A PMS-modified silica sol inorganic waterproof coating, its preparation method and application

By combining PMS and dual-terminated monohydroxy organosilicon, an organic-inorganic hybrid Si-O-Si crosslinking network was constructed, which solved the problems of high brittleness, easy cracking, and insufficient interfacial adhesion of PMS-modified silica sol inorganic coatings, and achieved simultaneous improvement in high hardness, flexibility and water resistance.

CN123107425APending Publication Date: 2026-11-17NINGDE NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611522617.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PMS-modified silica sol inorganic coatings, while maintaining high hardness and dense inorganic cross-linking network, suffer from problems such as high coating brittleness, easy cracking, easy migration and precipitation of flexible components, and poor dispersion of pigments and fillers. In particular, they have insufficient interfacial adhesion performance on porous, weakly alkaline cementitious substrates.

Method used

Using PMS and dual-terminated monohydroxy organosilicon as composite modifiers, flexible siloxane segments are chemically bonded into a rigid inorganic siloxane framework through a dehydration condensation reaction to construct an organic-inorganic hybrid Si-O-Si crosslinked network. During the film formation process, a low surface energy hydrophobic layer is constructed to improve the interfacial adhesion performance.

Benefits of technology

This achievement simultaneously enhances the coating's high hardness and flexibility. The flexible segments remain stable within the cross-linked network over a long period, strengthening the interfacial adhesion between the coating and the substrate, and improving the coating's water resistance and storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107425A_ABST
    Figure CN123107425A_ABST
Patent Text Reader

Abstract

This invention provides a PMS-modified silica sol inorganic waterproof coating, its preparation method, and its application. Using alkaline silica sol with a solid content of 25-30% and a pH of 9.0-10.5 as raw material, and potassium methylsilicate and α,ω-dihydroxy-terminated alkyl-modified polydimethylsiloxane as composite modifiers, a stepwise dropwise addition and ultrasonic dispersion modification process is employed. Flexible silica segments are chemically bonded to the inorganic silica skeleton through a dehydration condensation reaction, yielding a PMS-modified silica sol. This modified silica sol is then used as a film-forming substance, compounded with titanium dioxide, talc, quartz sand, quartz powder, and hydroxyethyl cellulose, and prepared through a stepwise formulation process to obtain an inorganic waterproof coating. The resulting coating exhibits no blistering, peeling, or wrinkling defects after 48 hours of water immersion, a contact angle retention rate ≥95%, adhesion grade 1, a pencil hardness of 4H-5H, and no cracks when bent with a 3 mm shaft, demonstrating both high hardness and flexible crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic waterproof coating technology, and specifically relates to a PMS-modified silica sol inorganic waterproof coating, its preparation method, and its application. Background Technology

[0002] Building leakage is a major technical challenge that has long plagued the construction industry. Waterproof coatings, as key materials for solving building leakage problems, play a decisive role in the quality and durability of waterproofing projects. Organic waterproof coatings are highly flexible but have high VOC content, which does not meet current green building and environmental protection policies. Inorganic waterproof coatings have the advantages of low VOC and high weather resistance, but generally suffer from poor water resistance and are prone to cracking.

[0003] Silica sol-based coatings use nano-sized silica sol as the main film-forming substance, and have advantages such as being green and environmentally friendly, having high mechanical strength, and strong permeability. They are representative products of the third generation of inorganic coatings. However, during the film formation process of silica sol, the silicon-oxygen bonds cross-link to form a dense film. The silicon-oxygen bonds themselves are relatively rigid, which increases the brittleness of the coating and reduces its impact resistance. In addition, traditional silica sol has poor water resistance.

