Biodegradable and environmentally friendly lighter casing materials and their manufacturing process

By introducing chain extenders containing phosphorus-containing phenanthrene structures and thiophene groups into PLA materials and combining them with PBAT materials to construct a conjugated conductive network, the problems of insufficient toughness, poor flame retardancy, and insufficient antistatic properties of PLA materials in lighter casings are solved. This achieves high-efficiency flame retardancy, antistatic properties, and solvent resistance, meeting the comprehensive performance requirements of lighter casings.

CN123107326APending Publication Date: 2026-11-17CIXI SANQI SMOKING SET CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611231826.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

PLA materials suffer from problems such as poor toughness, insufficient impact resistance, low heat resistance, easy accumulation of static electricity, and difficulty in flame retardancy when used in lighter casings, which limits their widespread application in the lighter casing field.

Method used

By using a diol initiator with a phosphorus-containing phenanthrene structure and a chain extender with a thiophene group, a conjugated conductive network is constructed through ring-opening polymerization, cross-linking reaction, and subcritical carbon dioxide medium polymerization. Combined with PBAT material, PLA material with flame retardancy, antistatic properties, and solvent resistance is prepared.

Benefits of technology

It achieves high-efficiency flame retardancy and antistatic properties of PLA material, enhances the material's impact toughness and solvent erosion resistance, maintains good processing fluidity and thermal stability, and meets the comprehensive performance requirements of lighter housing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a preparation process for a biodegradable and environmentally friendly lighter casing material, comprising the following steps: S1: ring-opening polymerization of lactide, diol initiator, and catalyst; S2: cross-linking reaction of dicarboxylic acid chain extender to obtain a prepolymer of modified PLA material; S3: polymerization reaction of thiophene monomer, oxidant, and organic solvent under subcritical carbon dioxide to obtain a primary product of modified PLA material; S4: uniformly mixing the primary product with unmodified PLA masterbatch, PBAT masterbatch, and additives, followed by melt extrusion and granulation to finally obtain the biodegradable and environmentally friendly lighter casing material. This preparation process not only achieves good biodegradability while possessing both high-efficiency flame retardancy and antistatic properties, but also significantly improves the material's impact toughness and resistance to organic solvent corrosion, exhibiting excellent overall performance and suitability for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of biodegradable polymer materials, and in particular to a biodegradable and environmentally friendly lighter casing material and its preparation process. Background Technology

[0002] Polylactic acid (PLA), as a biodegradable polymer material, is widely used in disposable consumer goods, packaging materials, and electronic appliance housings due to its good biocompatibility, renewability, and processing properties. However, PLA material itself has defects such as poor toughness, insufficient impact resistance, low heat resistance, and easy accumulation of static electricity, which seriously restricts its widespread application in fields with high requirements for comprehensive mechanical properties and safety, such as lighter housings.

[0003] As a daily consumer product, lighter casings not only need to possess good mechanical strength and impact resistance to withstand drops and collisions during daily use, but also need to meet safety performance requirements such as flame retardancy and antistatic properties to avoid safety accidents caused by static electricity accumulation. Currently, most commercially available lighter casings are made of non-degradable petroleum-based plastics such as polypropylene (PP) and acrylonitrile-butadiene-styrene copolymer (ABS), which are difficult to degrade naturally after disposal, posing a long-term pollution burden to the environment.

[0004] To address the aforementioned issues, existing technologies have reported methods to improve the toughness of lighter casings by blending PLA with flexible biodegradable materials such as polybutylene adipate / terephthalate (PBAT). However, such physical blending modifications often fail to simultaneously improve flame retardancy and antistatic properties. Furthermore, PLA exhibits poor resistance to organic solvents, easily swelling or even cracking when the lighter casing comes into contact with fuels such as butane and kerosene, further limiting its reliability in practical applications. Therefore, there is an urgent need to develop a lighter casing material that combines biodegradability, good mechanical properties, flame retardancy, antistatic properties, and solvent resistance. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the present invention provides a preparation process for a biodegradable and environmentally friendly lighter casing material to solve the technical problems of traditional lighter casing materials, such as difficulty in achieving biodegradability, flame retardancy and antistatic function, resistance to organic solvent corrosion and insufficient impact toughness.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A process for preparing a biodegradable and environmentally friendly lighter casing material, the process comprising the following steps: S1: Add the raw material lactide, diol initiator and catalyst to the reactor and carry out ring-opening polymerization under specific conditions; S2: After the polymerization reaction in step S1 has proceeded for a certain period of time, a dicarboxylic acid chain extender is added, and a crosslinking reaction is carried out under inert gas protection to obtain a prepolymer of modified PLA material; S3: Add thiophene monomer, oxidant and organic solvent to the prepolymer obtained in step S2, and carry out polymerization reaction under the action of subcritical carbon dioxide; after the reaction is completed, cast tape and pelletize to obtain the initial product of modified PLA material. S4: The primary product is mixed evenly with unmodified PLA masterbatch, PBAT masterbatch, and additives. After melt extrusion and granulation, a biodegradable and environmentally friendly lighter casing material is finally obtained. Melt extrusion is carried out at a temperature of 175–185℃ and a screw speed of 150–250 r / min.

