Metal-resin composite materials and their preparation methods, mid-frame components and electronic devices

By setting active molecules between the metal matrix and the thermoplastic resin layer and connecting them with chemical bonds, the problem of weak interfacial interaction between metal and resin composite materials is solved, resulting in stronger adhesion and a larger interaction area.

CN123107313APending Publication Date: 2026-11-17BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510625697.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the interfacial interaction between metal and resin composite materials is relatively weak, resulting in problems such as incomplete resin contact and uneven adhesion.

Method used

Active molecules are placed between the metal matrix and the thermoplastic resin layer and connected by chemical bonds to achieve physical anchoring and chemical cross-linking, thereby increasing the interaction area.

Benefits of technology

It significantly improves the bonding strength and interaction area between the metal matrix and the thermoplastic resin layer, and enhances the bonding strength and uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107313A_ABST
    Figure CN123107313A_ABST
Patent Text Reader

Abstract

This application discloses a metal-resin composite material and its preparation method, a mid-frame assembly, and an electronic device. The metal-resin composite material includes: a metal matrix, at least a portion of the surface of the metal matrix having pores; and a thermoplastic resin layer disposed on at least a portion of the surface of the metal matrix, with active molecules present between the thermoplastic resin layer and the metal matrix. The active molecules include at least one compound of Formula I: A-Q-R (Formula I), where A is a head group attached to the surface of the metal matrix, Q is an alkyl chain, and R is a terminal group connected to the thermoplastic resin layer. This application, by placing active molecules between the metal matrix and the thermoplastic resin layer, can significantly improve the adhesion strength between the metal matrix and the thermoplastic resin layer; simultaneously, it can also effectively increase the interaction area between the metal matrix and the thermoplastic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of materials, specifically relating to a metal-resin composite material and its preparation method, a mid-frame assembly, and an electronic device. Background Technology

[0002] Metal-resin composites are in high demand in the 3C electronics industry. Currently, the common method for bonding metal and resin involves first creating pores on the metal surface, then injecting fluid resin into these pores to produce a metal-resin composite. This method produces metal-resin composites with good bonding strength and high processing efficiency, but it still has the following drawbacks: firstly, the interfacial interaction between the resin and metal is weak; secondly, the micropores on the metal surface do not fully contact the resin, resulting in cavities and uneven surface adhesion. Summary of the Invention

[0003] This application aims to at least partially address one of the technical problems in the related art. Therefore, one objective of this application is to provide a metal-resin composite material and its preparation method, a mid-frame assembly, and an electronic device. By placing active molecules between the metal matrix and the thermoplastic resin layer, this application can significantly improve the adhesive strength between the metal matrix and the thermoplastic resin layer; simultaneously, it can also effectively increase the interaction area between the metal matrix and the thermoplastic resin.

[0004] This application firstly discloses a metal-resin composite material. According to embodiments of this application, the metal-resin composite material comprises:

[0005] A metal substrate, wherein at least a portion of the surface of the metal substrate is provided with pores;

[0006] A thermoplastic resin layer is disposed on at least a portion of the surface of the metal substrate, and the thermoplastic resin layer contains active molecules between the thermoplastic resin layer and the metal substrate;

[0007] The active molecule includes at least one of the compounds shown in Formula I:

[0008] AQR

[0009] Formula I

[0010] Wherein, A is a head group, which is attached to the surface of the metal matrix, Q is an alkyl chain, and R is a terminal group, which is connected to the thermoplastic resin layer.

[0011] According to the metal-resin composite material of the above embodiments of this application, active molecules are disposed between the metal matrix and the thermoplastic resin layer. These active molecules are chemically bonded between the metal matrix and the thermoplastic resin layer, achieving a synergistic effect of physical anchoring and chemical cross-linking between the metal matrix and the thermoplastic resin layer, thereby significantly improving the adhesive strength between the metal matrix and the thermoplastic resin layer. Simultaneously, the chemical bonding between the active molecules effectively increases the interaction area between the metal matrix and the thermoplastic resin.

[0012] In addition, the metal-resin composite material according to the above embodiments of this application may also have the following additional technical features:

[0013] In some embodiments of this application, the head group includes at least one selected from phosphate, carboxyl, silyl, amino, and hydroxyl groups.

[0014] In some embodiments of this application, the alkyl chain includes at least one of alkyl chains having 4 to 18 carbon atoms.

[0015] In some embodiments of this application, the terminal group includes at least one of epoxy, carboxyl, amino, silyl, and hydroxyl groups.

[0016] In some embodiments of this application, the active molecule includes at least one selected from 5-epoxypentyl phosphate, 6-epoxyhexanoic acid, 3-epoxypropyl-5-silylpentane, 6-epoxy-1-aminohexane, 6-epoxy-1-hexanol, 6-phosphohexanoic acid, 6-phospho-1-aminohexane, 6-phospho-1-silylpentane, and 6-phospho-1-hexanol.

[0017] In some embodiments of this application, the area ratio of the holes is 60% to 100% based on the surface area of ​​the metal substrate being 100%.

[0018] In some embodiments of this application, the pore size is in the nanometer to micrometer range.

[0019] In some embodiments of this application, the thermoplastic resin layer includes at least one of polyphenylene sulfide, polyphthalamide, polybutylene terephthalate, polyamide, polycarbonate, and polyolefin.

[0020] In some embodiments of this application, the thermoplastic resin layer further includes fibers, which include at least one of ceramic fibers, glass fibers, and carbon fibers.

[0021] In some embodiments of this application, the fiber accounts for 30% to 50% of the mass of the thermoplastic resin layer.

