Semiconducting shielding material and its preparation method and cable
By employing a core-shell structured antioxidant composition in a semiconductive shielding material, and utilizing chitosan and modified cellulose to form a three-dimensional cross-linked network, the slow-release function of the antioxidant is controlled, thus solving the problem of matrix resin aging caused by rapid antioxidant release and extending the service life of the cable.
Patent Information
- Application Number
- CN202611627587.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
The antioxidants in existing semiconductive shielding materials release rapidly, leading to a high risk of aging in the matrix resin and failing to meet the long-term service requirements of cables. Furthermore, conventional antioxidant compositions are prone to resin aging during the processing stage.
The antioxidant composition adopts a core-shell structure, with the shell consisting of chitosan, a first crosslinking agent, and modified cellulose, and the core being an antioxidant. The antioxidant is encapsulated through a three-dimensional crosslinking network to control its sustained-release function. A stable three-dimensional crosslinking network is formed by crosslinking the epoxy-based hydrophobic crosslinking agent with chitosan, which improves the compatibility and dispersibility with the matrix resin.
This reduces the rate of antioxidant depletion, slows down the aging of the semiconductive shielding matrix resin during preparation and long-term service, and improves the service life of cables.
Smart Images

Figure CN123107232A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of cable technology, and in particular to a semiconductive shielding material, its preparation method, and a cable. Background Technology
[0002] Semiconducting shielding material, as a core functional component of cables, is mainly used to protect the internal insulation layer of cables. Its performance stability directly determines the service life and operational safety of cables.
[0003] In related technologies, the antioxidants used in semiconductive shielding materials release relatively quickly, which cannot meet the requirements for long-term cable service. Meanwhile, conventional antioxidant compositions are prone to causing aging risks to the matrix resin during the processing of semiconductive shielding materials. Summary of the Invention
[0004] This application provides a semiconductive shielding material, its preparation method, and a cable, which reduces the risk of matrix resin aging during the processing of the semiconductive shielding material while controlling the release rate of antioxidants in the semiconductive shielding material layer during cable use, thereby meeting the long-term service requirements of the cable.
[0005] In a first aspect, embodiments of this application provide a semiconductive shielding material, comprising a matrix resin, conductive carbon black, a second crosslinking agent, an antioxidant composition, and a lubricant; The matrix resin is 100 parts by mass, the conductive carbon black is 35 to 65 parts by mass, the second crosslinking agent is 1 to 2 parts by mass, the antioxidant composition is 3 to 6 parts by mass, and the lubricant is 2 to 8 parts by mass. The antioxidant composition has a core-shell structure and includes a shell layer and a core layer. The shell layer includes chitosan, a first crosslinking agent, and modified cellulose. The core layer includes an antioxidant. The first crosslinking agent includes an epoxy-based hydrophobic crosslinking agent. Wherein, the mass ratio of the first crosslinking agent to the chitosan is (0.6~1):1, and the mass ratio of the chitosan to the modified cellulose is 1:(3~6); The modified cellulose is shear-resistant cellulose, which includes at least one of cellulose ether and cellulose ester, and the epoxy hydrophobic crosslinking agent includes at least one of epoxidized soybean oil and epoxidized sunflower seed oil.
[0006] Secondly, embodiments of this application also provide a method for preparing the semiconductive shielding material described in the first aspect, comprising: A semi-finished semi-conductive shielding material is obtained by mixing a matrix resin, conductive carbon black, lubricant and antioxidant composition using an internal mixer. The second crosslinking agent crosslinks with the semi-finished product of the semiconductive shielding material at the second crosslinking reaction temperature to obtain the semiconductive shielding material; The antioxidant composition has a core-shell structure and includes a shell layer and a core layer. The shell layer includes chitosan, a first crosslinking agent, and modified cellulose. The core layer includes an antioxidant. The first crosslinking agent includes an epoxy-based hydrophobic crosslinking agent. Wherein, the mass ratio of the first crosslinking agent to the chitosan is (0.6~1):1, and the mass ratio of the chitosan to the modified cellulose is 1:(3~6); The modified cellulose is shear-resistant cellulose, which includes at least one of cellulose ether and cellulose ester, and the epoxy hydrophobic crosslinking agent includes at least one of epoxidized soybean oil and epoxidized sunflower seed oil.
[0007] Thirdly, embodiments of this application also provide a cable including a semi-conductive shielding layer, wherein the semi-conductive shielding layer is the semi-conductive shielding material described in the first aspect.
[0008] Using one or more technical solutions in the embodiments of this application, the antioxidant composition has a core-shell structure. The chitosan in its shell layer can undergo a cross-linking reaction with a first cross-linking agent to form a three-dimensional cross-linked network of chitosan and the first cross-linking agent. This allows the antioxidant to be encapsulated within the three-dimensional cross-linked network, forming a core-shell structure antioxidant composition with sustained-release function. Modified cellulose can be added to the three-dimensional cross-linked network as a filler to improve its performance. When the antioxidant composition is added to a semiconductive shielding material, the composition can achieve good compatibility with the matrix resin in the semiconductive shielding material due to the good biocompatibility and film-forming properties of chitosan. This ensures the conductivity and mechanical properties of the semiconductive shielding material and avoids negatively impacting its conductivity and mechanical properties due to poor interfacial bonding between the antioxidant composition and the matrix resin.
[0009] The first crosslinking agent in this application embodiment is an epoxy-based hydrophobic crosslinking agent. During the crosslinking process with chitosan, it can also complete the curing and hydrophobic modification of the three-dimensional crosslinking network. The hydrophobic chain of the epoxy-based hydrophobic crosslinking agent has high chemical inertness and will not react chemically with the matrix resin and other components in the semiconductive shielding material. Therefore, the antioxidant composition is dispersed in the matrix resin. The antioxidant composition can maintain its original performance and will not adversely affect the components in the semiconductive shielding material.
[0010] This application embodiment also controls the degree of cross-linking between chitosan and the first cross-linking agent by controlling the mass ratio of the first cross-linking agent to chitosan to (0.6~1):1. This prevents the three-dimensional cross-linked network from becoming too dense due to excessive cross-linking, which would affect the sustained-release effect of the antioxidant. It also ensures that the number of amino groups retained in chitosan is sensitive to pH changes, giving the antioxidant composition a pH-responsive sustained-release effect. Furthermore, controlling the mass ratio of chitosan to modified cellulose to 1:(3~6) controls the amount of modified cellulose filling the three-dimensional cross-linked network, preventing excessive filling from clogging the gaps in the three-dimensional cross-linked network and thus affecting the sustained-release function of the antioxidant in the antioxidant composition.
[0011] As can be seen, the antioxidant composition of this application reduces the rate of antioxidant depletion, slows down the aging rate of the matrix resin of the semiconductive shielding material during the preparation process and long-term service, and improves the service life of the cable. Attached Figure Description
[0012] The above and other objects, features, and advantages of this application will become more apparent from the more detailed description of the embodiments of this application in conjunction with the accompanying drawings. The accompanying drawings are used to provide a further understanding of the embodiments of this application and form part of the specification. They are used together with the embodiments of this application to explain this application and do not constitute a limitation thereof. In the accompanying drawings, the same reference numerals generally represent the same components or steps.
