.16 kg conditions; and 37.5 kg is metallocene linear low-density polyethylene with a density of 0.918 g / cm³ and an MFR of 0.80 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0053] S1. Preparation of epoxy-functionalized block elastomer. Based on 100 parts by mass of ethylene / 1-octene block copolymer elastomer, 1.4 parts by mass of glycidyl methacrylate, 0.5 parts by mass of styrene, and 0.04 parts by mass of dicumyl peroxide were mixed to form a liquid grafting solution. The elastomer was fed into the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 170℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 0.72 wt%, and the pre-gel content was measured to be 0.8 wt% after extraction with xylene at 140℃.
[0054] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 48 was used, with the screw speed set at 300 r / min and the total output set at 110 kg / h. 58.75 kg of bimodal medium-density polyethylene, 37.5 kg of metallocene linear low-density polyethylene, and 10 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 35% of the effective screw length, 0.109 kg of hydrogenated C36 dimer fatty acid and 0.005 kg of zinc acetylacetonate were added via a metering pump kept at 80℃. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 188 mg KOH / g, an iodine value of 8 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.72. The reaction zone temperature between the first and second feed ports is 180℃, and the average material residence time is controlled to 35s by adjusting the output and screw configuration. Subsequently, 6.25kg of carbon black masterbatch is added at 70% of the effective screw length. This masterbatch contains 40.0wt% furnace black and 60.0wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.50kg of carbon black and 3.75kg of MPE. The furnace black has a native particle size of 22nm and a DBP oil absorption value of 100mL / 100g. Simultaneously added with the masterbatch are 0.10kg of antioxidant 1010, 0.11kg of antioxidant 168, 0.11kg of distearate thiodipropionate, 0.08kg of hydrotalcite, and 0.10kg of fluoropolymer processing aids. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.075MPa. The die head temperature is 180℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0055] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 1.50mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0056] Example 5
[0057] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 72.5 kg is bimodal medium-density polyethylene with a density of 0.944 g / cm³ and an MFR of 0.50 g / 10 min under 190℃ / 2.16 kg conditions; and 27.5 kg is metallocene linear low-density polyethylene with a density of 0.922 g / cm³ and an MFR of 1.70 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0058] S1. Preparation of epoxy-functionalized block elastomers. Based on 100 parts by mass of ethylene / 1-octene block copolymer elastomer, 2.3 parts by mass of glycidyl methacrylate, 1.1 parts by mass of styrene, and 0.075 parts by mass of dicumyl peroxide were mixed to form a liquid grafting solution. The elastomer was added through the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 186℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 1.38 wt%, and the pre-gel content was measured to be 2.4 wt% after extraction with xylene at 140℃.
[0059] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 52 was used, with the screw speed set at 450 r / min and the total output set at 70 kg / h. 69.2 kg of bimodal medium-density polyethylene, 27.5 kg of metallocene linear low-density polyethylene, and 14 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 42% of the effective screw length, 0.339 kg of hydrogenated C36 dimer fatty acid and 0.021 kg of zinc acetate were added via a metering pump kept at 80℃. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 198 mg KOH / g, an iodine value of 3 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.88. The temperature of the reaction zone between the first and second feed ports is 190℃, and the average residence time of the material is controlled to 70s by adjusting the output and screw configuration. Subsequently, 6kg of carbon black masterbatch is added at 78% of the effective screw length. This masterbatch contains 45.0wt% furnace black and 55.0wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.70kg of carbon black and 3.3kg of MPE. The furnace black has a native particle size of 18nm and a DBP oil absorption value of 120mL / 100g. Simultaneously added with the masterbatch are 0.14kg of antioxidant 1010, 0.17kg of antioxidant 168, 0.17kg of distearate thiodipropionate, 0.16kg of hydrotalcite, and 0.25kg of fluoropolymer processing aids. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.090MPa. The die head temperature is 188℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0060] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 2.50mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0061] Example 6
[0062] This embodiment uses 100 kg of final polyethylene matrix as the formulation basis, of which 75 kg is bimodal medium-density polyethylene with a density of 0.946 g / cm³ and an MFR of 0.25 g / 10 min under 190℃ / 2.16 kg conditions; and 25 kg is metallocene linear low-density polyethylene with a density of 0.924 g / cm³ and an MFR of 0.80 g / 10 min under the same conditions. The density of the ethylene / 1-octene block copolymer elastomer is 0.866–0.887 g / cm³, and the glass transition temperature of the soft segment is not higher than -58℃. All raw materials are dried in a 70℃ hot air circulating oven for 4 hours before use.
