A silicone rubber thermally conductive composite material and its preparation method

By introducing a bifunctional dynamic crosslinking agent and a surface hydroxylated thermally conductive filler into silicone rubber, a flexible, self-healing thermally conductive composite material is formed, which solves the contradiction between thermal conductivity and mechanical properties in the existing technology, achieves efficient heat dissipation and recyclability, and meets the requirements of green manufacturing.

CN123107360APending Publication Date: 2026-11-17HONG KONG UNIV OF SCI & TECH (GUANGZHOU)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202511791298.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

While existing silicone rubber thermally conductive composite materials improve thermal conductivity, their mechanical properties decrease, especially their flexibility and reliability. Furthermore, they are not self-healing or recyclable, making it difficult to meet the high-efficiency heat dissipation requirements and green manufacturing requirements of electronic devices.

Method used

A flexible self-healing material is formed by using silicone rubber containing carbon-carbon unsaturated bonds, a bifunctional dynamic crosslinking agent, and surface hydroxylated thermally conductive fillers through a dynamic crosslinking network. It is prepared through a specific process to achieve high thermal conductivity and reprocessability.

Benefits of technology

A silicone rubber thermally conductive composite material with excellent thermal conductivity (>5.0 W/mK), good mechanical properties, self-healing ability, and reprocessability has been developed, which improves the reliability and environmental friendliness of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The application discloses a silica gel heat-conducting composite material, which comprises the following components in parts by weight: 100 parts of carbon-carbon unsaturated bond-containing silicone rubber, 0.5-6 parts of vulcanizing agent, 2-10 parts of bifunctional dynamic crosslinking agent and 50-200 parts of heat-conducting filler. The dynamic boron-oxygen bond in the bifunctional dynamic crosslinking agent is used to realize dynamic crosslinking of the silicone rubber, so that the silicone rubber composite is endowed with better flexibility and self-healing capacity. The interaction between the filler and the base can be obviously increased, the mechanical property is improved, and the heat-conducting property is obviously improved. Meanwhile, the dynamic crosslinking can realize recycling of the silica gel heat-conducting composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and in particular to a silicone rubber thermally conductive composite material and its preparation method. Background Technology

[0002] With the increasing integration and miniaturization of electronic components and the rapid development of industries such as energy, electronic devices are increasingly designed to integrate high-energy-consuming and high-power components into small parts. This poses a significant challenge to the heat dissipation capabilities of these devices. High-energy-consuming, highly integrated devices generate a large amount of heat, causing a rapid rise in temperature, which can lead to abnormal operation or even malfunctions. Prolonged high-temperature operating environments directly damage operational stability and equipment lifespan. Efficient heat dissipation has become crucial for ensuring equipment reliability and lifespan. Thermal interface materials, such as silicone rubber gaskets, are widely used in heat sinks to fill micron-level air gaps, reduce contact thermal resistance, and improve heat dissipation efficiency. Silicone rubber (such as methyl vinyl silicone rubber), due to its excellent high and low temperature resistance, electrical insulation, and flexibility, can perform functions such as heat dissipation, shock absorption, puncture resistance, and sealing, and is considered an ideal matrix for thermal interface materials.

[0003] However, intrinsic silicone rubber has extremely low thermal conductivity (typically between 0.1-0.3 W / m·K), which cannot meet the heat dissipation requirements of modern electronic devices. To improve its thermal conductivity, the most common strategy is to fill the silicone rubber matrix with highly thermally conductive functional fillers, such as alumina, aluminum nitride, zinc oxide, and boron nitride. For example, patent CN201911190641.7 discloses modified boron nitride particles and its preparation method, wherein the modified boron nitride is encapsulated in a silicone rubber polymer. When the modified boron nitride content is 50%, the thermal conductivity of the material reaches 2.1 W / (m·K). Another example is patent CN201910131663.X, which discloses a silicone rubber-based thermally conductive material filled with functionalized boride and its preparation method. When the silicone rubber matrix contains 100 parts and the functionalized boride contains 170 parts, i.e., when the functionalized boron nitride content is approximately 65%, the thermal conductivity of the material reaches 1.1 W / (m·K).