[0022] In some embodiments of this application, the metal matrix includes at least one of titanium matrix, titanium alloy matrix, aluminum matrix, aluminum alloy matrix, stainless steel matrix, zinc matrix, and zinc alloy matrix.

[0023] A second aspect of this application provides a method for preparing the metal-resin composite material described in the above embodiments. According to an embodiment of this application, the method includes:

[0024] A pore-forming process is performed on the metal substrate to form pores on at least a portion of the surface of the metal substrate;

[0025] The metal substrate after pore-forming treatment is immersed in a treatment solution containing active molecules so that the active molecules can be adsorbed on the surface of the metal substrate.

[0026] The surface of the metal matrix is ​​injection molded with thermoplastic resin to form a metal-resin composite material.

[0027] According to the method for preparing metal-resin composite materials according to the above embodiments of this application, the metal matrix after pore formation is treated with a treatment solution to improve the wettability of the metal matrix. During injection molding, this not only makes it easier for the thermoplastic resin to wet the pores on the metal surface, but also, based on the physical adhesion (the formation of an interlocking structure between the metal matrix and the thermoplastic resin), the active molecules in the treatment solution can react with both the metal matrix and the thermoplastic resin, connecting the metal matrix and the thermoplastic resin in the form of chemical bonds. This achieves a synergistic effect of physical anchoring and chemical cross-linking between the metal matrix and the thermoplastic resin, thereby further improving the adhesion strength between the metal matrix and the thermoplastic resin. Furthermore, the reactions between the active molecules adsorbed on the metal surface and the thermoplastic resin are mostly exothermic, which can effectively maintain the fluidity of the thermoplastic resin, promote the flow of the thermoplastic resin into the pore microstructure of the metal matrix surface, and increase the interaction area between the metal matrix material and the thermoplastic resin. Simultaneously, the active molecules are connected between the metal matrix and the thermoplastic resin in the form of chemical bonds, which can effectively increase the interaction area between the metal matrix and the thermoplastic resin.

[0028] In addition, the method according to the above embodiments of this application may also have the following additional technical features:

[0029] In some embodiments of this application, the metal substrate is pore-forming process using chemical etching and / or electrochemical anodizing.

[0030] In some embodiments of this application, before immersing the pore-forming metal substrate in the treatment solution, the method further includes: activating the pore-forming metal substrate to form hydroxyl groups on the surface of the metal substrate.

[0031] In some embodiments of this application, the activation treatment includes: immersing the metal substrate after the pore-forming treatment in a mixed solution of concentrated sulfuric acid and hydrogen peroxide; or immersing the metal substrate after the pore-forming treatment in a phosphoric acid solution.

[0032] In some embodiments of this application, the mass ratio of concentrated sulfuric acid to hydrogen peroxide is (4-6):0.3, and the metal substrate after pore-forming treatment is immersed in the mixed solution of concentrated sulfuric acid and hydrogen peroxide for 1 min to 30 min; or, the concentration of phosphoric acid solution is 0.1 mol / L to 1 mol / L, and the metal substrate after pore-forming treatment is immersed in the phosphoric acid solution for 10 min to 60 min.

[0033] In some embodiments of this application, the mass concentration of active molecules in the treatment solution is 1% to 20%.

[0034] In some embodiments of this application, the soaking temperature of the treatment solution is 20°C to 60°C, and the soaking time is 10 min to 60 min.

[0035] A third aspect of this application discloses a mid-frame assembly. According to embodiments of this application, the mid-frame assembly comprises a metal-resin composite material as described in the first aspect or a metal-resin composite material prepared by the method of the second aspect. Consequently, the adhesive strength, mechanical properties, durability, and other performance characteristics of the mid-frame assembly are significantly improved.

[0036] A fourth aspect of this application provides an electronic device. According to embodiments of this application, the electronic device includes a metal-resin composite material of the first aspect, a metal-resin composite material prepared by the method of the second aspect, or a mid-frame assembly of the third aspect. It should be noted that the features and advantages described above for the metal-resin composite material or the mid-frame assembly also apply to this electronic device, and will not be repeated here.

[0037] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0038] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:

[0039] Figure 1 These are schematic diagrams of the structures of active molecules in some embodiments of this application;

[0040] Figure 2 This is a frontal view schematic diagram of the test of the bonding strength between titanium and plastic according to an embodiment of this application;

[0041] Figure 3This is a top view schematic diagram of the test of the bonding strength between titanium and plastic according to an embodiment of this application. Detailed Implementation

[0042] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0043] In this invention, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first" and "second" may explicitly or implicitly include at least one of those features.

[0044] The first aspect of this application discloses a metal-resin composite material. According to an embodiment of this application, the metal-resin composite material includes a metal matrix, at least a portion of the surface of the metal matrix having pores; a thermoplastic resin layer disposed on at least a portion of the surface of the metal matrix, and containing active molecules between the thermoplastic resin layer and the metal matrix; wherein, reference is made to the appendix... Figure 1 The active molecule includes at least one of the compounds shown in Formula I:

[0045] AQR

[0046] Formula I

[0047] In this design, A is the head group, which is attached to the surface of the metal matrix; Q is an alkyl chain; and R is the terminal group, which is connected to the thermoplastic resin layer.

[0048] It should be noted that the aforementioned thermoplastic resin layer is disposed on at least a portion of the surface of the porous region of the metal substrate, or the aforementioned thermoplastic resin layer is disposed on at least a portion of the surface of the porous region and at least a portion of the surface of the non-porous region of the metal substrate.