[0063] S1. Preparation of epoxy-functionalized block elastomers. Based on 100 parts by mass of ethylene / 1-octene block copolymer elastomer, 1.6 parts by mass of glycidyl methacrylate, 0.7 parts by mass of styrene, and 0.05 parts by mass of dicumyl peroxide were mixed to prepare a liquid grafting solution. The elastomer was added through the main feed port of a co-rotating twin-screw extruder with an aspect ratio of 40. After melting, the grafting solution was metered and injected at 30% of the effective screw length. The main reaction zone was controlled at 176℃ and the screw speed at 220 r / min. After the reaction, unreacted monomers were removed at -0.085 MPa, and the pellets were granulated underwater. After Soxhlet extraction with acetone for 8 hours and drying, the GMA grafting rate was measured to be 0.90 wt%, and the pre-gel content was measured to be 1.1 wt% after extraction with xylene at 140℃.
[0064] S2. In-situ construction of dynamic micro-crosslinked phase and completion of sheath material blending. A co-rotating twin-screw extruder with an aspect ratio of 50 was used, with the screw speed set at 375 r / min and the total output set at 90 kg / h. 70.8 kg of bimodal medium-density polyethylene, 25 kg of metallocene linear low-density polyethylene, and 8 kg of epoxy functionalized block elastomer obtained in step S1 were continuously added to the main feed port to form a continuous polyethylene phase and a dispersed elastomer phase. At 37.5% of the effective screw length, 0.118 kg of hydrogenated C36 dimer fatty acid and 0.008 kg of zinc acetylacetonate were added via a metering pump kept at 80℃. The dimer fatty acid used had a C36 dimer acid content of not less than 95 wt%, an acid value of 192 mg KOH / g, an iodine value of 5 g I2 / 100 g, and a carboxyl / epoxy equivalent ratio of 0.80. The reaction zone temperature between the first and second feed ports is 185℃, and the average material residence time is controlled to 52s by adjusting the output and screw configuration. Subsequently, 7kg of carbon black masterbatch is added at 72.5% of the effective screw length. This masterbatch contains 40.0wt% furnace black and 60.0wt% bimodal medium-density polyethylene (MDPE) as a carrier, corresponding to 2.80kg of carbon black and 4.2kg of MPE. The furnace black has a native particle size of 20nm and a DBP oil absorption value of 110mL / 100g. Simultaneously, 0.12kg of antioxidant 1010, 0.14kg of antioxidant 168, 0.14kg of distearate thiodipropionate, 0.12kg of hydrotalcite, and 0.15kg of fluoropolymer processing aids are added along with the masterbatch. A distribution mixing element is set downstream of the second side feed port, and the material is devolatilized under a vacuum of -0.080MPa. The die head temperature is 185℃. After extrusion, water cooling and granulation, black sheath material is obtained.
[0065] S3. Sample Preparation. After drying the sheath material at 70℃ for 4 hours, it was applied to a circular non-metallic simulated cable core with an outer diameter of 10mm using a single-screw sheath extruder at barrel / die temperatures of 170℃, 180℃, 185℃, and 185℃, forming a simulated optical cable outer sheath with a nominal thickness and a measured average thickness of 1.80mm. Separately, density, MFR, tensile, ESCR, and embrittlement temperature samples were pressed or cut according to relevant national standards. All samples were conditioned for 48 hours at 23±2℃ and 50±10% relative humidity before testing.
[0066] Unless otherwise specified in the comparative examples below, the raw material specifications, dosage, screw assembly, temperature, residence time, sample preparation, and condition adjustment conditions are exactly the same as in Example 3.
[0067] Comparative Example 1
[0068] The epoxy-functionalized elastomer of Example 3 was replaced with an equal mass of ethylene / 1-octene block copolymer elastomer that was not grafted with GMA; 0.207 kg of hydrogenated C36 dimer fatty acid and 0.012 kg of zinc acetylacetonate were added as in Example 3.
