A composite material motor shaft, its preparation method and application

By using plasma activation and covalent bridging technology to form multi-level chemical bonds at the interface between carbon fiber and resin, the problem of debonding at the interface of carbon fiber composite motor shafts was solved, and the high strength, lightweight and fatigue resistance were improved.

CN123107312APending Publication Date: 2026-11-17EXTREME LIGHT POWER (BEIJING) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611481223.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing carbon fiber composite motor shafts are prone to interfacial debonding under long-term cyclic loads, leading to shaft delamination failure, weak interfacial bonding, and insufficient interfacial wettability and adhesion between carbon fiber and resin matrix.

Method used

A three-step interface engineering strategy of plasma activation → chemical grafting → covalent bridging was adopted to introduce reactive functional groups on the surface of carbon fibers and covalently bridge them with carbon nanotubes to form a multi-level chemical bonding interface, thereby enhancing the bonding between carbon fibers and resin.

Benefits of technology

It significantly improves the interfacial bonding strength and interlaminar shear strength, enhances the fatigue resistance and corrosion resistance of composite materials, reduces rotational inertia, and improves the lightweight and high power density performance of the motor shaft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107312A_ABST
    Figure CN123107312A_ABST
Patent Text Reader

Abstract

This invention provides a composite material motor shaft, its preparation method, and its application, belonging to the field of motor component manufacturing. The invention involves plasma surface activation treatment of carbon fibers; when the plasma treatment has introduced target carboxyl groups onto the carbon fiber surface, carbon fibers containing a first reactive functional group are directly obtained, or the surface-activated carbon fibers are chemically grafted in a grafting reaction solution to introduce amino, epoxy, or isocyanate groups; the first carbon nanotube is chemically modified to introduce a second reactive functional group, causing the second reactive functional group to undergo a covalent bridging reaction with the first reactive functional group; the resulting carbon fiber reinforcement with surface-grafted carbon nanotubes is then composited with a resin composite layer, molded, and cured to obtain the composite material motor shaft. This invention, through plasma activation, selective functionalization, and nano-interface bridging, forms a multi-layered chemical coupling interface between the carbon fiber and the resin, significantly enhancing the interfacial bonding performance of the composite material motor shaft.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of motor component technology, and in particular to a composite material motor shaft, its preparation method, and its application. Background Technology

[0002] The motor shaft is a core transmission component in an electric motor that transmits electromagnetic torque to the load. Its performance directly determines the motor's maximum speed, power density, operational smoothness, and service life. Currently, traditional motor shafts are mainly made of metal materials such as alloy steel and stainless steel, manufactured through processes such as forging, turning, grinding, and heat treatment. With the urgent need for lightweight and high power density in fields such as new energy vehicle drive motors, aerospace electric drive systems, and high-speed spindle motors, carbon fiber reinforced resin matrix composites (CFRP) have become a research hotspot for alternatives to metal motor shafts due to their high specific strength, high specific modulus, and excellent fatigue resistance. However, existing carbon fiber composite motor shafts suffer from weak interfacial bonding because the carbon fiber surface is chemically inert, has low surface energy, and insufficient interfacial wettability and bonding force with the resin matrix. Under long-term cyclic loading, interfacial debonding easily occurs, leading to shaft delamination failure. Related technologies disclose plasma treatment for carbon fiber surface activation, but the problem of low reinforcement potential at the carbon fiber-matrix interface still exists. Summary of the Invention

[0003] In view of this, the purpose of this invention is to provide a composite material motor shaft, its preparation method, and its application. This invention employs a three-step interface engineering strategy of plasma activation → chemical grafting → covalent bridging, forming a multi-layered chemical bonding interface between carbon fibers and resin, extending from the carbon fiber surface through covalently linked carbon nanotubes to the resin, thereby improving the interfacial bonding strength.

[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing a composite material motor shaft, comprising the following steps: Carbon fiber (CF) is subjected to plasma surface activation treatment to obtain surface-activated carbon fiber; when the plasma surface activation treatment is to introduce carboxyl groups on the surface of the carbon fiber, the surface-activated carbon fiber is directly used as a carbon fiber with a first reactive functional group on the surface; or, the surface-activated carbon fiber is immersed in a grafting reaction solution to carry out a chemical grafting reaction to introduce the first reactive functional group and obtain a carbon fiber with a first reactive functional group on the surface. The first carbon nanotube (CNT) is chemically modified to introduce a second reactive functional group, resulting in a carbon nanotube dispersion containing a second reactive functional group on its surface. The carbon fiber with a first reactive functional group on its surface is mixed with the carbon nanotube dispersion with a second reactive functional group on its surface. The second reactive functional group and the first reactive functional group undergo a covalent bridging reaction to obtain a carbon fiber reinforced with surface-grafted carbon nanotubes. Using the carbon fiber reinforcement with surface-grafted carbon nanotubes as the core layer and the resin composite layer as the outer layer, the carbon fiber reinforcement with surface-grafted carbon nanotubes is combined with the resin composite slurry, and then molded and cured sequentially to obtain the composite material motor shaft, wherein the resin composite layer contains a second carbon nanotube.

[0005] Preferably, the grafting reaction solution comprises a silane coupling agent solution or an isocyanate-based compound solution.

[0006] Preferably, the silane coupling agent in the silane coupling agent solution includes γ-aminopropyltriethoxysilane and / or γ-glycidoxypropyltrimethoxysilane.

[0007] Preferably, the first reactive functional group includes one or more of carboxyl, amino, isocyanate, and epoxy groups.

[0008] Preferably, the second reactive functional group includes one or more of carboxyl, amino, and epoxy groups.

[0009] Preferably, the concentration of the carbon nanotube dispersion containing a second reactive functional group on its surface is 0.01~1.0 mg / mL.

[0010] Preferably, the temperature of the covalent bridging reaction is 25~80℃, and the reaction time is 2~24h.

[0011] Preferably, the covalent bridging reaction further includes a carboxyl activation system, which includes 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide (EDC / NHS carboxyl activation system).

[0012] The present invention also provides a composite material motor shaft prepared by the preparation method described above, comprising a core layer and an outer layer, wherein the outer layer encapsulates the core layer, and the outer layer is a resin composite layer comprising resin and a second carbon nanotube. The core layer comprises, from the inside out, a carbon fiber layer, an interface bridging layer and a carbon nanotube layer, wherein the interface bridging layer is obtained by a covalent bridging reaction between a second reactive functional group and a first reactive functional group.

[0013] The present invention also provides the application of the composite material motor shaft described in the above technical solution in the field of electric drive.

