A halogen-free flame-retardant SBS polymer blend and its vacuum preparation method
By introducing double-bond functionalized intumescent flame-retardant microcapsules and end-capped multi-thiol siloxane crosslinking agents into SBS polymer blends, and utilizing thiol-ene addition reaction and gradient blending process, the problem of weak interfacial bonding between flame retardant and matrix was solved, achieving synergistic improvement in flame retardant performance and mechanical properties, as well as enhanced stability.
Patent Information
- Application Number
- CN202611387998.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
In existing halogen-free flame-retardant SBS blends, the bonding between the flame-retardant filler and the matrix is weak, making it difficult to balance flame-retardant performance with mechanical toughness and long-term stability.
A double-bond functionalized expandable flame-retardant microcapsule is combined with a capped multi-thiol siloxane crosslinking agent. The flame retardant and the matrix are covalently bonded at the interface through a thiol-ene addition reaction. The timing and rate of the crosslinking reaction are precisely controlled by a gradient blending extrusion process.
While ensuring stable material processing, the synergistic improvement of flame retardant and mechanical properties was achieved, reducing interfacial stress concentration and the migration and precipitation of flame retardants, and improving the long-term stability of the material.
Smart Images

Figure CN123107291A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of polymer material modification and processing technology, and more specifically, it relates to a halogen-free flame-retardant SBS polymer blend and a vacuum preparation method thereof. Background Technology
[0002] Styrene-butadiene-styrene block copolymers are a class of widely used thermoplastic elastomers that combine the high elasticity of rubber with the easy processing properties of plastics. They are commonly used to manufacture products such as wire and cable sheaths, building seals, and automotive interior parts. In these applications, to meet relevant fire safety regulations, the matrix material needs to be modified to produce a flame-retardant rating, thereby reducing the risk of fire occurrence and spread.
[0003] Existing halogen-free flame retardant modifications mostly employ physical blending to directly introduce flame retardant fillers into the matrix system. The flame retardant particles and the polymer matrix only have a physical bonding effect, and the interfacial compatibility is relatively limited. This can easily lead to stress concentration points at the interface, causing a decrease in the mechanical toughness of the material, and can also cause flame retardant migration and precipitation during long-term use. It is difficult to maintain good mechanical properties and service stability of the material while achieving flame retardancy standards. Summary of the Invention
[0004] To address the issues in existing technologies where the flame-retardant filler in halogen-free flame-retardant SBS blends exhibits weak interfacial bonding with the matrix, making it difficult to balance flame retardant performance with mechanical toughness and long-term stability, this application provides a halogen-free flame-retardant SBS polymer blend and a vacuum preparation method therein.
[0005] In a first aspect, this application provides a halogen-free flame-retardant SBS polymer blend, employing the following technical solution: A halogen-free flame-retardant SBS polymer blend, comprising, by weight, the following components: 70 to 85 parts of a styrene-butadiene-styrene block copolymer matrix, 12 to 18 parts of double-bond functionalized intumescent flame-retardant microcapsules, 3 to 6 parts of a capped polythiol siloxane crosslinking agent, 0.1 to 0.3 parts of an alkenyl functionalized semi-hindered phenol regulator, 0.3 to 0.8 parts of a composite antioxidant, and 0.5 to 1.2 parts of a silicone lubricant; The surface of the capsule wall of the double-bond functionalized expandable flame-retardant microcapsule is grafted with carbon-carbon double bonds and short-chain polymer compatible anchor points. The thiol groups of the terminated polythiol siloxane crosslinking agent are terminated by a blocking agent. The alkenyl-functionalized semi-hindered phenol regulator molecule contains both a hindered phenolic hydroxyl group and a terminal allyl double bond.
[0006] By employing the above technical solution, double-bond functionalized intumescent flame-retardant microcapsules, end-capped multi-thiol siloxane crosslinking agents, and alkenyl functionalized semi-hindered phenol regulators are compounded. During the melt blending process, the flame-retardant particles are covalently linked to the polymer matrix through a thiol-alkene addition reaction. At the same time, the density and uniformity of the crosslinking network are moderately controlled, so that the flame-retardant components can be stably distributed at the interface between the two phases of the matrix. While imparting reliable flame-retardant properties to the material, the elasticity and toughness of the matrix itself are maintained to the greatest extent. This alleviates the problems of weak interfacial bonding, obvious stress concentration, and large toughness loss that are common in conventional physically filled flame-retardant systems, and achieves a synergistic improvement in flame-retardant performance and mechanical properties.
[0007] Preferably, the double-bond functionalized expandable flame-retardant microcapsules have calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell layer; the short-chain polymer compatibility anchor is a polystyrene segment.
[0008] By adopting the above technical solution, calcium phytate, as the bio-based phosphorus-based flame retardant core, can release phosphorus-containing active groups after thermal decomposition, catalyzing the rapid char formation of the matrix and capsule wall material. Its decomposition temperature matches the processing temperature of the SBS matrix, preventing premature decomposition and failure during conventional blending. Allyl ether-modified melamine-formaldehyde resin, as the capsule wall shell, possesses the characteristic of thermal expansion and foaming. During combustion, it can form a dense expanded char layer to block heat and oxygen. At the same time, carbon-carbon double bonds are introduced into the side chains of the capsule wall molecules through ether bonds, enabling the double bonds to stably participate in subsequent cross-linking reactions. Polystyrene segments, as compatibility anchors, have good thermodynamic compatibility with the styrene hard segments in the SBS matrix. Through segment entanglement, it can reduce the interfacial tension between the two phases, guide the microcapsules to spontaneously accumulate at the interface between the two phases, improve the interfacial bonding state between the flame retardant particles and the matrix, reduce interfacial voids and stress concentration points, and inhibit the migration and precipitation of flame retardant particles during long-term use.
[0009] Preferably, the end-capped polythiol siloxane crosslinking agent uses polythiol cage-type silsesquioxane as the base material and acetone oxime as the blocking agent to end-cap the thiol groups.
