A thermally conductive pad and its preparation method
By introducing negative thermal expansion regulators such as zirconium tungstate and zirconium vanadate, the thermal expansion coefficient of the thermally conductive pad is adjusted, which solves the problem of poor thermal cycling reliability caused by thermal expansion coefficient mismatch and achieves high thermal conductivity, low thermal expansion coefficient and excellent thermal cycling stability.
Patent Information
- Application Number
- CN202611320848.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing high thermal conductivity interface materials suffer from poor thermal cycling reliability due to the mismatch in thermal expansion coefficients, and are prone to problems such as interface delamination and increased thermal resistance.
By using negative thermal expansion regulators such as zirconium tungstate and zirconium vanadate, the thermal expansion coefficient of the material is adjusted to be close to that of metal heat sinks and chips. Combined with polymer matrix and thermally conductive filler, a dense stacked structure is formed, reducing the accumulation of thermal stress.
It significantly reduces the coefficient of thermal expansion of materials, improves the reliability of thermal cycling, reduces the accumulation of thermal stress, suppresses excessive expansion of materials at high temperatures and excessive contraction at low temperatures, alleviates the oil pumping effect, and ensures the stability of geometric structure.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application belongs to the field of electronic packaging materials technology, and relates to a thermally conductive pad and its preparation method, specifically a thermally conductive pad with high thermal conductivity, low coefficient of thermal expansion and excellent thermal cycling stability and its preparation method. Background Technology
[0002] With the rapid development of 5G communication, new energy vehicles, and high-performance computing (HPC), the power density of electronic components is increasing exponentially. Thermal interface materials (TIMs), as key materials for filling the micro-gaps between heat-generating chips and heat sinks, directly determine the operational stability of electronic devices.
[0003] Currently, most mainstream thermal interface materials on the market use polymers (such as silicone rubber and epoxy resin) as the matrix and high thermal conductivity ceramic powders such as alumina, aluminum nitride, and boron nitride as fillers. To keep up with the increasing demand for heat dissipation and achieve higher thermal conductivity, a very high filler ratio (typically exceeding 85 wt%) or the use of fillers with larger particle sizes is required. However, this design approach and technical method have the following drawbacks: the coefficient of thermal expansion (CTE) of the polymer matrix is typically between 200-300 ppm / K, while the coefficients of thermal expansion of chips (silicon, approximately 2.6 ppm / K) and heat sinks (copper / aluminum, approximately 17-23 ppm / K) are extremely low.
[0004] During long-term operation or thermal shock testing, this significant difference in thermal expansion coefficients generates substantial thermal stress at the interface. This cyclical thermal stress leads to: (1) Interface debonding: The filler separates from the matrix, generating microcracks, which leads to the interruption of the thermal path and a sharp increase in thermal resistance.
[0005] (2) Pumping effect: The material is squeezed out of the contact area during repeated expansion and contraction, resulting in drying failure.
[0006] (3) Warping deformation: This leads to the breakage of the connection between the chip and the substrate, and the expansion of the interface gap.
[0007] For such problems, most solutions focus on modifying the filler surface or selecting coupling agents, which improves the interfacial bonding to some extent, but does not solve the problem of the matrix itself having an excessively high coefficient of thermal expansion.
[0008] Therefore, developing a thermally conductive composite material that can actively adjust the coefficient of thermal expansion and maintain dimensional stability during thermal cycling as a thermally conductive pad has significant practical implications. Summary of the Invention
[0009] To address the shortcomings of existing technologies, the purpose of this application is to provide a thermally conductive pad and its preparation method, specifically a thermally conductive pad with high thermal conductivity, low coefficient of thermal expansion, and excellent thermal cycling stability, as well as its preparation method. This application aims to solve the problems of poor thermal cycling reliability, easy interface delamination, and increased thermal resistance caused by the mismatch of thermal expansion coefficients in existing high thermal conductivity interface materials.
[0010] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a thermally conductive pad, wherein the raw materials for preparing the thermally conductive pad, by weight, include the following raw materials: Polymer matrix: 2-10 parts; Thermally conductive filler: 85-95 parts; Negative thermal expansion regulator: 1-10 parts.