[0069] Comparative Example 2
[0070] Hydrogenated C36 dimer fatty acids were not added. All other raw materials and processes were the same as in Example 3. Zinc acetylacetonate was still added at 0.012 kg.
[0071] Comparative Example 3
[0072] Instead of adding dimer fatty acids and catalyst at 37.5% screw length, both are added together with carbon black masterbatch at 72.5% screw length; the dosage, total temperature, and screw speed remain unchanged.
[0073] Comparative Example 4
[0074] Only 0.012 kg of zinc acetylacetone was added to the first feeding port; after extrusion granulation was completed and the particles were cooled to 40°C, 0.207 kg of hydrogenated C36 dimer fatty acid was atomized and sprayed onto the particle surface and rolled for 30 min.
[0075] Comparative Example 5
[0076] The amount of epoxy functionalized elastomer was reduced from 12 kg to 4 kg, and the dimer fatty acid and catalyst were adjusted synchronously according to the same GMA grafting rate, the same carboxyl / epoxy equivalent ratio and the same relative amount of catalyst, while the polyethylene matrix remained at 100 kg.
[0077] Comparative Example 6
[0078] The amount of epoxy functionalized elastomer was increased from 12 kg to 20 kg, and the amount of dimer fatty acid and catalyst was adjusted synchronously according to the same GMA grafting rate, the same carboxyl / epoxy equivalent ratio and the same relative amount of catalyst, while the amount of polyethylene matrix remained at 100 kg.
[0079] Comparative Example 7
[0080] The amount of hydrogenated C36 dimer fatty acid was adjusted to make the carboxyl / epoxy equivalent ratio 0.45, and other raw materials and processes were the same as in Example 3.
[0081] Comparative Example 8
[0082] The amount of hydrogenated C36 dimer fatty acid was adjusted to make the carboxyl / epoxy equivalent ratio 1.20, and other raw materials and processes were the same as in Example 3.
[0083] Performance testing methods
[0084] Density: Tested according to the immersion method of GB / T 1033.1—2008. The sample was equilibrated at 23±2℃, and the average value of three independent batches of samples was reported.
[0085] Melt mass flow rate: Tested according to GB / T 3682.1—2018, under the conditions of 190℃ and 2.16kg, in g / 10min.
[0086] Tensile properties: Specimens shall be cut from a simulated sheath with a thickness of 1.8±0.1mm in accordance with GB / T 2951.11—2008, and the tensile strength and elongation at break shall be determined in accordance with the standard; no less than 5 valid specimens shall be taken from each batch.
[0087] Environmental stress cracking: Conducted according to the general rules of GB / T 1842—2008 and in conjunction with GB / T 43316.1—2023, selecting test condition B. The medium, bending specimen, notch and temperature shall be performed in accordance with the standard, and the report shall be F50.
[0088] Low-temperature impact: According to GB / T 2951.14—2008, the simulated optical cable sheaths of different thicknesses obtained in Example S3 were pre-cooled at -50±2℃ for 16 hours, and the impact hammer mass specified in the standard was selected according to the outer diameter of the finished product; 30 samples were tested in each batch, and the number of samples with visible cracks was recorded. The comparative example used the same sheath thickness of 2.10 mm as in Example 3.
[0089] Impact embrittlement temperature: Tested according to GB / T 5470—2008, the embrittlement temperature is the temperature at which 50% of the sample fails.
[0090] Carbon black content and dispersion: determined according to GB / T 2951.41—2008; the smaller the dispersion grade number, the more uniform the dispersion.
[0091] Melt fracture rating: As a supplementary internal process evaluation, the sheath surface is observed under fixed extrusion rates and traction speeds. Grade 0 indicates no visible sharkskin, while grades 1 through 5 increase with the degree of periodic surface roughness and spiral fracture. This internal evaluation does not replace the national standard items.
[0092] Free component migration: The sheathed sample was sandwiched between two sheets of quantitative filter paper and placed at 70℃ and 0.2MPa for 168 hours. Based on the presence of oil stains on the filter paper and the stickiness of the sample surface, it was classified as none, slight, or significant. This test is used to distinguish between covalently fixed and free dimer acids.
[0093] The test results are shown in Tables 1-3.
