A phosphating-reinforced composite carbon mineralization anti-corrosion coating and its preparation method
By introducing a phosphating-enhanced interface layer and a calcium-magnesium composite carbon mineralization protective layer into the carbon mineralization coating, the problems of poor adhesion and insufficient density of the carbon mineralization coating in steel structure protection are solved. Carbonization priority and polymer film formation lag are achieved under high polymer doping, which improves the adhesion, density and toughness of the coating and extends the anti-corrosion performance.
Patent Information
- Application Number
- CN202611427995.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing carbon mineralization coatings suffer from poor adhesion, insufficient density, and brittleness in steel structure protection. They cannot coordinate polymer film formation and inorganic carbonization reactions at high polymer dosages, resulting in insufficient corrosion protection performance.
A composite coating system combining a phosphate-reinforced interface layer and a calcium-magnesium composite carbon mineralization protective layer is adopted. A "two-way bridging" interface layer is formed on the steel surface through a phosphoric acid + phosphate system. The reaction sequence is controlled by a water-based epoxy resin + polyamide curing agent system, which achieves preferential carbonization and delayed polymer film formation under high polymer content, resulting in a dense and tough coating.
It significantly improves the chemical bonding strength between the coating and the steel, ensures the carbonization reaction under high polymer content, enhances the coating's adhesion, density, and toughness, extends its anti-corrosion performance, and meets the requirements for long-term service of steel structures.
Smart Images

Figure CN123107424A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of anti-corrosion coating technology, specifically relating to an anti-corrosion coating and its preparation method. Background Technology
[0002] Steel faces severe corrosion problems in high-humidity, high-salt, and high-UV environments such as marine and industrial settings, making coating protection a primary means of protection. Traditional organic coatings have poor aging resistance, poor high-temperature resistance, and are prone to causing pollution. Inorganic carbon mineralization coatings (such as γ-C2S-based coatings) can fix carbon and form a stable calcium carbonate protective layer, exhibiting excellent UV aging resistance, temperature resistance, environmental friendliness, and long-term chemical stability, making them highly promising protective materials for steel structures.
[0003] However, existing carbon mineralization coating technology faces three major challenges in steel protection applications: (1) poor adhesion. Carbon mineralization coatings adhere primarily to smooth steel surfaces through physical bonding, lacking strong chemical bonds, and are prone to peeling under stress or environmental erosion. (2) inability to form a continuous film. Carbide products are difficult to completely fill the pores left by particle accumulation and moisture evaporation. Existing research shows that the impedance value of unmodified carbon mineralization coatings on steel surfaces is typically below 10. 4 Ω·cm 2 There are continuous channels for the corrosive medium to penetrate. (3) Inherent brittleness. The inorganic carbon mineral coating has a high modulus and poor deformation capacity, which does not match the thermal expansion coefficient and elongation at break of the steel. The small deformations that occur in the steel structure during service can easily lead to penetrating microcracks in the brittle coating, causing the anti-corrosion barrier to fail.
[0004] Phosphating is a mature and effective solution for addressing poor adhesion issues on metal surfaces. Traditional phosphating technology reacts phosphoric acid with the metal surface to generate an insoluble phosphate conversion film. This film has a micro-rough structure, enabling mechanical interlocking with subsequent coatings, and the phosphate layer itself possesses a certain degree of corrosion resistance. However, existing phosphating technologies are primarily geared towards organic coating systems (such as epoxy and polyurethane), with the composition and structural design of the phosphate film focused on interfacial compatibility with the organic coating. Carbon mineralization coatings are highly alkaline inorganic systems (pH>12), with calcium carbonate as the main reaction product. This calcium carbonate has poor chemical affinity with conventional phosphating films (such as zinc-based phosphates), and the phosphate film may chemically dissolve in the highly alkaline slurry environment of carbon mineralization coatings, leading to the failure of the interfacial transition layer. Therefore, conventional phosphating treatment is difficult to directly apply to carbon mineralization coating systems, necessitating the development of novel interfacial reinforcement layers that are chemically compatible with carbon mineralization coatings.