[0011] The thermal pad provided in this application significantly reduces the coefficient of thermal expansion of the material by introducing a negative thermal expansion regulator, making it closer to the coefficient of thermal expansion of metal heat sinks and chips. This greatly reduces the accumulation of thermal stress during thermal cycling, giving the thermal pad excellent thermal cycling reliability. In addition, the addition of the negative thermal expansion regulator can effectively suppress the excessive expansion of the material at high temperatures and the excessive contraction at low temperatures, alleviating the oil pumping effect.
[0012] In this application, the raw materials for preparing the thermal pad can be in the following quantities by weight: 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0013] In this application, the raw materials for preparing the thermal pad are in parts by weight, and the amount of thermally conductive filler can be 85 parts, 86 parts, 88 parts, 90 parts, 92 parts, 94 parts, 95 parts, etc.
[0014] In this application, the amount of negative thermal expansion regulator used in the preparation of the thermal pad can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc., according to the weight parts of the raw materials.
[0015] In some embodiments, the negative thermal expansion regulator has a negative coefficient of thermal expansion in the range of -50°C to 150°C.
[0016] In some embodiments, the negative thermal expansion regulator includes any one or a combination of at least two of zirconium tungstate, zirconium vanadate, zirconium phosphate, and cyanide complexes, preferably zirconium tungstate.
[0017] In some embodiments, the D50 particle size of the negative thermal expansion regulator is 0.5-3 μm, such as 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc. This application controls the D50 particle size of the negative thermal expansion regulator within a specific range, enabling it to fill the voids in the thermally conductive filler, forming a dense "packed structure." If the D50 particle size of the negative thermal expansion regulator is too small, the specific surface area will be too large, resulting in a high oil absorption value, which will hinder the formation of the thermally conductive network; if the D50 particle size of the negative thermal expansion regulator is too large, it will not be able to fill the voids and will easily cause stress concentration.
[0018] In some embodiments, the polymer matrix includes vinyl silicone oil, a crosslinking agent, and a catalyst.
[0019] In some embodiments, the polymer matrix comprises component A and component B, wherein component A comprises vinyl silicone oil and a crosslinking agent, and component B comprises vinyl silicone oil and a catalyst.
[0020] In some embodiments, based on the total mass of component A as 100%, the content of the vinyl silicone oil is 92%-97%, such as 92%, 93%, 94%, 95%, 96%, 97%, etc., and the content of the crosslinking agent is 3%-8%, such as 3%, 4%, 5%, 6%, 7%, 8%, etc.
[0021] In some embodiments, the content of the vinyl silicone oil is 92%-97% based on the total mass of the B component as 100%, for example 92%, 93%, 94%, 95%, 96%, 97%, etc., and the content of the catalyst is 3%-8%, for example 3%, 4%, 5%, 6%, 7%, 8%, etc.
[0022] In some embodiments, the crosslinking agent includes hydrogen-containing silicone oil.
[0023] In some embodiments, the catalyst comprises a platinum catalyst. In some embodiments, the mass ratio of component A to component B is (0.8-1.2):1, for example, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, etc.
[0024] In some embodiments, the thermally conductive filler comprises any one or a combination of at least two of aluminum nitride, aluminum oxide, and zinc oxide, preferably a combination of aluminum nitride, aluminum oxide, and zinc oxide. The thermally conductive filler preferably has a bimodal or multimodal particle size distribution.
[0025] In some embodiments, based on the total weight of the thermally conductive filler as 100%, the weight percentage of aluminum nitride is 40%-60% (e.g., 40%, 42%, 44%, 45%, 46%, 48%, 50%, 52%, 54%, 55%, 56%, 58%, 60%, etc.), the weight percentage of alumina is 20%-40% (e.g., 20%, 22%, 24%, 25%, 26%, 28%, 30%, 32%, 34%, 35%, 36%, 38%, 40%, etc.), and the weight percentage of zinc oxide is 10%-30% (e.g., 10%, 12%, 14%, 15%, 16%, 18%, 20%, 22%, 24%, 25%, 26%, 28%, 30%, etc.).
[0026] In some embodiments, the aluminum nitride comprises spherical aluminum nitride.
[0027] In some embodiments, the alumina includes spherical alumina.