[0004] Typically, as in the aforementioned patents, introducing a high content of thermally conductive fillers is the main strategy to achieve good thermal conductivity. However, this inevitably leads to a significant decrease in the mechanical properties of the composite material, especially a reduction in flexibility. This trade-off in mechanical properties for high thermal conductivity is substantial, manifested as a significant decrease in tensile properties and a sharp increase in modulus. For example, in patent CN201710038586.4, using 64g of silicone rubber and 30g of boron nitride, the resulting thermally conductive composite has only 195% elongation at break and a tensile strength as high as 5.4 MPa. The silicone rubber matrix used in this patent is TPSIV4200-70A, with theoretical values ​​for elongation at break and tensile modulus of 554% and 3.9 MPa, respectively. The original elastic silicone is transformed into a "hard and brittle" composite material with limited ductility, severely affecting its ability to adhere to the heat source during use as a thermally conductive composite material. Typically, when the BN filler content exceeds 50 wt%, although the thermal conductivity of the composite material is improved (even reaching over 5.0 W / mK), its mechanical properties, especially elongation at break, decrease sharply. The material becomes hard and brittle, with significantly reduced flexibility, making it prone to cracking or permanent damage under bending or tensile stress. Furthermore, high filler content leads to excessive rubber density, failing to meet the demands of increasingly lightweight electronic components. The large-scale introduction of high-density fillers also results in poor interfacial compatibility of the bulk components. Even so, the thermal conductivity of existing silicone rubber thermally conductive composite products is generally mediocre, increasingly lagging behind the growing heat dissipation requirements of devices.

[0005] In addition, existing thermally conductive silicone rubbers based on permanent covalent cross-linked networks have a significant limitation: the materials lack dynamic self-healing properties and recyclability.

[0006] During assembly, transportation, or use, thermal interface materials in electronic devices may develop microcracks due to scratches, compression, or fatigue stress. Once this physical damage occurs, the cracks in traditional thermally conductive silicone rubber continue to propagate due to the rigidity of its permanently cross-linked network, failing to heal on their own. This leads to interruptions in heat conduction paths, a sharp increase in localized thermal resistance, the formation of overheating hotspots, and ultimately, jeopardizing the safety and lifespan of the entire electronic device. Repairing or replacing these built-in gaskets is often costly and difficult. Furthermore, the three-dimensional network structure of traditional thermosetting silicone rubber cannot be melted or reshaped after cross-linking and curing. This means that scraps, defective products, and end-of-life waste generated during production cannot be recycled using simple thermal processing methods. These materials typically end up in landfills or incinerators, resulting in resource waste and increasing environmental pressure. This contradicts the globally advocated principles of green and sustainable manufacturing.

[0007] Therefore, there is an urgent need in this field for a breakthrough solution that can achieve high thermal conductivity and high flexibility while endowing materials with intelligent self-healing capabilities to improve their reliability and service life, and possess reprocessing / recyclability to meet the requirements of green manufacturing. Developing such a dynamically cross-linked thermally conductive composite material that integrates multiple superior properties has become a clearly existing and pressing technical challenge in this field. Summary of the Invention

[0008] The purpose of this invention is to provide a silicone rubber thermally conductive composite material with self-healing ability, reprocessability, good thermal conductivity (>5.0W / mK), and good mechanical properties, as well as its preparation method.

[0009] This invention is achieved through the following technical solution: A silicone thermally conductive composite material, by weight, comprises the following components: 100 parts of silicone rubber containing carbon-carbon unsaturated bonds; 0.5-6 parts of vulcanizing agent; 2-10 parts of a bifunctional dynamic crosslinking agent; 50-200 parts of thermally conductive filler; The chemical formula of the aforementioned bifunctional dynamic crosslinking agent is as follows: Formula I or Formula II: Formula I; Formula II; Wherein, R1 is at least one of phenylene, biphenyl, naphthyl, alkylene with 1-8 carbon atoms, and cycloalkyl with 4-6 carbon atoms, R2 is an alkylene with 1-8 carbon atoms, and R3 is an alkylene with 1-8 carbon atoms.

