A method for preparing an antibacterial polypropylene material
By modifying nano-zinc oxide and forming chemical bonds with quaternized chitosan, the problems of insufficient antibacterial effect and poor mechanical properties of antibacterial polypropylene materials are solved, achieving a synergistic improvement in both long-lasting antibacterial properties and excellent mechanical properties.
Patent Information
- Application Number
- CN202611332364.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing antibacterial polypropylene materials are insufficient in terms of antibacterial effect and durability, and also have poor mechanical properties.
By modifying nano-zinc oxide, quaternary ammonium salt groups are introduced, and chemical bonds are formed with components such as quaternized chitosan, compatibilizer, antioxidant, and toughening agent during melt blending. This improves the dispersibility and interfacial compatibility of nano-zinc oxide in the polypropylene matrix, forming a synergistic antibacterial system.
It achieves durable antibacterial effect and excellent mechanical properties, avoids the migration and loss of antibacterial components, improves the toughness and antibacterial durability of the material, and maintains the mechanical strength of the material.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polypropylene materials technology, specifically to a method for preparing an antibacterial polypropylene material. Background Technology
[0002] Polypropylene (PP) is a semi-crystalline thermoplastic resin that is abundant, inexpensive, and easy to process and mold. It possesses excellent acid and alkali resistance, heat resistance, electrical insulation, mechanical properties, and processing performance, and is widely used in the automotive industry, home appliances, food packaging, and medical and hygiene products. However, polypropylene plastic itself does not have antibacterial properties and is prone to the growth of bacteria, mold, and other microorganisms during use, posing potential health and safety hazards. In today's society, people are increasingly concerned about hygiene; therefore, developing polypropylene materials with excellent antibacterial effects is of significant practical importance for public health and environmental hygiene.
[0003] Numerous reports on antibacterial polypropylene materials exist in the prior art. Chinese patent application CN121519191A discloses an antibacterial polypropylene fiber and its preparation method. This antibacterial polypropylene fiber comprises polypropylene, modified chitosan, zinc oxide, toughening agent, lubricant, and antioxidant. It is prepared by melt blending and exhibits good antibacterial and mechanical properties. However, zinc oxide has poor dispersibility in the matrix, and the antibacterial components are prone to migration and loss after long-term use. Chinese patent application CN122278058A discloses an antibacterial polypropylene material and its preparation method. This antibacterial polypropylene material is prepared by melt blending polypropylene, inorganic filler, hydrated calcium silicate, antibacterial agent, nucleating agent, antioxidant, and dispersant. The hydrated calcium silicate and antibacterial agent are only physically mixed, lacking chemical bonding, resulting in limited synergistic antibacterial effect. Furthermore, the poor dispersibility of the inorganic filler affects the mechanical properties of the polypropylene material. Chinese patent application CN103059405A discloses an antibacterial polypropylene plastic, comprising polypropylene and a composite antibacterial agent. The composite antibacterial agent is composed of cypress oil, chitosan, nano-titanium dioxide, nano-zeolite, polyhexamethylene guanidine phosphate, and N-(trichloromethylthio)phthalimide. This antibacterial polypropylene plastic has a strong effect of inhibiting bacteria, killing bacteria, and preventing mold. However, the antibacterial agent has too many components, a complex formula, poor compatibility, and affects mechanical strength. In addition, cypress oil has poor thermal stability and is easy to decompose and fail.
[0004] Therefore, it is of great significance to provide a polypropylene material with excellent antibacterial effect, long-lasting antibacterial effect and excellent mechanical properties.
[0005] Summary of the Invention (a) Technical problems to be solved To address the shortcomings of existing technologies, this invention provides a method for preparing antibacterial polypropylene materials, which solves the problems of poor antibacterial effect and insufficient antibacterial durability of polypropylene materials.
[0006] (II) Technical Solution To achieve the above objectives, this invention discloses a method for preparing an antibacterial polypropylene material, comprising the following steps: Step 1: Disperse nano zinc oxide in dichloromethane using ultrasonication at 500W for 60 minutes. After uniform dispersion, add 4-dimethylaminopyridine (DMAP) and triethylamine (Et3N) and stir until homogeneous. Then, slowly add 4-bromomethylbenzoyl chloride to initiate the reaction. After the reaction is complete, filter the mixture and wash it successively with anhydrous ethanol and deionized water. Finally, vacuum dry the mixture at 60℃ for 12 hours to obtain modified nano zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline are stirred and mixed, heated, and reacted. After the reaction is completed, the mixture is filtered, washed with acetone and carbon tetrachloride, and dried under vacuum at 60°C for 12 hours to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add polypropylene resin, quaternary ammonium salt modified zinc oxide, compatibilizer, quaternized chitosan, antioxidant, toughening agent, lubricant, and initiator to a high-speed mixer, mix evenly, melt-blend in a twin-screw extruder, extrude and granulate, and cool to obtain antibacterial polypropylene material.