[0049] According to the metal-resin composite material of the above embodiments of this application, active molecules (as shown in Formula I) are disposed between the metal matrix and the thermoplastic resin layer. The active molecules include head groups, alkyl chains, and terminal groups. The head groups are attached to the surface of the metal matrix by chemical bonds, the alkyl chains interact with adjacent active molecules through van der Waals forces, and the terminal groups are connected to the thermoplastic resin layer by chemical bonds. Thus, the active molecules are chemically bonded between the metal matrix and the thermoplastic resin layer, achieving a synergistic effect of physical anchoring and chemical cross-linking between the metal matrix and the thermoplastic resin layer, thereby significantly improving the adhesive strength between the metal matrix and the thermoplastic resin layer. Simultaneously, the chemical bonded connection of the active molecules between the metal matrix and the thermoplastic resin layer effectively increases the interaction area between the metal matrix and the thermoplastic resin.

[0050] Specifically, the metal substrate and the thermoplastic resin layer of this application can achieve a seamless bond, and the shear strength of the bond between the metal substrate and the thermoplastic resin layer can reach over 25 MPa. Even after the bond between the metal substrate and the thermoplastic resin layer fails, the adhesive area of ​​the metal substrate can reach over 95%. The adhesive area percentage refers to the proportion of residual thermoplastic resin on the contact surface between the metal substrate and the thermoplastic resin layer after separation.

[0051] According to some specific embodiments of this application, the head group includes at least one selected from phosphate (-PO3H2), carboxyl (-COOH), silyl (-Si(OR)3), amino (-NH2), and hydroxyl (-OH), and the head group is capable of chemical adsorption with the metal matrix. Phosphate (-PO3H2) is preferred, as it has a strong affinity for the metal surface and can form stable phosphates or compounds.

[0052] According to some specific embodiments of this application, the alkyl chain includes at least one of alkyl chains having 4 to 18 carbon atoms, and the alkyl chain can interact with adjacent active molecules through van der Waals forces.

[0053] According to some specific embodiments of this application, the terminal groups include at least one selected from epoxy (-CH(O)CH2), carboxyl (-COOH), amino (-NH2), silyl (-Si(OR)3), and hydroxyl (-OH), and the aforementioned terminal groups can be chemically bonded to the thermoplastic resin layer. Epoxy (-CH(O)CH2) is preferred, as epoxy groups have high reactivity and readily undergo ring-opening reactions with hydroxyl, carboxyl, and other groups of the thermoplastic resin.

[0054] According to further specific embodiments of this application, the aforementioned active molecules include at least one selected from 5-epoxypentylphosphonic acid, 6-epoxyhexanoic acid, 3-epoxypropyl-5-silylpentane, 6-epoxy-1-aminohexane, 6-epoxy-1-hexanol, 6-phosphohexanoic acid, 6-phospho-1-aminohexane, 6-phospho-1-silylpentane, and 6-phospho-1-hexanol. All of the above active molecules can be chemically bonded between the metal matrix and the thermoplastic resin layer, achieving a synergistic effect of physical anchoring and chemical cross-linking between the metal matrix and the thermoplastic resin layer, thereby significantly improving the adhesive strength between the metal matrix and the thermoplastic resin layer.

[0055] According to some specific embodiments of this application, based on the surface area of ​​the metal substrate being 100%, the area ratio of the holes is 60% to 100%, for example, it can be 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc. By limiting the area ratio of the holes to the above range, the metal and resin can be further bonded more firmly through the anchor bolt effect.

[0056] According to some specific embodiments of this application, the pore size is in the nanometer to micrometer range, that is, the pore size can be in the nanometer and / or micrometer range. Hole formation is performed using chemical etching, resulting in pores with a micrometer-level pore size; while hole formation is performed using electrochemical anodizing, resulting in pores with a nanometer-level pore size. In some specific embodiments, the pore size is 10 μm-30 μm; in still other specific embodiments, the pore size is 15 nm-30 nm.

[0057] In the embodiments of this application, the type of material for the thermoplastic resin layer is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred embodiments, the thermoplastic resin layer includes at least one of polyphenylene sulfide, polyphthalamide, polybutylene terephthalate, polyamide, polycarbonate, and polyolefin. More preferably, polybutylene terephthalate resin has excellent mechanical properties, heat resistance, electrical properties, chemical corrosion resistance, processing properties, and flame retardant properties.

[0058] In the embodiments of this application, during the cooling process of injection molding, the volume shrinkage caused by the difference in thermal expansion coefficients between the metal and the resin can significantly disrupt the bond between the resin and the metal, resulting in voids or even detachment at the two-phase interface. Adding fibers can improve the thermal expansion coefficient of the thermoplastic resin, making it closer to that of the metal. According to some specific embodiments of this application, the aforementioned fibers include at least one of ceramic fibers, glass fibers, and carbon fibers. Glass fibers are preferred because they have advantages such as a thermal expansion coefficient similar to that of metals, low cost, good mechanical properties, high dimensional stability, excellent processing performance, strong chemical corrosion resistance, and good insulation properties, making them a preferred reinforcing fiber material in metal-resin composite materials.

[0059] According to some specific embodiments of this application, the mass percentage of the above-mentioned fiber in the thermoplastic resin layer is 30% to 50%, for example, it can be 30%, 35%, 40%, 45%, 50%, etc. By limiting the mass percentage of the fiber in the thermoplastic resin layer to the above range, the coefficient of thermal expansion of the thermoplastic resin can be further improved, making it close to the coefficient of thermal expansion of metal.

[0060] In the embodiments of this application, the specific types of the metal substrates are not particularly limited, and those skilled in the art can select them according to actual needs. As some specific embodiments, the metal substrates include at least one of titanium substrates, titanium alloy substrates, aluminum substrates, aluminum alloy substrates, stainless steel substrates, zinc substrates, and zinc alloy substrates.