[0014] This invention provides a method for preparing a composite material motor shaft, comprising the following steps: subjecting carbon fibers to plasma surface activation treatment; directly obtaining carbon fibers with a first reactive functional group on the surface when the plasma treatment has introduced target carboxyl groups, or chemically grafting the surface-activated carbon fibers in a grafting reaction solution to introduce amino, epoxy, or isocyanate groups; chemically modifying the first carbon nanotubes to introduce a second reactive functional group; causing the second reactive functional group to undergo a covalent bridging reaction with the first reactive functional group to obtain a carbon fiber reinforcement with surface-grafted carbon nanotubes; using the reinforcement as the core layer and a resin composite layer containing the second carbon nanotubes as the outer layer, and then sequentially molding and curing to obtain a composite material motor shaft.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Significantly improved interfacial bonding strength. Through a three-step interfacial engineering strategy of plasma activation → chemical grafting → covalent bridging, a multi-level chemical bonding interface is formed between carbon fiber and resin, extending from the carbon fiber surface to the resin matrix via covalent bonds. The interfacial shear strength (IFSS) is increased by 80% to 200% compared to untreated carbon fiber composites.

[0016] (2) Efficient dispersion and full utilization of carbon nanotubes. CNTs are anchored to the surface of carbon fibers through covalent bonds, effectively overcoming the agglomeration problem of CNTs when freely dispersed in resin. At the same time, the "brush-like" extended configuration of CNTs allows for full utilization of their specific surface area, maximizing their contact area with the resin matrix and load transfer efficiency.

[0017] (3) Construction of a three-dimensional continuous reinforcement network. A three-dimensional continuous reinforcement network is formed between carbon fiber (micron-scale reinforcing phase) → covalently bridged CNT (nano-scale reinforcing phase) → resin matrix, realizing a synergistic reinforcement effect across micro and nano scales. The interlaminar shear strength (ILSS) and flexural strength of the composite material motor shaft are improved.

[0018] (4) Significantly reduces rotational inertia and increases critical speed. The composite material motor shaft has a lower density, which greatly reduces the rotor's rotational inertia.

[0019] (5) Reduce eddy current loss. Although carbon fiber and CNT have certain conductivity, the overall composite material is a non-magnetic material. Eddy current loss of the composite material motor shaft described in this invention was not detected, which is beneficial to improving motor efficiency.

[0020] (6) Excellent fatigue resistance and corrosion resistance. The covalently bridged interface effectively inhibits interface debonding and microcrack propagation under cyclic loading, thus improving fatigue life. The resin matrix endows the motor shaft with excellent resistance to acid and alkali, salt spray and organic solvent corrosion.

[0021] (7) The process is highly adaptable and easy to scale up. The process conditions of each step are mild and controllable. Plasma treatment and chemical grafting can be carried out on a continuous production line, and it is directly compatible with existing carbon fiber composite molding processes (winding, pultrusion, RTM, etc.).

[0022] This invention also provides a composite material motor shaft prepared by the preparation method described above. It constructs a strong chemical bonding interface between carbon fiber and resin matrix, significantly improves the interfacial shear strength and interlaminar shear strength of composite material, realizes uniform dispersion and efficient chemical bonding of single-walled carbon nanotubes in resin matrix, gives full play to their nano-reinforcing effect, establishes a covalent bridging structure between carbon fiber and carbon nanotube, and forms a three-dimensional continuous reinforcement network of carbon fiber-carbon nanotube-resin / carbon nanotube. It is a motor shaft with lightweight, high strength, high modulus, high critical speed and excellent fatigue resistance. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the composite material motor shaft of the hollow cylindrical structure of the present invention; Figure 2 The image shows the morphological characteristics of carbon fiber using a scanning electron microscope. Figure 3 The image shows the scanning electron microscope (SEM) morphology of the carbon fiber / SWCNT interface. Figure 4 The surface morphology of the resin / / SWCNT is shown. In the diagram, 1 represents the core layer, 2 represents the outer layer, and 3 represents the hollow section. Detailed Implementation

[0024] This invention provides a method for preparing a composite material motor shaft, comprising the following steps: Carbon fibers are subjected to plasma surface activation treatment to obtain surface-activated carbon fibers; when the plasma surface activation treatment is to introduce carboxyl groups on the surface of the carbon fibers, the surface-activated carbon fibers are directly used as carbon fibers with a first reactive functional group on the surface; or, the surface-activated carbon fibers are immersed in a grafting reaction solution to carry out a chemical grafting reaction to introduce the first reactive functional group and obtain carbon fibers with a first reactive functional group on the surface. The first carbon nanotubes are chemically modified to introduce a second reactive functional group, resulting in a carbon nanotube dispersion containing a second reactive functional group on its surface. The carbon fiber with a first reactive functional group on its surface is mixed with the carbon nanotube dispersion with a second reactive functional group on its surface. The second reactive functional group and the first reactive functional group undergo a covalent bridging reaction to obtain a carbon fiber reinforced with surface-grafted carbon nanotubes. Using the carbon fiber reinforcement with surface-grafted carbon nanotubes as the core layer and the resin composite layer as the outer layer, the carbon fiber reinforcement with surface-grafted carbon nanotubes is combined with the resin composite slurry, and then molded and cured sequentially to obtain the composite material motor shaft, wherein the resin composite layer contains a second carbon nanotube.

[0025] Unless otherwise specified, all raw materials used in this invention are commercially available products in the field.

[0026] This invention involves plasma surface activation treatment of carbon fibers to obtain surface-activated carbon fibers. The plasma surface activation treatment introduces active functional groups, including hydroxyl (-OH), carboxyl (-COOH), carbonyl (C=O), and amino (-NH2), onto the surface of the carbon fibers, thereby increasing the surface roughness and surface energy of the carbon fibers.

[0027] In this invention, the plasma type for the plasma surface activation treatment is preferably radio frequency (RF) glow discharge plasma or dielectric barrier discharge (DBD) atmospheric pressure plasma. In this invention, the processing atmosphere of the plasma surface activation treatment is preferably a mixture of argon and other gases, wherein the volume fraction of argon in the mixture is preferably 70% to 100%, and the other gases preferably include one or more of oxygen, nitrogen, and a nitrogen-hydrogen mixture. The volume ratio of nitrogen to hydrogen in the nitrogen-hydrogen mixture is preferably 1:1 to 10:1 to avoid the reducing properties of hydrogen inhibiting excessive oxidation and to promote stable grafting of amino groups. When the processing atmosphere preferably includes oxygen and argon, the plasma surface activation treatment introduces oxygen-containing groups (including -OH, -COOH, C=O). When the processing atmosphere preferably includes nitrogen and argon, the plasma surface activation treatment introduces nitrogen-containing groups (including -NH2, -CN, C=N). When the processing atmosphere preferably includes nitrogen, hydrogen, and argon, the plasma surface activation treatment synergistically introduces nitrogen-containing groups.

[0028] In this invention, the processing power of the plasma surface activation treatment is preferably 50~500W, specifically 50, 100, 200, 300, 400 or 500W.

[0029] In this invention, the processing pressure of the plasma surface activation treatment is preferably 10~200Pa (low-pressure plasma, specifically 10, 50, 100, 150 or 200Pa) or atmospheric pressure (DBD plasma).