[0005] To address the issues of insufficient density and brittleness, introducing polymers into inorganic coatings is a common strategy to simultaneously improve both. The idea is to introduce an organic polymer phase into the inorganic particle skeleton, filling pores to enhance density and utilizing the deformability of the organic phase to dissipate strain energy and improve toughness. However, this strategy faces a fundamental contradiction in the modification of carbon mineralization coatings: to achieve significant toughening and densification effects, the polymer must be present in sufficient quantities to ensure the formation of a connected organic network. However, during moisture evaporation and curing, the film-forming reaction of polymer particles often occurs before the carbonization reaction, blocking pore channels, hindering CO2 diffusion, and inhibiting the dissolution and migration of calcium ions, thus severely suppressing the carbonization reaction. Existing research often uses low-dosage (<10%) acrylic emulsions to introduce carbon mineralization coatings (Chinese invention patents CN112897966B, CN116891647B), while at high dosages, the organic-inorganic two-phase reaction is difficult to balance.
[0006] In summary, existing technologies lack both a steel interface reinforcement scheme that is chemically compatible with carbon mineralization coatings and an effective means to coordinate organic film formation and inorganic carbonization reactions with high polymer content. As a result, it is difficult to improve density, adhesion and toughness simultaneously, which has become a technical bottleneck restricting the application of carbon mineralization coatings in the field of steel structure corrosion protection. Summary of the Invention
[0007] The existing technology mainly has the following three problems: (1) Insufficient adhesion between the coating and the steel substrate. Carbon mineralization coatings are highly alkaline inorganic systems, lacking strong chemical bonds with smooth steel surfaces. The interfacial bonding mainly relies on physical anchoring, making them prone to interfacial peeling under stress or environmental corrosion. Although existing phosphating technologies can improve the surface activity of steel, their phosphating film composition and structural design are mainly geared towards organic coating systems, resulting in poor chemical compatibility with carbon mineralization coatings. In highly alkaline slurry environments, the phosphating film is prone to dissolution and failure, making direct application difficult.
[0008] (2) There is a conflict in reaction timing between polymer modification and carbonization, which leads to a significant decrease in the degree of carbonization at high dosages. Introducing polymers into carbon mineralization coatings is a necessary means to improve density and toughness, and a high dosage (usually >10%) is required to form an effective interconnected organic network. However, in existing polymer systems, the film-forming / crosslinking reaction rate during moisture evaporation and curing is often faster than or equal to the carbonization reaction rate, resulting in premature film formation of the organic phase, blocking the pore channels between inorganic particles, hindering the gas phase diffusion and dissolution of CO2, and inhibiting the dissolution and migration of calcium ions, thus severely suppressing the carbonization reaction. This contradiction limits the polymer dosage in existing technologies to a low level (usually <10%), making it impossible to achieve effective toughening and densification modification.
[0009] (3) The density, toughness and carbonization degree of the coating are difficult to improve simultaneously. Due to the coupling of the two aspects of interface adhesion and reaction time, the lack of interface layer makes the coating easy to peel off. Polymer modification is limited by carbonization inhibition and cannot be added in high dosage. Therefore, carbon mineralized coating cannot obtain high adhesion, high density, high toughness and sufficient carbonization degree at the same time under high polymer dosage conditions. The overall anti-corrosion performance cannot meet the requirements of long-term service of steel structure.
[0010] To address the aforementioned problems, the present invention aims to provide a novel composite coating system and its preparation method that achieves both strong chemical bonding between the carbon mineralization coating and the steel interface and coordinates the reaction sequence of high-dosage polymer film formation and inorganic carbon mineralization. A "two-way bridging" interface layer is constructed on the steel surface using a phosphoric acid + phosphate system. This phosphate layer forms Fe-OP chemical bonds through the reaction of phosphoric acid with the steel. Furthermore, the residual phosphate and calcium ions on its surface can chemically react with the upper high-alkalinity carbon mineralization coating, achieving a gradual change in composition and interface enhancement from the metal substrate to the inorganic protective layer. Simultaneously, by controlling the polymer crosslinking reaction rate, the carbonization reaction occurs preferentially, while polymer film formation is delayed, thereby achieving a synergistic effect of sufficient carbonization and efficient toughening at high polymer dosage.