[0007] As a preferred technical solution, the lactide is at least one of L-lactide, D-lactide, and D,L-lactide.

[0008] As a preferred technical solution, the diol initiator is a mixture of dihydroxyphenylphosphine and butanediol.

[0009] As a preferred technical solution, the catalyst is at least one of stannous octoate, stannous acetate, and stannous chloride.

[0010] As a preferred technical solution, in step S1, the reaction conditions for the ring-opening polymerization reaction are: inert atmosphere protection, reaction temperature 120-160℃, and reaction time 1-6 hours.

[0011] As a preferred technical solution, the dicarboxylic acid chain extender is composed of 3-thiophene malonic acid, 1,5-glutaric acid, and / or 1,6-adipic acid.

[0012] As a preferred technical solution, in step S2, the reaction conditions for the crosslinking reaction are: reaction temperature 150-180℃, reaction pressure less than or equal to 1000Pa, and reaction time 1-2 hours.

[0013] As a preferred technical solution, the thiophene monomer is at least one of thiophene, 3-pentylthiophene, 3-hexylthiophene, and 3-heptylthiophene.

[0014] As a preferred technical solution, the oxidant is at least one of anhydrous ferric chloride, ammonium persulfate, and sodium persulfate.

[0015] As a preferred technical solution, the additive is one or more of antioxidants, lubricants, ultraviolet light stabilizers, and hydrolysis stabilizers.

[0016] As a preferred technical solution, the mass ratio of the primary product to unmodified PLA masterbatch, PBAT masterbatch and additives is 15-20:50-55:23-27:3-7.

[0017] Another aspect of the present invention is to provide a biodegradable and environmentally friendly lighter casing material, wherein the casing material is prepared by the above-described biodegradable and environmentally friendly lighter casing material preparation process.

[0018] The beneficial effects of this invention are: This invention discloses a novel process for preparing a biodegradable and environmentally friendly lighter casing material. It innovatively introduces a diol initiator (ODOPB) containing a phosphorus-phenanthrene structure and a chain extender containing a thiophene group into the PLA molecular chain. Furthermore, it utilizes a subcritical carbon dioxide medium to achieve in-situ polymerization of the thiophene monomer, thereby further constructing a conjugated conductive network structure. This design allows the material to maintain excellent biodegradability while also possessing highly efficient flame retardant properties and antistatic properties (surface resistivity up to 10). 6 ~10 8 Furthermore, it significantly enhances the impact toughness and resistance to organic solvent corrosion of the shell material, while ensuring good processing flowability and thermal stability. Its excellent overall performance meets the durability and stability requirements of lighter shells during long-term storage and daily use. Detailed Implementation

[0019] The following description is intended to disclose the invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art.

[0020] Example 1 The preparation process of the biodegradable and environmentally friendly lighter casing material in this embodiment includes the following steps: S1: 100g of L-lactide, 8g of diol initiator, and 0.5g of stannous octoate catalyst were added to a reactor, and the ring-opening polymerization reaction was carried out at 140°C for 3 hours under a nitrogen atmosphere. The diol initiator was a mixture of dihydroxyphenylphosphaphenanthrene and butanediol in a molar ratio of 1:2. The dihydroxyphenylphosphaphenanthrene was 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide (ODOPB, CAS number 99208-50-1).

[0021] S2: After the polymerization reaction in step S1 has proceeded for 3 hours, 6g of dicarboxylic acid chain extender is added to the reactor. Under nitrogen atmosphere protection, the crosslinking reaction is carried out at 160°C and vacuum degree maintained below 800Pa for 1.5 hours to obtain the prepolymer of modified PLA material; wherein, the dicarboxylic acid chain extender is a mixture of 3-thiophene malonic acid and 1,6-adipic acid in a molar ratio of 1:1.

[0022] S3: After the crosslinking reaction in step S2 is completed, add 10g of thiophene monomer, 5g of anhydrous ferric chloride oxidant and 20g of organic solvent (tetrahydrofuran) to the reactor. In a subcritical carbon dioxide fluid medium, carry out the polymerization reaction at 40°C and 6MPa for 4 hours. After the reaction is completed, cast the product into strips and cut it into pellets to obtain the initial product of modified PLA material.