[0030] In this invention, the plasma surface activation treatment time is preferably 1 to 30 minutes, specifically 1, 5, 10, 20 or 30 minutes.

[0031] The present invention preferably places the carbon fiber in a low-temperature plasma treatment device to perform the plasma surface activation treatment.

[0032] In this invention, the carbon fiber is preferably carbon fiber fabric or carbon fiber tow.

[0033] After obtaining surface-activated carbon fibers, when the plasma surface activation treatment introduces carboxyl groups on the surface of the carbon fibers, the surface-activated carbon fibers are directly used as carbon fibers with a first reactive functional group on the surface; or, the surface-activated carbon fibers are immersed in a grafting reaction solution to carry out a chemical grafting reaction, introducing the first reactive functional group, and obtaining carbon fibers with a first reactive functional group on the surface.

[0034] In this invention, the first reactive functional group preferably includes one or more of carboxyl, amino, isocyanate and epoxy groups.

[0035] In this invention, when the first reactive functional group is a carboxyl group, it is preferable to directly introduce the carboxyl group using oxygen / argon plasma treatment, that is, the carboxyl group is introduced during the plasma surface activation treatment. When it is necessary to increase the carboxyl group density, this invention preferably further uses concentrated nitric acid for oxidation, that is, the carbon fiber after the carboxyl group is introduced by oxygen / argon plasma treatment is oxidized in concentrated nitric acid, the concentration of the concentrated nitric acid is preferably 68 wt%, and the oxidation is preferably refluxed at 65~90°C for 2~8 hours.

[0036] When the first reactive functional group is an amino, epoxy, or isocyanate group, the grafting reaction solution is preferably a solution of the corresponding silane coupling agent or an isocyanate compound solution.

[0037] In this invention, the mass ratio of the surface-activated carbon fiber to the grafting reagent is preferably 1:2 to 1:8, and the grafting reagent is a silane coupling agent or an isocyanate-based compound.

[0038] In this invention, the silane coupling agent in the silane coupling agent solution preferably includes γ-aminopropyltriethoxysilane (KH-550) and / or γ-glycidoxypropyltrimethoxysilane (KH-560), wherein KH-550 is used to introduce amino groups and KH-560 is used to introduce epoxy groups.

[0039] In this invention, the concentration of the silane coupling agent solution is preferably 0.5 to 5 wt%, specifically 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%, and the solute of the silane coupling agent solution is preferably ethanol, more preferably a 95 vol% aqueous solution of ethanol.

[0040] In this invention, the isocyanate-based compound in the isocyanate-based compound solution preferably includes one or more of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI).

[0041] In this invention, the concentration of the isocyanate-based compound solution is preferably 0.1-2 wt%, and the solute of the isocyanate-based compound solution is preferably anhydrous toluene or acetone.

[0042] In this invention, the temperature of the chemical grafting reaction is preferably room temperature to 80°C, and the reaction time is preferably 1 to 12 hours, specifically 1, 4, 8 or 12 hours.

[0043] After the chemical grafting reaction is completed, the present invention preferably subjectes the obtained grafted product to ultrasonic washing and vacuum drying in sequence to obtain carbon fibers with the first reactive functional group on the surface.

[0044] In this invention, the detergent used for ultrasonic cleaning is preferably anhydrous ethanol or acetone.

[0045] The present invention introduces a second reactive functional group into the first carbon nanotube by chemical modification, thereby obtaining a carbon nanotube dispersion containing the second reactive functional group on its surface.

[0046] In this invention, the first carbon nanotube is preferably a single-walled carbon nanotube (SWCNT), and the diameter of the single-walled carbon nanotube is preferably 0.7~3nm, and the length is preferably 1~100μm.

[0047] In this invention, the second reactive functional group preferably includes one or more of carboxyl, amino, and epoxy groups.

[0048] When the second reactive functional group is a carboxyl group, the chemical modification preferably includes the following steps: refluxing the CNT in concentrated nitric acid, wherein the mass fraction of the concentrated nitric acid is preferably 68%, the reflux temperature is preferably 65~90℃, and the time is preferably 2~8h, to obtain carboxyl CNT.

[0049] When the second reactive functional group is amino, the chemical modification preferably includes the following steps: dispersing the carboxyl CNT in a buffer solution with a pH of 5.0 to 6.0, mixing it with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC·HCl) and N-hydroxysuccinimide (NHS) to activate the carboxyl group, and then mixing it with ethylenediamine to carry out an amidation reaction to obtain amino-modified CNT.

[0050] In this invention, the buffer solution preferably includes MES (2-morpholinoethanesulfonic acid) buffer.

[0051] In this invention, the molar ratio of carboxyl group, EDC·HCl and NHS in the carboxyl CNT is preferably 1:1:1.

[0052] In this invention, the temperature for activating the carboxyl group is preferably 20~30℃, more preferably 25℃, and the time is preferably 0.5~2h, more preferably 1h.

[0053] In this invention, the mass ratio of ethylenediamine to carboxyl CNT is preferably 5:1 to 30:1, more preferably 15:1. In this invention, the temperature of the amidation reaction is preferably 20~60°C, more preferably 20, 30, 40, 50 or 60°C, and the time is preferably 4~24h, more preferably 4, 12 or 24h.

[0054] After the amidation reaction is completed, the product is preferably filtered and washed with water and ethanol in sequence, and then vacuum dried at 50-80°C for 6-24 hours to obtain amino-modified CNTs.

[0055] When the second reactive functional group is an epoxy group, the chemical modification preferably includes the following steps: An epoxy-containing silane coupling agent is dispersed in a dispersant, the pH is adjusted to 4.0~5.5, and then hydrolyzed to obtain the hydrolysis product. The carboxyl CNTs were mixed with the hydrolysis products and reacted to obtain epoxy-modified CNTs, namely CNT-EP.

[0056] In this invention, the epoxy-containing silane coupling agent preferably includes γ-glycidoxypropyltrimethoxysilane.

[0057] In this invention, the dispersant preferably comprises ethanol and water.

[0058] The present invention preferably uses acetic acid to adjust the pH value, and the pH value is preferably 4.5.

[0059] In this invention, the temperature of the hydrolysis treatment is preferably 20~30℃, more preferably 25℃, and the time is preferably 20~60min, more preferably 30min.

[0060] In this invention, the mass ratio of the epoxy-containing silane coupling agent to the carboxyl CNT is preferably 1:1 to 10:1, more preferably 5:1.

[0061] In this invention, the reaction temperature is preferably 50~80℃, more preferably 60℃, and the reaction time is preferably 2~12h, more preferably 6h.

[0062] After the reaction is completed, the product is preferably filtered and washed with ethanol and deionized water in sequence, and then dried under vacuum at 50~80°C for 6~24h to obtain the epoxy-modified CNT.

[0063] In this invention, the concentration of the carbon nanotube dispersion containing a second reactive functional group on its surface is preferably 0.01~1.0 mg / mL, specifically 0.01, 0.1, 0.2, 0.4, 0.6, 0.8 or 1.0 mg / mL.