[0007] Preferably, in step one, the mass ratio of nano zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:(800~1200):(1~5):(12~25):(16~24).
[0008] Preferably, the reaction temperature in step one is 25~40℃, and the reaction time is 12~18h.
[0009] Preferably, in step two, the mass ratio of acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline is (1000~1400):100:(30~50).
[0010] Preferably, the reaction temperature in step two is 50~60℃, and the reaction time is 24~36h.
[0011] Preferably, in step three, the mass ratio of polypropylene resin, quaternary ammonium salt modified zinc oxide, compatibilizer, quaternized chitosan, antioxidant, toughening agent, lubricant, and initiator is (70~90):(3~8):(15~24):(1~3):(0.3~0.5):(5~9):(0.2~0.8):(0.1~0.2).
[0012] Preferably, in step three, the high-speed mixer operates at a speed of 800-1000 r / min, and the mixing time is 20-40 min. During the melt blending process, the screw speed of the twin-screw extruder is 200-240 r / min. The twin-screw extruder is configured with five temperature zones according to the material's forward direction, with temperatures of 165-180℃, 185-200℃, 205-220℃, 195-210℃, and 180-195℃, respectively.
[0013] Preferably, the quaternized chitosan in step three is glycidyltriethylammonium chloride-modified chitosan.
[0014] Preferably, the preparation method of the glycidyltriethylammonium chloride modified chitosan includes the following steps: drying chitosan in a vacuum drying oven at 60°C for 12 hours, dispersing the dried chitosan in isopropanol to swell, adding 30wt% sodium hydroxide solution for alkalization, and then adding glycidyltriethylammonium chloride, wherein the mass ratio of dried chitosan, isopropanol, 30wt% sodium hydroxide solution, and glycidyltriethylammonium chloride is 100:(800~1200):(200~320):(120~250), reacting at 60~75°C for 12~24 hours, after the reaction is completed, adjusting the pH of the system to neutral with dilute hydrochloric acid, dialysis to remove small molecule salts, and drying to obtain glycidyltriethylammonium chloride modified chitosan.
[0015] Preferably, the compatibilizer in step three is maleic anhydride-grafted polypropylene.
[0016] Preferably, the antioxidant in step three is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.
[0017] Preferably, the toughening agent in step three is POE-g-MAH.
[0018] Preferably, the lubricant in step three is zinc stearate.
[0019] Preferably, the initiator in step three is dicumyl peroxide.
[0020] (iii) Beneficial technical effects
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) In this invention, 4-bromomethylbenzoyl chloride is first used to modify nano-zinc oxide. The acyl chloride on 4-bromomethylbenzoyl chloride reacts with the hydroxyl group on nano-zinc oxide, introducing bromine atoms and phenyl groups onto the surface of nano-zinc oxide, giving the surface of nano-zinc oxide active sites that can chemically bond with quaternized chitosan, thus obtaining modified zinc oxide. The modified zinc oxide undergoes a quaternization reaction with N,N-dimethyl-4-vinylaniline to obtain quaternary ammonium salt modified zinc oxide, introducing quaternary ammonium salt and vinyl groups onto the surface of nano-zinc oxide. Modification of nano-zinc oxide effectively avoids agglomeration, allowing it to be uniformly dispersed in the matrix and improving the mechanical properties of the matrix. Polypropylene resin, quaternary ammonium salt modified zinc oxide, compatibilizer, quaternized chitosan, antioxidant, toughening agent, lubricant, and initiator are mixed, melt-blended, extruded and granulated, and cooled to obtain antibacterial polypropylene material. During melt extrusion, under the initiation of dicumyl peroxide, quaternary ammonium salt modified zinc oxide can undergo free radical grafting with polypropylene and maleic anhydride-grafted polypropylene, which significantly improves the interfacial compatibility of nano zinc oxide in the polypropylene matrix, improves the problem of inorganic particle agglomeration, and reduces the deterioration of the mechanical properties of the material by the filler.