[0011] To achieve the above objectives, the following technical solution is adopted: A phosphate-reinforced composite carbon mineralization anti-corrosion coating includes a phosphate-reinforced interface layer and a calcium-magnesium composite carbon mineralization protective layer. The phosphate-reinforced interface layer is coated on the steel surface and is a chemical conversion film formed by reacting a mixed slurry composed of 50 parts dilute phosphoric acid, 10-25 parts phosphate, 5-30 parts silica fume, and 0-20 parts water by weight. The calcium-magnesium composite carbon mineralization protective layer is coated on the phosphate-reinforced interface layer. It is formed by carbonization curing and polymer crosslinking reaction of 100 parts calcium carbonization cementitious material, 10-50 parts magnesium carbonization cementitious material, 25-60 parts water, 0.5-3.0 parts water-reducing agent and 12-60 parts polymer modifier by mass. The polymer modifier is a water-based epoxy resin + polyamide curing agent system.
[0012] According to the above scheme, the thickness of the phosphating-enhanced interface layer is 0.05~0.5mm; the thickness of the calcium-magnesium composite carbon mineralization protective layer is 0.2~3.0mm.
[0013] According to the above scheme, the concentration of the dilute phosphoric acid is 10%~30%, preferably 15%~25%.
[0014] According to the above scheme, the phosphate is specifically one or more of calcium dihydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate, with calcium dihydrogen phosphate being preferred. Silica fume is used as a physical filler to adjust the slurry properties; the amount of water added is determined to make the slurry coatable.
[0015] According to the above scheme, the preferred calcium carbonized cementitious material is dicalcium silicate (γ-C2S), with a fineness passing through a 200-mesh sieve.
[0016] According to the above scheme, the magnesium carbonized cementitious material is a compound mixture of light-burned magnesium oxide and dark-burned magnesium oxide, with a light-burned / dark-burned mass ratio of 1:(0.3~3), preferably 1:(0.5~2).
[0017] According to the above scheme, in the waterborne epoxy resin + polyamide curing agent system, the amount of polyamide curing agent is 20%~50% of the stoichiometric ratio of epoxy groups, calculated based on active hydrogen. Under carbonization curing conditions, a low-activity polyamide curing agent is used to replace the conventional aliphatic amine curing agent, while the dosage is reduced (the conventional dosage is 80%~100% of the stoichiometric ratio of epoxy groups). The crosslinking reaction rate of the waterborne epoxy resin + polyamide curing agent system is controlled to be lower than the carbonization reaction rate, thereby achieving the effect of preferential carbonization reaction and delayed polymer crosslinking film formation until after carbonization curing is completed.
[0018] This invention also provides a method for preparing the above-mentioned phosphating-reinforced composite carbon mineralization anti-corrosion coating, comprising the following steps: S1. Mix dilute phosphoric acid, phosphate, silica fume and water in a certain proportion to prepare a phosphate-reinforced interface layer slurry. Coat the slurry onto the surface of the steel after surface cleaning and allow it to set at room temperature. S2. Mix the calcium carbonized cementitious material, magnesium carbonized cementitious material, water, and water-reducing agent in proportion, add the polymer modifier and stir again until the slurry is uniform, and coat it on the surface of the initially set phosphated reinforced interface layer to obtain a composite coating. S3. The coated composite coating is placed in a CO2 environment for carbonization curing. The carbonization reaction is preferentially carried out by adjusting the reaction conditions, and the crosslinking reaction of the polymer modifier is delayed. S4: After carbonization curing is completed, continue curing to allow the polymer modifier to fully react and form a film.
[0019] According to the above scheme, in step S3, the CO2 concentration for carbonization curing is 20%~100%, the temperature is 10~40 ℃, the relative humidity is 45%~100%, the pressure is atmospheric pressure~0.4 MPa, and the curing time is 6~72 hours.
[0020] According to the above plan, the conditions for continued curing in step S4 are normal temperature natural curing for 3 to 14 days, or accelerated curing at 40 to 60℃ for 24 to 72 hours.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Phosphating Reinforced Interface Layer: A "two-way bridging" conversion film is formed on the steel surface using a phosphoric acid + phosphate system. Dilute phosphoric acid etches the steel surface and reacts with iron to generate an iron phosphate conversion film, which forms a strong bond with the steel substrate through Fe-OP chemical bonds. The phosphate layer surface is rich in phosphate ions (PO4). 3- Calcium phosphate and calcium ions, through an acid-base neutralization-precipitation reaction at the interface with the upper calcium-magnesium composite carbon mineralization protective layer, form a calcium phosphate / magnesium phosphate transition layer, achieving a gradual change in composition and chemical bonding. This "two-way bridging" mechanism makes the phosphate layer a "chemical link" connecting the metal substrate and the inorganic carbon mineralization coating, fundamentally solving the problem of poor adhesion of traditional carbon mineralization coatings on steel surfaces due to reliance solely on physical adhesion.