[0010] The phenylene oxide can be 1,4-phenylene oxide, 1,3-phenylene oxide, etc.

[0011] Alkylenes with 1-8 carbon atoms can be butylene, methylene, ethylene, propylene, hexene, octylene, etc., and can be straight-chain alkyl or branched alkyl.

[0012] In Formula I, the substitution positions of R2 and R3 can be arbitrarily the 4th or 5th position of dioxoborane.

[0013] In Formula II, the mercapto substitution position can be any position 4 or 5 of dioxoborane.

[0014] The silicone rubber containing carbon-carbon unsaturated bonds is selected from at least one of vinyl silicone rubber, methyl vinyl silicone rubber, terminal vinyl silicone oil, phenyl vinyl silicone rubber, fluorovinyl silicone rubber, and acryloyloxy silicone rubber.

[0015] In the silicone rubber thermally conductive composite material of the present invention, the silicone rubber containing carbon-carbon unsaturated bonds accounts for not less than 25 wt% of the total weight.

[0016] The vulcanizing agent used in this field can be selected from at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,4-dichlorobenzoyl peroxide, bis(2,4-dichlorobenzoyl peroxide), benzoyl peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and dicumyl peroxide.

[0017] The thermally conductive filler is selected from at least one of metal oxides, metal nitrides, carbon materials, metal thermally conductive fillers, carbides and their derivatives.

[0018] Optionally, the metal oxide is selected from at least one of aluminum oxide, zinc oxide, and magnesium oxide; the metal nitride is selected from at least one of aluminum nitride, boron nitride, and silicon nitride; the carbon material is selected from at least one of graphite, graphene, carbon nanotubes, carbon fibers, carbon dots, and diamond; the metallic thermally conductive filler is selected from at least one of copper powder, aluminum powder, and silver powder; and the carbide is selected from at least one of silicon carbide, boron carbide, and two-dimensional carbides (MXenes).

[0019] Boron nitride is selected from at least one of hexagonal boron nitride, rhombohedral boron nitride, cubic boron nitride, and wurtzite boron nitride.

[0020] Preferably, the thermally conductive filler is selected from surface-hydroxylated thermally conductive fillers, which are selected from at least one of surface-hydroxylated metal oxides, surface-hydroxylated metal nitrides, surface-hydroxylated carbon materials, surface-hydroxylated metallic thermally conductive fillers, surface-hydroxylated carbides, and their derivatives. Specifically, the surface-hydroxylated metal oxides are selected from at least one of surface-hydroxylated alumina, surface-hydroxylated zinc oxide, and surface-hydroxylated magnesium oxide; the surface-hydroxylated metal nitrides are selected from at least one of surface-hydroxylated aluminum nitride, surface-hydroxylated boron nitride, and surface-hydroxylated silicon nitride; the surface-hydroxylated carbon materials are selected from at least one of surface-hydroxylated graphite, surface-hydroxylated graphene, surface-hydroxylated carbon nanotubes, surface-hydroxylated carbon fibers, surface-hydroxylated carbon dots, and surface-hydroxylated diamond; the surface-hydroxylated metallic thermally conductive fillers are selected from at least one of surface-hydroxylated copper powder, surface-hydroxylated aluminum powder, and surface-hydroxylated silver powder; and the surface-hydroxylated carbides are selected from at least one of surface-hydroxylated silicon carbide, surface-hydroxylated boron carbide, and surface-hydroxylated two-dimensional carbides (MXenes).

[0021] More preferably, the surface-hydroxylated thermally conductive filler is selected from surface-hydroxylated boron nitride. Surface-hydroxylated boron nitride is selected from at least one of hydroxylated hexagonal boron nitride, hydroxylated rhombohedral boron nitride, hydroxylated cubic boron nitride, and hydroxylated wurtzite boron nitride. More preferably, the modified boron nitride is hydroxylated hexagonal boron nitride.