[0013] Figure 1 This paper illustrates a schematic diagram of the generation principle of a three-dimensional cross-linked network using epoxidized soybean oil as an example in an embodiment of this application. Figure 2 Scanning electron microscope images of the antioxidant compositions of embodiments of this application are shown; Figure 3 A schematic flowchart of the preparation method of the antioxidant composition according to an embodiment of this application is shown; Figure 4 A schematic flowchart of a method for preparing a semiconductive shielding material according to an embodiment of this application is shown. Detailed Implementation
[0014] To make the objectives, technical solutions, and advantages of this application more apparent, exemplary embodiments according to this application will be described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments of this application. It should be understood that this application is not limited to the exemplary embodiments described herein.
[0015] As a core functional component of cables, cable shielding materials are primarily used to protect the internal insulation layer of cables, and their performance stability directly determines the cable's service life and operational safety. With the rapid development of industrial technology, the service scenarios for cables are becoming increasingly complex, especially for long-term service scenarios such as ultra-high voltage cables, outdoor cables, and submarine cables, which place higher demands on the oxidation resistance, processing stability, and service life of cable shielding materials.
[0016] Semiconducting shielding materials are highly susceptible to thermo-oxidative aging during processing, extrusion, prolonged operation at high temperatures, high-temperature extrusion, and high-voltage electric field coupling. While small-molecule antioxidants or liquid nonpolar core-shell slow-release antioxidants can be used to mitigate aging, these solutions have significant drawbacks, which are illustrated below.
[0017] Liquid nonpolar polymer core-shell antioxidants rely solely on the melting of polyolefins to achieve single-thermal controlled slow release. When used in high carbon black-filled semiconductive shielding materials, the numerous active sites on the carbon black surface catalyze the rapid decomposition of small-molecule antioxidants. Moreover, the shell layer melts instantaneously under high-temperature extrusion, resulting in a large-scale release of antioxidants at once. Within a few years of service (e.g., 3 years), the antioxidant components are significantly depleted, failing to meet the long-term service requirements (e.g., 30 years) of high-voltage cables.
[0018] Meanwhile, the application of antioxidants in the industry is limited to simple compounding of different types of antioxidants, and the potential risk that "using conventional slow-release antioxidants alone may lead to resin aging during the processing stage" has not been realized, and no targeted solutions have been developed.
[0019] To address the aforementioned problems, embodiments of this application provide a cable that may include a semi-conductive shielding layer. This semi-conductive shielding layer may be an insulating semi-conductive shielding layer or a conductive semi-conductive shielding layer. Taking an insulating semi-conductive shielding layer as an example, the insulating semi-conductive shielding layer may be located on the surface of the insulation layer away from the conductor.
[0020] In some embodiments, the antioxidant contained in the semiconductive shielding layer of this application can be the antioxidant composition of this application, which can reduce the risk of matrix resin aging during the processing of semiconductive shielding material, while controlling the release rate of antioxidant in the semiconductive shielding material layer during cable use, thereby meeting the long-term service requirements of the cable.
[0021] In other embodiments, the semiconductive shielding layer of this application contains a semiconductive shielding material containing an antioxidant composition of this application; thus, during the processing of the semiconductive shielding material, the aging risk of the matrix resin is relatively low, and the release rate of the antioxidant during cable use can be controlled, thereby meeting the long-term service requirements of the cable.
[0022] This application provides an antioxidant composition with a core-shell structure. In this case, the antioxidant composition can be an antioxidant slow-release capsule. Utilizing the slow-release capability of the capsule, the antioxidant is gradually released during the preparation and use of the semiconductive shielding material, thereby slowing down the aging rate of the matrix resin and meeting the long-term service requirements of the cable.
[0023] The antioxidant composition of this application embodiment includes a shell layer and a core layer. The shell layer includes chitosan, a first crosslinking agent, and modified cellulose. The core layer includes an antioxidant. The chitosan can undergo a crosslinking reaction with the first crosslinking agent to form a three-dimensional crosslinked network (also known as a crosslinked polysaccharide gradient microporous structure). This allows the antioxidant to be encapsulated within the three-dimensional crosslinked network, forming a core-shell structure antioxidant composition with sustained-release function. The modified cellulose can fill the three-dimensional crosslinked network, improving the properties of the shell layer, such as mechanical strength and temperature resistance.
[0024] When an antioxidant composition is added to a semiconductive shielding material, the antioxidant composition can achieve good compatibility with the matrix resin in the semiconductive shielding material through the good biocompatibility, film-forming properties and environmental friendliness of chitosan. This ensures the conductivity and mechanical properties of the semiconductive shielding material and avoids the impact on the conductivity and mechanical properties of the semiconductive shielding material due to poor interfacial bonding between the antioxidant composition and the matrix resin.
[0025] Optionally, when the first crosslinking agent includes an epoxy-based hydrophobic crosslinking agent, the epoxy-based hydrophobic crosslinking agent can be a mono-epoxy hydrophobic crosslinking agent or a poly-epoxy hydrophobic crosslinking agent. The hydrophobic chain in the molecular skeleton of the epoxy-based hydrophobic crosslinking agent can be an alkyl chain, for example, the alkyl chain has 4 to 20 carbon atoms, further, 4 to 18 carbon atoms. The epoxy-based hydrophobic crosslinking agent includes at least one of epoxidized soybean oil, epoxidized sunflower seed oil, and diol diglycidyl ether. For example, the diol diglycidyl ether can be 1,4-butanediol diglycidyl ether and / or 1,6-hexanediol diglycidyl ether.
[0026] Figure 1 This illustration shows a schematic diagram illustrating the generation principle of a three-dimensional cross-linked network using epoxidized soybean oil as an example from an embodiment of this application. Figure 1 As shown, when chitosan A undergoes a crosslinking reaction with epoxidized soybean oil (ESO), the epoxy functional groups in the ESO can undergo ring-opening and addition crosslinking reactions with the primary amino and hydroxyl groups of the chitosan molecules, thereby obtaining a first shell composite material B constructed from chitosan and epoxidized soybean oil. This first shell composite material B has a three-dimensional crosslinked network structure. Furthermore, the amino and hydroxyl groups of the chitosan molecules can be connected through intermolecular hydrogen bonds to further construct a second shell composite material C. Figure 1In the first shell composite material B and the second shell composite material C, R represents an alkyl chain.
[0027] The aforementioned epoxidized soybean oil's molecular backbone possesses hydrophobic chains that, during the chitosan crosslinking process, complete the curing and hydrophobic modification of the three-dimensional crosslinked network, making the cable suitable for underwater or high-humidity environments. Furthermore, the hydrophobic chains of epoxidized soybean oil are highly chemically inert and will not chemically react with the matrix resin or other components in the semiconductive shielding material. Therefore, when this antioxidant composition is dispersed in the matrix resin, it maintains its original properties without adversely affecting the components in the semiconductive shielding material.