[0022] (2) The nano-zinc oxide in this invention possesses excellent antibacterial and mechanical properties. Nano-zinc oxide releases Zn... 2+ Ions disrupt bacterial cell membranes. Under light, electrons in the valence band of nano-zinc oxide can be excited to the conduction band, forming positively charged holes that can generate reactive oxygen species that kill bacteria. Under non-light conditions, free zinc ions in zinc oxide, upon contact with bacteria, can inactivate bacterial proteases, thus killing the bacteria. Introducing quaternary ammonium salts onto the surface of nano-zinc oxide allows the cations on the quaternary ammonium salts to adsorb onto the negatively charged bacterial cell membranes, thereby altering the permeability of the bacterial cell wall, causing a charge imbalance in the cell membrane, and effectively killing the bacteria. Organic and inorganic antibacterial components work synergistically to exhibit excellent antibacterial properties. Chitosan itself has excellent antibacterial efficacy. Quaternary ammonium salt modification of chitosan effectively prevents its aggregation. Simultaneously, the positively charged quaternary ammonium groups of quaternized chitosan adsorb onto the negatively charged bacterial surface through electrostatic interactions, disrupting the cell membrane structure. The two antibacterial agents work synergistically to give polypropylene materials excellent antibacterial properties. By chemically bonding the antibacterial components into the polymer matrix, the defects of easy migration and loss of antibacterial agents in physical blending systems are avoided, and the slow release and long-lasting antibacterial effect of the antibacterial components are achieved.
[0023] (3) In this invention, maleic anhydride-grafted polypropylene is used as a compatibilizer, and its anhydride groups can react with the active groups of quaternized chitosan. POE-g-MAH is used as a toughening component, which can effectively improve the embrittlement problem of the matrix and increase toughness. At the same time, the interfacial bonding force between the antibacterial component and the matrix is strong, and it is not easy to form stress concentration points. The resulting polypropylene material has excellent and long-lasting antibacterial effect as well as excellent mechanical properties. Detailed Implementation
[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0025] Example 1 A method for preparing glycidyltriethylammonium chloride-modified chitosan includes the following steps: Chitosan was dried in a vacuum drying oven at 60℃ for 12 hours. The dried chitosan was then dispersed in isopropanol to swell, alkalized with 30wt% sodium hydroxide solution, and then glycidyltriethylammonium chloride was added. The mass ratio of dried chitosan, isopropanol, 30wt% sodium hydroxide solution, and glycidyltriethylammonium chloride was 100:800:200:120. The mixture was reacted at 60℃ for 24 hours. After the reaction was completed, the pH of the system was adjusted to neutral using dilute hydrochloric acid, and small molecule salts were removed by dialysis. The mixture was then dried to obtain glycidyltriethylammonium chloride-modified chitosan.
[0026] Example 2 A method for preparing glycidyltriethylammonium chloride-modified chitosan includes the following steps: Chitosan was dried in a vacuum drying oven at 60℃ for 12 hours. The dried chitosan was dispersed in isopropanol to swell, and then alkalized with 30wt% sodium hydroxide solution. Glycidyltriethylammonium chloride was then added. The mass ratio of dried chitosan, isopropanol, 30wt% sodium hydroxide solution, and glycidyltriethylammonium chloride was 100:1000:260:200. The mixture was reacted at 70℃ for 18 hours. After the reaction was completed, the pH of the system was adjusted to neutral with dilute hydrochloric acid, and small molecule salts were removed by dialysis. The mixture was then dried to obtain glycidyltriethylammonium chloride-modified chitosan.
[0027] Example 3 A method for preparing glycidyltriethylammonium chloride-modified chitosan includes the following steps: Chitosan was dried in a vacuum drying oven at 60℃ for 12 hours. The dried chitosan was then dispersed in isopropanol to swell, alkalized with 30wt% sodium hydroxide solution, and then glycidyltriethylammonium chloride was added. The mass ratio of dried chitosan, isopropanol, 30wt% sodium hydroxide solution, and glycidyltriethylammonium chloride was 100:1200:320:250. The mixture was reacted at 75℃ for 12 hours. After the reaction was completed, the pH of the system was adjusted to neutral using dilute hydrochloric acid, and small molecule salts were removed by dialysis. The mixture was then dried to obtain glycidyltriethylammonium chloride-modified chitosan.