[0061] A second aspect of this application provides a method for preparing the metal-resin composite material of the above embodiments. According to an embodiment of this application, the method includes:

[0062] S100: Hole-forming treatment of the metal substrate;

[0063] In this step, a pore-forming process is performed on the metal substrate to etch holes into at least a portion of the surface of the metal substrate.

[0064] According to some specific embodiments of this application, pores can be formed in a metal substrate by chemical etching and / or electrochemical anodizing. It should be noted that chemical etching produces pores with diameters in the micrometer range, while electrochemical anodizing produces pores with diameters in the nanometer range.

[0065] According to further specific embodiments of this application, the above-mentioned chemical etching can be performed using a solution containing acid and / or oxidizing agent. The acid solution can be one or more of sulfuric acid solution, hydrochloric acid solution, hydrofluoric acid solution, nitric acid solution, and phosphoric acid solution. The oxidizing agent solution can be one or more of ferric chloride solution, copper chloride solution, persulfate solution, hydrogen peroxide solution, persulfate solution, perphosphoric acid solution, and peracetic acid solution. As a specific embodiment, chemical etching can be performed using a mixed solution of hydrofluoric acid and nitric acid (mass ratio of hydrofluoric acid to nitric acid is (9-11):1), or a mixed solution of hydrofluoric acid and ferric chloride (mass ratio of hydrofluoric acid to ferric chloride is 1:(4-6)). The temperature of the chemical etching solution can be 20°C to 50°C, and the immersion etching time can range from a few seconds to several minutes as needed.

[0066] According to some specific embodiments of this application, the above-described electrochemical anodic oxidation method can use a titanium alloy as the anode and graphite as the cathode. The electrolyte is composed of fluorides, weak acids and their salts, surfactants, etc. The fluorides can be one or more of potassium fluoride, sodium fluoride, ammonium fluoride, ammonium hydrogen fluoride, and hydrofluoric acid. The weak acids and their salts can be one or more of carbonates, bicarbonates, phosphoric acid and their salts. Depending on the electrolyte formulation, the applied voltage range can be 5V to 50V, the time can be 1min to 60min, and the temperature can be 5℃ to 80℃.

[0067] According to some specific embodiments of this application, before performing hole-forming treatment on the metal substrate, the above method may further include:

[0068] The metal substrate undergoes degreasing, alkaline washing, and neutralization treatments. Degreasing removes oil stains from the substrate surface, alkaline washing removes the oxide layer to facilitate adsorption of active molecules, and neutralization neutralizes any alkaline solutions on the substrate surface.

[0069] In addition, each step includes a water wash to remove the solution brought out from the previous steps of material processing, thus preventing the solutions from mixing and affecting the actual use effect.

[0070] As some specific embodiments, a mixed solution of an alkaline substance and a surfactant can be used for degreasing. The alkaline substance includes at least one selected from NaOH, Na2CO3, NaHCO3, and Na3PO4, and the concentration of the alkaline substance can range from 10 g / L to 80 g / L. The surfactant can be sodium dodecyl sulfate, and the mass concentration of the surfactant can be from 1% to 10%. The temperature of the degreasing solution can be from 50°C to 70°C, and the soaking time can be from 1 min to 10 min.

[0071] The above-mentioned alkaline washing method is not particularly limited, and conventional methods in the field can be used. For example, the metal can be soaked in an aqueous solution of NaOH containing 50 g / L to 70 g / L at 40℃ to 60℃ for 1 min to 20 min.

[0072] The above neutralization treatment can be achieved by using an acidic solution to neutralize the residual alkali solution. Common acids include hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.

[0073] S200: Immerse the metal substrate after the hole-forming process in the treatment solution;

[0074] In this step, the pore-forming metal substrate is immersed in a treatment solution containing active molecules that adsorb onto the surface of the metal substrate. These active molecules include head groups, alkyl chains, and terminal groups. After treatment with the solution, the head groups can chemically react with the metal substrate to form chemical bonds, attaching to the surface of the metal substrate in the form of chemical bonds. The alkyl chains can interact with adjacent active molecules through van der Waals forces, while the terminal groups, which can react with the resin, are exposed to the outside, enhancing the affinity between the metal and the resin and making it easier for the resin to flow into the metal surface.

[0075] According to some specific embodiments of this application, the above-mentioned active molecules include at least one selected from 5-epoxypentylphosphonic acid, 6-epoxyhexanoic acid, 3-epoxypropyl-5-silylpentane, 6-epoxy-1-aminohexane, 6-epoxy-1-hexanol, 6-phosphohexanoic acid, 6-phospho-1-aminohexane, 6-phospho-1-silylpentane, and 6-phospho-1-hexanol. All of the above-mentioned active molecules are compounds as shown in Formula I, and each includes a head group, an alkyl chain, and a terminal group.

[0076] According to some specific embodiments of this application, the mass concentration of active molecules in the treatment solution is 1% to 20%, for example, it can be 1%, 3%, 5%, 7%, 10%, 12%, 15%, 18%, 20%, etc., thereby further ensuring that the active molecules in the treatment solution are effectively adsorbed on the surface of the metal substrate, while ensuring that the surface of the metal substrate adsorbs an appropriate amount of active molecules.

[0077] In the embodiments of this application, the solvent in the above-mentioned treatment solution may be water or an organic solvent, or it may be a mixture of water and an organic solvent in a certain proportion. The organic solvent includes, but is not limited to, one or more of ethanol, propylene glycol, glycerol, 1,3-butanediol, propanol, and isopropanol.