[0028] In one example, the alkyl chain is relatively long and has good compatibility with the matrix resin. The epoxy hydrophobic crosslinking agent reacts with chitosan to form a three-dimensional crosslinking network and coats the antioxidant. Therefore, after the antioxidant composition is added to the semiconductive shielding material, it can improve the dispersibility of the antioxidant in the matrix resin, so that the antioxidant can be uniformly dispersed in the semiconductive shielding material.
[0029] For example, Figure 2 A scanning electron microscope (SEM) image of the antioxidant composition according to an embodiment of this application is shown. Figure 2 As shown, the core-shell structure of the antioxidant composition has a size of 0.5μm to 2.5μm. When the antioxidant composition is added to the semiconductive shielding material, the antioxidant is less likely to aggregate locally, ensuring that the antioxidant can be uniformly dispersed in the semiconductive shielding material, thereby better preventing the aging of the semiconductive shielding layer.
[0030] Optionally, in the embodiments of this application, if the content of the first crosslinking agent is too low, there are too few crosslinking sites, and the crosslinking reaction of chitosan amino and alcohol hydroxyl groups is incomplete, resulting in a low amount of hydrophobic alkyl grafting of the first crosslinking agent; if the content of the first crosslinking agent is too high, there is excessive crosslinking, the amount of amino residue is too low, the pH-responsive slow-release mechanism is lost, and the three-dimensional crosslinking network is too dense, resulting in poor antioxidant slow-release effect. Therefore, the degree of crosslinking between chitosan and the first crosslinking agent can be controlled by controlling the mass ratio of the first crosslinking agent to chitosan to (0.6~1):1 (such as 0.6:1, 0.8:1 or 1:1). This can prevent the three-dimensional crosslinking network from becoming too dense due to excessive crosslinking degree, which would affect the slow-release effect of antioxidant, and can also ensure that the number of amino groups retained by chitosan is sensitive to pH changes, so that the antioxidant composition has a pH-responsive slow-release effect.
[0031] The pH-responsive slow-release effect of the antioxidant composition in this application embodiment can be understood as follows: Long-term thermo-oxidative aging of the matrix resin included in the cable will slowly generate trace amounts of acidic degradation molecules of carboxylic acids. Under acidic conditions, the amino groups on the chitosan of the antioxidant composition that penetrates into the semiconductive shielding material undergo protonation (-NH2+H2O).+ →NH 3+ ), making Figure 1 The hydrogen bonding between different chitosan molecules weakens, causing the chitosan polysaccharide chains to stretch, the gradient micropore size to increase significantly, and the antioxidant release rate to automatically increase. When the acidity of the system is neutralized by the antioxidant and free radicals are consumed, the environmental pH rises, the amino groups deprotonate, the chain segments contract again, and the antioxidant release rate decreases. Furthermore, the hydrophobic chain of the first crosslinking agent can increase the dispersibility of the antioxidant composition in the matrix resin, preventing the hydrophilicity of the amino groups from affecting the dispersibility of the antioxidant composition in the matrix resin.
[0032] As can be seen, the antioxidant composition of this application embodiment can reduce the rate of antioxidant depletion, slow down the aging rate of the matrix resin of the semiconductive shielding material during the preparation process and long-term service, and improve the service life of the cable.
[0033] In some embodiments, the mass ratio of chitosan to modified cellulose is controlled to be 1:(3~6), and the amount of modified cellulose in the three-dimensional cross-linked network is controlled to prevent excessive filling from blocking the gaps in the three-dimensional cross-linked network and thus affecting the sustained-release function of the antioxidant in the antioxidant composition.
[0034] Optionally, the modified cellulose is shear-resistant cellulose, which can be used as a filler material to fill the three-dimensional cross-linked network constructed by chitosan and the first cross-linking agent. By utilizing the shear resistance of the shear-resistant cellulose, the shell strength of the antioxidant composition can be improved. Therefore, during the preparation of the semiconductive shielding material, even if the antioxidant composition is in a strong shear environment during the mixing process, the shear-resistant cellulose in the shell of the antioxidant composition can ensure the integrity of the three-dimensional cross-linked network constructed by chitosan and the first cross-linking agent, preventing the sudden leakage of the core antioxidant caused by shell breakage, thereby reducing the rate of antioxidant loss. This can slow down the aging rate of the matrix resin of the semiconductive shielding material during the preparation process and long-term service, and extend the service life of the cable.
[0035] Optionally, the shear-resistant cellulose also has temperature resistance. In the process of preparing semiconductive shielding material, the excellent high temperature resistance and shear resistance of shear-resistant cellulose can be utilized. This not only ensures the integrity of the coating structure during high-temperature mixing and prevents the three-dimensional cross-linked network (shell) from breaking, but also ensures that the shell of the three-dimensional cross-linked network in the antioxidant composition is not destroyed by high temperature during the high-temperature extrusion process of the semiconductive shielding material through the high content of shear-resistant cellulose.
[0036] In one example, shear-resistant cellulose includes at least one of cellulose ethers and cellulose esters, for example, cellulose ethers include ethyl cellulose, and cellulose esters include at least one of cellulose acetate propionate and cellulose acetate butyrate.
[0037] The degree of substitution (the degree of substitution of each repeating unit of modified cellulose) affects the compatibility of modified cellulose in hydrophilic systems. For example, when the number of substituents in modified cellulose is relatively high, it is more compatible with organic systems; when the number of substituents in modified cellulose is relatively low, it is more compatible with hydrophilic systems.
[0038] In the embodiments of this application, the epoxy-based hydrophobic crosslinking agent used to construct the three-dimensional crosslinked network can modify the three-dimensional network structure. This not only makes the three-dimensional crosslinked network hydrophobic but also ensures that the antioxidant composition has better shear resistance and temperature resistance. Therefore, the degree of substitution of modified cellulose can be controlled to be 2.4~2.6. At this point, the modified cellulose has good hydrophobicity and can better fill the three-dimensional crosslinked network. Taking ethyl cellulose as an example, its degree of substitution is 2.4~2.6, such as 2.4, 2.5, or 2.6.
[0039] In one embodiment, when the mass ratio of chitosan to antioxidant is 1:(1.5~2.5) (e.g., 1:1.5, 1:2.2 or 1:2.5), the antioxidant composition is uniformly dispersed in the matrix resin, making it less likely for antioxidants to aggregate at a single location. This effectively coordinates the aging rate of different areas of the matrix resin and avoids excessively rapid local aging of the matrix resin.
[0040] Antioxidants include one or more of hindered phenolic antioxidants and phosphite antioxidants. Optionally, antioxidants may include one or more of antioxidants 1010, 1076, 264, 168, and 626. Antioxidants 1010, 1076, and 264 are hindered phenolic primary antioxidants, while antioxidants 168 and 626 are phosphite secondary antioxidants.
[0041] This application also provides a method for preparing an antioxidant composition. Figure 3 A schematic flowchart illustrating the preparation method of the antioxidant composition according to an embodiment of this application is shown. Figure 3 As shown, the preparation method 300 of the antioxidant composition includes steps 301 to 303.