[0022] (2) The reaction timing control strategy is achieved by adding a waterborne epoxy resin + polyamide curing agent system. By reducing the amount of curing agent and selecting a low-activity curing agent, the crosslinking rate of the polymer is made lower than the carbonization reaction rate, realizing the timing separation of "carbonization priority and film formation lag", breaking the technical bottleneck of high-dosage polymer inhibiting carbonization. At the same time, the addition of the waterborne epoxy resin + polyamide curing agent system allows the polymer dosing to reach 10%~40%, forming a connected organic network, and simultaneously improving density and toughness. Attached Figure Description
[0023] Figure 1 : Schematic diagram of the composite carbon mineralization anti-corrosion coating structure of the present invention.
[0024] Figure 2 Comparison of backscattered electron (BSE) images of the coating cross sections of Example 1 with those of Comparative Examples 2A, 2B, and 3. Detailed Implementation
[0025] The following embodiments further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0026] A specific embodiment provides a composite carbon mineralization anti-corrosion coating, as shown in the attached figure. Figure 1 As shown, it is prepared through the following steps: S1: Preparation of Phosphating Reinforced Interface Layer (A): Dilute phosphoric acid solution, phosphate, silica fume and water are mixed evenly in proportion to prepare phosphating reinforced interface layer slurry. The slurry is coated on the surface of steel that has undergone surface cleaning treatment and left to stand at room temperature for 10~50 minutes to allow it to dry. The coating thickness is 0.05~0.5mm.
[0027] S2: Preparation of calcium-magnesium composite carbon mineralization protective layer (B): Mix calcium carbonization cementitious material, magnesium carbonization cementitious material, water and water-reducing agent in proportion, and mechanically stir at 350~500 r / min for 3~10 minutes until uniform. Then add waterborne epoxy resin + polyamide curing agent system and stir again until the slurry is uniform. Coat the surface of the initially set phosphated reinforced interface layer with a coating thickness of 0.2~3.0 mm.
[0028] S4: Carbonization Curing + Time Control: The coated composite coating is placed in a CO2 environment for carbonization curing. Conditions include CO2 concentration of 20%–100%, temperature of 10–40 °C, relative humidity of 45%–100%, pressure of atmospheric pressure to 0.4 MPa, and curing time of 6–72 hours. During this stage, the carbonization reaction occurs preferentially, and the crosslinking reaction of the waterborne epoxy resin + polyamide curing agent system is significantly delayed.
[0029] S5: Polymer Crosslinking Film Formation: After carbonization curing, continue curing the coating to allow the waterborne epoxy resin + polyamide curing agent system to fully crosslink and form a film. Conditions are: natural curing at room temperature for 3-14 days, or accelerated curing at 40-60℃ for 24-72 hours.
[0030] In the specific implementation, the calcium-based carbonized cementing material used is dicalcium silicate (γ-C2S), with a fineness passing through a 200-mesh sieve.
[0031] In the specific implementation, the magnesium carbide cementing material used is a compound mixture of light-burned magnesium oxide and dark-burned magnesium oxide, with a light-burned / dark-burned mass ratio of 1:(0.3~3).
[0032] The specific product selection in the epoxy resin + polyamide curing agent system shall be based on the following parameters: waterborne epoxy resin emulsion: solid content 40%~60%, epoxy equivalent 500~1200g / Eq; polyamide curing agent: active hydrogen equivalent 100~300g / Eq, amine value 150~400mg KOH / g; any commercially available waterborne epoxy resin and amine curing agent products that meet the above parameter range can achieve the technical effects of this invention.
[0033] The specific product models used in the examples and comparative examples are as follows: waterborne epoxy resin emulsion: Shenzhen Borui Technology, BH-WSEP-1050; polyamide curing agent: Shenzhen Borui Technology, BH-WEC-2015B; fatty amine curing agent: Shenzhen Borui Technology, BH-WEC-101B.
[0034] The specific products used in the examples and comparative examples are for illustrative purposes only and do not constitute a limitation on the source of the products. Unless otherwise specified, all other raw materials were obtained commercially.