[0064] In this invention, the dispersant of the carbon nanotube dispersion containing a second reactive functional group on its surface preferably includes anhydrous dimethylformamide (DMF) or N-methylpyrrolidone (NMP).

[0065] After obtaining a dispersion of carbon fibers with a first reactive functional group on their surface and a dispersion of carbon nanotubes with a second reactive functional group on their surface, the present invention mixes the carbon fibers with the first reactive functional group and the dispersion of carbon nanotubes with the second reactive functional group on their surface. The second reactive functional group and the first reactive functional group undergo a covalent bridging reaction to obtain a carbon fiber reinforcement with surface-grafted carbon nanotubes. A schematic diagram of the structure of the formed carbon fiber reinforcement with surface-grafted carbon nanotubes is shown below. Figure 1 As shown.

[0066] In this invention, the covalent bridging reaction preferably includes the following types: Carbon fiber surface -COOH + CNT surface -NH2 → amide bond (-CO-NH-); Carbon fiber surface -NH2+CNT surface -COOH→amide bond (-CO-NH-); Carbon fiber surface -NCO+CNT surface -NH2→urea bond (-NH-CO-NH-); Carbon fiber surface - epoxy group + CNT surface -NH2 → secondary amine bond (-CH(OH)-CH2-NH-); Carbon fiber surface -NH2+CNT surface -epoxy group → secondary amine bond (-CH(OH)-CH2-NH-).

[0067] In this invention, the temperature of the covalent bridging reaction is preferably 25~80℃, and the reaction time is preferably 2~24h. During the covalent bridging reaction, CNTs are anchored to the carbon fiber surface at one end through covalent bonds, while the other end extends freely to form a "brush-like" or "cluster-like" nano-interface structure.

[0068] In this invention, the covalent bridging reaction is preferably carried out with the addition of a corresponding catalyst or activator according to the functional group combination; in the amidation reaction of carboxyl and amino groups, the EDC / NHS activation system is preferably used, and triethylamine can be added to adjust the reaction system; in the isocyanate reaction, dibutyltin dilaurate is preferably used.

[0069] In this invention, the molar ratio of carboxyl groups, EDC·HCl and NHS in the system undergoing the covalent bridging reaction is preferably 1:1:1.

[0070] In this invention, the amount of the amine catalyst is preferably 5-25% of the mass of the carbon fiber containing the first reactive functional group on its surface. When the amine catalyst is added, the temperature of the covalent bridging reaction is preferably 20-60°C, and the time is preferably 12 hours.

[0071] In this invention, the amount of the tin catalyst is preferably 0.001 to 0.5% of the mass of the carbon fiber containing the first reactive functional group on its surface. When the tin catalyst is added, the temperature of the covalent bridging reaction is preferably 20 to 60°C, and the time is preferably 12 hours.

[0072] The present invention preferably involves impregnating the carbon fibers containing a first reactive functional group on their surface with a dispersion of carbon nanotubes containing a second reactive functional group on their surface to carry out the covalent bridging reaction.

[0073] After the covalent bridging reaction is completed, the present invention preferably removes unreacted CNTs by washing with DMF or NMP, and then vacuum drying to obtain the carbon fiber reinforcement with CNT grafted on the surface.

[0074] After obtaining the carbon fiber reinforcement with surface-grafted carbon nanotubes, the present invention uses the carbon fiber reinforcement with surface-grafted carbon nanotubes as the core layer and the resin composite layer as the outer layer. The carbon fiber reinforcement with surface-grafted carbon nanotubes is compounded with the resin composite slurry and then molded and cured in sequence to obtain the composite material motor shaft. The resin composite layer contains a second carbon nanotube.

[0075] In this invention, the mass of the resin composite layer is preferably 30-50 wt% of the carbon fiber reinforcement with surface-grafted carbon nanotubes.

[0076] In this invention, the resin matrix in the resin composite slurry preferably includes one or more of epoxy resin, phenolic resin, bismaleimide resin, cyanate ester resin and polyether ether ketone (PEEK), and the epoxy resin preferably includes one or more of bisphenol A type, bisphenol F type and alicyclic epoxy resin, and the resin composite slurry forms the resin composite layer.

[0077] In this invention, the mass of the second carbon nanotube is preferably 0.05% to 2% of the mass of the resin matrix.

[0078] In this invention, the second carbon nanotube is preferably SWCNT.

[0079] In this invention, the resin composite slurry is preferably prepared by a method comprising the following steps: The second carbon nanotube and organic solvent were ultrasonically dispersed to obtain a carbon nanotube dispersion. The resin matrix is ​​pretreated to obtain a pretreated resin matrix; The carbon nanotube dispersion is mixed with a pretreated resin matrix to obtain the resin composite slurry.

[0080] The present invention involves ultrasonically dispersing the second carbon nanotube and an organic solvent to obtain a carbon nanotube dispersion.

[0081] In this invention, the organic solvent preferably includes one or more of anhydrous ethanol, DMF and N-methylpyrrolidone, and is preferably selected according to the resin system.

[0082] In this invention, the ultrasonic dispersion time is preferably 30-60 min. The ultrasonic dispersion is used to depolymerize and reduce carbon nanotube agglomeration, so as to obtain a uniform carbon nanotube dispersion.

[0083] In this invention, the dispersant is preferably added according to the resin system during ultrasonic dispersion, and the dispersant preferably includes one or more of polyvinylpyrrolidone (PVP), polyvinyl butyral (PVB), polyetherimide (PEI), and polymethyl methacrylate (PMMA).

[0084] In this invention, the amount of the dispersant is preferably 5 to 80% of the mass of the second carbon nanotube.

[0085] The present invention pretreats the resin matrix to obtain a pretreated resin matrix.

[0086] When the resin matrix is ​​preferably a liquid resin (including epoxy resin, cyanate ester resin, phenolic resin), the pretreatment preferably includes the following steps: constant temperature preheating to reduce viscosity, wherein the constant temperature preheating temperature is preferably 30~70℃; when the resin matrix is ​​preferably a solid resin (including PEEK, bismaleimide resin), the pretreatment preferably includes the following steps: pulverizing and grinding the solid resin matrix into micron-sized powder, wherein the particle size of the micron-sized powder is preferably 10~100μm, more preferably 20~75μm.

[0087] After obtaining the carbon nanotube dispersion and the pretreated resin matrix, the present invention mixes the carbon nanotube dispersion with the pretreated resin matrix to obtain the resin composite slurry.

[0088] In this invention, the carbon nanotube dispersion is preferably added to a pretreated resin matrix, and the mixture is stirred at high speed with a gradient increase in temperature. Solution blending or melt blending is selected according to the characteristics of the resin system to ensure that CNTs are uniformly dispersed in the resin system, thereby obtaining the resin composite slurry.