[0028] Example 4 A method for preparing an antibacterial polypropylene material includes the following steps: Step 1: Disperse nano-zinc oxide in dichloromethane using ultrasonication at 500W for 60 minutes. After uniform dispersion, add 4-dimethylaminopyridine and triethylamine and stir until homogeneous. Then, slowly add 4-bromomethylbenzoyl chloride. The mass ratio of nano-zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:800:1:12:16. React at 25℃ for 18 hours. After the reaction, filter the solution and wash with anhydrous ethanol and deionized water sequentially. Dry under vacuum at 60℃ for 12 hours to obtain modified nano-zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline in a mass ratio of 1000:100:30 are stirred and mixed, heated, and reacted at 50°C for 36 hours. After the reaction is completed, the mixture is filtered, washed with acetone and carbon tetrachloride, and dried under vacuum at 60°C for 12 hours to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add polypropylene resin (mass ratio 70:3:15:1:0.3:5:0.2:0.1), quaternary ammonium salt modified zinc oxide, maleic anhydride grafted polypropylene compatibilizer, glycidyl triethylammonium chloride modified chitosan, antioxidant, toughening agent POE-g-MAH, lubricant zinc stearate, and initiator dicumyl peroxide to a high-speed mixer. The antioxidant consists of antioxidant 1010 and antioxidant 168 in a 1:1 mass ratio. Mix thoroughly at 800 r / min for 40 min. Then, melt-blend in a twin-screw extruder at 200 r / min. The twin-screw extruder is set with five temperature zones according to the material's direction of travel: 165℃, 185℃, 205℃, 195℃, and 180℃. Extrude, granulate, and cool to obtain antibacterial polypropylene material.
[0029] The preparation method of glycidyltriethylammonium chloride modified chitosan in this embodiment is completely consistent with the preparation method of glycidyltriethylammonium chloride modified chitosan in Example 1.
[0030] Example 5 A method for preparing an antibacterial polypropylene material includes the following steps: Step 1: Disperse nano-zinc oxide in dichloromethane using ultrasonication at 500W for 60 minutes. After uniform dispersion, add 4-dimethylaminopyridine and triethylamine and stir until homogeneous. Then, slowly add 4-bromomethylbenzoyl chloride. The mass ratio of nano-zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:1000:3:20:20. React at 35℃ for 14 hours. After the reaction, filter the solution and wash with anhydrous ethanol and deionized water sequentially. Dry under vacuum at 60℃ for 12 hours to obtain modified nano-zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline in a mass ratio of 1200:100:40 are stirred and mixed, heated, and reacted at 55°C for 30 hours. After the reaction is completed, the mixture is filtered, washed with acetone and carbon tetrachloride, and dried under vacuum at 60°C for 12 hours to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add the following components to a high-speed mixer in a mass ratio of 82:5:18:1.5:0.4:6:0.4:0.15: quaternary ammonium salt modified zinc oxide, maleic anhydride-grafted polypropylene compatibilizer, glycidyl triethylammonium chloride-modified chitosan, antioxidant, toughening agent POE-g-MAH, lubricant zinc stearate, and initiator dicumyl peroxide. The antioxidant is prepared by mixing antioxidant 1010 and antioxidant 1 in a 1:1 mass ratio. The mixture consists of 68 components, which are mixed evenly in a high-speed mixer at a speed of 900 r / min for 30 min. The mixture is then melt-blended in a twin-screw extruder at a screw speed of 220 r / min. The twin-screw extruder is equipped with five temperature zones along the material's direction of travel: 170℃, 190℃, 210℃, 200℃, and 185℃. After extrusion granulation and cooling, an antibacterial polypropylene material is obtained.
[0031] The preparation method of glycidyltriethylammonium chloride modified chitosan in this embodiment is completely consistent with the preparation method of glycidyltriethylammonium chloride modified chitosan in Example 2.