[0078] According to some specific embodiments of this application, the immersion temperature of the treatment solution is 20℃~60℃ (e.g., 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, etc.), and the immersion time is 10min~60min (e.g., 10min, 20min, 30min, 40min, 50min, 60min, etc.). This further ensures that the active molecules in the treatment solution are effectively adsorbed on the surface of the metal substrate.

[0079] According to some specific embodiments of this application, before immersing the metal substrate after the pore-forming treatment into the treatment solution, the method further includes:

[0080] The metal substrate after the pore-forming process is activated to form hydroxyl groups on the surface of the metal substrate. This effectively promotes the chemical reaction between the head group and the hydroxyl groups on the surface of the metal substrate to form chemical bonds, which then attach to the surface of the metal substrate in the form of chemical bonds.

[0081] According to some specific embodiments of this application, the activation treatment includes: immersing the pore-forming metal substrate in a mixed solution of concentrated sulfuric acid and hydrogen peroxide, thereby effectively forming hydroxyl groups on the surface of the metal substrate. Alternatively, immersing the pore-forming metal substrate in a phosphoric acid solution, thereby effectively forming hydroxyl groups on the surface of the metal substrate.

[0082] As some specific embodiments, the mass ratio of concentrated sulfuric acid to hydrogen peroxide is (4-6):0.3 (e.g., 4:0.3, 5:0.3, or 6:0.3, etc.). The metal substrate after pore-forming treatment is immersed in the mixed solution of concentrated sulfuric acid and hydrogen peroxide for 1 min to 30 min (e.g., 1 min, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.). This can further effectively ensure the formation of hydroxyl groups on the surface of the metal substrate.

[0083] In some further specific embodiments, the concentration of the phosphoric acid solution is 0.1 mol / L to 1 mol / L (e.g., 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, etc.). The metal substrate after pore-forming treatment is immersed in the phosphoric acid solution for 10 min to 60 min (e.g., 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, etc.). This can further effectively ensure the formation of hydroxyl groups on the surface of the metal substrate.

[0084] According to some specific embodiments of this application, after immersing the metal substrate after the hole-forming treatment in the treatment solution, the following steps may also be included:

[0085] Clean the surface of the metal substrate and dry it;

[0086] In this step, the surface of the metal substrate can be cleaned with deionized water to remove unreacted active molecules, followed by drying. In some specific embodiments, the surface of the metal substrate can be cleaned with room temperature deionized water for 5 to 10 minutes. In still other specific embodiments, the drying process is low-temperature drying, such as heating to 40°C to 60°C and drying for 10 to 60 minutes.

[0087] S300: The surface of the metal substrate is injection molded using thermoplastic resin.

[0088] In this step, thermoplastic resin is used to injection mold the surface of the metal substrate to form an integrated metal-resin composite material.

[0089] In the embodiments of this application, the type of thermoplastic resin is not particularly limited, and those skilled in the art can select it according to actual needs. As some preferred embodiments, the thermoplastic resin includes at least one of polyphenylene sulfide, polyphthalamide, polybutylene terephthalate, polyamide, polycarbonate, and polyolefin. More preferably, polybutylene terephthalate resin has excellent mechanical properties, heat resistance, electrical properties, chemical corrosion resistance, processing properties, and flame retardant properties.

[0090] In the embodiments of this application, during the cooling process of injection molding, the volume shrinkage caused by the difference in thermal expansion coefficients between the metal and the resin can significantly disrupt the bond between the resin and the metal, resulting in voids or even detachment at the two-phase interface. Adding fibers can improve the thermal expansion coefficient of the thermoplastic resin, making it closer to that of the metal. According to some specific embodiments of this application, the aforementioned fibers include at least one of ceramic fibers, glass fibers, and carbon fibers. Glass fibers are preferred because they have advantages such as a thermal expansion coefficient similar to that of metals, low cost, good mechanical properties, high dimensional stability, excellent processing performance, strong chemical corrosion resistance, and good insulation properties, making them a preferred reinforcing fiber material in metal-resin composite materials.

[0091] In the embodiments of this application, the above-mentioned injection molding conditions are not particularly limited, and those skilled in the art can select them according to actual needs. As some preferred embodiments, the above-mentioned injection molding conditions can be: barrel temperature set at 200℃~500℃, injection pressure at 75MPa~300MPa, mold temperature at 80℃~350℃, and holding pressure at 40MPa~250MPa. Preferred injection molding conditions are: barrel temperature set at 250℃~380℃, injection pressure at 120MPa~200MPa, mold temperature at 130℃~230℃, and holding pressure at 80MPa~200MPa.

[0092] According to the method for preparing metal-resin composite materials according to the above embodiments of this application, the metal matrix after pore formation is treated with a treatment solution to improve the wettability of the metal matrix. During injection molding, this not only makes it easier for the thermoplastic resin to wet the pores on the metal surface, but also, based on the physical adhesion (the formation of an interlocking structure between the metal matrix and the thermoplastic resin), the active molecules in the treatment solution can react with both the metal matrix and the thermoplastic resin, connecting the metal matrix and the thermoplastic resin in the form of chemical bonds. This achieves a synergistic effect of physical anchoring and chemical cross-linking between the metal matrix and the thermoplastic resin, thereby further improving the adhesion strength between the metal matrix and the thermoplastic resin. Furthermore, the reactions between the active molecules adsorbed on the metal surface and the thermoplastic resin are mostly exothermic, which can effectively maintain the fluidity of the thermoplastic resin, promote the flow of the thermoplastic resin into the pore microstructure of the metal matrix surface, and increase the interaction area between the metal matrix material and the thermoplastic resin. Simultaneously, the active molecules are connected between the metal matrix and the thermoplastic resin in the form of chemical bonds, which can effectively increase the interaction area between the metal matrix and the thermoplastic resin.