[0035] Example 1 (1) Preparation and coating of phosphating reinforced interface layer (A): Mix 50 parts of 20% dilute phosphoric acid, 15 parts of calcium dihydrogen phosphate, and 18 parts of silica fume, and mechanically stir for 10 minutes until the silica fume is fully dispersed and the slurry is uniform to obtain component A slurry. Apply component A slurry to the surface of the steel after grinding and rust removal to a thickness of 0.2 mm, and let it stand at room temperature for 30 minutes to dry.
[0036] (2) Preparation of calcium-magnesium composite carbon mineralization protective layer (B): 100 parts of γ-C2S, 15 parts of lightly calcined magnesium oxide, 15 parts of heavily calcined magnesium oxide, 40 parts of water, 1.3 parts of polycarboxylate superplasticizer, after mechanically stirring evenly, add 40 parts of waterborne epoxy resin (solid content 50%) and polyamide curing agent (added at 40% of the stoichiometric ratio of epoxy groups according to the active hydrogen), and stir evenly again to obtain component B slurry.
[0037] (3) Coating and curing of protective layer (B): The composite slurry of component B is coated on the surface of layer A with a thickness of 1.5 mm; it is placed in an environment with CO2 concentration of 99%, temperature of 25℃, relative humidity of 70% and pressure of 0.2 MPa for carbonization and curing for 24 hours; after removal, it is naturally cured at room temperature for 7 days.
[0038] Example 2 (1) Mix 50 parts of 25% dilute phosphoric acid, 22 parts of potassium dihydrogen phosphate, 30 parts of silica fume, and 10 parts of water. Stir mechanically for 10 minutes until the silica fume is fully dispersed and the slurry is uniform to obtain component A slurry. Apply component A slurry to the surface of the steel after grinding and rust removal to a thickness of 0.4 mm, and let it stand at room temperature for 20 minutes to dry.
[0039] (2) 100 parts of γ-C2S, 23 parts of lightly calcined magnesium oxide, 18 parts of heavily calcined magnesium oxide, 57 parts of water, 1.5 parts of polycarboxylate superplasticizer, after mechanically stirring evenly, 58 parts of waterborne epoxy resin (solid content 50%) and polyamide curing agent (added at 25% of the stoichiometric ratio of epoxy groups according to the active hydrogen) are added, and stirred evenly again to obtain component B slurry.
[0040] (3) The remaining steps are the same as in Example 1.
[0041] Example 3 Steps (1) and (2) are the same as in Example 1.
[0042] (3) Coat the surface of layer A with component B composite slurry to a thickness of 0.8 mm; place it in an environment with CO2 concentration of 99%, temperature of 25℃, relative humidity of 80%, and normal pressure (0.1MPa) for carbonization and curing for 48 hours; remove it and allow it to cure at room temperature for 7 days.
[0043] Comparative Example 1 (1) Phosphating Enhanced Interface Layer (A) Preparation and Coating: Not set.
[0044] (2) The calcium-magnesium composite carbon mineralization protective layer (B) is prepared in the same way as in Example 1.
[0045] (3) Coating and curing of protective layer (B): The composite slurry of component B is directly scraped onto the steel surface after grinding and rust removal, with a thickness of 1.0 mm; it is placed in an environment with CO2 concentration of 99%, temperature of 25℃, relative humidity of 70%, and pressure of 0.2 MPa for carbonization and curing for 24 hours; after removal, it is naturally cured at room temperature for 7 days.
[0046] Comparative Example 2A (1) Formulation and coating of phosphating reinforced interface layer (A): Same as in Example 1.
[0047] (2) Preparation of calcium-magnesium composite carbon mineralization protective layer (B): Same as in Example 1, but the amount of polyamide curing agent is added at 100% of the stoichiometric ratio of epoxy groups based on the active hydrogen.
[0048] (3) Coating and curing of the protective layer (B): Same as in Example 1.
[0049] Comparative Example 2B (1) Phosphating reinforced interface layer (A) preparation and coating: same as in Example 1.
[0050] (2) Preparation of calcium-magnesium composite carbon mineralization protective layer (B): Same as in Example 1, but aliphatic amine curing agent is used instead of polyamide curing agent (40% of the stoichiometric ratio of epoxy groups is added according to the active hydrogen).