[0032] Example 6 A method for preparing an antibacterial polypropylene material includes the following steps: Step 1: Disperse nano-zinc oxide in dichloromethane using ultrasonication at 500W for 60 minutes. After uniform dispersion, add 4-dimethylaminopyridine and triethylamine and stir until homogeneous. Then, slowly add 4-bromomethylbenzoyl chloride. The mass ratio of nano-zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:1000:4:21:22. React at 35℃ for 16 hours. After the reaction, filter the solution and wash with anhydrous ethanol and deionized water sequentially. Dry under vacuum at 60℃ for 12 hours to obtain modified nano-zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline in a mass ratio of 1200:100:45 are stirred and mixed, heated, and reacted at 55°C for 34 hours. After the reaction is completed, the mixture is filtered, washed with acetone and carbon tetrachloride, and dried under vacuum at 60°C for 12 hours to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add the following components to a high-speed mixer in a mass ratio of 82:6:20:2:0.4:7:0.5:0.15: quaternary ammonium salt modified zinc oxide, maleic anhydride-grafted polypropylene compatibilizer, glycidyl triethylammonium chloride-modified chitosan, antioxidant, toughening agent POE-g-MAH, lubricant zinc stearate, and initiator dicumyl peroxide. The antioxidant is prepared by mixing antioxidant 1010 and antioxidant 16 in a 1:1 mass ratio. The mixture consists of 8 components, which are thoroughly mixed. The mixing speed is 900 r / min in a high-speed mixer for 30 min. The mixture is then melt-blended in a twin-screw extruder at a screw speed of 220 r / min. The twin-screw extruder is set with five temperature zones according to the material's direction of travel, with temperatures of 175℃, 195℃, 215℃, 205℃, and 190℃. After extrusion granulation and cooling, an antibacterial polypropylene material is obtained.
[0033] The preparation method of glycidyltriethylammonium chloride modified chitosan in this embodiment is completely consistent with the preparation method of glycidyltriethylammonium chloride modified chitosan in Example 2.
[0034] Example 7 A method for preparing an antibacterial polypropylene material includes the following steps: Step 1: Disperse nano-zinc oxide in dichloromethane using ultrasonication at 500W for 60 minutes. After uniform dispersion, add 4-dimethylaminopyridine and triethylamine and stir until homogeneous. Then, slowly add 4-bromomethylbenzoyl chloride. The mass ratio of nano-zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:1200:5:25:24. React at 40℃ for 12 hours. After the reaction, filter the solution and wash with anhydrous ethanol and deionized water sequentially. Dry the solution under vacuum at 60℃ for 12 hours to obtain modified nano-zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline in a mass ratio of 1400:100:50 are stirred and mixed, heated, and reacted at 60°C for 24 hours. After the reaction is completed, the mixture is filtered, washed with acetone and carbon tetrachloride, and dried under vacuum at 60°C for 12 hours to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add the following components to a high-speed mixer in a mass ratio of 90:8:24:3:0.5:9:0.8:0.2: polypropylene resin, quaternary ammonium salt modified zinc oxide, maleic anhydride grafted polypropylene compatibilizer, glycidyl triethylammonium chloride modified chitosan, antioxidant, toughening agent POE-g-MAH, lubricant zinc stearate, and initiator dicumyl peroxide. The antioxidant is prepared by mixing antioxidant 1010 and antioxidant 168 in a 1:1 mass ratio. The mixture was prepared and thoroughly mixed in a high-speed mixer at a speed of 1000 r / min for 20 min. The mixture was then melt-blended in a twin-screw extruder at a screw speed of 240 r / min. The twin-screw extruder was equipped with five temperature zones along the material's direction of travel: 180℃, 200℃, 220℃, 210℃, and 195℃. The mixture was then extruded, granulated, and cooled to obtain an antibacterial polypropylene material.
[0035] The preparation method of glycidyltriethylammonium chloride modified chitosan in this embodiment is completely consistent with the preparation method of glycidyltriethylammonium chloride modified chitosan in Example 3.
[0036] Comparative Example 1 A method for preparing an antibacterial polypropylene material, compared with the method for preparing the antibacterial polypropylene material in Example 6, differs in that glycidyltriethylammonium chloride-modified chitosan is replaced with an equal amount of chitosan, while the other preparation methods are completely consistent with Example 6.
[0037] Comparative Example 2 A method for preparing an antibacterial polypropylene material is provided. Compared with the method for preparing the antibacterial polypropylene material in Example 6, the difference is that the quaternary ammonium salt modified zinc oxide is replaced with an equal amount of nano zinc oxide, while the other preparation methods are completely consistent with those in Example 6.
[0038] Comparative Example 3 A method for preparing an antibacterial polypropylene material is provided. Compared with the method for preparing the antibacterial polypropylene material in Example 6, the difference is that the quaternary ammonium salt modified zinc oxide is replaced with modified nano zinc oxide in equal amounts. The other preparation methods are completely consistent with those in Example 6.