[0093] A third aspect of this application discloses a mid-frame assembly. According to embodiments of this application, the mid-frame assembly comprises a metal-resin composite material as described in the first aspect or a metal-resin composite material prepared by the method of the second aspect. Consequently, the adhesive strength, mechanical properties, durability, and other performance characteristics of the mid-frame assembly are significantly improved.

[0094] In the embodiments of this application, the mid-frame assembly is a key structural component located between the front panel (screen) and the back cover of the mobile phone, mainly serving the following functions: 1) Support and fixation: The mid-frame is the mounting base for various internal components of the mobile phone, including the battery, motherboard, camera, flex cable, various sensors, microphone, earpiece, etc. It provides stable support and fixing points for these components, ensuring that they do not loosen or shift during use. 2) Protection: The mid-frame protects the internal electronic components of the mobile phone from external impacts, collisions, and damage. In short, the mid-frame assembly is an indispensable part of the mobile phone structure. It not only bears the functions of mounting and protecting internal components, but also has an important impact on the overall performance, appearance, and user experience of the mobile phone.

[0095] A fourth aspect of this application provides an electronic device. According to embodiments of this application, the electronic device includes a metal-resin composite material of the first aspect, a metal-resin composite material prepared by the method of the second aspect, or a mid-frame assembly of the third aspect. It should be noted that the features and advantages described above for the metal-resin composite material or the mid-frame assembly also apply to this electronic device, and will not be repeated here.

[0096] It is understood that there are no particular limitations on the specific types of the aforementioned electronic devices, as long as the electronic devices require the aforementioned metal-resin composite material. For example, the aforementioned electronic devices may be smartphones, automobiles, cellular phones, cordless phones, Session Initiation Protocol (SIP) phones, tablets, Personal Digital Assistants (PADs), laptops, digital cameras, e-book readers, portable multimedia players, handheld devices with wireless communication capabilities, computing devices or other processing devices connected to a wireless modem, in-vehicle devices, wearable devices, 5G terminal devices, etc., and this application embodiment does not limit these categories.

[0097] The embodiments of this application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. In addition, unless otherwise specified, all reagents used in the following embodiments are commercially available or can be synthesized according to the methods described herein or known methods. For reaction conditions not listed, they are also readily available to those skilled in the art.

[0098] Example 1

[0099] This embodiment provides a metal-resin composite material, the preparation method of which includes the following steps:

[0100] (1) Samples made of TC4 titanium alloy with dimensions of 40mm×12mm×3mm were subjected to degreasing, alkaline washing, neutralization, and chemical etching. Degreasing was performed using a solution containing 40g / L NaOH and 1wt% sodium dodecyl sulfate at a solution temperature of 50℃ for 10min. Alkaline washing involved immersion in a 60g / L NaOH aqueous solution at 50℃ for 5min. Neutralization involved immersion in a 30g / L sulfuric acid solution at room temperature for 5min. The etching solution was a mixed solution of hydrofluoric acid and ferric chloride (mass ratio of hydrofluoric acid to ferric chloride of 1:5) with a total concentration of 300g / L at room temperature for 30s. Overflow rinsing was performed between each step to remove black ash and other solutions from the product surface.

[0101] (2) Immerse the titanium alloy in a mixed solution of concentrated sulfuric acid and 30% hydrogen peroxide solution (mass ratio of concentrated sulfuric acid to hydrogen peroxide solution is 5:1) for 5 minutes.

[0102] (3) Soak in a 5-epoxypentylphosphoric acid (one end is phosphoric acid, the other end is an epoxy group, and the middle is connected by 5 carbon chains) solution at 40℃ for 10 min, with a mass concentration of 5% and water as the solvent.

[0103] (4) Remove from the water, wash with deionized water for 10 minutes, and dry at 50°C for 35 minutes.

[0104] (5) Polybutylene terephthalate resin (containing 40% glass fiber) is used for injection molding. The barrel temperature is set at 260°C, the injection pressure is 120MPa, the mold temperature is 150°C, and the holding pressure is 100MPa. After injection molding, a titanium alloy and resin composite material can be obtained.

[0105] Example 2

[0106] This embodiment is basically the same as embodiment 1, except for step (3):

[0107] The active molecule is 6-epoxyhexanoic acid (one end is a carboxyl group, the other end is an epoxy group, and the middle is connected by five carbon chains).

[0108] Example 3

[0109] This embodiment is basically the same as embodiment 1, except for step (3):

[0110] The active molecule is 3-epoxypropyl-5-silylpentane (one end is silyl, the other end is epoxy, and the middle is connected by five carbon chains), and the solvent is a mixed solution of ethanol and water (the mass ratio of ethanol to water is 1:1).

[0111] Example 4

[0112] This embodiment is basically the same as embodiment 1, except for step (3):

[0113] The active molecule is 6-epoxy-1-aminohexane (one end is an amino group, the other end is an epoxy group, and the middle is connected by five carbon chains).

[0114] Example 5

[0115] This embodiment is basically the same as embodiment 1, except for step (3):

[0116] The active molecule is 6-epoxy-1-hexanol (one end is a hydroxyl group, the other end is an epoxy group, and the middle is connected by five carbon chains).

[0117] Example 6

[0118] This embodiment is basically the same as embodiment 1, except for step (3):

[0119] The active molecule is 6-phosphohexanoic acid (one end is a phosphate group, the other end is a carboxyl group, and the middle is connected by five carbon chains).