[0010] By adopting the above technical solution, the multi-thiol cage-like silsesquioxane has multiple reactive thiol sites, which can simultaneously undergo addition reactions with matrix double bonds and microcapsule double bonds to construct a multi-site interfacial cross-linking network. Its cage-like siloxane structure can also form a siliceous carbon layer skeleton during combustion, improving the density and anti-dripping performance of the carbon layer, and playing a synergistic flame-retardant role with phosphorus-based flame retardants. After acetone oxime is used as a sealing agent to end-cap the thiol groups, the oxime groups and thiol groups form stable thiooxime ether bonds, so that the thiol groups are in an inert dormant state under low temperature conditions. After reaching a specific temperature range, the chemical bonds gradually break, and the thiol group reactivity is released in an orderly manner, realizing the controllable timing of the cross-linking reaction, reducing the possibility of premature cross-linking and agglomeration of materials in the early stage of processing and abnormal increase in screw torque, and broadening the processing window of the material.
[0011] Preferably, the styrene-butadiene-styrene block copolymer matrix has a linear structure, and the styrene mass percentage is 30% to 40%; the alkenyl functionalized semi-hindered phenol regulator is 2-tert-butyl-6-methyl-4-allylphenol.
[0012] By adopting the above technical solution, the butadiene segments of the linear styrene-butadiene-styrene block copolymer have uniformly distributed unsaturated double bonds, which can directly participate in the interfacial addition reaction as active sites for crosslinking reactions. This eliminates the need for additional solution grafting modification of the matrix, avoiding problems such as solvent residue, complicated processes, and increased costs. The allyl double bonds in 2-tert-butyl-6-methyl-4-allylphenol can participate in the thiol-ene addition reaction, consuming some of the thiol active sites. At the same time, the sterically hindered thiol alkylphenols generated after the reaction reduce free radical activity, playing a role in chain transfer and soft termination. This adjusts the overall crosslinking density and avoids excessive crosslinking that leads to material embrittlement and decreased toughness. The semi-hindered phenolic hydroxyl groups in the molecule can capture peroxide free radicals generated during thermal processing and aging, protecting the SBS butadiene segments from oxidative chain scission and synergistically improving the thermo-oxidative stability of the material.
[0013] Preferably, the composite antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1 to 2:1.2.
[0014] By adopting the above technical solution, two antioxidants are compounded in proportion to form a highly efficient synergistic thermo-oxidative stabilization system. The hindered phenolic primary antioxidant can capture macromolecular peroxide free radicals through hydrogen transfer reaction, terminating the oxidation chain reaction. The phenolic oxygen free radicals generated after the reaction have a stable structure and are not prone to initiating new active chains. The phosphite auxiliary antioxidant can decompose the hydroperoxides in the system into inactive stable products, and at the same time, it can reduce the oxidized phenolic oxygen free radicals and regenerate the activity of the primary antioxidant. The synergistic effect of the two can significantly improve the thermo-oxidative stabilization efficiency, reduce yellowing and mechanical property degradation of materials during high-temperature processing, and extend the long-term service life of materials.
[0015] Secondly, this application provides a vacuum preparation method for halogen-free flame-retardant SBS polymer blends, employing the following technical solution: A vacuum preparation method for a halogen-free flame-retardant SBS polymer blend includes the following steps: S1. Vacuum pre-drying: Vacuum drying is performed on all component raw materials to control the moisture content of the raw materials to meet the processing requirements; S2, Nitrogen premixing: All dried raw materials are placed in a nitrogen-protected environment for low-temperature mixing to obtain a uniform premixed material; S3, Gradient Blending Extrusion: The premixed material is fed into a co-rotating parallel twin-screw extruder and a gradient process with coordinated matching of temperature, vacuum and shear rate is adopted. The material passes through the feeding and conveying section, plasticizing and venting section, core reaction section, homogenization and termination section and die head discharge section in sequence to complete the end-capped thiol desealing and interfacial covalent cross-linking blending treatment. S4. Cooling, pelletizing and collecting: The continuous strip extruded from the die head is cooled and shaped, and after air drying, it is cut into pellets to obtain the finished blend.
[0016] By adopting the above technical solution, a gradient extrusion process with coordinated matching of temperature, vacuum degree, and shear rate is used to achieve stable material conveying, plasticizing and degassing, interfacial crosslinking, and homogenized discharge in different functional sections. This allows the decapping process of end-capped thiol groups and the interfacial covalent crosslinking reaction to proceed step by step according to a set time sequence. The temperature gradient matches the decapping law of end-capped groups, the vacuum gradient regulates the lifetime and reaction rate of free radicals, and the shear gradient adapts to the dispersion requirements of each stage. The three work together to complete the interfacial crosslinking network construction in situ during melt blending without the need for additional initiators. This simplifies the processing flow while improving the uniformity and controllability of the reaction, ensuring stable and uniform performance of the finished product.
[0017] Preferably, in step S2, the nitrogen-protected low-temperature mixing specifically involves: purging high-purity nitrogen to replace the air for 2 to 4 minutes before mixing, ensuring that the oxygen concentration in the mixing chamber is no greater than 500 ppm; and ensuring that the material temperature does not exceed 50°C during the mixing process.
[0018] By adopting the above technical solution, high-purity nitrogen is introduced to replace the air in the mixing chamber before mixing, which can significantly reduce the oxygen concentration in the mixing environment, reduce the oxidative loss of thiol activity by oxygen, and avoid thermal oxidative aging of materials during the mixing friction heating process. The mixing process controls the material to be at a low temperature, ensuring that the temperature is always lower than the initial unsealing temperature of the end-capping groups, so that the end-capping structure remains intact and stable. All components achieve only macroscopic and microscopic physical uniform dispersion in the premixing stage, without chemical reaction, ensuring that the crosslinking reaction can be started synchronously in the subsequent extrusion process, avoiding uneven material properties caused by local premature crosslinking.
[0019] Preferably, in step S3, the feeding and conveying section maintains a normal pressure nitrogen atmosphere, with an oxygen content in the cavity not exceeding 500 ppm and a temperature of 130 to 140°C; the plasticizing and exhaust section has an absolute vacuum of 0.05 to 0.06 MPa and a temperature of 145 to 155°C.
[0020] By adopting the above technical solution, the feeding and conveying section maintains a normal pressure nitrogen atmosphere and sets a low temperature. On the one hand, this prevents air from continuously entering the extrusion system with the material, and on the other hand, it ensures that the end-capping groups remain stable during the initial melting process, preventing premature decapping reactions and maintaining good material flowability, thus achieving stable feeding and initial plasticization. The plasticizing and venting section is set with a moderate vacuum and a medium temperature, which can remove residual air, adsorbed moisture, and low-boiling-point volatile impurities from the system during the gradual melting and plasticization of the material, avoiding bubble defects in subsequent reaction sections. At the same time, the temperature in this section is close to the initial decapping temperature of the end-capping groups. After the material is fully plasticized, the microcapsules can be uniformly dispersed in the matrix, preparing the phase state for interfacial crosslinking in subsequent reaction sections. The reactivity in this stage is extremely low, and there is no obvious premature crosslinking phenomenon.