[0039] Comparative Example 4 A method for preparing an antibacterial polypropylene material is provided. Compared with the method for preparing the antibacterial polypropylene material in Example 6, the difference is that the toughening agent POE-g-MAH is replaced with maleic anhydride-grafted polypropylene in equal amounts. The other preparation methods are completely consistent with those in Example 6.
[0040] The nano zinc oxide used in the examples and comparative examples of this invention was purchased from Nanjing Baoket New Materials Co., Ltd., with an average particle size of 30 nm; polypropylene was purchased from Daqing Petrochemical Company of China National Petroleum Corporation, model T30S; maleic anhydride-grafted polypropylene was purchased from Shanghai Rizhisheng New Technology Development Co., Ltd., model CMG9801; chitosan was purchased from Sinopharm Chemical Reagent Co., Ltd.; POE-g-MAH was purchased from Dalian Haizhou Chemical Co., Ltd., brand HZPA101; and other reagents were commercially available.
[0041] The antibacterial polypropylene materials prepared in Examples 4-7 and Comparative Examples 1-4 were subjected to relevant performance tests, the specific tests of which are as follows: (1) Antibacterial performance test: The test standard refers to GB / T 31402-2023 "Determination of antibacterial activity of plastics and other non-porous materials", and the concentration is 1.5×10 5 CFU / mL bacterial suspension was dropped onto the surface of the sample to be tested, covered with a covering film, and incubated in an incubator at 37℃ and 90% relative humidity for 24 hours. After incubation, 10mL of sterile physiological saline was added, and the sample was shaken to wash away bacteria. The number of viable bacteria was counted using the plate count method, and the antibacterial rate was calculated. Antibacterial rate (%) = (average number of viable bacteria in blank sample - average number of viable bacteria on antibacterial sample) / average number of viable bacteria in blank sample × 100%. The blank sample was a polypropylene resin sample without any antibacterial agent. The test strains were Escherichia coli (ATCC 25922) and Staphylococcus aureus (ATCC 6538). (2) Antibacterial durability test: In order to evaluate the anti-migration and anti-leakage performance of the antibacterial components of the material, a hot water circulation immersion durability test was conducted to simulate the long-term use rinsing environment. The antibacterial polypropylene materials prepared in each example and comparative example were injection molded into test samples of 50mm×50mm×2mm. Each sample was placed in a constant temperature water bath at 50℃ and continuously immersed. The deionized water was replaced every 24 hours. The antibacterial rate was tested after immersion for 60 days and the antibacterial rate retention rate was calculated. Antibacterial rate retention rate (%) = (antibacterial rate after water washing / initial antibacterial rate) × 100%. The test strains were Escherichia coli (ATCC 25922) and Staphylococcus aureus (ATCC 6538). The test method for antibacterial rate after water washing was the same as the antibacterial performance test method. (3) Mechanical property testing: The test standard refers to GB / T 1843-2008 "Determination of impact strength of plastic cantilever beam", and the impact strength test is carried out on the XCJD model pendulum impact tester. Each sample is tested 3 times and the average value is taken. The test standard refers to GB / T 1040.2-2022 "Determination of tensile properties of plastics - Part 2: Test conditions for molding and extruded plastics", and the tensile properties test is carried out on the WDW-1000G universal testing machine. Each sample is tested 3 times and the average value is taken.