[0051] (3) Coating and curing of the protective layer (B): Same as in Example 1.
[0052] Comparative Example 3 (1) Formulation and coating of phosphating reinforced interface layer (A): Same as in Example 1.
[0053] (2) Preparation of calcium-magnesium composite carbon mineralization protective layer (B): 100 parts of γ-C2S, 15 parts of lightly calcined magnesium oxide, 15 parts of heavily calcined magnesium oxide, 35 parts of water, 1.2 parts of polycarboxylate superplasticizer, after mechanically stirring evenly, add 40 parts of acrylic emulsion (solid content 50%), and stir evenly again to obtain component B slurry.
[0054] (3) Coating and curing of the protective layer (B): Same as in Example 1.
[0055] Comparative Example 4 (1) Phosphating Enhanced Interface Layer (A) Preparation and Coating: Not set.
[0056] (2) Preparation of calcium-magnesium composite carbon mineralization protective layer (B): 100 parts of γ-C2S, 15 parts of lightly calcined magnesium oxide, 15 parts of heavily calcined magnesium oxide, 35 parts of water, 1.2 parts of polycarboxylate superplasticizer, after mechanically stirring evenly, 9 parts of acrylic emulsion (solid content 50%) are added, and stirred evenly again to obtain component B slurry.
[0057] (3) Coating and curing of protective layer (B): The composite slurry of component B is directly scraped onto the steel surface after grinding and rust removal, with a thickness of 1.0 mm; it is placed in an environment with CO2 concentration of 99%, temperature of 25℃, relative humidity of 70%, and pressure of 0.2 MPa for carbonization and curing for 24 hours; after removal, it is naturally cured at room temperature for 7 days.
[0058] The coatings obtained in Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests, and the results are shown in Table 1. The test methods and standards are as follows: The degree of carbonization (DOC) is determined by calcination and calculated according to formula (1): Equation (1) Where, Δ m Loss on ignition (g) at 300-1000℃. m 1 and m 2 represents the mass (g) of γ-C2S and magnesium cementitious material (MgO) before carbonization. Pull-out bond strength test was performed according to GB / T 5210-2006; water absorption test according to HG / T 3344-2012; flexural strength test according to GB / T 6742-2007; impact resistance test according to GB / T 20624.2-2006; salt spray test according to GB / T1771-2007.
[0059] Table 1
[0060] BSE microscopy was performed on Examples 1 and Comparative Examples 2-3 to observe the carbonization products, the microstructure of the coating cross-section, and the porosity distribution. The results are shown in the appendix. Figure 2 As shown, the strategy of delayed polymer film formation increases the carbonization products in the composite coating and reduces the remaining unreacted γ-C2S, indicating that it is beneficial to improve the degree of carbonization; at the same time, the longitudinal porosity of the coating is significantly reduced, and the structural distribution is more uniform.
[0061] As shown in Table 1, the pull-out bond strength of Example 1 was 4.1 MPa, while that of Comparative Example 1 (without phosphate layer) was only 0.9 MPa under the same B group ratio, representing an approximately 4.5-fold increase in adhesion. The pull-out bond strength of Comparative Example 4 (without phosphate layer + low-dosage acrylic acid) was only 0.6 MPa, reflecting the lack of effective chemical bonding between the inorganic coating and the steel substrate without phosphate layer; the interfacial bonding mainly relied on physical anchoring, resulting in severely insufficient adhesion. Meanwhile, Comparative Example 3, using acrylic emulsion instead of the epoxy system, although having a phosphate layer, also only achieved a pull-out strength of 3.3 MPa, lower than the levels of the examples, indicating that the synergistic effect between the phosphate layer and the epoxy system was optimal. This invention utilizes the "bidirectional bridging" mechanism of the phosphate-reinforced interfacial layer (A) to form Fe-OP chemical bonds downwards with the steel and a calcium phosphate / magnesium phosphate homologous transition layer upwards with the carbon mineralization protective layer, significantly improving the pull-out bond strength between the coating and the steel.