[0094] Table 1
[0095] Table 2
[0096] Table 3
[0097] Examples 1 through 6 cover the lower, upper, and middle regions of the elastomer content, grafting rate, carboxyl / epoxy equivalence ratio, reaction temperature, carbon black and stabilizer dosage as specified in the independent claims. Examples 4 and 5 further cover the two ends of the preferred reaction temperature of 180–190°C, equivalence ratio of 0.72–0.88, and gel content of 25–55 wt%. The results show that all examples can meet the requirements of F50 not less than 1000h, tensile strength not less than 18 MPa, elongation at break not less than 450%, and no cracking upon impact at -50°C.
[0098] Compared with Comparative Examples 1 and 2, Example 3, with the same content of polyethylene matrix and elastomer, reduced the gel content to near zero by only lacking epoxy functional groups or dimer acid crosslinking bridges, the dispersion domain D90 exceeded 2.50 μm, and the F50 and low-temperature impact were significantly reduced. This indicates that the effect comes from the micro-crosslinking structure formed by epoxy-dimer acid, rather than the simple blending of elastomers.
[0099] Compared with Comparative Example 3, Example 3 only changed the timing of adding dimer acid / catalyst, which reduced the dimer acid conversion rate from the predicted 93% to 56%, changed the carbon black dispersion grade from level 1 to level 4, and produced low-temperature impact cracks. This shows that "forming a network first and then adding carbon black" has a synergistic contribution to selective reaction and carbon black dispersion.
[0100] Compared with Comparative Example 4, Example 3 used the same total amount of dimer acid, but when it was added in a free coating manner, significant migration was observed, and the ESCR and embrittlement temperature both deteriorated significantly. This proves that hydrogenated C36 dimer fatty acid needs to be fixed in the elastomer phase as a covalent crosslinking bridge, rather than being used as a general processing aid.
[0101] Comparative Example 5 shows that although the dynamic phase has a smaller particle size when it is less than 8 parts, it is insufficient to establish an effective crack passivation volume fraction; Comparative Example 6 shows that although the dynamic phase has a higher low-temperature elongation and F50 when it is more than 16 parts, the tensile strength decreases and melt fracture is aggravated. This demonstrates that the present invention balances the window of low-temperature toughness, strength and processability.
[0102] The equivalent ratio of Comparative Example 7 was too low, resulting in insufficient gelation; the equivalent ratio of Comparative Example 8 was too high, resulting in excessive gelation, decreased MFR and elongation. Examples 3 to 5 had a more balanced network density and processing performance.
[0103] Depend on Figure 1 As can be seen, the regions with different elastic moduli in the cross-section of the sheath in Example 3 exhibit a refined, continuous, and interconnected distribution at the nanoscale, without large-sized, sharply defined extremely high-modulus agglomerates or extremely low-modulus defect regions. This result indicates that a relatively uniform nanomechanical transition structure is formed between the polyethylene matrix, toughening phase, confined molecular chain regions, and filler interface regions in the sheath material. Figure 1The continuous intermediate modulus region indicates that the different phases are not completely separated, but rather form a mechanical transition interface with a certain width, which helps to reduce local modulus abrupt changes and interface stress concentration under external forces. When the sheath is subjected to bending, impact, or residual internal stress at low temperatures, this structure can gradually transfer the load from the local area to the surrounding matrix, thereby reducing the possibility of crack initiation preferentially at the edge of hard agglomerates or at the interface between soft and hard phases.
[0104] Depend on Figure 2 As can be seen, carbon black is dispersed in the continuous polyethylene phase in the form of small aggregates, with relatively uniform spacing between the aggregates, without forming large carbon black agglomerates or obvious local enrichment zones that penetrate the field of view. The relatively continuous interface between the aggregate edges and the surrounding polyethylene matrix indicates that the formulation and mixing process used in Example 3 can suppress secondary agglomeration of carbon black. Uniform carbon black dispersion reduces local stress concentration caused by large rigid agglomerates, lowering the probability of microcracks initiating at the edges of carbon black agglomerates under low-temperature conditions. The uniformly distributed carbon black aggregates also allow cracks to deflect, branch, or circumvent, extending the crack propagation path. Simultaneously, this dispersion state helps avoid excessive carbon black agglomeration, which can cause abnormal local melt viscosity and defects on the extruded sheath surface.