[0004] Potassium methylsilicate (PMS) contains silanol groups similar to those in silica sol, and the two can form a Si-O-Si coating through dehydration condensation. Tian Zhenkun's article "Preparation of PMS-Modified Silica Sol and Its Application in Inorganic Coatings," published in *Modern Chemical Industry*, Vol. 41, No. 8, 2021, discloses the preparation of PMS-modified silica sol and its application in inorganic coatings. A 20% PMS solution was prepared and ultrasonically dispersed. This solution was then slowly added dropwise to an alkaline silica sol and ultrasonically dispersed at 50°C to obtain a modified silica sol with a PMS content of 0%–5%. Fillers were then added and dispersed to obtain an inorganic coating. The literature reports that coatings with a PMS content of 3%–5% showed no significant abnormalities after 48 hours of water immersion, and the pencil hardness was not adversely affected. However, this existing technology still has the following technical defects: (1) The modification target is singular and does not involve the flexibility and interfacial adhesion performance of the coating. The prior art only modifies silica sol with PMS, and the improvement direction is focused on the hydrophobicity and water resistance of the coating surface. It does not involve the flexibility and crack resistance of the coating under the deformation conditions of the substrate, nor does it involve the interfacial adhesion performance between the coating and the substrate (especially porous, weakly alkaline concrete substrate). For the long-standing technical problem of silica sol inorganic coatings being "hard and brittle and prone to cracking under substrate deformation or temperature stress", the prior art does not provide a solution. (2) The introduction of flexible components is limited. To improve the flexibility of inorganic coatings, the art typically uses physical blending to introduce organosilicon components (e.g., silicone-acrylic emulsion, silicone oil, methyl-terminated polydimethylsiloxane), or uses common silane coupling agents to modify the surface of silica sol. However, the organosilicon components introduced by physical blending do not have chemical bonds with the inorganic network, and are prone to migration and precipitation during service. Their hydrophobic and toughening effects decay rapidly with the service time, and affect the storage stability of the coating. When modified with common silane coupling agents, the flexible segments are only connected to the inorganic network at one end and are free at the other end, in a suspended state, making it difficult to effectively buffer and dissipate stress within the crosslinked network. Introducing organosilicon with active hydroxyl groups at both ends into the inorganic silicon-oxygen network by double-end covalent bonding, so that the flexible segments become the bridging structure embedded in the network, has not yet been found in the prior art. (3) The effects of the modifier addition method and the pigment and filler dispersion method on the system uniformity have not been recognized. When the composite modifier is added to the alkaline silica sol in one go using the post-modification method, it is difficult to achieve uniform coating of the modifier on the surface of the silica sol particles and effective cross-linking between particles. At the same time, if fillers such as quartz sand, quartz powder, and talc are directly mixed and stirred with silica sol without pre-dispersion and the amount of water added is not controlled, it is easy to cause uneven dispersion of fillers, resulting in accumulation defects and capillary pores inside the coating, and poor storage stability.

[0005] Therefore, there is an urgent need in this field for a PMS-modified silica sol inorganic waterproof coating, its preparation method and application, which can solve the problems of high brittleness and easy cracking of inorganic coatings, easy migration and precipitation of flexible components, poor dispersion of pigments and fillers and insufficient interfacial adhesion while maintaining the low VOC, high hardness and dense inorganic network of silica sol coatings. Summary of the Invention

[0006] The purpose of this invention is to provide a PMS-modified silica sol inorganic waterproof coating, its preparation method, and its application. It addresses how to achieve sufficient flexibility and impact resistance to withstand substrate deformation and temperature stress while maintaining the high hardness and dense inorganic cross-linked network of the silica sol inorganic coating, while preventing the introduced flexible components from migrating and precipitating during service, and improving the interfacial adhesion between the coating and porous, weakly alkaline cementitious substrates.

[0007] The core concept of this invention is to use PMS and dual-terminated monohydroxy organosilicon as composite modifiers, and to utilize the dehydration condensation reaction between the potassium methylsilicate hydrolysis product and the active silanol groups at both ends of the dual-terminated monohydroxy organosilicon, as well as the co-condensation reaction between the two and the silanol groups on the surface of silica sol particles and inorganic fillers, to covalently integrate flexible siloxane segments into the rigid inorganic siloxane framework formed by the self-condensation of PMS through chemical bonding, thereby constructing an organic-inorganic hybrid Si-O-Si crosslinking network with "rigid framework-flexible segments" synergistic support, and to construct a low surface energy hydrophobic layer by means of surface migration during the film formation of siloxane segments, thereby simultaneously achieving high hardness, high water resistance, strong adhesion and flexible crack resistance.

[0008] The technical solution of the present invention: In a first aspect, the present invention provides a PMS-modified silica sol inorganic waterproof coating, comprising, by weight: 28-33 parts of PMS-modified silica sol; 8-10 parts of titanium dioxide; 3-5 parts of talc; 12-15 parts of quartz sand; 18-22 parts of quartz powder; 1-3 parts of hydroxyethyl cellulose; and 20-25 parts of deionized water. The PMS-modified silica sol is prepared by dehydration condensation reaction using alkaline silica sol with a solid content of 25-30% and a pH of 9.0-10.5 as raw material and potassium methylsilicate and double-terminated monohydroxy organosilicon as composite modifiers. The effective solid content of potassium methylsilicate is 0.5-1.0% based on the total mass of the PMS-modified silica sol, and the mass ratio of potassium methylsilicate to double-terminated monohydroxy organosilicon is (1-5):1 based on the effective solid content. The dual-terminated monohydroxy organosilicon is a hydroxyl-terminated alkyl-modified polydimethylsiloxane, having the general formula shown in formula (I): HO-R¹-[Si(CH3)2-O] m -[Si(CH3)(R 5 )-O] n -R²-OH formula (I) In equation (I), R¹ and R² are both chemical bonds; R 5 It is a straight-chain alkyl group with 6 to 10 carbon atoms; m and n are number-average degrees of polymerization (statistical average), m:n = (15 to 25):1; the number-average molecular weight of the dual-terminal monohydroxy organosilicon is 500 to 2000.