[0062] As shown in Table 1, the degree of carbonization (DOC) of Examples 1-3 reached 56%, 49%, and 50%, respectively, indicating that the carbonization reaction still proceeded sufficiently under high polymer dosing conditions. Comparative Examples 2A and 2B employed a single control strategy using 100% low-activity curing agent and 40% high-activity aliphatic amine curing agent, respectively. The degree of carbonization still significantly decreased to below 30%. In particular, the aliphatic amine curing agent caused a rapid crosslinking reaction of the epoxy resin, resulting in a higher degree of inhibition of the carbonization reaction. Therefore, simply reducing the amount of curing agent reduced the crosslinking component while film formation still preferentially involved the carbonization reaction, resulting in a more porous coating structure in Comparative Example 2B. This comparison directly demonstrates the synergistic control effect of the "low-activity + low-dosage" curing agent. This invention, by using an aqueous epoxy resin + polyamide curing agent system and reducing the amount of polyamide curing agent (40% and 25% of the stoichiometry), actively controls the crosslinking reaction rate of the polymer to be lower than the carbonization reaction rate, achieving a temporal separation of "carbonization priority, film formation lag."
[0063] As shown in Table 1, the water absorption rates of Examples 1-3 were 1.2%, 1.4%, and 0.9%, respectively, all significantly lower than those of Comparative Examples 2A (5.9%), 2B (7.0%), 3 (7.1%), and 4 (11.2%). In the salt spray test, Examples 1-3 all exhibited excellent anti-corrosion performance with no blistering or rust for over 1440 hours. In contrast, Comparative Examples 2A and 2B, controlled by a single strategy, showed rust spots after 720 hours and 576 hours, respectively. Comparative Example 3, using an acrylic emulsion substitute, failed after only 648 hours, and Comparative Example 4, with no phosphate layer and low acrylic acid content, showed rust spots after only 504 hours. The salt spray life of the embodiments of this invention is nearly three times longer than that of Comparative Example 4 (previous technology) and more than twice as long as that of Comparative Example 2 (controlled by a single strategy), fully demonstrating the significant improvement in anti-corrosion performance resulting from the synergistic effect of phosphate enhancement and reaction sequence control. This invention employs a dual densification mechanism: "carbonation reaction preferentially forms a dense inorganic calcium carbonate skeleton + polymer delayed cross-linking forms a film to fill pores," resulting in a coating with extremely low water absorption and excellent resistance to corrosive media penetration.
[0064] Bending tests (referencing GB / T 6742-2007) showed that the minimum diameter of the shaft through which Examples 1-3 passed was 12 mm, while Comparative Examples 2A and 2B, controlled by a single strategy, had diameters of 16 and 25 mm, respectively. Comparative Example 3, which used an acrylic emulsion as a substitute, had a diameter of 25 mm. Comparative Example 4, with no phosphate layer and low acrylic acid content, exhibited extremely brittle coating, resulting in through-cracks under a maximum shaft diameter of 32 mm, making it impossible to determine the minimum diameter through. Although Comparative Example 1 had the same B-group ratio as Example 1, the lack of a phosphate layer resulted in extremely low adhesion, causing the coating to peel off completely from the substrate interface during bending (peeling off under a 32 mm shaft). This fundamentally differed from the microcrack failure mode of Example 1, further demonstrating the fundamental role of the phosphate layer in the cooperative deformation capability of the coating and substrate. Impact resistance tests (referencing GB / T 20624.2-2006) also verified the toughening effect of the present invention: the impact resistance of Examples 1-3 were 58 kg·cm, 50 kg·cm, and 52 kg·cm, respectively, significantly higher than that of Comparative Example 3 (35 kg·cm) and Comparative Example 4 (10 kg·cm). These results indicate that the synergistic effect of the phosphating-reinforced interface layer and reaction timing regulation—the phosphating layer providing strong interfacial chemical bonds enabling the coating to deform in tandem with the substrate, and the timing regulation ensuring sufficient carbonization and a dense inorganic framework—is indispensable. Together, they endow the carbon mineralized coating with significantly improved flexibility and crack resistance, effectively overcoming the inherent brittleness of traditional inorganic carbon mineralized coatings.
[0065] This invention uses a calcareous carbonized cementitious material as the main component (100 parts γ-C2S) to ensure the stability and degree of carbonization of the main carbonization reaction framework. The magnesium component (a mixture of lightly calcined magnesia and heavily calcined magnesia, totaling 30-41 parts) reacts with phosphate ions in the phosphate layer to form a magnesium phosphate transition layer, strengthening the interfacial chemical continuity. Furthermore, the volume expansion effect of the magnesium component during carbonization effectively fills capillary pores. Combined with a polycarboxylate superplasticizer, the water-cement ratio is controlled within a reasonable range. The synergistic effect of these three components significantly reduces the coating porosity, lowering the water absorption rate to below 1.2%.