[0028] In some embodiments, the thermally conductive filler includes spherical aluminum nitride, spherical aluminum oxide, and zinc oxide.
[0029] In some embodiments, the thermally conductive filler has a D90 particle size of 110-130 μm (e.g., 110 μm, 115 μm, 120 μm, 125 μm, 130 μm, etc.), a D50 particle size of 5-10 μm (e.g., 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.), and a D10 particle size of 1-5 μm (e.g., 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc.). It should be noted that the D90, D50, and D10 particle sizes mentioned here refer to the particle size parameters of a mixed filler consisting of aluminum nitride, aluminum oxide, and zinc oxide.
[0030] Secondly, this application provides a method for preparing a thermally conductive pad as described in the first aspect, the method comprising the following steps: The polymer matrix, thermally conductive filler, and negative thermal expansion regulator are mixed, and the resulting mixture is added to a mold and cured to obtain the thermally conductive pad.
[0031] In some embodiments, the mixing includes: first stirring at a speed of 1400-1600 rpm (e.g., 1400 rpm, 1450 rpm, 1500 rpm, 1550 rpm, 1600 rpm, etc.) for 110-130 seconds (e.g., 110 seconds, 115 seconds, 120 seconds, 125 seconds, 130 seconds, etc.), repeating 2-4 times (e.g., 2 times, 3 times, 4 times, etc.), and then rolling for 10-20 minutes (e.g., 10 minutes, 15 minutes, 20 minutes, etc.). The stirring can be performed in a planetary mixer, and the rolling can be performed in an internal mixer (e.g., a three-roll internal mixer, etc.).
[0032] In some embodiments, the mixing process further includes a dispersion and degassing step, specifically including: stirring at a speed of 1500-2500 rpm (e.g., 1500 rpm, 1600 rpm, 1700 rpm, 1800 rpm, 1900 rpm, 2000 rpm, 2100 rpm, 2200 rpm, 2300 rpm, 2400 rpm, 2500 rpm, etc.) for 110-130 seconds (e.g., 110 seconds, 115 seconds, 120 seconds, 125 seconds, 130 seconds, etc.) under a vacuum of -0.098 MPa, repeating 2-4 times (e.g., 2 times, 3 times, 4 times, etc.) until the mixture is uniform and free of bubbles.
[0033] In some embodiments, the curing temperature is 140-160℃ (e.g., 140℃, 145℃, 150℃, 155℃, 160℃, etc.), the vacuum degree during curing is -0.098MPa, and the curing time is 1-3h (e.g., 1h, 1.5h, 2h, 2.5h, 3h, etc.).
[0034] Compared with the prior art, this application has the following advantages: (1) Excellent thermal cycling reliability: The thermal pad provided in this application significantly reduces the coefficient of thermal expansion of the material by introducing a negative thermal expansion regulator, making it closer to the coefficient of thermal expansion of metal heat sinks and chips, greatly reducing the accumulation of thermal stress during thermal cycling, so that the thermal pad has excellent thermal cycling reliability (thermal resistance growth rate after 1000 thermal cycles: 4.5%~11.5%).
[0035] (2) Geometric stability: It effectively suppresses the excessive expansion of the material at high temperature and the excessive contraction at low temperature, and alleviates the oil pumping effect. Detailed Implementation
[0036] The technical solution of this application will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of this application and should not be considered as specific limitations thereof. For example, in this application, the thermally conductive filler includes any one or a combination of at least two of aluminum nitride, alumina, and zinc oxide. This application only uses aluminum nitride and alumina as examples and does not mean that this application can only use aluminum nitride or alumina. In this application, aluminum nitride and alumina can also be replaced by alumina, zinc oxide, or a combination thereof. As another example, in this application, the negative thermal expansion regulator includes any one or a combination of at least two of zirconium tungstate, zirconium vanadate, zirconium phosphate, and cyanide complexes. This application only uses zirconium tungstate as an example and does not mean that this application can only use zirconium tungstate. In this application, zirconium tungstate can also be replaced by zirconium vanadate or zirconium phosphate, or a combination thereof. Other structures and raw materials in this application can also be understood in this way.