[0021] Preferably, in step S3, the absolute vacuum degree of the core reaction section is 0.02 to 0.03 MPa, the residual oxygen in the cavity is no more than 50 ppm, and the effective residence time of the material in the core reaction section is 3 to 5 minutes.
[0022] By adopting the above technical solution, the core reaction section is set with a high vacuum, which can significantly reduce the oxygen partial pressure in the cavity, weaken the quenching effect of oxygen on thiol free radicals, extend the survival life of free radicals, and enable the thiol free radicals generated by thermal initiation to effectively undergo addition reactions with double bonds without the need for additional thermal initiators, thus avoiding the negative impact of initiator residues on the aging resistance of the material. The temperature of this section matches the desealing temperature range of the capped thiol groups, which can continuously and stably release active thiol groups. Combined with appropriate shearing action, it can ensure full contact and reaction at the interface between the microcapsules and the matrix, forming a uniform interfacial cross-linking network, which firmly anchors the flame-retardant particles in the matrix. Controlling the effective residence time of the material in the core reaction section can ensure that the cross-linking reaction is fully carried out, while avoiding excessive reaction that would lead to excessive cross-linking and decreased fluidity of the material.
[0023] Preferably, in step S3, the absolute vacuum of the homogenization termination section is adjusted back to 0.06 to 0.07 MPa, and a trace amount of nitrogen is introduced simultaneously at a temperature of 150 to 155°C; the discharge section of the die head maintains a slight positive pressure discharge of nitrogen, with a gauge pressure of 0.01 to 0.02 MPa and a die head temperature of 145 to 150°C.
[0024] By adopting the above technical solutions, the vacuum level is adjusted back and a trace amount of nitrogen is introduced in the homogenization termination section, which can increase the oxygen concentration in the system. The free radical quenching effect of oxygen is used to inhibit the cross-linking reaction from continuing, so that the cross-linking reaction is gradually terminated, avoiding the material from continuing to react and causing excessive cross-linking during subsequent conveying. The appropriate temperature drop combined with weak shearing further homogenizes the cross-linked material system, eliminates local viscosity differences, and ensures a stable and smooth discharge process. The discharge section of the die head adopts a nitrogen micro-positive pressure setting, which can form a stable air seal effect, prevent outside air from entering the inside of the barrel, avoid oxidation and yellowing of the material surface when the material is discharged at high temperature, and at the same time stabilize the discharge pressure of the die head, ensuring continuous and uniform material strips, and improving the appearance quality and performance consistency of the finished granules.
[0025] In summary, this application has the following beneficial effects: 1. Because this application uses double-bond functionalized expandable flame-retardant microcapsules with surface-grafted short-chain polymer compatible anchors, and works in conjunction with end-capped multi-thiol siloxane crosslinking agents, the flame retardant and the matrix are covalently bonded at the interface through a mercaptoene addition reaction during gradient blending extrusion, which achieves the effect of synergistic improvement in flame retardant performance and mechanical toughness, and can alleviate the problems of weak interfacial bonding and easy loss of matrix elasticity of conventional filled flame retardants.
[0026] 2. In this application, acetone oxime-terminated polythiol cage-type silsesquioxane is preferably used as a crosslinking agent. By matching the extrusion temperature gradient with the unsealing temperature range of the terminated thiol groups, the crosslinking reaction proceeds step by step according to the set time sequence, resulting in more stable melt processing performance and reducing the risk of premature reaction and agglomeration of materials in the premixing stage.
[0027] 3. The method of this application precisely controls the amount of residual oxygen in the cavity by setting gradient vacuum in each functional segment of the extrusion process. It utilizes the quenching effect of oxygen on thiol free radicals to control the crosslinking reaction rate, thereby achieving a thermally initiated crosslinking effect without the need for an external initiator. This simplifies the processing flow and improves the uniformity of the reaction.
[0028] 4. In this application, 2-tert-butyl-6-methyl-4-allylphenol is preferably used as a regulator. The allyl double bond in its molecule can participate in the cross-linking reaction to regulate the cross-linking density. The sterically hindered phenolic hydroxyl group can synergistically enhance the thermal and oxygen stability of the material with the composite antioxidant, thus achieving a dual-effect application effect and optimizing the long-term performance of the material. Attached Figure Description
[0029] Figure 1 This is a flowchart of a halogen-free flame-retardant SBS polymer blend preparation process provided in this application; Figure 2 This is a comparison diagram of the tensile strength test results of the various embodiments and comparative examples provided in this application; Figure 3This is a comparison chart of the elongation at break test results of the various embodiments and comparative examples provided in this application; Figure 4 This is a comparison diagram of the tensile modulus of elasticity test results of the various embodiments and comparative examples provided in this application; Figure 5 This is a comparison chart of the tensile strength retention rate test results after hot air accelerated aging of the various embodiments and comparative examples provided in this application. Detailed Implementation
[0030] The present application will be further described in detail below with reference to embodiments and comparative examples. Unless otherwise specified, the experimental methods used below are conventional methods. Unless otherwise specified, the materials, reagents, methods and instruments used are all conventional materials, reagents, methods and instruments in the art, which can be obtained by those skilled in the art through commercial channels or prepared according to literature methods.
[0031] Technical Concept: Existing halogen-free flame-retardant SBS elastomers mostly employ physical blending to introduce intumescent flame-retardant fillers. The flame-retardant particles and the polymer matrix are bonded solely by physical forces, resulting in insufficient interfacial compatibility and a tendency for stress concentration points to form at the interface. This leads to a significant decrease in the material's tensile toughness and elasticity. Furthermore, during long-term use, the flame-retardant components are prone to migration and precipitation, causing a decline in flame-retardant performance and operational stability. Introducing a reactive crosslinking system to improve interfacial bonding is problematic because conventional highly reactive thiol crosslinking agents tend to react prematurely during premixing and plasticizing, causing issues such as material agglomeration and abnormally high processing torque. The timing and rate of the crosslinking reaction are difficult to precisely control, making it impossible to achieve interfacial compatibility enhancement and performance synergy while ensuring processing stability.