[0022] The average particle size of the thermally conductive filler is 1-20 micrometers.

[0023] The chemical formula I of the bifunctional dynamic crosslinking agent can be: R1 is 1,4-phenylene, R2 is methylene, and R3 is methylene; R1 is 1,3-phenylene, R2 is methylene, and R3 is methylene; R1 is phenylene, R2 is propylene, and R3 is propylene; R1 is phenylene, R2 is butylene, and R3 is butylene; R1 is butylene, R2 is methylene, and R3 is methylene; R1 is biphenyl, R2 is methylene, and R3 is methylene; R1 is cyclohexyl, R2 is ethylidene, and R3 is ethylidene.

[0024] Bifunctional dynamic crosslinking agent chemical formula II can be: R1 can be 1,4-phenylene, 1,3-phenylene, butylene, cyclohexyl, biphenyl, etc.

[0025] Preferably, the bifunctional dynamic crosslinking agent is selected from Formula II.

[0026] The mechanism is illustrated using 2,2'-(1,4-phenylene)bis(4-mercaptomethyl-1,3,2-dioxoborane) / vinyl silicone rubber / surface hydroxylated hexagonal boron nitride as an example: The molecular formula of dynamically cross-linked silicone rubber is: ; The roles of dynamically cross-linked silicone rubber and modified boron nitride: ; The product also includes 0-10 parts by weight of rubber reinforcing agent, which is a commonly used rubber reinforcing agent in the art. For example, the rubber reinforcing agent is selected from at least one of silica, diatomaceous earth, carbon black, calcium carbonate, titanium dioxide, diatomaceous earth, magnesium, and organic resin reinforcing agents.

[0027] The silicone rubber thermally conductive composite material can be modified according to actual needs. By weight, it also includes processing aids such as 3-8 parts of plasticizer methyl silicone oil, 1-5 parts of heat resistant agent such as iron oxide (Fe2O3), and 0.5-5 parts of colorant such as cobalt blue.

[0028] The method for preparing the silicone thermally conductive composite material of the present invention includes the following steps: Step A: According to the formula, the raw silicone rubber containing carbon-carbon unsaturated bonds, vulcanizing agent, bifunctional dynamic crosslinking agent, rubber reinforcing agent, and thermally conductive filler are mixed in an intensive mixing environment at a temperature of 80-160℃ for 20-120 minutes to obtain the precursor. Step B: Place the precursor in a mold and hot-press it at 100-200℃ for 10-120 minutes to obtain a silicone thermally conductive composite material.

[0029] The present invention has the following beneficial effects: First, the present invention utilizes the dynamic boron-oxygen bonds in a bifunctional dynamic crosslinking agent to achieve dynamic crosslinking of silicone rubber, thereby endowing the silicone rubber composite with better flexibility and self-healing ability.

[0030] Secondly, the improved flexibility of the silicone rubber composite allows for better bonding with the thermally conductive filler, effectively enhancing thermal conductivity. Furthermore, the edge boron atoms and hydroxyl groups of the surface-hydroxylated thermally conductive filler participate in dynamic cross-linking, further increasing the interaction between the filler and the substrate, significantly improving both mechanical properties and thermal conductivity.

[0031] Third, by utilizing a specific amount of dynamic cross-linking density, the recycling and reuse of silicone thermally conductive composite materials can be achieved. Detailed Implementation

[0032] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0033] The raw materials used in this invention are sourced from the following sources: Vinyl silicone rubber: Vinyl silicone rubber raw material DY-V110, Shandong Dayi Chemical Co., Ltd.; Bis(2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane, Shanghai Maclean Biochemical Technology Co., Ltd.; Dynamic crosslinking agent A: 2,2'-(1,4-phenylene)bis(4-mercaptomethyl-1,3,2-dioxoboronylpentane), prepared in-house, was prepared by accurately weighing phenyl-1,4-diboronic acid, 1-thioglycerol, and MgSO4 (mass ratio 3:4:5) and dissolving them in tetrahydrofuran. After stirring at room temperature for 24 hours, the mixture was filtered to remove MgSO4, and the crude product was obtained by evaporation and concentration. The crude product was then obtained by filtration, washing with heptane, and concentration and purification.