[0120] Example 7

[0121] This embodiment is basically the same as embodiment 1, except for step (3):

[0122] The active molecule is 6-phospho-1-aminohexane (one end is a phosphate group, the other end is an amino group, and the middle is connected by five carbon chains).

[0123] Example 8

[0124] This embodiment is basically the same as embodiment 1, except for step (3):

[0125] The active molecule is 6-phospho-1-silylpentane (one end is a phosphate group, the other end is a silyl group, and the middle is connected by five carbon chains), and the solvent is a mixed solution of ethanol and water (the mass ratio of ethanol to water is 1:1).

[0126] Example 9

[0127] This embodiment is basically the same as embodiment 1, except for step (3):

[0128] The active molecule is 6-phospho-1-hexanol (one end is a phosphate group, the other end is a hydroxyl group, and the middle is connected by five carbon chains).

[0129] Example 10

[0130] This embodiment is basically the same as embodiment 1, except for step (1):

[0131] Following the same chemical etching steps as in Example 1, an anodizing step was performed. The electrolyte for anodizing consisted of a mixture of ammonium hydrogen fluoride, phosphoric acid, and sodium dodecyl sulfate, with a hydrogen fluoride concentration of 10 g / L, a phosphoric acid concentration of 100 g / L, and a sodium dodecyl sulfate mass concentration of 1%. Water was used as the solvent. Anodizing was performed using a sample as the anode at a temperature of 40°C, a voltage of 30 V, and an oxidation time of 15 min.

[0132] Example 11

[0133] This embodiment is basically the same as embodiment 1, except for step (1):

[0134] The etching solution is a mixture of hydrofluoric acid and ferric chloride (mass ratio of hydrofluoric acid to ferric chloride is 1:5), with a total concentration of 400 g / L, at room temperature, and the processing time is 30 s.

[0135] Example 12

[0136] This embodiment is basically the same as embodiment 1, except for step (5):

[0137] Injection molding was performed using polybutylene terephthalate resin (containing 30% glass fiber).

[0138] Example 13

[0139] This embodiment is basically the same as embodiment 1, except for step (5):

[0140] Injection molding was performed using polybutylene terephthalate resin (containing 50% glass fiber).

[0141] Example 14

[0142] This embodiment is basically the same as embodiment 1, except for step (5):

[0143] Injection molding was performed using polybutylene terephthalate resin (containing 40% ceramic fiber).

[0144] Example 15

[0145] This embodiment is basically the same as embodiment 1, except for step (5):

[0146] Injection molding was performed using polybutylene terephthalate resin (containing 40% carbon fiber).

[0147] Example 16

[0148] This embodiment is basically the same as embodiment 1, except for step (3):

[0149] The mass concentration of 5-epoxypentylphosphoric acid in the 5-epoxypentylphosphoric acid solution is 1%.

[0150] Example 17

[0151] This embodiment is basically the same as embodiment 1, except for step (3):

[0152] The mass concentration of 5-epoxypentylphosphoric acid in the 5-epoxypentylphosphoric acid solution is 20%.

[0153] Example 18

[0154] This embodiment is basically the same as embodiment 1, except for step (3):

[0155] Immerse in a solution of 5-epoxypentylphosphoric acid (one end is phosphoric acid, the other end is epoxy group, and the middle is connected by 5 carbon chains) at 20℃ for 60 min.

[0156] Example 19

[0157] This embodiment is basically the same as Embodiment 1, except that:

[0158] This embodiment does not go through step (2).

[0159] Comparative Example 1

[0160] This comparative example is basically the same as Example 1, except that:

[0161] This comparative example does not go through step (3).

[0162] Comparative Example 2

[0163] This comparative example is basically the same as Example 1, except that:

[0164] This comparative example does not go through steps (2) and (3).

[0165] The pore size of the metal substrates in Examples 1-9, Examples 11-19 and Comparative Examples 1-2 was tested using a light microscope. The pore size of the metal substrate in Example 10 was tested using a scanning electron microscope (SEM). The results are shown in Table 1.

[0166] The surfaces of the metal substrates in Examples 1-19 and Comparative Examples 1-2 were photographed under a metallographic microscope. The pores on the metal substrate surfaces were binarized using image processing software (Matlab), and the pore area percentage was calculated (pore area percentage = total pore area / total field of view × 100%). The results are shown in Table 1.

[0167] Metal-plastic bond strength test:

[0168] The shear strength of samples from Examples 1-19 and Comparative Examples 1-2 was tested on a universal testing machine. A schematic diagram of the test for the metal-plastic composite material is shown below. Figure 2 and Figure 3 The adhesive area ratio was statistically analyzed. The shear strength test method was as follows: a universal testing machine equipped with a tensile clamp was used. The specimen was clamped in the clamp, ensuring the force direction was parallel to the adhesive surface. The specimen was stretched at a constant rate until the adhesive layer failed. The maximum load was recorded, and the shear strength was obtained by dividing the load by the adhesive area. The results are shown in Table 1. The adhesive area ratio refers to the proportion of residual thermoplastic resin on the contact surface between the metal substrate and the thermoplastic resin layer after separation (the surface of the metal after adhesive separation was photographed using a metallographic microscope, and the proportion of residual resin on the contact surface was calculated using Matlab simulation).

[0169] Table 1

[0170]

[0171]

[0172] It should be noted that in Example 10, the pores were first chemically etched and then anodized. The pores obtained by chemical etching had a diameter of 10 μm-30 μm, while the pores obtained by anodizing had a diameter of 15 nm-30 nm.

[0173] As can be seen from Table 1, compared with Comparative Examples 1-2, the shear strength and adhesive area ratio of Examples 1-19 were significantly improved. This shows that by setting active molecules between the metal matrix and the thermoplastic resin layer, the shear strength and adhesive area ratio of the metal-resin composite material can be effectively improved.