[0032] This technical solution adopts a design approach that combines functional modification with gradient processes. It functionalizes the flame-retardant microcapsules with double bonds and grafts polystyrene compatibility anchors, leveraging segment compatibility to drive interfacial enrichment and provide covalent reaction sites. Simultaneously, it uses acetone oxime to end-cap siloxanes, endowing the crosslinking agent with temperature-controlled desealing properties. Based on this, a gradient extrusion process with synergistic matching of temperature, vacuum, and shear rate is constructed. The oxygen concentration within the cavity is controlled by vacuum to precisely control the mercapto-olefin radical reaction process. During melt blending, in-situ interfacial covalent crosslinking between the flame retardant and the matrix is completed. The crosslinking density is further regulated by a bifunctional semi-hindered phenol. Ultimately, without sacrificing processing stability, the flame-retardant properties and mechanical toughness of the material are synergistically improved.
[0033] Preparation Example 1: The preparation method of double-bond functionalized expandable flame-retardant microcapsules is as follows: 15 parts of calcium phytate were dispersed in deionized water to prepare a 15% (w / w) suspension. Sodium dodecylbenzenesulfonate emulsifier was added, and the mixture was stirred and emulsified at 300 r / min for 20 min. Separately, 8 parts of melamine, 12 parts of 37% (w / w) formaldehyde solution, and 3 parts of ethylene glycol monoallyl ether were added to a reaction vessel. Triethanolamine was added dropwise to adjust the pH of the system to 8.5. The temperature was raised to 75℃ and stirred for 30 min to obtain an allyl ether-modified melamine-formaldehyde resin prepolymer. The prepolymer was slowly added dropwise to the calcium phytate suspension. After the addition was complete, the pH of the system was adjusted to 5.0 with dilute hydrochloric acid. The temperature was further raised to 80℃ and kept at that temperature for 3 h to form an in-situ expanded flame-retardant microcapsule. Microcapsules with calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell were prepared. Two parts of terminally hydroxyl polystyrene with a number-average molecular weight of 2500 were then added, and the reaction was continued at a constant temperature for 2 hours to fix the polystyrene linkages onto the capsule wall surface, forming compatible anchor points for the polystyrene chains. After the reaction, the capsules were cooled to room temperature, filtered, washed three times with deionized water, and vacuum dried at 60°C to obtain the target microcapsules. Particle size analysis using a laser particle size analyzer revealed a median particle size of 6.5 μm. Transmission electron microscopy was used to observe the capsule wall cross-section and calculate that the shell thickness accounted for 12% of the total particle size. X-ray photoelectron spectroscopy was used to quantitatively analyze the elements on the capsule wall surface, calculating a carbon-carbon double bond grafting density of 0.45 bonds per square nanometer.
[0034] Preparation Example 2: The preparation method of the end-capped polythiol siloxane crosslinking agent is as follows: 5 parts of octamercaptopropyl cage-type silsesquioxane were dispersed in anhydrous ethanol and stirred to form a uniform dispersion. 2.5 parts of acetone oxime were added, and glacial acetic acid was added dropwise to adjust the pH of the system to 5.5. The temperature was raised to 35℃ and stirred for 4 hours to complete the end-capping modification of the thiol group. After the reaction, the solvent and unreacted acetone oxime were removed by vacuum distillation. The product was dried under vacuum at 80℃ to obtain the end-capped polythiol siloxane crosslinking agent. The particle size of the powder was measured by a laser particle size analyzer, and the average particle size was found to be 1.5 μm. The thiol content was determined by iodometric titration and the molecular thiol functionality was calculated to be 7. Differential scanning calorimetry was used to test the decapping temperature of the end-capped thiol group at a heating rate of 10℃ / min, and the decapping temperature was found to be 152℃.
[0035] Preparation Example 3: The preparation method of the alkenyl-functionalized semi-hindered phenol regulator is as follows: 10 parts of 2-tert-butyl-6-methylphenol were dissolved in toluene solvent, and 4.5 parts of sodium hydroxide were added as an acid-binding agent. After stirring evenly, 5.2 parts of allyl chloride were slowly added dropwise. After the addition was completed, the temperature was raised to 55℃ and the reaction was maintained for 5 hours to complete the Williamson etherification reaction. The reaction solution was washed three times with deionized water, separated, and the solvent and low-boiling point impurities were removed under reduced pressure to obtain 2-tert-butyl-6-methylphenylene. Crude propyl ether was transferred to a pressure-resistant reactor, and the air inside the reactor was replaced three times with high-purity nitrogen. The reactor was then heated to 190°C and held for 3.5 hours for rearrangement. The product was purified by vacuum distillation to obtain 2-tert-butyl-6-methyl-4-allylphenol. The purity of the product was tested by gas chromatography, and the purity was found to be 98.2%. The structure was characterized by Fourier transform infrared spectroscopy and nuclear magnetic resonance hydrogen spectroscopy, which verified that the molecule contains both a sterically hindered phenolic hydroxyl group and a terminal allyl double bond.
[0036] Example 1: This example provides a halogen-free flame-retardant SBS polymer blend, comprising the following raw materials in parts by weight: 77.5 parts of styrene-butadiene-styrene block copolymer matrix, 15 parts of double-bond functionalized intumescent flame-retardant microcapsules, 4.5 parts of end-capped polythiol siloxane crosslinking agent, 0.2 parts of alkenyl functionalized semi-hindered phenol regulator, 0.55 parts of composite antioxidant, and 0.85 parts of silicone lubricant.
[0037] Among them, the double-bond functionalized intumescent flame-retardant microcapsules have calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell layer, with polystyrene segments as short-chain polymer compatibility anchors. These microcapsules are prepared using the process described in Preparation Example 1 above. The end-capped polythiol siloxane crosslinking agent has polythiol cage-type silsesquioxane as the base material and acetone oxime as the blocking agent to end-cap the thiol groups. This crosslinking agent is prepared using the process described in Preparation Example 2 above. The styrene-butadiene-styrene block copolymer matrix has a linear structure, with styrene accounting for 35% by mass. The alkenyl functionalized semi-hindered phenol regulator is 2-tert-butyl-6-methyl-4-allylphenol, prepared using the process described in Preparation Example 3 above. The composite antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1.1.