[0034] Dynamic crosslinking agent B: 2,2'-(1,4-phenylene)bis(5-mercapto-1,3,2-dioxoboronylpentane), self-made; Dynamic crosslinking agent C: 2,2'-(1,3-phenylene)bis(4-mercaptomethyl-1,3,2-dioxoboronylpentane), prepared in-house; Dynamic crosslinking agent D: 2,2'-(1,4-phenylene)bis(5-mercaptopropyl-1,3,2-dioxoborhexane), self-made; Dynamic crosslinking agent E: 2,2'-(1,4-butylene)bis(4-mercaptomethyl-1,3,2-dioxoboronyl pentane), self-made; Dynamic crosslinking agent F: 2,2'-(1,4-cyclohexyl)bis(4-mercaptoethyl-1,3,2-dioxoborhecyclopentane), self-made; Thermally conductive filler A: Alumina, particle size 2 micrometers, Dongguan Dongchao New Material Technology Co., Ltd.; Thermally conductive filler B: Copper powder, particle size 1-3 microns, Shanghai Pantian Powder Co., Ltd.; Thermally conductive filler C: Silicon carbide, particle size 1-3 micrometers, Shandong Jinmeng New Material Co., Ltd.

[0035] Thermally conductive filler D: Hexagonal boron nitride, particle size 1~5 micrometers, Shanghai Maclean Biochemical Technology Co., Ltd.; Thermally conductive filler E: Rhombohedral boron nitride, particle size 2~4 micrometers, Shanghai Xiaohuang Nanotechnology Co., Ltd.; Thermally conductive filler F: Cubic boron nitride micro powder, 8-10 microns, Henan Xinyang Delong Superhard Materials Co., Ltd.; Thermally conductive filler G: Zinc ore boron nitride, 3-5 microns, Shenzhen Guangxinyuan Chemical Co., Ltd.; Thermally conductive filler H: Surface-hydroxylated alumina. Alumina powder was added to 2 mol / mL hydrochloric acid and reacted for 3 hours at 60-80 ℃ with magnetic stirring. The solvent was removed by filtration, and the mixture was repeatedly washed with deionized water until neutral, then dried at 60-100 ℃.

[0036] Thermally conductive filler I: Surface-hydroxylated copper powder, hydrogen peroxide oxidation method. First, briefly soak the copper powder in dilute hydrochloric acid or dilute acetic acid (about 30-60 seconds) to remove the natural oxide layer and contaminants on the surface. Add the treated copper powder to a 30% H2O2 solution and stir to react at room temperature or 40℃ for 5-30 minutes.

[0037] Thermally conductive filler J: Surface hydroxylated hexagonal boron nitride, ball milling method: Hexagonal boron nitride and urea (mass ratio 8:2) are put into a planetary ball mill for high-intensity mechanical grinding (200-500 rpm) for 20 hours.

[0038] Thermally conductive filler K: Surface hydroxylated cubic boron nitride, chemical oxidation method, cubic boron nitride powder is mixed with a strong oxidant (concentrated nitric acid: 30% hydrogen peroxide = 1:2), placed in a reactor and reacted at a high temperature of 180-250℃ for 24-72 hours, and the raw material is obtained after filtration and drying.

[0039] Thermally conductive filler L: Surface hydroxylated wurtzite boron nitride, chemical oxidation method, wurtzite boron nitride is mixed with a strong oxidant (concentrated nitric acid: 30% hydrogen peroxide = 1:2), placed in a reactor and reacted at a high temperature of 200-300℃ for 48-120 hours, and the raw material is obtained after filtration and drying.

[0040] Thermally conductive filler M: Surface-hydroxylated rhombic boron nitride, produced by hydrothermal method. Rhombic boron nitride powder is mixed with deionized water (1:40) and ultrasonically treated for 30-60 minutes to form a homogeneous suspension. The suspension is transferred to a polytetrafluoroethylene-lined high-pressure reactor and reacted at 150-200℃ for 6-24 hours. After the reaction is complete, it is allowed to cool naturally, repeatedly centrifuged and washed with deionized water and ethanol until neutral, and finally vacuum dried at 60-80℃.