[0089] In this invention, the preferred heating rate of the gradient heating and high-speed stirring mixture is 2~10℃ / min, the preferred holding temperature is 40~100℃, and the preferred stirring rate is 1000~10000r / min, more preferably 2000~8000r / min.

[0090] When the resin matrix is ​​preferably bismaleimide resin, melt blending is preferably performed at 120~165°C; when the resin matrix is ​​PEEK, melt blending is preferably performed at 380~400°C using a twin-screw extruder, wherein the screw speed of the twin-screw extruder is preferably 50~300 r / min.

[0091] The present invention does not impose any particular limitation on the specific method of solution blending or melt blending, and any method known to those skilled in the art can be used.

[0092] In this invention, the mixing process preferably includes the addition of one or more of a curing agent, an accelerator, and a defoamer.

[0093] When the resin matrix is ​​a thermosetting resin, it is preferable to add the curing agent, accelerator and defoamer; when the resin matrix is ​​a PEEK thermoplastic resin, it is preferable not to add the curing agent, and to use melt molding and cooling to set the shape.

[0094] In this invention, the mixing process preferably includes vacuum degassing for 10-30 minutes to remove air bubbles from the system and obtain the resin composite slurry.

[0095] In a specific embodiment of the present invention, the resin composite slurry preferably includes the following: (1) Bisphenol F type epoxy resin / SWCNT composite material Raw material ratio (parts by weight): 100 parts bisphenol F type epoxy resin, 0.3 parts SWCNT, 65 parts curing agent (polythiol), 0.3 parts accelerator (2,4,6-tris(dimethylaminomethyl)phenol (DMP-30)), 25 parts anhydrous ethanol; The preparation steps of the bisphenol F type epoxy resin / SWCNT composite material include the following steps: SWCNT was added to anhydrous ethanol and ultrasonically dispersed for 35 min to prepare a dispersion. The bisphenol F epoxy resin was stirred at room temperature for 10 minutes, and the dispersion was mixed in. The mixture was stirred at 60°C for 45 minutes until the solvent was completely evaporated. Add curing agent and accelerator, stir evenly, and then degas under vacuum for 15 minutes.

[0096] (2) Alicyclic epoxy resin / SWCNT composite material Raw material ratio (parts by weight): 100 parts alicyclic epoxy resin, 0.8 parts SWCNT, 75 parts acid anhydride curing agent, and 0.4 parts curing accelerator (N,N-dimethylbenzylamine (BDMA)).

[0097] Preparation steps: SWCNTs were surface modified with silane coupling agent to obtain modified SWCNTs. SWCNTs were mixed with an ethanol solution of silane coupling agent and stirred for 30 min. After drying, they were mixed with alicyclic epoxy resin, acid anhydride curing agent and curing accelerator, and then vacuum degassing was performed.

[0098] (3) Phenolic resin / SWCNT composite material Raw material ratio (parts by weight): 100 parts phenolic resin, 0.6 parts SWCNT, 5 parts hexamethylenetetramine curing agent, and 40 parts ethanol.

[0099] Preparation steps: SWCNT is ultrasonically dispersed in ethanol, thoroughly mixed with phenolic resin, stirred at 70°C to evaporate the solvent, hexamethylenetetramine curing agent is added and mixed evenly, and then vacuum degassing is performed.

[0100] (4) Bismaleimide resin / SWCNT composite material Raw material ratio (parts by weight): 100 parts bismaleimide resin, 0.4 parts SWCNT, and 15 parts allylphenol modifier.

[0101] Preparation steps: Grind bismaleimide resin into powder, mix with SWCNT powder dry powder for 30 min, add allylphenol, heat to 130~140℃ and stir for 20~30 min to fully mix the components and carry out prepolymerization reaction; then heat to 180℃ to obtain uniformly molten bismaleimide resin / SWCNT composite material.

[0102] (5) Cyanate ester resin / SWCNT composite material Raw material ratio (parts by weight): 100 parts of cyanate ester resin, 0.5 parts of SWCNT, and 0.2 parts of stannous octoate catalyst. The role of the stannous octoate catalyst is to improve the degree of curing of the resin.

[0103] Preparation steps: Melt and preheat cyanate resin at 80℃, add ultrasonically dispersed SWCNT suspension, stir at constant temperature for 50 min, add catalyst and mix well, and degas under vacuum.

[0104] (6) PEEK / SWCNT thermoplastic composite material Raw material ratio (parts by weight): 100 parts of PEEK ultrafine powder (particle size 2~100μm), 0.7 parts of SWCNT, and 0.2 parts of antioxidant (antioxidant 1010).

[0105] Preparation steps: PEEK powder, SWCNT and antioxidant are dry premixed using a melt blending process to obtain a premix; the premix is ​​fed into a twin-screw extruder and melt blended at 380~400℃ and screw speed 50~300r / min; the extrudate is water-cooled and pelletized to obtain PEEK / SWCNT thermoplastic composite granules; the PEEK / SWCNT thermoplastic composite granules are melted and coated onto the surface of a pre-prepared core layer; after injection molding and cooling, the composite motor shaft is obtained.

[0106] (7) Resin compounding system (bisphenol A epoxy + cyanate ester) / SWCNT composite material Raw material ratio (parts by weight): 60 parts of bisphenol A type epoxy resin, 40 parts of cyanate ester resin, 0.6 parts of SWCNT, and composite curing agent (40~50 parts of methyltetrahydrophthalic anhydride + 0.2~1.0 parts of 2-ethyl-4-methylimidazolium).

[0107] Preparation steps: First, bisphenol A type epoxy resin and cyanate ester resin are blended and melted uniformly at 70°C. Then, SWCNT dispersion is added (the dispersant of the SWCNT dispersion preferably includes one or more of acetone, anhydrous ethanol and NMP). The mixture is stirred and dispersed at a constant temperature. A composite curing agent is added, and the mixture is degassed under vacuum to balance the high adhesion of epoxy resin with the low dielectric and high heat resistance of cyanate ester resin.

[0108] (8) Resin compounding system (phenolic + bismaleimide) / SWCNT composite material Raw material ratio (parts by weight): 50 parts phenolic resin, 50 parts bismaleimide resin, 0.5 parts SWCNT.

[0109] Preparation steps: Powder blending + solution-assisted dispersion. After premixing the two resin powders, CNT dispersion is added for wetting and mixing, and then dried to remove solvent, thereby improving the high temperature resistance and aging resistance of the composite material.

[0110] In this invention, the carbon fiber reinforcement with surface-grafted carbon nanotubes is preferably impregnated in the resin composite slurry.

[0111] In this invention, the molding process is preferably filament winding, pultrusion, resin transfer molding (RTM), vacuum-assisted resin injection (VARI), or prepreg compression molding.