[0038] The vacuum preparation method of the above-mentioned halogen-free flame-retardant SBS polymer blend includes the following steps: S1. Vacuum pre-drying: Vacuum drying is performed on all components of the raw materials to control the moisture content of the raw materials to meet the processing requirements.
[0039] The styrene-butadiene-styrene block copolymer matrix was placed in a vacuum drying oven and dried for 5 hours at 65°C and 0.08 MPa absolute vacuum, with the final moisture content controlled to be no more than 0.05%. The double-bond functionalized intumescent flame-retardant microcapsules, the end-capped polythiol siloxane crosslinking agent, the alkenyl functionalized semi-hindered phenol regulator, the composite antioxidant, and the silicone lubricant were dried for 2 hours at 80°C and 0.08 MPa absolute vacuum to remove adsorbed moisture.
[0040] S2. Nitrogen premixing: All dried raw materials are placed in a nitrogen-protected environment for low-temperature mixing to obtain a uniform premixed material.
[0041] Before mixing, high-purity nitrogen is introduced to replace the air for 3 minutes to control the oxygen concentration in the mixing chamber to be no more than 500 ppm; the stirring speed is set to 350 r / min and the mixing time is 6.5 minutes; the temperature is controlled by jacket cooling water throughout the process to ensure that the material temperature does not exceed 50℃, so as to avoid premature desealing of the end-capped thiol groups.
[0042] S3. Gradient blending extrusion: The premixed material is fed into a co-rotating parallel twin-screw extruder and a gradient process with coordinated matching of temperature, vacuum and shear rate is adopted. The material passes through the feeding and conveying section, plasticizing and venting section, core reaction section, homogenization and termination section and die head discharge section in sequence to complete the desealing of end-capped thiol groups and interfacial covalent cross-linking blending treatment.
[0043] The feeding and conveying section maintains a normal pressure nitrogen atmosphere, with an oxygen content not exceeding 500 ppm and a temperature of 135°C. It employs a low-shear conveying thread configuration with a shear rate of 40 s⁻¹. The plasticizing and venting section has an absolute vacuum of 0.055 MPa and a temperature of 150°C. It employs a weak-shear mixing thread configuration with a shear rate of 90 s⁻¹. The core reaction section has an absolute vacuum of 0.025 MPa, with residual oxygen not exceeding 50 ppm and a temperature of 160°C. It employs a medium-shear mixing thread configuration with a shear rate of 90 s⁻¹. The rate is 175s⁻¹, and the effective residence time of the material in the core reaction section is 4 minutes, which can simultaneously complete the desealing of end-capped thiol groups and the cross-linking reaction of thiol-ene addition interface, thereby strengthening the interfacial bonding strength between the flame retardant and the matrix; the homogenization termination section adjusts the absolute vacuum to 0.065MPa, and simultaneously introduces a trace amount of nitrogen gas at a temperature of 152.5℃, adopting a weak shear conveying screw configuration with a shear rate of 70s⁻¹; the discharge section at the die head maintains a slight positive pressure discharge of nitrogen gas at a gauge pressure of 0.015MPa and a die head temperature of 147.5℃.
[0044] S4. Cooling, pelletizing and collecting: The continuous strip extruded from the die head is cooled and shaped, and after air drying, it is cut into pellets to obtain the finished blend.
[0045] In this process, the material strip is cooled and shaped by circulating cooling water at room temperature. After the surface moisture is dried by compressed air, it is sent to a pelletizer to be pelletized, resulting in cylindrical pellets with uniform particle size.
[0046] Example 2: This example provides a halogen-free flame-retardant SBS polymer blend, comprising the following raw materials in parts by weight: 70 parts of styrene-butadiene-styrene block copolymer matrix, 12 parts of double-bond functionalized intumescent flame-retardant microcapsules, 3 parts of end-capped polythiol siloxane crosslinking agent, 0.1 parts of alkenyl functionalized semi-hindered phenol regulator, 0.3 parts of composite antioxidant, and 0.5 parts of silicone lubricant.
[0047] Among them, the double-bond functionalized intumescent flame-retardant microcapsules have calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell layer, with polystyrene segments as short-chain polymer compatibility anchors. These microcapsules are prepared using the process described in Preparation Example 1 above. The end-capped polythiol siloxane crosslinking agent has polythiol cage-type silsesquioxane as the base material and acetone oxime as the blocking agent to end-cap the thiol groups. This crosslinking agent is prepared using the process described in Preparation Example 2 above. The styrene-butadiene-styrene block copolymer matrix has a linear structure, with styrene accounting for 30% by mass. The alkenyl functionalized semi-hindered phenol regulator is 2-tert-butyl-6-methyl-4-allylphenol, prepared using the process described in Preparation Example 3 above. The composite antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1.
[0048] The vacuum preparation method of the above-mentioned halogen-free flame-retardant SBS polymer blend includes the following steps: S1. Vacuum pre-drying: Vacuum drying is performed on all components of the raw materials to control the moisture content of the raw materials to meet the processing requirements.
[0049] The styrene-butadiene-styrene block copolymer matrix was placed in a vacuum drying oven and dried at 60°C and 0.07 MPa absolute vacuum for 4 hours to control the final moisture content to be no more than 0.05%. The double bond functionalized intumescent flame retardant microcapsules, the end-capped multi-thiol siloxane crosslinking agent, the alkenyl functionalized semi-hindered phenol regulator, the composite antioxidant, and the silicone lubricant were dried at 80°C and 0.07 MPa absolute vacuum for 1.5 hours to remove adsorbed moisture.
[0050] S2. Nitrogen premixing: All dried raw materials are placed in a nitrogen-protected environment for low-temperature mixing to obtain a uniform premixed material.
[0051] The process involves purging high-purity nitrogen to replace the air for 2 minutes before mixing, controlling the oxygen concentration in the mixing chamber to be no more than 500 ppm; setting the stirring speed to 300 r / min and the mixing time to 5 minutes; and controlling the temperature throughout the process using jacketed cooling water to ensure that the material temperature does not exceed 50℃.