[0037] Unless otherwise specified, the following information pertains to some of the raw materials used in the embodiments and comparative examples of this application: (1) Polymer matrix Component A: A mixture of vinyl silicone oil and hydrogen-containing silicone oil (mass ratio of 95:5), brand name HANTEK9125-A; Component B: A mixture of vinyl silicone oil and platinum catalyst (mass ratio 95:5), brand name HANTEK9125-B.
[0038] (2) Thermally conductive filler A mixture of spherical aluminum nitride, spherical alumina, and zinc oxide in a weight ratio of 50:30:20 has the following particle size distribution: D90=120μm, D50=10μm, D10=5μm, and a thermal conductivity of 30W / (m·K).
[0039] (3) Negative thermal expansion regulator NTE-1: Zirconium tungstate, D50=2μm, CTE≈-9×10 -6 / K; NTE-2: Zirconium vanadate, D50 = 2 μm, CTE ≈ -8 × 10⁻⁸ -5 / K; NTE-3: Zirconium tungstate, D50=0.5μm, CTE≈-9×10 -6 / K; NTE-4: Zirconium vanadate, D50 = 0.5 μm, CTE ≈ -8 × 10⁻⁸ -5 / K.
[0040] Example 1 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 92 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 3 parts.
[0041] The preparation method includes the following steps: (1) Mixing: Add the polymer matrix, thermally conductive filler and negative thermal expansion regulator into the planetary mixer according to the formula ratio, stir at 1500 rpm for 120 seconds, repeat 3 times, and then run through a three-roll mixer for 15 minutes. (2) Dispersion and degassing: Stir at 2000 rpm for 120 seconds under a vacuum of -0.098 MPa, repeat 3 times until the mixture is uniform and free of bubbles; (3) Curing: The mixture is coated into a mold, a mold with a fixed thickness of 2 mm is selected, and the mixture is cured at 150℃ and vacuum degree -0.098MPa for 2 hours to obtain the thermal pad.
[0042] Example 2 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 90 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 5 parts.
[0043] The preparation method is the same as in Example 1.
[0044] Example 3 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 88 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 7 parts.
[0045] The preparation method is the same as in Example 1.
[0046] Example 4 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 86 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 9 parts.
[0047] The preparation method is the same as in Example 1.
[0048] Example 5 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 92 parts; Negative thermal expansion regulator (zirconium tungstate, 0.5 μm): 3 parts.
[0049] The preparation method is the same as in Example 1.
[0050] Example 6 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 90 parts; Negative thermal expansion regulator (zirconium tungstate, 0.5 μm): 5 parts.
[0051] The preparation method is the same as in Example 1.
[0052] Example 7 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 88 parts; Negative thermal expansion regulator (zirconium tungstate, 0.5 μm): 7 parts.
[0053] The preparation method is the same as in Example 1.
[0054] Example 8 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 92 parts; Negative thermal expansion regulator (zirconium vanadate, 2μm): 3 parts.
[0055] The preparation method is the same as in Example 1.
[0056] Example 9 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 90 parts; Negative thermal expansion regulator (zirconium vanadate, 2μm): 5 parts.
[0057] The preparation method is the same as in Example 1.
[0058] Example 10 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 92 parts; Negative thermal expansion regulator (zirconium vanadate, 0.5 μm): 3 parts.
[0059] The preparation method is the same as in Example 1.
[0060] Example 11 This embodiment provides a thermally conductive pad, the raw materials for which are prepared include the following by weight: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 90 parts; Negative thermal expansion regulator (zirconium vanadate, 0.5 μm): 5 parts.
[0061] The preparation method is the same as in Example 1.
[0062] Example 12 The only difference between this embodiment and Example 1 is that the D50 particle size of zirconium tungstate is 0.3 μm.
[0063] Example 13 The only difference between this embodiment and Example 1 is that the D50 particle size of zirconium tungstate is 5 μm.
[0064] Comparative Example 1 This comparative example provides a thermally conductive pad, the raw materials for which are prepared, by weight, include the following: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 95 parts.