[0042] The test results are shown in Table 1: Table 1 Test item Antibacterial rate against E. coli (%) Antibacterial rate against S. aureus (%) Antibacterial rate against E. coli (%) Antibacterial rate against S. aureus (%) impact strength (kJ / m 2 ) Tensile strength (MPa) Example 4 98.5 98.2 98.1 97.7 12.9 43.8 Example 5 99.5 99.3 98.9 98.6 13.8 44.6 Example 6 99.9 99.8 99.2 99.0 14.2 45.1 Example 7 99.7 99.5 98.7 98.4 13.3 44.3 Comparative Example 1 94.8 94.3 78.9 76.5 11.2 38.5 Comparative Example 2 91.5 91.1 73.0 70.9 7.8 29.7 Comparative Example 3 95.1 94.8 84.1 82.8 11.3 39.1 Comparative Example 4 99.5 99.3 98.5 98.2 6.5 34.0 As can be seen from the test results in Table 1, the samples corresponding to Examples 4-7 of this invention exhibit excellent antibacterial properties, excellent tensile and impact resistance, good toughness, and excellent mechanical properties. In Comparative Example 1, the chitosan was not modified, resulting in a decrease in overall performance, with reduced antibacterial rate and antibacterial retention rate, and decreased mechanical properties. This is mainly due to the weak antibacterial activity of chitosan itself, poor compatibility with the polypropylene matrix, and interface defects leading to reduced mechanical properties. Furthermore, it cannot form an effective synergistic antibacterial system, and the antibacterial components are easily lost after long-term washing, resulting in insufficient antibacterial retention. In Comparative Example 2, nano-zinc oxide was directly used instead of quaternary ammonium salt-modified zinc oxide, significantly reducing the overall performance of the polypropylene material. Nano-zinc oxide has poor dispersion in the matrix, easily agglomerates, has a small exposed antibacterial surface area, and lacks the synergistic effect of quaternary ammonium salt, resulting in poor antibacterial effect and durability, and significantly reduced mechanical properties. In Comparative Example 3, the modified zinc oxide showed improved dispersion and compatibility compared to Comparative Example 2, but the synergistic antibacterial effect was insufficient, and the overall performance of the corresponding sample was still lower than that of Example 6. Comparative Example 4 lacks toughening agents, resulting in a lower impact on antibacterial effects. The system also lacks flexible toughening components, and the inorganic fillers easily cause stress concentration in the matrix, leading to a significant decrease in the material's impact toughness, impact resistance, and tensile strength.
[0043] Although embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.
Claims
1. A method for preparing an antibacterial polypropylene material, characterized in that: Includes the following steps: Step 1: Disperse nano zinc oxide in dichloromethane using ultrasonication. After uniform ultrasonic dispersion, add 4-dimethylaminopyridine and triethylamine and stir until uniformly mixed. Then, slowly add 4-bromomethylbenzoyl chloride to induce a reaction. After the reaction is complete, filter, wash, and dry to obtain modified nano zinc oxide. Step 2: Acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline are stirred and mixed, heated, and reacted. After the reaction is completed, the mixture is filtered, washed, and dried to obtain quaternary ammonium salt modified zinc oxide. Step 3: Add polypropylene resin, quaternary ammonium salt modified zinc oxide, compatibilizer, quaternized chitosan, antioxidant, toughening agent, lubricant, and initiator to a high-speed mixer, mix evenly, melt-blend in a twin-screw extruder, extrude and granulate, and cool to obtain antibacterial polypropylene material.
2. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step one, the mass ratio of nano zinc oxide, dichloromethane, 4-dimethylaminopyridine, triethylamine, and 4-bromomethylbenzoyl chloride is 100:(800~1200):(1~5):(12~25):(16~24).
3. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: The reaction temperature in step one is 25~40℃, and the reaction time is 12~18h.
4. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step two, the mass ratio of acetone, modified nano zinc oxide, and N,N-dimethyl-4-vinylaniline is (1000~1400):100:(30~50).
5. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: The reaction temperature in step two is 50~60℃, and the reaction time is 24~36h.
6. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step three, the mass ratio of polypropylene resin, quaternary ammonium salt modified zinc oxide, compatibilizer, quaternized chitosan, antioxidant, toughening agent, lubricant, and initiator is (70~90):(3~8):(15~24):(1~3):(0.3~0.5):(5~9):(0.2~0.8):(0.1~0.2).
7. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step three, the high-speed mixer operates at a speed of 800-1000 r / min and a mixing time of 20-40 min. During the melt blending process, the screw speed of the twin-screw extruder is 200-240 r / min. The twin-screw extruder is equipped with five temperature zones according to the material's forward direction, with temperatures of 165-180℃, 185-200℃, 205-220℃, 195-210℃, and 180-195℃, respectively.
8. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step three, the quaternized chitosan is glycidyltriethylammonium chloride-modified chitosan.
9. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: In step three, the compatibilizer is maleic anhydride-grafted polypropylene; the antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; the toughening agent is POE-g-MAH; and the lubricant is zinc stearate.
10. The method for preparing the antibacterial polypropylene material according to claim 1, characterized in that: The initiator in step three is dicumyl peroxide.
Citation Information
Patent Citations
Antibacterial polypropylene plastic
CN103059405A
Antibacterial polypropylene fiber and preparation method thereof
CN121519191A
Antibacterial polypropylene material and preparation method thereof
CN122278058A