[0042] In step 301, the mixed solution of chitosan and modified cellulose is premixed with the first crosslinking agent under alkaline conditions to obtain a homogeneous composite polysaccharide solution. It should be understood that the mass ratio of chitosan to modified cellulose, and the specific amount of modified cellulose, can be found in the preceding descriptions and will not be repeated here.
[0043] Optionally, the chitosan solution and the modified cellulose solution can be mixed evenly to obtain a mixed solution of chitosan and modified cellulose; then, at the first crosslinking reaction temperature, the first crosslinking agent is added to the mixed solution of chitosan and modified cellulose under alkaline conditions to obtain a homogeneous composite polysaccharide solution.
[0044] When the first crosslinking agent is added to a mixed solution of chitosan and modified cellulose under alkaline conditions at the first crosslinking reaction temperature, it can gradually react with chitosan during the addition process. During the reaction, the amount of chitosan and modified cellulose is relatively large, while the amount of the first crosslinking agent is relatively small. Therefore, in the process of constructing a three-dimensional crosslinked network, modified cellulose can fill the three-dimensional crosslinked network to enhance the shell properties of the network.
[0045] In one example, the chitosan solution can be a glacial acetic acid solution of chitosan with a concentration ranging from 0.5 g / 100 mL to 2.0 g / 100 mL. For example, 0.5 g / 100 mL, 1.0 g / 100 mL, 1.5 g / mL, or 2.0 g / mL. For instance, chitosan can be dissolved in a 2% (w / w) aqueous solution of glacial acetic acid and stirred at room temperature until a clear chitosan solution is obtained. Modified cellulose can also be first dispersed in an organic solvent to form a stable dispersion; for example, ethyl cellulose can be dispersed in isopropanol.
[0046] In one example, the temperature of the first crosslinking reaction is 60°C to 75°C, and the pH value of the alkaline conditions is 7.5 to 8.5. For example, dilute ammonia can be added dropwise to a mixed solution of chitosan and modified cellulose until the pH value of the mixed solution of chitosan and modified cellulose is equal to 8.0, and the mixed solution of chitosan and modified cellulose is heated to 60°C to 75°C, and then the first crosslinking agent is slowly added dropwise.
[0047] In step 302, an antioxidant solution is added to a homogeneous complex polysaccharide solution, and the homogeneous complex polysaccharide solution with added antioxidant is homogenized and emulsified at a first crosslinking reaction temperature to obtain a crosslinking reaction solution.
[0048] In the embodiments of this application, the antioxidant can be dissolved in an organic solvent to obtain an antioxidant solution. The mass ratio of the antioxidant to chitosan in the antioxidant solution and the selection of the antioxidant can be referred to the relevant description above, and will not be repeated here.
[0049] Optionally, the antioxidant solution can be uniformly added dropwise to the homogeneous complex polysaccharide solution so that the three-dimensional network structure can controllably encapsulate the antioxidant, ensuring that the core-shell structure of the subsequently formed antioxidant composition has an appropriate particle size, neither too large nor too small.
[0050] Optionally, the homogenization emulsification is performed at a speed of 500 rpm to 1000 rpm for a duration of 1 h to 3 h, in order to further control the particle size of the core-shell structure of the antioxidant composition.
[0051] In step 303, the crosslinking reaction solution is treated to obtain a core-shell structured antioxidant composition. Here, the crosslinking reaction solution can be cured to obtain a cured mixture, and then the core-shell structured antioxidant composition can be separated from the cured mixture.
[0052] Optionally, the crosslinking reaction solution can be allowed to stand and solidify at room temperature to obtain a solidified mixture. The solidified mixture can then be dialyzed to remove free small molecules contained therein. The dialyzed solidified mixture can then be vacuum dried to obtain a core-shell structured antioxidant composition.
[0053] This application provides a semiconductive shielding material, which may include a matrix resin, conductive carbon black, a second crosslinking agent, an antioxidant composition, and a lubricant. The matrix resin is in the form of 100 parts by weight, the conductive carbon black is in the form of 35 to 65 parts by weight, the second crosslinking agent is in the form of 1 to 2 parts by weight, the antioxidant composition is in the form of 3 to 6 parts by weight, and the lubricant is in the form of 2 to 8 parts by weight.
[0054] In one embodiment, the matrix resin may include at least one of ethylene-butyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-vinyl acetate copolymer.
[0055] In some embodiments, the mass fraction of conductive carbon black can be 40 to 65 parts, for example, 35, 46, 50, 55, 60, or 65 parts. This ensures that the conductive carbon black can form a continuous conductive network within the semiconductive shielding material, thereby better achieving interface equipotentiality and electric field homogenization, and enhancing the shielding function of the semiconductive shielding layer.
[0056] For example, the conductive carbon black has an oil absorption value of 150mL / 100g to 220mL / 100g, a particle size of 30nm to 50nm, and an ash content of <0.1% by mass. In this case, the conductive carbon black can improve the dispersion of the antioxidant composition in the matrix resin without disrupting the conductive pathways of the carbon black, thus alleviating the localized aging weaknesses of the semi-conductive shielding layer caused by the localized large-scale adsorption of the antioxidant composition.
[0057] In some embodiments, the second crosslinking agent may be a peroxide crosslinking agent, such as at least one of dicumyl peroxide and bis-tert-butyl peroxide. The lubricant may be at least one of microcrystalline wax and polyethylene wax.
[0058] In some embodiments, the antioxidant composition added to the semiconductive shielding material of this application is the same as that of this application. Testing revealed that the oxidation induction period of this semiconductive shielding material is 32.4 min to 32.9 min, the decrease in tensile strength before and after aging is less than or equal to 5%, and the decrease in elongation at break before and after aging is 5.2% to 5.4%. Therefore, when the antioxidant composition of this application is added, the semiconductive shielding material exhibits good anti-aging properties.
[0059] It should be noted that the chitosan, first crosslinking agent, modified cellulose and antioxidant involved in the preparation method of the antioxidant composition in the embodiments of this application can be referred to the relevant description of the antioxidant composition in the embodiments of this application, and will not be repeated here.
[0060] This application also provides a method for preparing a semiconductive shielding material. Figure 4 A schematic flowchart illustrating the preparation method of the semiconductive shielding material according to an embodiment of this application is shown. Figure 4 As shown, the preparation method 400 of the semiconductive shielding material includes steps 401 and 402.
[0061] In step 401, the matrix resin, conductive carbon black, lubricant and antioxidant composition are mixed using an internal mixer to obtain a semi-finished product of semi-conductive shielding material.
[0062] Optionally, the matrix resin, conductive carbon black, lubricant and antioxidant composition can be added to a mixer and mixed at 150℃~180℃ for 20min~40min. Then, after single-screw extrusion granulation, a semi-finished product of semi-conductive shielding material can be obtained.
[0063] In step 402, at the second crosslinking reaction temperature, the semi-finished product of the semiconductive shielding material is treated with a second crosslinking agent to obtain the semiconductive shielding material.
[0064] The semi-finished semi-conductive shielding material is cross-linked with a second cross-linking agent at 50℃~80℃ for 1h~4h to obtain the semi-conductive shielding material.