[0105] Depend on Figure 3 As can be seen, the low-temperature impact fracture surface of the sheath in Example 3 is generally rough, with overlapping tear ridges, microfibers and polymer ligaments formed under tension, irregular cavitation depressions, and obvious crack deflection paths. Some polymer ligaments bridge adjacent fracture areas, indicating that the material still underwent a certain degree of plastic tension and local shear yielding during the −50 °C impact. This morphology differs from the typical rapid brittle fracture surface, which is flat, continuous, and lacks tensile ligaments. This demonstrates that Example 3 can dissipate impact energy during low-temperature impact through processes such as molecular chain stretching, controlled cavitation after interfacial debonding, ligament necking, and crack deflection, thus delaying the rapid penetration of the main crack through the sheath. This proves that Example 3 does not merely rely on reducing material stiffness to achieve apparent softness, but rather forms an effective low-temperature plastic energy dissipation mechanism while maintaining the structural integrity of the sheath.
[0106] Depend on Figure 4It is evident that the tip of the original notch undergoes a certain degree of rounding, forming a plastic deformation region of a certain width in front of the notch. Within this region, several short, tortuous, and discontinuous microcracks exist, and tensile microfibers or polymer ligaments connecting the two sides of some cracks can be observed; no single straight main crack extends directly forward from the notch tip and traverses the field of view. The rounding of the notch tip reduces local stress intensity, while the dispersion of microcracks and the inter-crack ligaments consumes crack opening energy and hinders the rapid merging of adjacent microcracks. These results indicate that the sheathing material of Example 3, under the combined action of surfactant medium and continuous bending stress, can still slow crack growth through local plastic deformation, microfiber stretching, and crack deflection.
[0107] The above are merely specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent substitutions, or modifications made based on the present invention to solve essentially the same technical problems and achieve essentially the same technical effects are all covered within the protection scope of the present invention.
Claims
1. A method for preparing low-temperature crack-resistant polyethylene sheath material for optical cables, characterized in that, Includes the following steps: S1. Ethylene / 1-octene block copolymer elastomer, glycidyl methacrylate, free radical initiator and styrene grafting agent are reacted, extruded and devolatilized to obtain epoxy-functionalized ethylene / 1-octene block copolymer elastomer with glycidyl methacrylate grafting rate of 0.6-1.5 wt%. S2. Using 100 parts by weight of polyethylene matrix, 8-16 parts by weight of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer and the polyethylene matrix are added and melt-dispersed through the main feed port of a co-rotating twin-screw extruder. Then, hydrogenated C36 dimer fatty acid and epoxy-carboxyl addition and transesterification catalyst are added through the first side feed port located downstream of the melt dispersion section. The equivalent ratio of the carboxyl group of the hydrogenated C36 dimer fatty acid to the epoxy group in the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.65-0.
95. The hydrogenated C36 dimer fatty acid reacts with the epoxy group in the dispersed elastomer phase at 175-195°C to form a dynamic micro-crosslinked phase connected by β-hydroxy ester bonds in situ. S3. After the formation of the dynamic micro-crosslinked phase, carbon black masterbatch, antioxidant, acid absorbent, and processing aid are added from the second feed port located downstream of the reaction section, so that the carbon black content is 2.4-2.8 parts by mass, the antioxidant content is 0.25-0.55 parts by mass, the acid absorbent content is 0.05-0.20 parts by mass, and the processing aid content is 0.05-0.30 parts by mass per 100 parts by mass of the polyethylene matrix. After melt mixing, vacuum devolatilization, extrusion, and granulation, the sheath material is obtained.
2. The preparation method according to claim 1, characterized in that, The polyethylene matrix is composed of 60-75 parts by mass of bimodal medium-density polyethylene and 25-40 parts by mass of metallocene linear low-density polyethylene; the bimodal medium-density polyethylene has a melt flow rate of 0.10-0.60 g / 10 min and a density of 0.938-0.946 g / cm³ at 190°C and 2.16 kg, and the metallocene linear low-density polyethylene has a melt flow rate of 0.50-2.00 g / 10 min and a density of 0.915-0.924 g / cm³ at 190°C and 2.16 kg.