[0174] As can be seen from Table 1, in Examples 1-9, the effect of the head group in the active molecule is phosphate group > carboxyl group > silyl group > amino group > hydroxyl group, and the effect of the terminal group is epoxy group > carboxyl group > amino group > silyl group > hydroxyl group.

[0175] As can be seen from Table 1, compared with the chemical etching method used in Example 1, the titanium alloy with better adhesion to the resin was formed by chemical etching + anodizing in Example 10.

[0176] As can be seen from Table 1, compared with Example 19, Example 1 has better shear strength and adhesive area ratio. It can be seen that activation treatment of the metal matrix after pore-forming treatment can further improve the shear strength and adhesive area ratio of the metal-resin composite material.

[0177] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0178] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A metal-resin composite material, characterized in that, include: A metal substrate, wherein at least a portion of the surface of the metal substrate is provided with pores; A thermoplastic resin layer is disposed on at least a portion of the surface of the metal substrate, and the thermoplastic resin layer contains active molecules between the thermoplastic resin layer and the metal substrate; The active molecule includes at least one of the compounds shown in Formula I: AQR Formula I Wherein, A is a head group, which is attached to the surface of the metal matrix, Q is an alkyl chain, and R is a terminal group, which is connected to the thermoplastic resin layer.

2. The metal-resin composite material according to claim 1, characterized in that, The head group includes at least one of phosphate, carboxyl, silyl, amino, and hydroxyl groups.

3. The metal-resin composite material according to claim 1, characterized in that, The alkyl chain includes at least one of alkyl chains having 4 to 18 carbon atoms.

4. The metal-resin composite material according to claim 1, characterized in that, The terminal group includes at least one of epoxy, carboxyl, amino, silyl, and hydroxyl groups.

5. The metal-resin composite material according to claim 1, characterized in that, The active molecule includes at least one of 5-epoxypentyl phosphate, 6-epoxyhexanoic acid, 3-epoxypropyl-5-silylpentane, 6-epoxy-1-aminohexane, 6-epoxy-1-hexanol, 6-phosphohexanoic acid, 6-phospho-1-aminohexane, 6-phospho-1-silylpentane, and 6-phospho-1-hexanol.

6. The metal-resin composite material according to any one of claims 1 to 5, characterized in that, The surface area of ​​the metal substrate is 100%, and the area ratio of the holes is 60% to 100%.

7. The metal-resin composite material according to any one of claims 1 to 5, characterized in that, The pore size is in the nanometer to micrometer range.

8. The metal-resin composite material according to any one of claims 1 to 5, characterized in that, The thermoplastic resin layer includes at least one of polyphenylene sulfide, polyphthalamide, polybutylene terephthalate, polyamide, polycarbonate, and polyolefin.

9. The metal-resin composite material according to claim 8, characterized in that, The thermoplastic resin layer further includes fibers, which include at least one of ceramic fibers, glass fibers, and carbon fibers.

10. The metal-resin composite material according to claim 9, characterized in that, The fiber accounts for 30% to 50% of the mass of the thermoplastic resin layer.

11. The metal-resin composite material according to any one of claims 1 to 5, characterized in that, The metal matrix includes at least one of titanium matrix, titanium alloy matrix, aluminum matrix, aluminum alloy matrix, stainless steel matrix, zinc matrix, and zinc alloy matrix.

12. A method for preparing the metal-resin composite material according to any one of claims 1 to 11, characterized in that, include: A pore-forming process is performed on the metal substrate to form pores on at least a portion of the surface of the metal substrate; The metal substrate after pore-forming treatment is immersed in a treatment solution containing active molecules so that the active molecules can be adsorbed on the surface of the metal substrate. The surface of the metal matrix is ​​injection molded with thermoplastic resin to form a metal-resin composite material.

13. The method according to claim 12, characterized in that, The metal substrate is subjected to pore-forming treatment by chemical etching and / or electrochemical anodizing.

14. The method according to claim 12, characterized in that, Before immersing the metal substrate after the pore-forming treatment into the treatment solution, the process further includes: The metal substrate after the pore-forming treatment is activated to form hydroxyl groups on the surface of the metal substrate.

15. The method according to claim 14, characterized in that, The activation process includes: The metal substrate after the pore-forming treatment is immersed in a mixed solution of concentrated sulfuric acid and hydrogen peroxide. Alternatively, the metal substrate after the pore-forming treatment can be immersed in a phosphoric acid solution.

16. The method according to claim 15, characterized in that, The mass ratio of concentrated sulfuric acid to hydrogen peroxide is (4-6):0.

3. The metal substrate after the pore-forming treatment is immersed in the mixed solution of concentrated sulfuric acid and hydrogen peroxide for 1 min to 30 min. Alternatively, the concentration of the phosphoric acid solution is 0.1 mol / L to 1 mol / L, and the metal substrate after pore-forming treatment is immersed in the phosphoric acid solution for 10 min to 60 min.

17. The method according to any one of claims 12 to 16, characterized in that, The mass concentration of active molecules in the treatment solution is 1% to 20%.

18. The method according to claim 17, characterized in that, The soaking temperature of the treatment solution is 20℃~60℃, and the soaking time is 10min~60min.

19. A mid-frame component, characterized in that, The metal resin composite material includes any one of claims 1 to 11 or the metal resin composite material prepared by the method described in any one of claims 12 to 18.

20. An electronic device, characterized in that, Includes the metal resin composite material according to any one of claims 1 to 11, or the metal resin composite material prepared by the method according to any one of claims 12 to 18, or the middle frame assembly according to claim 19.