[0041] Thermally conductive filler N: Surface-hydroxylated silicon carbide, thermally oxidized. The silicon carbide powder is placed in a tube furnace and heated for 1-4 hours in an oxygen or air atmosphere at 800-1100℃. The oxidized sample is then immersed in deionized water or boiling water for 4-6 hours and dried at low temperature (e.g., 60-100℃).

[0042] Silica: Particle size 0.5-2 microns, Guangdong Lvwei New Material Technology Co., Ltd.; Fe2O3: Iron oxide, 99.95%, particle size 1 micrometer, Shanghai Maclean Biochemical Technology Co., Ltd.

[0043] Preparation method of silicone rubber thermally conductive composite material in the examples and comparative examples: According to the formula, raw silicone rubber containing carbon-carbon unsaturated bonds, vulcanizing agent, bifunctional dynamic crosslinking agent, rubber reinforcing agent and boron nitride are mixed in an intensive mixing temperature of 110°C for 60 min to obtain a precursor; the precursor is placed in a mold and hot-pressed at 160°C and 15 MPa for 80 min to obtain silicone thermally conductive composite material.

[0044] Test methods: (1) Thermal conductivity: HotDisk TPS 2500 transient method, sample size 40 mm*40 mm*2 mm; (2) Elongation at break: Instron-68TM universal testing machine, ASTM D412; (3) Self-healing: The sample size is 40 mm*40 mm*2 mm, the penetrating scratch length is 10 mm, and 5 scratches are made at 5 mm intervals. Then, it is heat-healed at 140℃ and 10MPa for 20 minutes. After the healing treatment, the elongation at break is tested and calculated as follows: the elongation at break before and after self-healing = elongation at break after self-healing test / elongation at break before self-healing test * 100%. >90% is excellent, 80-90% is good, 30-80% is poor, and less than 30% indicates no self-healing.

[0045] (4) Recyclability: Hot pressing of fragments, same as step B, placing fragments with a diameter of less than 5 mm in a mold, hot pressing at 150-170℃ and 10-25MPa for 40-120 min, to obtain recycled silicone thermally conductive composite material, measuring the change rate of thermal conductivity and elongation at break before and after, change rate = (thermal conductivity and elongation at break after self-healing test - thermal conductivity and elongation at break before test) / thermal conductivity and elongation at break before self-healing test * 100%, less than 5% indicates good recyclability.

[0046] Table 1: Component content and test results of silicone rubber thermally conductive composite materials in Examples 1-7 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Vinyl silicone rubber 100 100 100 100 100 100 100 Bis(2,5) sulfide 1 2 3 1 1 1 1 Dynamic crosslinking agent selection B B B A C D E Dynamic crosslinking agent content 2 5 10 2 2 2 2 Thermally conductive filler J 100 50 200 100 100 100 100 precipitate 10 2 0 10 10 10 10 <![CDATA[Fe2O3]]> 0.5 Thermal conductivity, W / (m·K) 6.41 2.98 8.63 6.23 6.17 6.33 6.12 Elongation at break, % 486 279 192 459 438 411 463 Self-healing, % 95.83 90.1 87.5 92.0 92.2 91.7 91.1 Recovery thermal conductivity change rate, % -1.3 -7.6 -11.1 -2.7 -2.4 -3.7 -4.6 Change in elongation at break after recovery, % -2.7 -8.9 -17.4 -3.9 -3.4 -4.1 -5.2 As can be seen from Examples 1 / 4 / 5 / 6 / 7 / 8, the bifunctional dynamic crosslinking agent is selected from Formula II.