[0052] S3. Gradient blending extrusion: The premixed material is fed into a co-rotating parallel twin-screw extruder and a gradient process with coordinated matching of temperature, vacuum and shear rate is adopted. The material passes through the feeding and conveying section, plasticizing and venting section, core reaction section, homogenization and termination section and die head discharge section in sequence to complete the desealing of end-capped thiol groups and interfacial covalent cross-linking blending treatment.
[0053] The feeding and conveying section maintains a normal pressure nitrogen atmosphere, with an oxygen content of no more than 500 ppm and a temperature of 130°C. It adopts a low-shear conveying thread configuration with a shear rate of 30 s⁻¹. The plasticizing and venting section has an absolute vacuum of 0.05 MPa and a temperature of 145°C. It adopts a weak-shear mixing thread configuration with a shear rate of 80 s⁻¹. The core reaction section has an absolute vacuum of 0.02 MPa, with residual oxygen of no more than 50 ppm and a temperature of 155°C. It adopts a medium-shear mixing thread configuration with a shear rate of 150 s⁻¹, and the effective residence time of the material in the core reaction section is 3 minutes. The homogenization termination section adjusts the absolute vacuum to 0.06 MPa, simultaneously introduces a trace amount of nitrogen, maintains a temperature of 150°C, adopts a weak-shear conveying thread configuration, and a shear rate of 60 s⁻¹. The die head discharge section maintains a slightly positive nitrogen discharge pressure, with a gauge pressure of 0.01 MPa and a die head temperature of 145°C.
[0054] S4. Cooling, pelletizing and collecting: The continuous strip extruded from the die head is cooled and shaped, and after air drying, it is cut into pellets to obtain the finished blend.
[0055] In this process, the material strip is cooled and shaped by circulating cooling water at room temperature. After the surface moisture is dried by compressed air, it is sent to a pelletizer to be pelletized, resulting in cylindrical pellets with uniform particle size.
[0056] Example 3: This example provides a halogen-free flame-retardant SBS polymer blend, comprising the following raw materials in parts by weight: 85 parts of styrene-butadiene-styrene block copolymer matrix, 18 parts of double-bond functionalized intumescent flame-retardant microcapsules, 6 parts of end-capped polythiol siloxane crosslinking agent, 0.3 parts of alkenyl functionalized semi-hindered phenol regulator, 0.8 parts of composite antioxidant, and 1.2 parts of silicone lubricant.
[0057] Among them, the double-bond functionalized intumescent flame-retardant microcapsules have calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell layer, with polystyrene segments as short-chain polymer compatibility anchors. These microcapsules are prepared using the process described in Preparation Example 1 above. The end-capped polythiol siloxane crosslinking agent has polythiol cage-type silsesquioxane as the base material and acetone oxime as the blocking agent to end-cap the thiol groups. This crosslinking agent is prepared using the process described in Preparation Example 2 above. The styrene-butadiene-styrene block copolymer matrix has a linear structure, with styrene accounting for 40% by mass. The alkenyl functionalized semi-hindered phenol regulator is 2-tert-butyl-6-methyl-4-allylphenol, prepared using the process described in Preparation Example 3 above. The composite antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1.2.
[0058] The vacuum preparation method of the above-mentioned halogen-free flame-retardant SBS polymer blend includes the following steps: S1. Vacuum pre-drying: Vacuum drying is performed on all components of the raw materials to control the moisture content of the raw materials to meet the processing requirements.
[0059] The styrene-butadiene-styrene block copolymer matrix was placed in a vacuum drying oven and dried at 70°C and 0.09 MPa absolute vacuum for 6 hours to control the final moisture content to be no more than 0.05%. The double bond functionalized intumescent flame retardant microcapsules, the end-capped polythiol siloxane crosslinking agent, the alkenyl functionalized semi-hindered phenol regulator, the composite antioxidant, and the silicone lubricant were dried at 80°C and 0.09 MPa absolute vacuum for 2.5 hours to remove adsorbed moisture.
[0060] S2. Nitrogen premixing: All dried raw materials are placed in a nitrogen-protected environment for low-temperature mixing to obtain a uniform premixed material.
[0061] The process involves purging high-purity nitrogen to replace the air for 4 minutes before mixing, controlling the oxygen concentration in the mixing chamber to be no more than 500 ppm; setting the stirring speed to 400 r / min and the mixing time to 8 minutes; and controlling the temperature throughout the process using jacketed cooling water to ensure that the material temperature does not exceed 50℃.
[0062] S3. Gradient blending extrusion: The premixed material is fed into a co-rotating parallel twin-screw extruder and a gradient process with coordinated matching of temperature, vacuum and shear rate is adopted. The material passes through the feeding and conveying section, plasticizing and venting section, core reaction section, homogenization and termination section and die head discharge section in sequence to complete the desealing of end-capped thiol groups and interfacial covalent cross-linking blending treatment.
[0063] The feeding and conveying section maintains a normal pressure nitrogen atmosphere, with an oxygen content not exceeding 500 ppm and a temperature of 140℃. It employs a low-shear conveying thread configuration with a shear rate of 50 s⁻¹. The plasticizing and venting section has an absolute vacuum of 0.06 MPa and a temperature of 155℃, employing a weak-shear mixing thread configuration with a shear rate of 100 s⁻¹. The core reaction section has an absolute vacuum of 0.03 MPa, with residual oxygen in the cavity not exceeding 50 ppm and a temperature of 165℃, employing a medium-shear mixing... The refining thread configuration has a shear rate of 200 s⁻¹, and the effective residence time of the material in the core reaction section is 5 minutes, which can fully complete the construction of the interfacial covalent cross-linking network and improve the long-term stability of the material. In the homogenization termination section, the absolute vacuum is adjusted back to 0.07 MPa, and a trace amount of nitrogen is introduced simultaneously. The temperature is 155℃, and a weak shear conveying thread configuration is adopted with a shear rate of 80 s⁻¹. The discharge section of the die head maintains a slight positive pressure discharge of nitrogen, with a gauge pressure of 0.02 MPa and a die head temperature of 150℃.
[0064] S4. Cooling, pelletizing and collecting: The continuous strip extruded from the die head is cooled and shaped, and after air drying, it is cut into pellets to obtain the finished blend.
[0065] In this process, the material strip is cooled and shaped by circulating cooling water at room temperature. After the surface moisture is dried by compressed air, it is sent to a pelletizer to be pelletized, resulting in cylindrical pellets with uniform particle size.