[0065] It should be noted that the matrix resin, conductive carbon black, lubricant, antioxidant composition and second crosslinking agent involved in the preparation method of the semiconductive shielding material in the embodiments of this application can be referred to the relevant description of the semiconductive shielding material in the embodiments of this application, and will not be repeated here.
[0066] To clearly explain the role of the antioxidant composition in the semiconductive shielding material according to the embodiments of this application, the preparation process of the antioxidant composition and the preparation process of the semiconductive shielding material are described below with reference to specific embodiments and comparative examples. In the following embodiments, the preparation process of the antioxidant composition is directly integrated into the preparation process of the semiconductive shielding material, and the antioxidant composition is referred to as an antioxidant sustained-release capsule.
[0067] Example 1 The main raw materials and their mass proportions in the preparation method of the antioxidant sustained-release capsules of this application embodiment include: 10 parts of chitosan, 30 parts of ethyl cellulose (the mass ratio of chitosan to ethyl cellulose is 1:3), 8 parts of epoxidized sunflower seed oil (epoxidized sunflower seed oil to chitosan = 0.8:1), 15 parts of antioxidant 1010 and 5 parts of antioxidant 626. The specific steps include steps one to four, and the degree of substitution of ethyl cellulose is 2.6.
[0068] In step one, 10 parts of chitosan were dissolved in 100 parts of glacial acetic acid aqueous solution with a mass concentration of 2wt%, and stirred at room temperature for 2 hours to obtain a transparent chitosan solution; 30 parts of ethyl cellulose were dispersed in 60 parts of isopropanol, stirred for 40 minutes, and then slowly added to the transparent chitosan solution to obtain a mixed solution of chitosan and modified cellulose.
[0069] In step two, dilute ammonia water is added dropwise to the mixed solution of chitosan and modified cellulose to adjust the pH value of the mixed solution to 7.5, and the temperature is raised to 75°C. Eight parts of epoxidized sunflower seed oil are then slowly added dropwise to obtain a homogeneous complex polysaccharide solution.
[0070] In step three, 15 parts of antioxidant 1010 and 5 parts of antioxidant 626 are dissolved together in 30 parts of dichloromethane, and then added dropwise to a homogeneous complex polysaccharide solution at a uniform rate. The mixture is then homogenized and emulsified at 500 rpm for 1 hour to complete the cross-linking reaction and obtain the cross-linking reaction solution.
[0071] In step four, the cross-linking reaction solution is allowed to stand and solidify at room temperature for 2 hours, then dialyzed for 24 hours to remove free small molecules, and finally vacuum dried at 45°C to obtain antioxidant sustained-release capsules.
[0072] The main raw materials and their mass fractions in the preparation method of the semiconductive shielding material in this application embodiment include: 100 parts of ethylene-ethyl acrylate copolymer, 65 parts of conductive carbon black VXC500, 6 parts of polyethylene wax, 5 parts of antioxidant sustained-release capsules (Example 1), and 2 parts of dicumyl peroxide.
[0073] The preparation method of the semiconductive shielding material includes: adding 100 parts of ethylene-ethyl acrylate copolymer, 65 parts of conductive carbon black VXC500, 6 parts of polyethylene wax and 5 parts of antioxidant sustained-release capsules into a mixer, mixing at 180°C for 20 minutes, and then extruding and granulating by a single screw to obtain a semi-finished product of the semiconductive shielding material; after absorbing the semi-finished product of the semiconductive shielding material with 2 parts of dicumyl peroxide at 50°C for 4 hours, the semiconductive shielding material is obtained.
[0074] Example 2 The main raw materials and their mass proportions in the preparation method of the antioxidant sustained-release capsules of this application embodiment include: 10 parts chitosan, 20 parts ethyl cellulose, 40 parts cellulose acetate butyrate (the mass ratio of chitosan to ethyl cellulose and cellulose acetate butyrate is 1:2:4), 9 parts 1,6-hexanediol diglycidyl ether (1,6-hexanediol diglycidyl ether: chitosan = 0.9:1), 20 parts antioxidant 1076 and 5 parts antioxidant 168. The specific steps include steps one to four. The degree of substitution of ethyl cellulose is 2.4 and the degree of substitution of cellulose acetate butyrate is 2.5.
[0075] In step one, 10 parts of chitosan were dissolved in 200 parts of glacial acetic acid aqueous solution with a mass concentration of 2wt%, and stirred at room temperature for 2 hours to obtain a transparent chitosan solution; 20 parts of ethyl cellulose and 40 parts of cellulose acetate butyrate were dispersed in 80 parts of isopropanol, stirred for 50 minutes, and then slowly added to the transparent chitosan solution to obtain a mixed solution of chitosan and modified cellulose.
[0076] In step two, dilute ammonia water is added dropwise to the mixed solution of chitosan and modified cellulose to adjust the pH value of the mixed solution to 8.5, and the temperature is raised to 60°C. Nine parts of 1,6-hexanediol diglycidyl ether are slowly added dropwise to obtain a homogeneous complex polysaccharide solution.
[0077] In step three, 20 parts of antioxidant 1076 and 5 parts of antioxidant 168 are dissolved together in 45 parts of dichloromethane, and then added dropwise to a homogeneous complex polysaccharide solution at a uniform rate. The mixture is then homogenized and emulsified at 750 rpm for 3 hours to complete the cross-linking reaction and obtain the cross-linking reaction solution.
[0078] In step four, the cross-linking reaction solution is allowed to stand and solidify at room temperature for 2 hours, then dialyzed for 24 hours to remove free small molecules, and finally vacuum dried at 45°C to obtain antioxidant sustained-release capsules.
[0079] The main raw materials and their mass fractions in the preparation method of the semiconductive shielding material in this application embodiment include: 100 parts of ethylene-vinyl acetate copolymer, 35 parts of conductive carbon black VXC500, 2 parts of polyethylene wax, 4 parts of antioxidant sustained-release capsules (Example 2), and 1 part of dicumyl peroxide.
[0080] The preparation method of the semi-conductive shielding material includes: adding 100 parts of ethylene-vinyl acetate copolymer, 35 parts of conductive carbon black VXC500, 2 parts of polyethylene wax and 4 parts of antioxidant slow-release capsules into a mixer, mixing at 170°C for 35 minutes, and then extruding and granulating by a single screw to obtain a semi-finished product of the semi-conductive shielding material; and then absorbing the semi-finished product of the semi-conductive shielding material with 1 part of dicumyl peroxide at 80°C for 1 hour to obtain the semi-conductive shielding material.
[0081] Example 3 The main raw materials and their mass proportions for preparing the antioxidant sustained-release capsules according to this application include: 10 parts chitosan, 50 parts cellulose acetate propionate (the mass ratio of chitosan to cellulose acetate propionate is 1:5), 6 parts 1,4-butanediol diglycidyl ether (1,4-butanediol diglycidyl ether: chitosan = 0.6:1), and 15 parts antioxidant 264. The specific steps include steps one to four, and the degree of substitution of cellulose acetate propionate is 2.4.