[0023] S4: The modified PLA material pre-product obtained in step S3 is mixed evenly with unmodified PLA masterbatch, PBAT masterbatch and additives in a weight ratio of 15:55:23:7; wherein the additives are a composite additive system composed of antioxidant 1010, tristearate lubricant, UV-327 ultraviolet light stabilizer and polycarbodiimide hydrolysis stabilizer in a mass ratio of 3:2:1:2; the mixture is added to a twin-screw extruder and melt-extruded and granulated at a temperature of 180℃ and a screw speed of 200r / min to finally obtain a biodegradable and environmentally friendly lighter shell material.

[0024] Example 2 The preparation process of the biodegradable and environmentally friendly lighter casing material in this embodiment includes the following steps: S1: 100g of D,L-lactide, 8g of diol initiator and 0.5g of stannous acetate catalyst are added to the reactor and the ring-opening polymerization reaction is carried out at 130°C for 4 hours under nitrogen atmosphere protection; wherein, the diol initiator is a mixture of dihydroxyphenylphosphaphenanthrene and butanediol in a molar ratio of 1:2.

[0025] S2: After the polymerization reaction in step S1 has proceeded for 4 hours, 6g of dicarboxylic acid chain extender is added to the reactor. Under nitrogen atmosphere protection, the crosslinking reaction is carried out at 170°C and vacuum degree maintained below 800Pa for 1 hour to obtain the prepolymer of modified PLA material; wherein, the dicarboxylic acid chain extender is a mixture of 3-thiophene malonic acid and 1,5-glutaric acid in a molar ratio of 1:1.

[0026] S3: After the crosslinking reaction in step S2 is completed, add 10g of 3-hexylthiophene monomer, 5g of ammonium persulfate oxidant and 20g of organic solvent (tetrahydrofuran) to the reactor. In a subcritical carbon dioxide fluid medium, carry out the polymerization reaction at 45°C and 5MPa for 3 hours. After the reaction is completed, cast the product into strips and cut them into pellets to obtain the initial product of modified PLA material.

[0027] S4: The modified PLA material pre-processed product obtained in step S3 is mixed evenly with unmodified PLA masterbatch, PBAT masterbatch and additives in a weight ratio of 18:52:25:5; wherein the additives are a composite additive system composed of antioxidant 1010, tristearate glyceryl ester lubricant, UV-327 ultraviolet light stabilizer and polycarbodiimide hydrolysis stabilizer in a mass ratio of 3:2:1:2; the mixture is added to a twin-screw extruder and melt-extruded and granulated at a temperature of 175℃ and a screw speed of 220r / min to finally obtain a biodegradable and environmentally friendly lighter shell material.

[0028] Example 3 The preparation process of the biodegradable and environmentally friendly lighter casing material in this embodiment includes the following steps: S1: 100g of D-lactide, 8g of diol initiator and 0.5g of stannous chloride catalyst are added to the reactor and the ring-opening polymerization reaction is carried out at 150°C for 2 hours under nitrogen atmosphere protection; wherein, the diol initiator is a mixture of dihydroxyphenylphosphaphenanthrene and butanediol in a molar ratio of 1:2.

[0029] S2: After the polymerization reaction in step S1 has proceeded for 2 hours, 6g of dicarboxylic acid chain extender is added to the reactor. Under nitrogen atmosphere protection, the crosslinking reaction is carried out at 155°C and vacuum degree maintained below 800Pa for 2 hours to obtain the prepolymer of modified PLA material; wherein, the dicarboxylic acid chain extender is a mixture of 3-thiophene malonic acid and 1,5-glutaric acid in a molar ratio of 1:1.

[0030] S3: After the crosslinking reaction in step S2 is completed, add 10g of 3-heptylthiophene monomer, 5g of sodium persulfate oxidant and 20g of organic solvent (tetrahydrofuran) to the reactor. In a subcritical carbon dioxide fluid medium, carry out the polymerization reaction at 35°C and 7MPa for 5 hours. After the reaction is completed, cast the product into strips and cut them into pellets to obtain the initial product of modified PLA material.

[0031] S4: The modified PLA material pre-processed product obtained in step S3 is mixed evenly with unmodified PLA masterbatch, PBAT masterbatch and additives in a weight ratio of 20:50:27:3; wherein the additives are a composite additive system composed of antioxidant 1010, tristearate glyceryl ester lubricant, UV-327 ultraviolet light stabilizer and polycarbodiimide hydrolysis stabilizer in a mass ratio of 3:2:1:2; the mixture is added to a twin-screw extruder and melt-extruded and granulated at a temperature of 185℃ and a screw speed of 180r / min to finally obtain a biodegradable and environmentally friendly lighter shell material.