[0065] The preparation method includes the following steps: (1) Mixing: Add the polymer matrix and thermally conductive filler into the planetary mixer according to the formula ratio, stir at 1500 rpm for 120 seconds, repeat 3 times, and then run through a three-roll mixer for 15 minutes. (2) Dispersion and degassing: Stir at 2000 rpm for 120 seconds under a vacuum of -0.098 MPa, repeat 3 times until the mixture is uniform and free of bubbles; (3) Curing: The mixture is coated into a mold, a mold with a fixed thickness of 2 mm is selected, and the mixture is cured at 150℃ and vacuum degree -0.098MPa for 2 hours to obtain the thermal pad.
[0066] Comparative Example 2 This comparative example provides a thermally conductive pad, the raw materials for which are prepared, by weight, include the following: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 83 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 12 parts.
[0067] The preparation method includes the following steps: (1) Mixing: Add the polymer matrix, thermally conductive filler and negative thermal expansion regulator into the planetary mixer according to the formula ratio, stir at 1500 rpm for 120 seconds, repeat 3 times, and then run through a three-roll mixer for 15 minutes. (2) Dispersion and degassing: Stir at 2000 rpm for 120 seconds under a vacuum of -0.098 MPa, repeat 3 times until the mixture is uniform and free of bubbles; (3) Curing: The mixture is coated into a mold, a mold with a fixed thickness of 2 mm is selected, and the mixture is cured at 150℃ and vacuum degree -0.098MPa for 2 hours to obtain the thermal pad.
[0068] Comparative Example 3 This comparative example provides a thermally conductive pad, the raw materials for which are prepared, by weight, include the following: Polymer matrix: 5 parts (2.5 parts each of component A and component B); Thermally conductive filler: 94.5 parts; Negative thermal expansion regulator (zirconium tungstate, 2μm): 0.5 parts.
[0069] The preparation method includes the following steps: (1) Mixing: Add the polymer matrix, thermally conductive filler and negative thermal expansion regulator into the planetary mixer according to the formula ratio, stir at 1500 rpm for 120 seconds, repeat 3 times, and then run through a three-roll mixer for 15 minutes. (2) Dispersion and degassing: Stir at 2000 rpm for 120 seconds under a vacuum of -0.098 MPa, repeat 3 times until the mixture is uniform and free of bubbles; (3) Curing: The mixture is coated into a mold, a mold with a fixed thickness of 2 mm is selected, and the mixture is cured at 150℃ and vacuum degree -0.098MPa for 2 hours to obtain the thermal pad.
[0070] The performance of the thermal pads provided in the embodiments and comparative examples of this application was tested, as follows: (1) Thermal conductivity test Test Principles Based on Fourier's law, the thermal resistance (R=ΔT / Q) is calculated by measuring the temperature difference (ΔT) and heat flow (Q) on both sides of the sample.
[0071] Equipment and Standards Equipment: Dual-plate thermal conductivity meter (such as Gardon heat flow meter), constant temperature hot plate, temperature sensor (thermocouple).
[0072] Standard: ASTM D5470 (Thermal transfer properties of insulating materials).
[0073] (2) Test of thermal resistance growth rate under cyclic pressure Instrumentation: TIMA5 thermal interface material analyzer.
[0074] Test standard: Compress the thermal pad by 50% and test the thermal resistance, which is recorded as the initial thermal resistance; then increase the height to 75% of the initial thickness and test the thermal resistance; compress the thermal pad to 50% of the initial thickness again and increase the height to 75% of the initial thickness again, and perform a total of 1000 cycles. Calculate the ratio of the final change in thermal resistance to the initial thermal resistance, which is the thermal resistance growth rate.
[0075] The performance test results are shown in Table 1.
[0076] Table 1 As can be seen from Table 1, the thermal pads provided in Examples 1-11 of this application all have high thermal conductivity (5.36~6.02W / (m·K)) and high thermal cycling reliability (thermal resistance growth rate after 1000 thermal cycles: 4.5%~8.6%).
[0077] Compared with Example 1, the thermal resistance growth rate of the thermal pad provided in Example 12 after 1000 thermal cycles is slightly higher; the thermal resistance growth rate of the thermal pad provided in Example 13 is higher.
[0078] Compared with Examples 1-11, no negative thermal expansion regulator was added in Comparative Example 1. Although the thermal conductivity of the thermal pad was high, the thermal resistance growth rate after 1000 thermal cycles was as high as 22%, which shows that the material is prone to failure in thermal cycling when there is no negative thermal expansion regulator.