[0082] In step one, 10 parts of chitosan were dissolved in 50 parts of glacial acetic acid aqueous solution with a mass concentration of 2wt%, and stirred at room temperature for 2 hours to obtain a transparent chitosan solution; 50 parts of cellulose acetate propionate were dispersed in 60 parts of isopropanol, stirred for 350 minutes, and then slowly added to the transparent chitosan solution to obtain a mixed solution of chitosan and modified cellulose.
[0083] In step two, dilute ammonia water is added dropwise to the mixed solution of chitosan and modified cellulose to adjust the pH value of the mixed solution to 8.0, and the temperature is raised to 70°C. Six parts of 1,4-butanediol diglycidyl ether are slowly added dropwise to obtain a homogeneous complex polysaccharide solution.
[0084] In step three, 15 parts of antioxidant 264 were dissolved in 20 parts of dichloromethane and added dropwise to a homogeneous complex polysaccharide solution at a uniform rate. The mixture was then homogenized and emulsified at 850 rpm for 3 hours to complete the cross-linking reaction and obtain the cross-linking reaction solution.
[0085] In step four, the cross-linking reaction solution is allowed to stand and solidify at room temperature for 2 hours, then dialyzed for 24 hours to remove free small molecules, and finally vacuum dried at 45°C to obtain antioxidant sustained-release capsules.
[0086] The main raw materials and their mass fractions in the preparation method of the semiconductive shielding material of this application embodiment include: 40 parts of ethylene-ethyl acrylate copolymer, 60 parts of ethylene-ethyl acrylate copolymer, 46 parts of conductive carbon black VXC500, 6 parts of polyethylene wax, 6 parts of antioxidant sustained-release capsules (Example 3), 1 part of dicumyl peroxide, and 0.5 parts of bis-tert-butyl peroxide.
[0087] The preparation method of this semi-conductive shielding material includes: adding 40 parts of ethylene-ethyl acrylate copolymer, 60 parts of ethylene-ethyl acrylate copolymer, 46 parts of conductive carbon black VXC500, 6 parts of polyethylene wax and 6 parts of antioxidant sustained-release capsules into a mixer, mixing at 150°C for 40 minutes, and then granulating by single-screw extrusion to obtain a semi-finished product of the semi-conductive shielding material; after absorbing the semi-finished product of the semi-conductive shielding material with 1 part of dicumyl peroxide and 0.5 parts of di-tert-butyl peroxide at 70°C for 2 hours, the semi-conductive shielding material is obtained.
[0088] Example 4 Compared with Example 3, the preparation method of the antioxidant sustained-release capsule in this application embodiment is different in that the antioxidant includes 11 parts of antioxidant 264 and 7 parts of antioxidant 626.
[0089] Compared with Example 3, the difference in the preparation method of the semiconductive shielding material in this application is that the antioxidant sustained-release capsules used are the antioxidant sustained-release capsules prepared in Example 4.
[0090] Example 5 Compared with Example 3, the preparation method of the antioxidant sustained-release capsule in this application differs in that the antioxidant includes 13 parts of antioxidant 1076 and 7 parts of antioxidant 264.
[0091] Compared with Example 3, the difference in the preparation method of the semiconductive shielding material in this application is that the antioxidant sustained-release capsules used are the antioxidant sustained-release capsules prepared in Example 5.
[0092] Example 6 The main raw materials and their mass fractions in the preparation method of the antioxidant sustained-release capsules of this application embodiment include: 10 parts of chitosan, 40 parts of ethyl cellulose (the mass ratio of chitosan to ethyl cellulose is 1:4), 8 parts of epoxidized soybean oil (epoxidized soybean oil to chitosan = 0.8:1), and 22 parts of antioxidant 1010. The specific steps include steps one to four, and the degree of substitution of ethyl cellulose is 2.4.
[0093] In step one, 10 parts of chitosan were dissolved in 100 parts of glacial acetic acid aqueous solution with a mass concentration of 2wt%, and stirred at room temperature for 2 hours to obtain a transparent chitosan solution; 40 parts of ethyl cellulose were dispersed in 60 parts of isopropanol, stirred for 40 minutes, and then slowly added to the transparent chitosan solution to obtain a mixed solution of chitosan and modified cellulose.
[0094] In step two, dilute ammonia water is added dropwise to the mixed solution of chitosan and modified cellulose to adjust the pH value of the mixed solution of chitosan and modified cellulose to 8.0, and the temperature is raised to 70°C. Eight parts of epoxidized soybean oil are then slowly added dropwise to obtain a homogeneous complex polysaccharide solution.
[0095] In step three, 22 parts of antioxidant 1010 were dissolved in 30 parts of dichloromethane and added dropwise to a homogeneous complex polysaccharide solution at a uniform rate. The mixture was then homogenized and emulsified at 1000 rpm for 3 hours to complete the cross-linking reaction and obtain the cross-linking reaction solution.
[0096] In step four, the cross-linking reaction solution is allowed to stand and solidify at room temperature for 2 hours, then dialyzed for 24 hours to remove free small molecules, and finally vacuum dried at 45°C to obtain antioxidant sustained-release capsules.
[0097] Antioxidant content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant content in the antioxidant sustained-release capsules was analyzed by HPLC: 19.1%.
[0098] The main raw materials and their mass fractions in the preparation method of the semiconductive shielding material in this application embodiment include: 100 parts of ethylene-butyl acrylate, 45 parts of conductive carbon black VXC500, 3 parts of microcrystalline wax, 3 parts of antioxidant sustained-release capsules (Example 6), and 1.5 parts of bis-tert-butylperoxyisopropylbenzene.
[0099] The preparation method of the semi-conductive shielding material includes: adding 100 parts of ethylene-butyl acrylate copolymer, 45 parts of conductive carbon black VXC500, 3 parts of microcrystalline wax and 3 parts of antioxidant sustained-release capsules into a mixer, mixing at 150°C for 30 minutes, and then granulating by single-screw extrusion to obtain a semi-finished product of the semi-conductive shielding material; and then absorbing the semi-finished product of the semi-conductive shielding material with 1.5 parts of di-tert-butyl peroxide isopropylbenzene at 60°C for 2 hours to obtain the semi-conductive shielding material.
[0100] Example 7 Compared with Example 6, the main raw materials and processes for preparing the antioxidant sustained-release capsules in this application are the same, except that: 6 parts of epoxidized soybean oil (epoxidized soybean oil: chitosan = 0.6:1).
[0101] Antioxidant mass content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant mass content in the antioxidant sustained-release capsules was analyzed by HPLC: 18.9%.
[0102] Compared with Example 6, the difference in the preparation method of the semiconductive shielding material in this application is that the antioxidant sustained-release capsules used are the antioxidant sustained-release capsules prepared in Example 7.
[0103] Example 8 Compared with Example 6, the main raw materials and processes for preparing the antioxidant sustained-release capsules in this application are the same, except that: 10 parts of epoxidized soybean oil (epoxidized soybean oil: chitosan = 1:1).
[0104] Antioxidant mass content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant mass content in the antioxidant sustained-release capsules was analyzed by HPLC: 18.7%.