[0066] The carbonization curing process of this invention can be flexibly adjusted within the range of atmospheric pressure to 0.4 MPa. In Example 3, after 48 hours of carbonization curing at atmospheric pressure (0.1 MPa), the carbonization degree still reached 50%, and the salt spray test exceeded 1440 hours, showing performance essentially equivalent to pressurized carbonization (Example 1). This fully demonstrates that the core technical solution of this invention does not rely on pressurized equipment, possessing good process tolerance and promising prospects for industrial application. Carbonization curing can be carried out in an industrial waste gas atmosphere (CO2 concentration 20%~100%), taking into account both CO2 resource utilization and coating preparation, resulting in significant environmental benefits.
Claims
1. A phosphate-reinforced composite carbon mineralization anti-corrosion coating, characterized in that... This includes a phosphate-reinforced interface layer and a calcium-magnesium composite carbon mineralization protective layer; The phosphate-reinforced interface layer is coated on the steel surface and is a chemical conversion film formed by reacting a mixed slurry composed of 50 parts dilute phosphoric acid, 10-25 parts phosphate, 5-30 parts silica fume, and 0-20 parts water by weight. The calcium-magnesium composite carbon mineralization protective layer is coated on the phosphate-reinforced interface layer. It is formed by carbonization curing and polymer crosslinking reaction of 100 parts calcium carbonization cementitious material, 10-50 parts magnesium carbonization cementitious material, 25-60 parts water, 0.5-3.0 parts water-reducing agent and 12-60 parts polymer modifier by mass. The polymer modifier is a water-based epoxy resin + polyamide curing agent system.
2. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... The thickness of the phosphating-reinforced interface layer is 0.05~0.5mm; the thickness of the calcium-magnesium composite carbon mineralization protective layer is 0.2~3.0mm.
3. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... The concentration of the dilute phosphoric acid is 10% to 30%.
4. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... The phosphate is specifically one or more of calcium dihydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate.
5. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... The calcium-carbonized cementitious material is dicalcium γ-silicate with a fineness passing through a 200-mesh sieve.
6. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... The magnesium-based carbonized cementitious material is a compound mixture of light-burned magnesium oxide and dark-burned magnesium oxide, with a light-burned / dark-burned mass ratio of 1:(0.3~3).
7. The phosphate-reinforced composite carbon mineralization anti-corrosion coating as described in claim 1, characterized in that... In the waterborne epoxy resin + polyamide curing agent system, the amount of polyamide curing agent is calculated based on the active hydrogen and is 20% to 50% of the stoichiometric ratio of epoxy groups.
8. The method for preparing the composite carbon mineralization anti-corrosion coating according to claim 1, characterized in that... Includes the following steps: S1. Mix dilute phosphoric acid, phosphate, silica fume and water in a certain proportion to prepare a phosphate-reinforced interface layer slurry. Coat the slurry onto the surface of the steel after surface cleaning and allow it to set at room temperature. S2. Mix the calcium carbonized cementitious material, magnesium carbonized cementitious material, water, and water-reducing agent in proportion, add the polymer modifier and stir again until the slurry is uniform, and coat it on the surface of the initially set phosphated reinforced interface layer to obtain a composite coating. S3. The coated composite coating is placed in a CO2 environment for carbonization curing. The carbonization reaction is preferentially carried out by adjusting the reaction conditions, and the crosslinking reaction of the polymer modifier is delayed. S4: After carbonization curing is completed, continue curing to allow the polymer modifier to fully react and form a film.
9. The method for preparing the composite carbon mineralization anti-corrosion coating as described in claim 8, characterized in that... In step S3, the CO2 concentration for carbonization curing is 20%~100%, the temperature is 10~40 ℃, the relative humidity is 45%~100%, the pressure is atmospheric pressure~0.4 MPa, and the curing time is 6~72 hours.
10. The method for preparing the composite carbon mineralization anti-corrosion coating as described in claim 8, characterized in that... In step S4, the continued curing conditions are normal temperature natural curing for 3 to 14 days, or accelerated curing at 40 to 60℃ for 24 to 72 hours.