[0047] Table 2: Component content and test results of silicone rubber thermally conductive composite materials in Examples 8-14 Example 8 Example 9 Example 10 Example 11 Example 12 Example 13 Example 14 Vinyl silicone rubber 100 100 100 100 100 100 100 Bis(2,5)sulfide 1 1 1 1 1 1 1 Dynamic crosslinking agent A 2 2 2 2 2 2 Dynamic crosslinking agent F 2 Thermally conductive filler serial number J M K L H I N thermally conductive filler content 100 100 100 100 100 100 100 precipitate 10 10 10 10 10 10 10 Thermal conductivity, W / (m·K) 6.03 6.23 6.17 6.02 5.76 5.92 5.23 Elongation at break, % 441 424 394 403 441 417 416 Self-healing, % 90.7 91.7 92.0 91.6 91.1 91.0 91.3 Recovery thermal conductivity change rate, % -2.7 -1.7 -2.2 -3.2 -3.7 -4.1 -4.4 Change in elongation at break (%) -4.1 -3.4 -4.6 4.9 -5.2 -9.2 -7.6 Table 3: Component content and test results of silicone rubber thermally conductive composite materials in Examples 14-21 Example 15 Example 16 Example 17 Example 18 Example 19 Example 20 Example 21 Vinyl silicone rubber 100 100 100 100 100 100 100 Bis(2,5)sulfide 1 1 1 1 1 1 1 Dynamic crosslinking agent A 2 2 2 2 2 2 2 Thermally conductive filler serial number D E F G A B C thermally conductive filler content 100 100 100 100 100 100 100 precipitate 10 10 10 10 10 10 10 Thermal conductivity, W / (m·K) 4.67 4.28 4.32 4.27 3.88 4.13 3.97 Elongation at break, % 384 378 297 311 339 347 302 Self-healing, % 87.6 88.1 86.4 85.1 88.4 83.7 82.9 Recovery thermal conductivity change rate, % -3.4 -4.8 -6.1 -5.3 -5.7 -5.2 -5.9 Change in elongation at break (%) -7.9 -8.6 -9.2 -7.6 -7.2 -9.2 -10.1 As can be seen from Examples 4 / 8-21, surface-hydroxylated thermally conductive fillers are preferred, surface-hydroxylated boron nitride is even more preferred, and surface-hydroxylated hexagonal boron nitride is even more preferred.

[0048] Table 4: Component content and test results of comparative silicone rubber thermally conductive composite materials Comparative Example 1 Comparative Example 2 Comparative Example 3 Vinyl silicone rubber 100 100 100 Bis(2,5)sulfide 2 7 0 Dynamic crosslinking agent B / 5 5 Hexagonal boron nitride 50 50 50 precipitate 2 2 2 Thermal conductivity, W / (m·K) 1.84 2.42 2.34 Elongation at break, % 157 268 109 Self-healing, % 7.3 64.7 91.3 Recovery thermal conductivity change rate, % - -13.2 -1.9 Change in elongation at break after recovery, % - -23.3 -3.6 As shown in Comparative Example 1, the product without dynamic cross-linking agent has almost no self-healing properties and cannot be recycled.

[0049] As can be seen from Comparative Example 2, when the vulcanizing agent content is too high, the elongation at break, self-healing property, and recyclability all decrease significantly, and the thermal conductivity is significantly lower than that of Example 2.

[0050] As can be seen from Comparative Example 3, when no vulcanizing agent is present, the self-healing and recyclability are good, but the elongation at break is too low, and the thermal conductivity is significantly reduced compared to Example 2.

Claims

1. A silica gel thermally conductive composite material, characterized in that, By weight, it includes the following components: 100 parts of silicone rubber containing carbon-carbon unsaturated bonds; 0.5-6 parts of vulcanizing agent; 2-10 parts of a bifunctional dynamic crosslinking agent; 50-200 parts of thermally conductive filler; The chemical formula of the aforementioned bifunctional dynamic crosslinking agent is as follows: Formula I or Formula II: Formula I; Formula II; Wherein, R1 is at least one of phenylene, biphenyl, naphthyl, alkylene with 1-8 carbon atoms, and cycloalkyl with 4-6 carbon atoms, R2 is an alkylene with 1-8 carbon atoms, and R3 is an alkylene with 1-8 carbon atoms.