[0105] Compared with Example 6, the difference in the preparation method of the semiconductive shielding material in this application is that the antioxidant sustained-release capsules used are the antioxidant sustained-release capsules prepared in Example 8.
[0106] Comparative Example 1 Compared with Example 6, the preparation method of the antioxidant sustained-release capsules in Comparative Example 1 uses the same main raw materials and processes, but differs in that: the amount of ethyl cellulose is 20 parts (the mass ratio of chitosan to ethyl cellulose is 1:2), and the amount of epoxidized soybean oil is 8 parts (epoxidized soybean oil to chitosan = 0.8:1).
[0107] Antioxidant mass content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant mass content in the antioxidant sustained-release capsules was analyzed by HPLC: 20.7%.
[0108] Compared with Example 6, the difference in the preparation method of the semiconductive shielding material in Comparative Example 1 is that the antioxidant sustained-release capsules used are the same as those prepared in Comparative Example 1.
[0109] Comparative Example 2 Compared with Example 6, the preparation method of the antioxidant sustained-release capsules in Comparative Example 2 has the same main raw materials and the same process, except that: 4 parts of epoxidized soybean oil (epoxidized soybean oil: chitosan = 0.4:1).
[0110] Antioxidant mass content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant mass content in the antioxidant sustained-release capsules was analyzed by HPLC: 16.7%.
[0111] Compared with Example 6, the difference in the preparation method of the semiconductive shielding material in Comparative Example 2 is that the antioxidant sustained-release capsules used are the same as those prepared in Comparative Example 2.
[0112] Comparative Example 3 Compared with Example 6, the preparation method of the antioxidant sustained-release capsules in Comparative Example 3 has the same main raw materials and the same process, except that: 15 parts of epoxidized soybean oil (epoxidized soybean oil: chitosan = 1.5:1).
[0113] Antioxidant mass content determination: After washing and drying, the antioxidant sustained-release capsules were added to a mixed solvent of dichloromethane and tetrahydrofuran, and heated under reflux for 2 hours in a sealed container. The polysaccharide shell of the antioxidant sustained-release capsules swelled and ruptured, and all the antioxidants in the core were fully dissolved. The polysaccharide solid residue was removed by filtration, and the antioxidant mass content in the antioxidant sustained-release capsules was analyzed by HPLC: 19.2%.
[0114] Compared with Example 6, the difference in the preparation method of the semiconductive shielding material of Comparative Example 3 is that the antioxidant sustained-release capsules used are the same as those prepared in Comparative Example 3.
[0115] Comparative Example 4 Compared with Example 6, the preparation method of the semiconductive shielding material in Comparative Example 4 is different in that antioxidant sustained-release capsules are not used, but antioxidant 1010 is used directly, with a quantity of 0.573 parts (the mass is obtained by proportional conversion of the effective antioxidant content in the antioxidant sustained-release capsules).
[0116] It should be noted that the degree of substitution of ethyl cellulose used in Examples 6 to 8 and Comparative Examples 1 to 3 of this application is 2.4.
[0117] The oxidation induction period and aging tests were conducted on the semiconductive shielding materials of Examples 6 to 8 and Comparative Examples 1 to 4. The oxidation induction period test conditions were: test temperature 220℃, standard GB / T19466.3-2009; the aging test conditions were: aging in a forced-air oven at 150℃ for 30 days. After aging, the samples were removed and their tensile strength and elongation at break were tested. The test results are shown in Table 1.
[0118] Table 1 Performance test results of semiconductive shielding material
[0119] Analysis of Table 1 shows that when the mass ratio of epoxidized soybean oil to chitosan is (0.6~1):1, the oxidation induction period can reach 32.4 min or more, and the elongation at break and tensile strength before and after aging do not change much.
[0120] Compared to the examples and comparative examples using antioxidant sustained-release capsules, Comparative Example 4 had a shorter oxidation induction period (only 15.1 min), and its elongation at break and tensile strength changed significantly before and after aging. Furthermore, its elongation at break and tensile strength were relatively low before aging. Therefore, compared to using small-molecule antioxidants, the semiconductive shielding material using antioxidant sustained-release capsules exhibits better anti-aging performance.
[0121] If the mass ratio of epoxidized soybean oil to chitosan is too high (such as 1.5:1 in Example 3), the three-dimensional cross-linked network formed by the high degree of cross-linking between chitosan and epoxidized soybean oil will be relatively dense. Although the mass content of antioxidant is relatively high (such as 19.2%), its oxidation induction period is only 16.5 min, and the elongation at break and tensile strength before and after aging change greatly. The reason for this is that the overly dense three-dimensional cross-linked network inhibits the release of antioxidant 1010, resulting in poor performance.
[0122] If the mass ratio of epoxidized soybean oil to chitosan is (0.6~1):1, but the amount of ethyl cellulose added is relatively low (e.g., in Comparative Example 1, the mass ratio of chitosan to ethyl cellulose is 1:2), although the mass ratio of epoxidized soybean oil to chitosan ensures a relatively high antioxidant content in the antioxidant sustained-release capsules (e.g., the antioxidant content in Comparative Example 1 is 20.7%), the low mass content of ethyl cellulose results in insufficient filling of the three-dimensional cross-linked network. This leads to low shear strength and temperature resistance of the three-dimensional cross-linked network. Therefore, when the mass content of ethyl cellulose is low, taking Comparative Example 1 as an example, its oxidation induction period is only 15.7 min, and the elongation at break and tensile strength before and after aging change significantly.
[0123] The antioxidant composition of this application embodiment possesses a dual adaptive sustained-release mechanism based on heat and pH, exhibiting outstanding long-term protective capabilities. This is manifested in the following ways: the sustained-release antioxidant capsule achieves controlled release through the cross-linked polysaccharide gradient microporous structure of the core-shell capsule. During normal cable operation at 90°C, the molecular chains contract and the micropores narrow, resulting in a continuous, minute release of the antioxidant. At the high extrusion temperature of 120–160°C, the chain segments expand, releasing sufficient amounts in a short time to inhibit processing degradation. Simultaneously, the chitosan retains free amino groups, automatically increasing the release rate in response to acidic degradation products generated by thermal aging. This overcomes the shortcomings of traditional sustained-release systems that rely solely on high-temperature melting for single-time release, lack continuous replenishment at low temperatures, and cannot match the aging rhythm of materials, thus meeting the 30-year long-term antioxidant requirements of cables.
[0124] In the antioxidant composition of this application embodiment, crosslinking and hydrophobic modification with chitosan can be completed in one step using an epoxy-based hydrophobic crosslinking agent. The water absorption rate is extremely low, effectively suppressing cable water tree defects. This is manifested by: using an epoxy-based crosslinking agent to undergo a ring-opening reaction with the amino and alcohol hydroxyl groups of chitosan, covalently grafting long alkyl hydrophobic chains, and compounding with a high proportion of modified cellulose with a high degree of substitution to synergistically improve hydrophobicity. This solves the problems of traditional polysaccharide carriers being severely hydrophilic, easily generating water trees under high voltage electric fields, and reducing cable breakdown strength, making it suitable for long-term humid and high-voltage service conditions of cables.