[0112] In this invention, the curing is carried out based on the resin composite slurry, and preferably includes the following methods: When the resin composite slurry is preferably a bisphenol F type epoxy resin / SWCNT composite material, the molding is preferably a molding process, and the curing includes the following steps: curing at 90°C for 1.5 hours, curing at 130°C for 2.5 hours, and then cooling and demolding to obtain the composite material motor shaft; When the resin composite slurry is preferably an alicyclic epoxy resin / SWCNT composite material, the curing is a segmented high-temperature curing, the highest temperature of the segmented high-temperature curing is 180℃, and the segmented high-temperature curing process is to keep at 80℃ for 1 hour, keep at 120℃ for 2 hours, keep at 150℃ for 2 hours, keep at 180℃ for 2 hours, and then cool to room temperature. When the resin composite slurry is preferably a phenolic resin / SWCNT composite material, the curing is performed by first pre-curing at 100°C for 1 hour, then hot-pressing at 150°C for 3 hours at a pressure of 5 MPa, followed by cooling, to obtain the composite material motor shaft. When the resin composite slurry is preferably a bismaleimide resin / SWCNT composite material, the molding is plasticizing, and the curing is hot-pressing curing at 220°C for 4 hours at a pressure of 5MPa to obtain the composite material motor shaft. When the resin composite slurry is preferably a cyanate ester resin / SWCNT composite material, the curing is carried out in three stages: 120℃ / 2h, 160℃ / 2h, and 200℃ / 2h, with a total curing time of 6h, to obtain the composite material motor shaft. When the resin composite slurry is preferably a resin compound system (bisphenol A epoxy + cyanate ester) / SWCNT composite material, the curing is a segmented curing process, which is to keep the temperature at 100°C for 1 hour, at 130°C for 2 hours, at 160°C for 2 hours, at 190°C for 3 hours, and then cool it to room temperature in the furnace. When the resin composite slurry is preferably a resin compound system (phenolic + bismaleimide) / SWCNT composite material, the curing is high-temperature hot-press curing, the temperature of the high-temperature hot-press curing is 180~220℃, the time is 2~4h, and the pressure is 5~15MPa.

[0113] In this invention, the composite is preferably made by coating the resin composite slurry onto the surface of the carbon fiber reinforcement grafted with carbon nanotubes.

[0114] In this invention, the forming is preferably an alternating circumferential and helical winding, and the winding tension is preferably 5~15N.

[0115] This invention provides a plasma-activated carbon fiber-chemically modified carbon nanotube / resin-carbon nanotube composite motor shaft. The core technology concept is: plasma activation → double-end chemical modification → covalent bridging → resin coating integrated molding.

[0116] The present invention also provides a composite material motor shaft prepared by the preparation method described above, comprising a core layer and an outer layer, wherein the outer layer encapsulates the core layer, and the outer layer is a resin composite layer comprising resin and a second carbon nanotube. The core layer comprises, from the inside out, a carbon fiber layer, an interface bridging layer and a carbon nanotube layer, wherein the interface bridging layer is obtained by a covalent bridging reaction between a second reactive functional group and a first reactive functional group.

[0117] In this invention, the volume of the outer layer of the composite material motor shaft is preferably 50% to 70%.

[0118] In this invention, the composite material motor shaft is preferably a hollow cylindrical structure or a solid cylindrical structure.

[0119] When the composite material motor shaft is preferably a hollow cylindrical structure, it is produced by alternating circumferential and helical winding, resin impregnation, and curing using a core-pulling mold, followed by demolding.

[0120] In this invention, the resin content in the composite material motor shaft is preferably 20-35 wt%.

[0121] Figure 1 This is a schematic diagram of the composite material motor shaft of the hollow cylindrical structure of the present invention. In the figure, 1 is the core layer, 2 is the outer layer, and 3 is the hollow part.

[0122] The present invention also provides the application of the composite material motor shaft described in the above technical solution in the field of electric drive.

[0123] In this invention, the composite material motor shaft is preferably used in new energy vehicle drive motors, aerospace electric drive systems, and high-speed spindle motors to meet the urgent need for lightweight and high power density.

[0124] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0125] Example 1 Step (1) Carbon fiber plasma treatment Carbon fiber fabric was placed in a radio frequency plasma treatment device. Treatment parameters: oxygen / argon mixture (argon 70% by volume, oxygen 30% by volume), radio frequency power 200W, chamber pressure 50Pa, treatment time 10min. The water contact angle on the carbon fiber surface decreased from 85° to 25° after treatment.

[0126] Step (2) Grafting amino functional groups onto the surface of carbon fibers The plasma-treated carbon fibers were immersed in an ethanol / water solution containing 2 wt% KH-550 (ethanol to water volume ratio 95:5) and reacted at room temperature for 4 h. After removal, they were ultrasonically washed three times with anhydrous ethanol (10 min each time) and vacuum dried at 60 °C for 2 h to obtain carbon fibers (CF-NH2) with amino grafts on the surface. Figure 2 The image shows the morphological characteristics of the carbon fiber using scanning electron microscopy. Note: The carboxyl group introduced in step (1) was not activated by EDC / NHS in the room temperature ethanol / water system in step (2), and will not undergo significant amidation with the amino group introduced by KH-550; this step is mainly due to the condensation of silanol formed by the hydrolysis of KH-550 with the oxygen-containing sites on the carbon fiber surface, and the terminal amino group of KH-550 is retained for the covalent bridging reaction in step (4).

[0127] Step (3) Carboxylation of single-walled carbon nanotubes Carboxylation: Take 1.0 g of single-walled carbon nanotubes (3 nm in diameter and 100 μm in length), add 100 mL of concentrated nitric acid (68 wt%), and reflux and stir at 80 °C for 6 h. After cooling, wash repeatedly with deionized water until neutral, filter under vacuum, and dry under vacuum at 60 °C to obtain carboxylated SWCNTs (SWCNT-COOH).

[0128] Step (4) Covalent bridging of carbon fiber and SWCNT SWCNT-COOH was ultrasonically dispersed in anhydrous DMF to prepare a dispersion with a concentration of 0.2 mg / mL. Based on the pre-determined carboxyl content on the surface of SWCNT-COOH, EDC·HCl and NHS were added in a molar ratio of 1:1:1. The mixture was stirred and activated at room temperature for 2 hours to obtain the activated SWCNT-COOH dispersion.

[0129] The obtained CF-NH2 was immersed in the above-activated SWCNT-COOH dispersion, and triethylamine was added at 0.1% of the total volume of the dispersion. The mixture was stirred at 40°C for 12 hours to allow the amino groups on the surface of CF-NH2 to undergo amidation with the activated carboxyl groups on the surface of SWCNT-COOH.

[0130] After the reaction, the carbon fibers were removed and washed three times each with DMF and deionized water, and then vacuum dried at 60°C to obtain carbon fibers (CF-g-SWCNT) with surface covalently grafted single-walled carbon nanotubes. The scanning electron microscope morphology of the carbon fiber / SWCNT interface is shown in the figure below. Figure 3 As shown.