2. The silicone thermally conductive composite material according to claim 1, characterized in that, The silicone rubber containing carbon-carbon unsaturated bonds is selected from at least one of vinyl silicone rubber, methyl vinyl silicone rubber, terminal vinyl silicone oil, phenyl vinyl silicone rubber, fluorovinyl silicone rubber, and acryloyloxy silicone rubber.

3. The silicone thermally conductive composite material according to claim 1, characterized in that, The vulcanizing agent is selected from at least one of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,4-dichlorobenzoyl peroxide, bis(2,4-dichlorobenzoyl peroxide), benzoyl peroxide, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and dicumyl peroxide.

4. The silicone thermally conductive composite material according to claim 1, characterized in that, The thermally conductive filler is selected from at least one of metal oxides, metal nitrides, carbon materials, metal-based thermally conductive fillers, carbides and their derivatives; the metal oxide is selected from at least one of aluminum oxide, zinc oxide, and magnesium oxide; the metal nitride is selected from at least one of aluminum nitride, boron nitride, and silicon nitride; the carbon material is selected from at least one of graphite, graphene, carbon nanotubes, carbon fibers, carbon dots, and diamond; the metal-based thermally conductive filler is selected from at least one of copper powder, aluminum powder, and silver powder; and the carbide is selected from at least one of silicon carbide, boron carbide, and two-dimensional carbides.

5. The silicone thermally conductive composite material according to claim 4, characterized in that, The thermally conductive filler is selected from surface-hydroxylated thermally conductive fillers, which are selected from at least one of surface-hydroxylated metal oxides, surface-hydroxylated metal nitrides, surface-hydroxylated carbon materials, surface-hydroxylated metal thermally conductive fillers, surface-hydroxylated carbides and their derivatives.

6. The silicone thermally conductive composite material according to claim 1, characterized in that, The average particle size of the thermally conductive filler is 1-20 micrometers.

7. The silicone thermally conductive composite material according to claim 1, characterized in that, In the aforementioned bifunctional dynamic crosslinking agent of formula I, R1 is 1,4-phenylene, R2 is methylene, and R3 is methylene; R1 is 1,3-phenylene, R2 is methylene, and R3 is methylene; R1 is phenylene, R2 is propylene, and R3 is propylene; R1 is phenylene, R2 is butylene, and R3 is butylene; R1 is butylene, R2 is methylene, and R3 is methylene; R1 is biphenyl, R2 is methylene, and R3 is methylene; R1 is cyclohexyl, R2 is ethylene, and R3 is ethylene; the aforementioned bifunctional dynamic crosslinking agent is selected from formula II, where R1 is phenylene.

8. The silicone thermally conductive composite material according to claim 1, characterized in that, The product also includes 0-10 parts by weight of a rubber reinforcing agent, wherein the rubber reinforcing agent is selected from at least one of silica, diatomaceous earth, carbon black, calcium carbonate, titanium dioxide, magnesium, and organic resin reinforcing agents.

9. The silicone thermally conductive composite material according to claim 1, characterized in that, Based on parts by weight, it also includes processing aids; said processing aids are selected from at least one of plasticizers, heat resistant agents, and colorants.

10. A method for preparing the silicone thermally conductive composite material according to any one of claims 1-9, characterized in that, Includes the following steps: Step A: According to the formula, the raw silicone rubber containing carbon-carbon unsaturated bonds, vulcanizing agent, bifunctional dynamic crosslinking agent, rubber reinforcing agent, and thermally conductive filler are mixed in an intensive mixing environment at a temperature of 80-160℃ for 20-120 minutes to obtain the precursor. Step B: Place the precursor in a mold and hot-press it at 100-200℃ for 10-120 minutes to obtain a silicone thermally conductive composite material.

Citation Information

Patent Citations

  • Heat-conducting silicone rubber composite material and preparation method thereof

    CN106810869A

  • Functionalized boride filled silicone rubber-based heat conduction material and preparation method thereof

    CN109777111A

  • Modified boron nitride particles, their preparation method and application

    CN110862576B