[0066] Comparative Example 1: The only difference between this comparative example and Example 1 is that the end-capped polythiol siloxane crosslinking agent is replaced with an equal mass of uncapped polythiol cage silsesquioxane, and octamercaptopropyl cage silsesquioxane is used directly without acetone oxime end-capping treatment. The other raw material types and amounts, and preparation process parameters are exactly the same as in Example 1.
[0067] Comparative Example 2: The only difference between this comparative example and Example 1 is that the double-bond functionalized intumescent flame-retardant microcapsules are replaced with an equal mass of ordinary calcium phytate microcapsules. The microcapsules have unmodified melamine-formaldehyde resin as the capsule wall, no polystyrene segment compatibility anchors are grafted on the surface, and no allyl ether double bond modification is performed. The other raw material types and amounts, as well as the preparation process parameters, are exactly the same as in Example 1.
[0068] Comparative Example 3: The only difference between this comparative example and Example 1 is that the alkenyl functionalized semi-hindered phenol regulator is replaced with an equal mass of 2,6-di-tert-butyl-p-cresol. This substance is a conventional hindered phenol antioxidant, which only has the antioxidant function of phenolic hydroxyl groups and has no allyl double bonds that participate in the cross-linking reaction. The other types and amounts of raw materials and preparation process parameters are exactly the same as those in Example 1.
[0069] Comparative Example 4: The only difference between this comparative example and Example 1 is that in step S3 gradient blending extrusion, the core reaction section maintains a normal pressure nitrogen atmosphere, an absolute vacuum of 0.1 MPa, and an oxygen content in the cavity of no more than 500 ppm. High vacuum settings are not used. The process parameters and operations of the other sections are exactly the same as those of Example 1.
[0070] Comparative Example 5: The only difference between this comparative example and Example 1 is that a commercially available general-purpose V-0 grade halogen-free flame-retardant SBS elastomer is used as the control sample, and the raw material system and vacuum gradient preparation process of this scheme are not used. All other performance test conditions and evaluation criteria are exactly the same as those of Example 1.
[0071] I. Vertical Burning Performance Test: In accordance with GB / T2408-2021 "Determination of Burning Performance of Plastics - Horizontal and Vertical Methods", the samples of Examples 1 to 3 and Comparative Examples 1 to 5 were prepared into standard vertical burning specimens with a length of 125 mm, a width of 13 mm, and a thickness of 3.2 mm using an injection molding machine. Five parallel specimens were prepared for each group of samples. All specimens were first placed in a standard environment at a temperature of 23°C and a relative humidity of 50% for 48 hours to adjust their condition. Then, a Class V burning performance test was carried out using a vertical burning tester. Each specimen was subjected to two ignition operations, with each ignition lasting for 10 seconds. After the ignition, the flame burning time and flameless burning time of each specimen were recorded. It was observed whether the specimen produced molten droplets and whether the molten droplets ignited the degreased cotton layer below. Finally, the corresponding vertical burning rating was evaluated based on the overall burning performance of each group of specimens.
[0072] II. Tensile mechanical property testing: In accordance with GB / T1040.1-2018 "Determination of tensile properties of plastics - Part 1: General rules", the samples of Examples 1 to 3 and Comparative Examples 1 to 5 were prepared into 1A type standard tensile specimens with a thickness of 4 mm using an injection molding machine. Five parallel specimens were prepared for each group of samples. All specimens were first placed in a standard environment at 23°C and 50% relative humidity for 48 hours for conditioning. Then, a universal electronic tensile testing machine was used for tensile testing. The test tensile rate was set to 50 mm / min. Load and displacement data were collected in real time during the test. The tensile strength, elongation at break and tensile modulus of elasticity of each group of specimens were automatically calculated by the equipment system. Finally, the arithmetic mean of the test results of the five parallel specimens was taken as the final mechanical property parameters of the group of samples.
[0073] III. Tensile Strength Retention Rate Test After Accelerated Air Aging: In accordance with GB / T7141-2023 "Plastics - Accelerated Air Aging and Heat Resistance Test Method", the Type 1A standard tensile specimens corresponding to Examples 1 to 3 and Comparative Examples 1 to 5 were placed in a hot air aging test chamber. The aging test temperature was set to 100℃, and the aging duration was 168h. During the aging process, forced air circulation was maintained in the test chamber, and the wind speed was uniform and stable. After aging, all specimens were removed and placed in a standard environment with a temperature of 23℃ and a relative humidity of 50% for 24h to allow them to return to room temperature. Subsequently, the tensile strength after aging was tested in accordance with the requirements of GB / T1040.1-2018 "Determination of Tensile Properties of Plastics - Part 1: General Rules". The tensile strength retention rate of each group of samples was calculated based on the initial tensile strength before aging. Finally, the arithmetic mean of the test results of 5 parallel specimens was taken as the final retention rate value of the group of samples.
[0074] Table 1: Performance test results of each embodiment and comparative example: sample Vertical flammability rating Tensile strength / MPa Elongation at break / % Tensile modulus of elasticity / MPa Tensile strength retention rate after aging / % Example 1 V-0 14.2 610 186 92.3 Example 2 V-0 13.7 645 179 91.4 Example 3 V-0 14.0 585 193 91.8 Comparative Example 1 V-1 11.6 390 174 82.1 Comparative Example 2 V-1 10.3 360 169 78.4 Comparative Example 3 V-0 13.1 345 206 86.0 Comparative Example 4 V-1 11.0 520 163 80.2 Comparative Example 5 V-0 9.7 315 213 75.0 ; Note: V-0 is the highest vertical flammability rating specified in this standard, and the test specimen thickness is 3.2 mm.
[0075] As can be seen from Examples 1-3 and Comparative Example 1, and Table 1, end-capping treatment of mercaptosiloxane is an important step in ensuring processing stability and overall material performance. The end-capping structure can keep the crosslinking activity stable during the low-temperature processing stage, and release the activity gradually only in the set reaction section, avoiding uneven plasticization and local gelation problems caused by premature crosslinking of materials. This allows for controllable timing of the crosslinking reaction and helps to simultaneously consider the flame retardant properties and mechanical toughness of the material.
[0076] As can be seen from Examples 1-3 and Comparative Example 2, and Table 1, the double bond functionalization modification of flame-retardant microcapsules and the introduction of polystyrene segment compatibility anchors can effectively improve the interfacial bonding state between flame-retardant particles and the matrix. By anchoring the flame retardant at the matrix interface through covalent bonding, the possibility of flame-retardant particle migration and precipitation can be reduced, and the interfacial stress concentration can be alleviated, thereby promoting the synergistic improvement of flame-retardant performance and mechanical properties.