[0131] Step (5) Resin impregnation and motor shaft molding Bisphenol F type epoxy resin / SWCNT composite material is used Raw material ratio (parts by weight): 100 parts bisphenol F type epoxy resin, 0.3 parts SWCNT, 65 parts polythiol curing agent, 0.3 parts accelerator DMP-30, and 25 parts anhydrous ethanol.

[0132] Preparation steps: SWCNT was added to anhydrous ethanol and ultrasonically dispersed for 35 min to prepare a uniform dispersion. Stir the bisphenol F epoxy resin at room temperature for 10 minutes, then mix in the dispersion and stir at 60°C for 45 minutes until the solvent is completely evaporated. Add curing agent and accelerator, stir evenly, and then degas under vacuum for 15 minutes to obtain bisphenol F type epoxy resin / SWCNT composite material; Step (6) Composite After coating the surface of the CF-g-SWCNT with the bisphenol F type epoxy resin / SWCNT composite material, it is molded and then cured at 90℃ for 1.5h and 130℃ for 2.5h respectively. After cooling and demolding, the composite material motor shaft is obtained. Figure 4 This is a surface morphology image of bisphenol F type epoxy resin / SWCNT.

[0133] Based on the cross-sectional dimensions of the motor shaft and the mass after curing, the outer layer of the composite material motor shaft has a volume of 60% and a resin content of 30wt%.

[0134] Example 2 (Example of Nitrogen-Containing Plasma Atmosphere) This embodiment is used to investigate the effect of plasma atmosphere on the degree of amination of carbon fiber surface and subsequent covalent bridging effect. Except for changing the plasma atmosphere in step (1) of Example 1 to a N2-H2-Ar mixture (N2, H2 and Ar volume ratio of 70:10:20), it is the same as Example 1, and the composite material motor shaft of Example 2 is obtained.

[0135] Example 3 (SWCNT dispersion concentration) Similar to Example 1, except that the concentration of the SWCNT-COOH dispersion used in step (4) is 0.40 mg / mL.

[0136] Example 4 Similar to Example 1, the difference is that the concentrations of the SWCNT-COOH dispersion used in step (4) are 0.01, 0.05, 0.10, 0.60, 0.80 and 1.00 mg / mL, respectively, and are recorded as Examples 4-1 to 4-6. The concentrations are compared with those of 0.20 mg / mL in Example 1 and 0.40 mg / mL in Example 3 by single-factor comparison, and the test results are shown in Table 2.

[0137] Comparative Example 1: Untreated virgin carbon fiber Material Scheme: Untreated virgin carbon fiber + epoxy resin / SWCNT matrix The process difference from Example 1 is that the carbon fiber has no surface modification, and SWCNTs are only dispersed freely in the resin without interfacial nanobridges.

[0138] Comparative Example 2: Plasma-activated carbon fibers only Material scheme: Plasma-activated carbon fiber + epoxy resin / SWCNT matrix only The process differs from Example 1 in that it involves only physical etching activation, without chemical grafting or covalent grafting of SWCNTs, relying solely on physical bonding through a rough surface. Comparative Example 3: Plasma activation + physical adsorption of SWCNTs (untreated SWCNTs) Material scheme: Plasma activated carbon fiber + physically impregnated free SWCNT + epoxy resin / SWCNT matrix The process difference from Example 1 is that SWCNTs are only ion-adsorbed on the carbon fiber surface and are easily detached by washing / ultrasound, and have no stable amide covalent bonds.

[0139] Comparative Example 4: 40Cr alloy steel metal shaft Material selection: 40Cr alloy steel motor shaft (traditional metal standard).

[0140] Example 5: Covalent bonding of carboxyl groups on carbon fiber surface with aminated SWCNTs Material scheme: Surface carboxylated carbon fiber (CF-COOH) + surface aminated SWCNT (SWCNT-NH2) + epoxy resin / SWCNT matrix Same as Example 1, except that: in step (2), KH-550 grafted amino groups are not used, but the carboxyl groups introduced on the carbon fiber surface after oxygen / argon plasma treatment are retained; in step (3), SWCNT-COOH is further activated by EDC / NHS and subjected to amidation reaction with ethylenediamine to obtain SWCNT-NH2; in step (4), CF-COOH and SWCNT-NH2 undergo amidation reaction to form -CO-NH- covalent bonds.

[0141] Specifically, step (3) is as follows: SWCNT-COOH is dispersed in MES buffer at pH 5.5, activated at 25°C for 1 h at a molar ratio of 1:1:1 for carboxyl, EDC·HCl and NHS, ethylenediamine is added (mass ratio of ethylenediamine to SWCNT-COOH is 15:1), reacted at 40°C for 12 h, and then washed and dried to prepare a 0.2 mg / mL SWCNT-NH2 dispersion.

[0142] Example 6: Covalent bonding of carbon fiber surface aminated and epoxy-modified SWCNTs Material scheme: Surface-aminated carbon fiber (CF-NH2) + surface-epoxy-modified SWCNT (SWCNT-EP) + epoxy resin / SWCNT matrix Same as Example 1, except that: in step (3), SWCNT-COOH is surface modified with KH-560 to obtain SWCNT-EP; in step (4), CF-NH2 and SWCNT-EP undergo an epoxy ring-opening reaction to form a -CH(OH)-CH2-NH- covalent bond, without adding EDC / NHS.

[0143] Specifically, step (3) is as follows: KH-560 is added to a mixed solvent of ethanol / deionized water, the pH value is adjusted to 4.5 with acetic acid, and hydrolyzed at 25℃ for 30 min; SWCNT-COOH is added, the mass ratio of KH-560 to SWCNT-COOH is 5:1, the reaction is carried out at 60℃ for 6 h, and after washing and drying, a 0.2 mg / mL SWCNT-EP dispersion is prepared.

[0144] The performance test results of the motor shaft are shown in Table 1.

[0145] Table 1 Performance test results of the motor shaft

[0146] As shown in Table 1, the present invention has the following advantages: 1. Improved interfacial bonding strength (IFSS / ILSS) Comparative Example 1: The surface of the virgin carbon fiber is inert and lacks active functional groups, allowing only physical adsorption. Comparative Example 2: Only plasma treatment was performed, without subsequent chemical grafting or covalent bridging. Comparative Example 3: No EDC / NHS was added, and SWCNTs were mainly physically adsorbed. Example 1: Plasma activation, KH-550 grafting of amino groups, and EDC / NHS-mediated amidation covalent bridging increased the IFSS from 32.5 MPa in Comparative Example 1 to 91.2 MPa, an increase of 180.6%; the ILSS increased from 47.8 MPa to 115.4 MPa, an increase of 141.4%. Example 5: CF-COOH and SWCNT-NH2 formed amide bonds, with IFSS and ILSS of 86.4 MPa and 108.7 MPa, respectively. Example 6: CF-NH2 and SWCNT-EP underwent an epoxy ring-opening reaction, with IFSS and ILSS of 82.7 MPa and 103.5 MPa, respectively. Both sets of results were significantly higher than those of Comparative Example 3, indicating that after changing the functional groups at the ends of carbon fibers or SWCNTs, interface reinforcement can still be achieved through stable covalent bonds; their performance was slightly lower than that of Example 1, indicating that the CF-NH2 / SWCNT-COOH amidation system has a high interface grafting efficiency under the process conditions of this set.