[0079] Compared with Example 1, the amount of negative thermal expansion regulator added in Comparative Example 2 was too high, and the thermal resistance growth rate of the thermal pad after 1000 thermal cycles was significantly increased. In Comparative Example 3, the amount of negative thermal expansion regulator added was too low, and the thermal resistance growth rate of the thermal pad after 1000 thermal cycles was also significantly increased.
[0080] The applicant declares that this application illustrates the thermally conductive pad and its preparation method through the above embodiments, but this application is not limited to the above embodiments, that is, it does not mean that this application must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of the raw materials used in this application, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of this application.
Claims
1. A thermally conductive pad, characterized in that, The raw materials for preparing the thermal pad include the following by weight: Polymer matrix: 2-10 parts; Thermally conductive filler: 85-95 parts; Negative thermal expansion regulator: 1-10 parts.
2. The thermally conductive pad according to claim 1, characterized in that, The negative thermal expansion regulator has a negative coefficient of thermal expansion in the range of -50°C to 150°C; And / or, the negative thermal expansion regulator includes any one or a combination of at least two of zirconium tungstate, zirconium vanadate, zirconium phosphate, and cyanide complexes, preferably zirconium tungstate.
3. The thermally conductive pad according to claim 1 or 2, characterized in that, The negative thermal expansion regulator has a D50 particle size of 0.5-3 μm.
4. The thermally conductive pad according to any one of claims 1-3, characterized in that, The polymer matrix includes vinyl silicone oil, a crosslinking agent, and a catalyst; And / or, the polymer matrix comprises component A and component B, wherein component A comprises vinyl silicone oil and a crosslinking agent, and component B comprises vinyl silicone oil and a catalyst; Based on the total mass of component A as 100%, the content of the vinyl silicone oil is 92%-97%, and the content of the crosslinking agent is 3%-8%. Based on the total mass of component B as 100%, the content of the vinyl silicone oil is 92%-97%, and the content of the catalyst is 3%-8%.
5. The thermally conductive pad according to claim 4, characterized in that, The crosslinking agent includes hydrogen-containing silicone oil; And / or, the catalyst includes a platinum catalyst; And / or, the mass ratio of component A to component B is (0.8-1.2):
1.
6. The thermally conductive pad according to any one of claims 1-5, characterized in that, The thermally conductive filler includes any one or a combination of at least two of aluminum nitride, aluminum oxide, and zinc oxide, preferably a combination of aluminum nitride, aluminum oxide, and zinc oxide.
7. The thermally conductive pad according to claim 6, characterized in that, Based on the total weight of the thermally conductive filler as 100%, the weight percentage of aluminum nitride is 40%-60%, the weight percentage of aluminum oxide is 20%-40%, and the weight percentage of zinc oxide is 10%-30%. And / or, the aluminum nitride comprises spherical aluminum nitride; And / or, the alumina includes spherical alumina; And / or, the thermally conductive filler includes spherical aluminum nitride, spherical aluminum oxide, and zinc oxide.
8. The thermally conductive pad according to any one of claims 1-7, characterized in that, The thermally conductive filler has a D90 particle size of 110-130 μm, a D50 particle size of 5-10 μm, and a D10 particle size of 1-5 μm.
9. A method for preparing a thermally conductive pad as described in any one of claims 1-8, characterized in that, The preparation method includes the following steps: The polymer matrix, thermally conductive filler, and negative thermal expansion regulator are mixed, and the resulting mixture is added to a mold and cured to obtain the thermally conductive pad.
10. The preparation method according to claim 9, characterized in that, The mixing process includes: first stirring at a speed of 1400-1600 rpm for 110-130 seconds, repeating 2-4 times, and then kneading for 10-20 minutes; And / or, the mixing process further includes a dispersion and degassing step, specifically including: stirring at a speed of 1500-2500 rpm for 110-130 seconds under a vacuum of -0.098 MPa, repeating 2-4 times until the mixture is uniform and free of bubbles; And / or, the curing temperature is 140-160℃, the vacuum degree during curing is -0.098MPa, and the curing time is 1-3h.