[0125] In the antioxidant composition of this application embodiment, the shell layer composed of chitosan, a first crosslinking agent, and shear-resistant cellulose exhibits excellent toughness, high capsule encapsulation efficiency, and stable structure during processing. Specifically, by controlling the mass ratio of chitosan to shear-resistant cellulose, shear-resistant cellulose (such as ethyl cellulose) is interpenetrated within the chitosan crosslinking network to form an interpenetrating toughening skeleton, constructing a gradient pore structure with a loose inner layer and a dense outer layer. This ensures high capsule integrity under high temperature and strong shear extrusion conditions, effectively preventing premature antioxidant leakage and surface blooming failure, and addressing the shortcomings of single polysaccharide shells, such as high brittleness, easy breakage, and poor drug loading stability.
[0126] Furthermore, by controlling the ratio of chitosan to epoxy-based hydrophobic crosslinking agents (such as epoxidized soybean oil), and precisely regulating the crosslinking density, the composite shell exhibits excellent toughness, high capsule encapsulation efficiency, and stable structure during processing. The density of the crosslinking network is precisely controlled by adjusting the amount of epoxidized soybean oil used, which, combined with ethyl cellulose, forms an interpenetrating toughening framework, creating a gradient porous structure with a loose inner layer and a dense outer layer. Insufficient crosslinking agent results in a loose network, making the capsule prone to breakage and leakage; excessive crosslinking agent leads to an overly dense network and insufficient long-term sustained-release supply.
[0127] As can be seen, the core technical concept of the antioxidant composition in this application is to address the core pain points of semiconductive shielding materials, namely, "easy loss of antioxidants during processing and insufficient antioxidant durability during long-term service." It constructs a synergistic antioxidant slow-release system that combines "a core-shell structure with gradient dense channels that slowly release antioxidants when the cable is in service at 90°C; and moderate expansion of the channels during extrusion at 110°C~160°C to release antioxidants, achieving thermal response slow release" with "protonation of chitosan amino groups, significantly weakening hydrogen bonding between molecular chains, stretching polysaccharide chains, significantly increasing gradient micropore size, and automatically improving the antioxidant release rate through pH response slow release capability." This achieves the triple goals of "processing anti-aging, long-term anti-aging, and no impact on core performance."
[0128] In the description of the above embodiments, specific features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments or examples.
[0129] The basic principles of this application have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in this application are merely examples and not limitations, and should not be considered as essential features of each embodiment of this application. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the application to the necessity of employing the aforementioned specific details for implementation.
[0130] The above description has been given for purposes of illustration and description. Furthermore, this description is not intended to limit the embodiments of this application to the forms disclosed herein. Although numerous exemplary aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, alterations, additions, and sub-combinations thereof.
Claims
1. A semiconductive shielding material, characterized in that, Includes a matrix resin, conductive carbon black, a second crosslinking agent, an antioxidant composition, and a lubricant; The matrix resin is 100 parts by mass, the conductive carbon black is 35 to 65 parts by mass, the second crosslinking agent is 1 to 2 parts by mass, the antioxidant composition is 3 to 6 parts by mass, and the lubricant is 2 to 8 parts by mass. The antioxidant composition has a core-shell structure and includes a shell layer and a core layer. The shell layer includes chitosan, a first crosslinking agent, and modified cellulose. The core layer includes an antioxidant. The first crosslinking agent includes an epoxy-based hydrophobic crosslinking agent. Wherein, the mass ratio of the first crosslinking agent to the chitosan is (0.6~1):1, and the mass ratio of the chitosan to the modified cellulose is 1:(3~6); The modified cellulose is shear-resistant cellulose, which includes at least one of cellulose ether and cellulose ester, and the epoxy hydrophobic crosslinking agent includes at least one of epoxidized soybean oil and epoxidized sunflower seed oil.
2. The semiconductive shielding material according to claim 1, characterized in that, The epoxy-based hydrophobic crosslinking agent is a polyepoxy-based hydrophobic crosslinking agent.
3. The semiconductive shielding material according to claim 1, characterized in that, The cellulose ether includes ethyl cellulose; and / or, The cellulose ester includes at least one of cellulose acetate propionate and cellulose acetate butyrate.
4. The semiconductive shielding material according to claim 1, characterized in that, The mass ratio of chitosan to antioxidant is 1:(1.5~2.5).
5. The semiconductive shielding material according to claim 1, characterized in that, The antioxidants include one or more of hindered phenolic antioxidants and phosphite antioxidants.
6. The semiconductive shielding material according to claim 1, characterized in that, The core-shell structure has a size of 0.5 μm to 2.5 μm.
7. The semiconductive shielding material according to any one of claims 1 to 6, characterized in that, The matrix resin includes at least one of ethylene-butyl acrylate copolymer, ethylene-ethyl acrylate copolymer and ethylene-vinyl acetate copolymer, and the second crosslinking agent is a peroxy crosslinking agent; The conductive carbon black has an oil absorption value of 150mL / 100g to 220mL / 100g, a particle size of 30nm to 50nm, an ash content of <0.1% by mass, and the lubricant is at least one of microcrystalline wax and polyethylene wax.
8. The semiconductive shielding material according to any one of claims 1 to 6, characterized in that, The oxidation induction period of the semiconductive shielding material is 32.4 min to 32.9 min, the tensile strength reduction rate of the semiconductive shielding material before and after aging is less than or equal to 5%, and the elongation at break reduction rate of the semiconductive shielding material before and after aging is 5.2% to 5.4%.
9. A method for preparing the semiconductive shielding material according to any one of claims 1 to 8, characterized in that, include: A semi-finished semi-conductive shielding material is obtained by mixing a matrix resin, conductive carbon black, lubricant and antioxidant composition using an internal mixer. The second crosslinking agent crosslinks with the semi-finished product of the semiconductive shielding material at the second crosslinking reaction temperature to obtain the semiconductive shielding material; The antioxidant composition has a core-shell structure and includes a shell layer and a core layer. The shell layer includes chitosan, a first crosslinking agent, and modified cellulose. The core layer includes an antioxidant. The first crosslinking agent includes an epoxy-based hydrophobic crosslinking agent. Wherein, the mass ratio of the first crosslinking agent to the chitosan is (0.6~1):1, and the mass ratio of the chitosan to the modified cellulose is 1:(3~6); The modified cellulose is shear-resistant cellulose, which includes at least one of cellulose ether and cellulose ester, and the epoxy hydrophobic crosslinking agent includes at least one of epoxidized soybean oil and epoxidized sunflower seed oil.
10. The method for preparing the semiconductive shielding material according to claim 9, characterized in that, The mixing temperature is 150℃~180℃, and the mixing time is 20min~40min; The second crosslinking reaction temperature is 50℃~80℃, and the crosslinking time between the second crosslinking agent and the semi-finished product of the semiconductive shielding material is 1h~4h.
11. A cable, characterized in that, It includes a semi-conductive shielding layer, wherein the semi-conductive shielding layer is the semi-conductive shielding material according to any one of claims 1 to 8.