[0147] 2. SWCNT dispersion and nano-reinforcement effect In Comparative Example 3, SWCNTs mainly relied on physical adsorption, with a fiber surface grafting efficiency of only 16.8%; the grafting efficiency in Example 1 was 74.3%. In Example 1, SWCNTs were covalently bridged and anchored to the carbon fiber surface and extended into the resin matrix, which is beneficial for constructing a three-dimensional continuous reinforcement network of carbon fiber-SWCNT-resin. The SWCNT fiber surface grafting efficiencies in Examples 5 and 6 were 68.9% and 64.7%, respectively, further demonstrating that both amide bonds and covalent bonds formed by epoxy ring opening can improve the stable anchoring degree of SWCNTs on the carbon fiber surface.

[0148] 3. Lightweight design and dynamic performance (moment of inertia, critical speed, eddy current loss) comparable to metal shafts. Comparative Example 4: Alloy steel density 7.85 g / cm³ 3 The moment of inertia of a shaft of the same size is 0.315 kg·mm. 2 The high-frequency magnetic field generates 128.6W of eddy current loss; the density of the composite material of this invention is only 1.58g / cm³. 3 The rotational inertia decreases, the dynamic response speed of the motor is significantly improved, and the composite material is non-magnetic throughout, which completely eliminates eddy current losses and improves the working efficiency of the motor.

[0149] 4. Improved fatigue and corrosion resistance Under alternating torsion / bending conditions, Comparative Example 1 exhibits rapid interface debonding and low fatigue life; the covalently bridged interface inhibits microcrack propagation, resulting in improved fatigue life. Salt spray corrosion tests show that metal shafts experience weight loss and are prone to corrosion and fatigue cracking. The resin matrix of this invention provides dense coating with minimal weight loss, making it suitable for marine and chemical corrosion conditions. In a 300MPa rotational bending test, Example 1 showed a fatigue life of 2.8 × 10⁻⁶. 7 Next, Comparative Example 1 is 2.1 × 10 6 In a 500-hour neutral salt spray test, the weight loss rate in Example 1 was 0.011 mg / cm³. 2 Comparative Example 1 was 0.026 mg / cm³. 2 .

[0150] 5. Process controllability A comparison between Example 1 and Example 2 shows that, under the same process conditions, the N2 / H2 / Ar nitrogen-containing plasma atmosphere is more conducive to improving the nitrogen-containing active sites on the fiber surface and the subsequent bridging effect than the O2 / Ar atmosphere. The IFSS, ILSS and grafting efficiency of Example 2 are all higher than those of Example 1.

[0151] 6. Single-factor analysis of SWCNT dispersion concentration: The point-by-point test results at different concentrations are shown in Table 2. IFSS, ILSS, and grafting efficiency increased with increasing concentration from 0.01 mg / mL to 0.40 mg / mL, and remained at a high level in the range of 0.20–0.60 mg / mL; after further increasing to 0.80–1.00 mg / mL, the relevant properties declined due to SWCNT aggregation and decreased utilization of effective reaction sites.

[0152] Table 2 shows the performance test results at different concentrations of SWCNT-COOH dispersions. As shown in Table 2, at concentrations of 0.01–0.10 mg / mL, the SWCNT coverage is insufficient, resulting in limited interfacial enhancement; at concentrations of 0.20–0.60 mg / mL, a relatively stable surface grafted layer is formed, with 0.40 mg / mL exhibiting the highest overall performance; when the concentration reaches 0.80–1.00 mg / mL, the dispersion viscosity increases and agglomeration occurs, leading to a decrease in effective grafting efficiency and shear strength.

[0153] Table 2 Performance test results at different SWCNT-COOH dispersion concentrations

[0154] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a composite material motor shaft, characterized in that, Includes the following steps: Surface-activated carbon fibers are obtained by plasma surface activation treatment of carbon fibers. When the plasma surface activation treatment is used to introduce carboxyl groups onto the surface of the carbon fiber, the surface-activated carbon fiber is directly used as a carbon fiber with a first reactive functional group on its surface. Alternatively, the surface-activated carbon fiber can be immersed in a grafting reaction solution to carry out a chemical grafting reaction, introducing a first reactive functional group to obtain carbon fiber with a first reactive functional group on its surface. The first carbon nanotubes are chemically modified to introduce a second reactive functional group, resulting in a carbon nanotube dispersion containing a second reactive functional group on its surface. The carbon fiber with a first reactive functional group on its surface is mixed with the carbon nanotube dispersion with a second reactive functional group on its surface. The second reactive functional group and the first reactive functional group undergo a covalent bridging reaction to obtain a carbon fiber reinforced with surface-grafted carbon nanotubes. Using the carbon fiber reinforcement with surface-grafted carbon nanotubes as the core layer and the resin composite layer as the outer layer, the carbon fiber reinforcement with surface-grafted carbon nanotubes is combined with the resin composite slurry, and then molded and cured sequentially to obtain the composite material motor shaft, wherein the resin composite layer contains a second carbon nanotube.

2. The preparation method according to claim 1, characterized in that, The grafting reaction solution includes a silane coupling agent solution or an isocyanate compound solution.

3. The preparation method according to claim 2, characterized in that, The silane coupling agent in the silane coupling agent solution includes γ-aminopropyltriethoxysilane and / or γ-glycidoxypropyltrimethoxysilane.

4. The preparation method according to claim 1, characterized in that, The first reactive functional group includes one or more of carboxyl, amino, isocyanate and epoxy groups.

5. The preparation method according to claim 1 or 4, characterized in that, The second reactive functional group includes one or more of carboxyl, amino, and epoxy groups.

6. The preparation method according to claim 1, characterized in that, The concentration of the carbon nanotube dispersion containing a second reactive functional group on its surface is 0.01~1.0 mg / mL.

7. The preparation method according to claim 1, characterized in that, The covalent bridging reaction is carried out at a temperature of 25-80℃ for 2-24 hours.

8. The preparation method according to claim 1 or 7, characterized in that, The covalent bridging reaction also includes a carboxyl activation system, which comprises 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide.

9. The composite material motor shaft prepared by the preparation method according to any one of claims 1 to 8, characterized in that, It includes a core layer and an outer layer, the outer layer encapsulating the core layer, the outer layer being a resin composite layer, the resin composite layer including resin and a second carbon nanotube, the core layer including a carbon fiber layer, an interface bridging layer and a carbon nanotube layer from the inside out, the interface bridging layer being obtained by a covalent bridging reaction between a second reactive functional group and a first reactive functional group.

10. The application of the composite material motor shaft according to claim 9 in the field of electric drive.