3. The preparation method according to claim 2, characterized in that, In step S1, based on 100 parts by mass of the ethylene / 1-octene block copolymer elastomer, the amount of glycidyl methacrylate is 1.2 to 2.5 parts by mass, the amount of the styrene grafting agent is styrene and it is 0.4 to 1.2 parts by mass, and the amount of the free radical initiator is 0.03 to 0.08 parts by mass; the temperature of the reactive extrusion is 165 to 190°C, and the gel content of the obtained epoxy-functionalized ethylene / 1-octene block copolymer elastomer, as measured by xylene extraction at 140°C, is less than 3 wt%.
4. The preparation method according to claim 3, characterized in that, The hydrogenated C36 dimer fatty acid contains a C36 dimer acid content of not less than 95 wt%, an acid value of 185-200 mg KOH / g, and an iodine value of not more than 10 g I2 / 100 g; the catalyst is zinc acetylacetone and / or zinc acetate, the amount of which is 0.03-0.20 wt% of the mass of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer, and the equivalence ratio of the carboxyl group to the epoxy group is 0.72-0.
88.
5. The preparation method according to claim 4, characterized in that, The reaction temperature in step S2 is 180–190°C, and the average residence time of the material from the addition of the hydrogenated C36 dimer fatty acid to the addition of the carbon black masterbatch is 35–70 s. After the obtained sheath material is extracted with xylene at 140°C for 24 h, the mass of insoluble matter is reduced by the mass of carbon black, acid absorbent and catalyst added, and the gel content is calculated based on the sum of the mass of the added epoxy functionalized ethylene / 1-octene block copolymer elastomer and hydrogenated C36 dimer fatty acid, which is 25–55 wt%.
6. The preparation method according to claim 1, characterized in that, The co-rotating twin-screw extruder has a length-to-diameter ratio of 44 to 56 and a screw speed of 250 to 500 r / min. With the effective screw length as 100%, the first side feed port is located at 30% to 45% and the second side feed port is located at 65% to 80%. A distribution mixing element and a kneading element are sequentially arranged between the first side feed port and the second side feed port. A devolatilization port with a vacuum degree of -0.06 to -0.095 MPa is arranged downstream of the second side feed port.
7. The preparation method according to claim 6, characterized in that, The carbon black masterbatch uses bimodal medium-density polyethylene as a carrier and contains 35-50 wt% furnace black. The original particle size of the furnace black is 15-25 nm, and the dibutyl phthalate oil absorption value is 90-130 mL / 100 g. The antioxidants include hindered phenolic antioxidants, phosphite antioxidants, and thiodipropionate antioxidants. The acid absorbent is hydrotalcite, and the processing aid is a fluoropolymer processing aid.
8. The low-temperature crack-resistant polyethylene sheath material for optical cables prepared by the method according to any one of claims 1-7, characterized in that, By weight, it comprises: 100 parts polyethylene matrix, 8-16 parts epoxy-functionalized ethylene / 1-octene block copolymer elastomer, hydrogenated C36 dimer fatty acid, 0.002-0.032 parts epoxy-carboxyl addition and transesterification catalyst, 2.4-2.8 parts carbon black, 0.25-0.55 parts antioxidant, 0.05-0.20 parts acid absorbent, and 0.05-0.30 parts processing aid; The glycidyl methacrylate grafting rate of the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.6–1.5 wt%, and the equivalent ratio of the carboxyl group of the hydrogenated C36 dimer fatty acid to the epoxy group in the epoxy-functionalized ethylene / 1-octene block copolymer elastomer is 0.65–0.
95. The epoxy-functionalized ethylene / 1-octene block copolymer elastomer forms a dynamic micro-crosslinked phase containing β-hydroxy ester bonds through the reaction of its epoxy groups with the hydrogenated C36 dimer fatty acid. The dynamic micro-crosslinked phase exists as dispersed domains in the polyethylene matrix, and the number-average equivalent diameter of the dispersed domains is 0.20–1.20 μm and the D90 is not greater than 2.50 μm.
9. The low-temperature crack-resistant polyethylene sheath material for optical cables according to claim 8, characterized in that, The polyethylene sheath material has a melt flow rate of 0.20-0.65 g / 10 min and a density of 0.932-0.946 g / cm³ at 190℃ and 2.16 kg. The environmental stress cracking time F50 is not less than 1000 h, the tensile strength is not less than 18 MPa, and the elongation at break is not less than 450%.