[0032] Example 4 The preparation process of the biodegradable and environmentally friendly lighter shell material in this embodiment is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation process of this embodiment, 3-pentyl-thiophene monomer is used instead of thiophene monomer.

[0033] Comparative Example 1 The preparation process of the biodegradable and environmentally friendly lighter casing material in this comparative example is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that dihydroxyphenylphosphine was not added in step S1 of the preparation process in this comparative example.

[0034] Comparative Example 2 The preparation process of the biodegradable and environmentally friendly lighter shell material in this comparative example is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that in the preparation process of this comparative example, in step S2, a dicarboxylic acid chain extender (a mixture of 3-thiophene malonic acid and 1,6-adipic acid in a molar ratio of 1:1) is not added.

[0035] Comparative Example 3 The preparation process of the biodegradable and environmentally friendly lighter casing material in this comparative example is basically the same as that in Example 1 in terms of raw material composition and preparation steps. The difference is that step S3 is not performed in the preparation process of this comparative example.

[0036] The biodegradable and environmentally friendly lighter casing materials prepared in Examples 1-4 and Comparative Examples 1-3 were subjected to performance tests, and the performance results are shown in Table 1. Among them, the flame retardant rating was tested according to UL-94 standard, with a sample thickness of 1.6 mm; the surface resistivity was tested according to GB / T 1410—2006 standard, using the ring electrode method, with a test voltage of 100V; the impact strength was tested according to GB / T 1043.1—2008 standard using a simply supported beam notched impact test, with a sample type of 1eA (notch depth 2.54 mm); the fuel compatibility was tested according to Clause 5.5 of GB 25722—2010 "Safety and Quality of Lighters", by contacting the shell material sample with n-butane fuel at (40±2)℃ for a certain period of time and evaluating its mass change and appearance integrity; the heat distortion temperature was tested according to GB / T 1634.2—2019 standard, with an applied load of 0.45 MPa and a heating rate of 120℃ / h.

[0037] Table 1

[0038] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A process for preparing a degradable and environment-friendly lighter housing material, characterized in that, The preparation process includes the following steps: S1: Add the raw material lactide, diol initiator and catalyst to the reactor and carry out ring-opening polymerization under specific conditions; S2: After the polymerization reaction in step S1 has proceeded for a certain period of time, a dicarboxylic acid chain extender is added, and a crosslinking reaction is carried out under the protection of an inert gas to obtain a prepolymer of modified PLA material; S3: Add thiophene monomer, oxidant and organic solvent to the prepolymer obtained in step S2, and carry out polymerization reaction under the action of subcritical carbon dioxide; after the reaction is completed, cast tape and pelletize to obtain the initial product of modified PLA material. S4: The primary product is mixed evenly with unmodified PLA masterbatch, PBAT masterbatch and additives, melt-extruded and granulated to finally obtain a biodegradable and environmentally friendly lighter shell material.

2. The preparation process of the degradable and environment-friendly lighter shell material according to claim 1, characterized in that, The lactide is at least one of L-lactide, D-lactide, and D,L-lactide.

3. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, The diol initiator is a mixture of dihydroxyphenylphosphine and butanediol.

4. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, The catalyst is at least one of stannous octoate, stannous acetate, and stannous chloride.

5. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, In step S1, the reaction conditions for the ring-opening polymerization reaction are: inert atmosphere protection, reaction temperature 120-160℃, and reaction time 1-6 hours.

6. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, The dicarboxylic acid chain extender is composed of 3-thiophene malonic acid, 1,5-glutaric acid, and / or 1,6-adipic acid.

7. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, In step S2, the reaction conditions for the crosslinking reaction are: reaction temperature 150-180℃, reaction pressure less than or equal to 1000Pa, and reaction time 1-2 hours.

8. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, The thiophene monomer is at least one of thiophene, 3-pentylthiophene, 3-hexylthiophene, and 3-heptylthiophene.

9. The preparation process of the biodegradable and environmentally friendly lighter casing material as described in claim 1, characterized in that, The oxidant is at least one of anhydrous ferric chloride, ammonium persulfate, and sodium persulfate.

10. A biodegradable and environmentally friendly lighter casing material, characterized in that, The shell material is prepared using the biodegradable and environmentally friendly lighter shell material preparation process described in any one of claims 1 to 9.