[0077] Combining Examples 1-3 and Comparative Example 3 with Table 1, it can be seen that the alkenyl functionalized semi-hindered phenol regulator has a dual effect. The allyl double bond in the molecule can participate in the thiol addition reaction, moderately consume crosslinking sites to regulate the overall crosslinking density, and avoid excessive crosslinking leading to material embrittlement. At the same time, the phenolic hydroxyl group can play a thermo-oxidative stabilizing role. Compared with ordinary hindered phenols, it is more suitable for the interfacial crosslinking system of this scheme, which is conducive to maintaining the toughness of the material.
[0078] As can be seen from Examples 1-3 and Comparative Example 4, and Table 1, the high vacuum setting in the core reaction section is crucial for the full advancement of the interfacial crosslinking reaction. The high vacuum environment can reduce the oxygen concentration in the reaction area and weaken the quenching effect of oxygen on thiol free radicals, thereby controlling the rate and extent of the free radical reaction and ensuring that the interfacial covalent crosslinking is successfully completed after the end-capped thiols are unsealed. This is the core process condition for improving material performance.
[0079] As can be seen from Examples 1-3 and Comparative Example 5, and Table 1, the functional flame retardant system of this scheme, combined with the vacuum gradient preparation process, can improve the tensile toughness and long-term aging resistance of the material while achieving the same flame retardant rating, compared with conventional commercial halogen-free flame retardant SBS products. The overall application advantages are more obvious.
[0080] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A halogen-free flame-retardant SBS polymer blend, characterized in that: By weight, it comprises the following components: 70 to 85 parts of styrene-butadiene-styrene block copolymer matrix, 12 to 18 parts of double bond functionalized intumescent flame-retardant microcapsules, 3 to 6 parts of end-capped polythiol siloxane crosslinking agent, 0.1 to 0.3 parts of alkenyl functionalized semi-hindered phenol regulator, 0.3 to 0.8 parts of composite antioxidant, and 0.5 to 1.2 parts of silicone lubricant; The surface of the capsule wall of the double-bond functionalized expandable flame-retardant microcapsule is grafted with carbon-carbon double bonds and short-chain polymer compatible anchor points. The thiol groups of the terminated polythiol siloxane crosslinking agent are terminated by a blocking agent. The alkenyl-functionalized semi-hindered phenol regulator molecule contains both a hindered phenolic hydroxyl group and a terminal allyl double bond.
2. The halogen-free flame-retardant SBS polymer blend according to claim 1, characterized in that: The double-bond functionalized expandable flame-retardant microcapsules have calcium phytate as the core layer and allyl ether-modified melamine-formaldehyde resin as the shell layer; the short-chain polymer compatibility anchor is a polystyrene segment.
3. The halogen-free flame-retardant SBS polymer blend according to claim 1, characterized in that: The terminated polythiol siloxane crosslinking agent uses polythiol cage-type silsesquioxane as the base material and acetone oxime as the blocking agent to terminate the thiol groups.
4. The halogen-free flame-retardant SBS polymer blend according to claim 1, characterized in that: The styrene-butadiene-styrene block copolymer matrix has a linear structure, and the styrene mass percentage is 30% to 40%; the alkenyl functionalized semi-hindered phenol regulator is 2-tert-butyl-6-methyl-4-allylphenol.
5. The halogen-free flame-retardant SBS polymer blend according to claim 1, characterized in that: The composite antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1 to 2:1.
2.
6. A vacuum preparation method for a halogen-free flame-retardant SBS polymer blend, characterized in that, The preparation of a halogen-free flame-retardant SBS polymer blend according to any one of claims 1 to 5 includes the following steps: S1. Vacuum pre-drying: Vacuum drying is performed on all component raw materials to control the moisture content of the raw materials to meet the processing requirements; S2, Nitrogen premixing: All dried raw materials are placed in a nitrogen-protected environment for low-temperature mixing to obtain a uniform premixed material; S3, Gradient Blending Extrusion: The premixed material is fed into a co-rotating parallel twin-screw extruder and a gradient process with coordinated matching of temperature, vacuum and shear rate is adopted. The material passes through the feeding and conveying section, plasticizing and venting section, core reaction section, homogenization and termination section and die head discharge section in sequence to complete the end-capped thiol desealing and interfacial covalent cross-linking blending treatment. S4. Cooling, pelletizing and collecting: The continuous strip extruded from the die head is cooled and shaped, and after air drying, it is cut into pellets to obtain the finished blend.
7. The vacuum preparation method of a halogen-free flame-retardant SBS polymer blend according to claim 6, characterized in that: In step S2, the nitrogen-protected low-temperature mixing specifically involves: purging high-purity nitrogen to replace the air for 2 to 4 minutes before mixing, ensuring that the oxygen concentration in the mixing chamber is no more than 500 ppm; and ensuring that the material temperature does not exceed 50°C during the mixing process.
8. The vacuum preparation method of a halogen-free flame-retardant SBS polymer blend according to claim 6, characterized in that: In step S3, the feeding and conveying section maintains a normal pressure nitrogen atmosphere, with an oxygen content of no more than 500 ppm and a temperature of 130 to 140°C; the plasticizing and exhaust section has an absolute vacuum of 0.05 to 0.06 MPa and a temperature of 145 to 155°C.
9. The vacuum preparation method of a halogen-free flame-retardant SBS polymer blend according to claim 6, characterized in that: In step S3, the absolute vacuum degree of the core reaction section is 0.02 to 0.03 MPa, the residual oxygen in the cavity is no more than 50 ppm, and the effective residence time of the material in the core reaction section is 3 to 5 minutes.
10. The vacuum preparation method of a halogen-free flame-retardant SBS polymer blend according to claim 6, characterized in that: In step S3, the absolute vacuum of the homogenization termination section is adjusted back to 0.06 to 0.07 MPa, and a trace amount of nitrogen is introduced simultaneously at a temperature of 150 to 155°C; the discharge section of the die head maintains a slight positive pressure discharge of nitrogen, with a gauge pressure of 0.01 to 0.02 MPa and a die head temperature of 145 to 150°C.