[0009] Preferably, the PMS-modified silica sol is prepared by a method comprising the following steps: (1) Mix potassium methylsilicate solution with deionized water to prepare a PMS stock solution with a mass fraction of 15-25%, and disperse it by ultrasonication; (2) The double-terminated monohydroxy organosilicon was mixed with deionized water and ultrasonically emulsified to obtain an organosilicon emulsion; (3) Weigh the alkaline silica sol and place it in a reactor. Heat the temperature to 45-60°C. Add the PMS mother liquor dropwise under stirring. After the addition is complete, ultrasonically disperse for 10-30 min. Then add the organosilicon emulsion dropwise. After the addition is complete, continue ultrasonically disperse for 30-60 min at 45-60°C to allow the potassium methylsilicate hydrolysis product, the double-terminated monohydroxy organosilicon, and the silica sol particles to undergo dehydration condensation reaction on the surface and between the particles. Add deionized water and stir evenly to obtain the PMS modified silica sol.

[0010] Preferably, the particle size of the quartz sand is 150 μm to 180 μm, and the particle size of the quartz powder is smaller than that of the quartz sand.

[0011] Preferably, the coating is applied to the surface of the substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm; after being immersed in water for 48 hours according to GB / T 1733-1993, the coating has a contact angle ≥88° and a contact angle retention rate ≥95%.

[0012] Preferably, the coating is applied to the surface of the substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm; the coating is bent 180° around a 3 mm diameter shaft according to GB / T 1731-2020 without cracking, has a pencil hardness of 4H~5H as measured according to GB / T 6739-2022, and shows no cracking or peeling after being impacted from a height of 50 cm with a 1 kg hammer according to GB / T 1732-2020.

[0013] Preferably, the coating is applied to the surface of a concrete substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm; the tensile bond strength of the coating, as measured by JGJ / T 70-2009, is ≥1.2 MPa, and after immersion in water for 48 h according to GB / T 1733-1993, there is no efflorescence or peeling.

[0014] Secondly, the present invention provides a method for preparing the above-mentioned PMS-modified silica sol inorganic waterproof coating, comprising the following steps: S1: First, mix titanium dioxide, talc, quartz sand, quartz powder, hydroxyethyl cellulose and the first part of deionized water, and stir at a speed of 600~900 r / min for 10~20 min to obtain pigment and filler slurry; S2: Under stirring conditions, the PMS modified silica sol as described in any one of claims 1 to 6 is added to the pigment and filler slurry. After the addition is complete, a second portion of deionized water is added, and stirring is continued at a speed of 800 to 1200 r / min for 30 to 60 min to obtain the PMS modified silica sol inorganic waterproof coating. The total amount of the first part of deionized water and the second part of deionized water is 20 to 25 parts by weight. The PMS-modified silica sol is prepared by a method comprising the following steps: (a) Mix potassium methylsilicate solution with deionized water to prepare a PMS stock solution with a mass fraction of 15-25%, and disperse it by ultrasonication; (b) A silicone emulsion was prepared by mixing a double-terminated monohydroxyl organosilicon with deionized water and ultrasonically emulsifying it. (c) Weigh the alkaline silica sol and place it in a reactor. Heat the temperature to 45-60°C. Under stirring conditions, first add the PMS mother liquor dropwise. After the addition is complete, ultrasonically disperse for 10-30 min. Then add the organosilicon emulsion dropwise. After the addition is complete, continue ultrasonic dispersion at 45-60°C for 30-60 min. This allows the potassium methylsilicate hydrolysis product, the double-terminated monohydroxy organosilicon, and the silica sol particles to undergo a dehydration condensation reaction on the surface and between the particles. Add deionized water and stir until homogeneous to obtain the PMS-modified silica sol.

[0015] Preferably, the amount of the first portion of deionized water is 60-80% of the total amount of deionized water.

[0016] Thirdly, the present invention provides a method for constructing a waterproof coating on a substrate surface, comprising: applying the above-mentioned PMS modified silica sol inorganic waterproof coating to the substrate surface, controlling the dry film thickness to be 100~150 μm, and curing at room temperature for 5~7 days under conditions of 20~25℃ and 50~70% relative humidity.

[0017] Fourthly, the present invention provides the application of the above-mentioned PMS modified silica sol inorganic waterproof coating in waterproofing projects for building roofs, basements, kitchens and bathrooms, or the backwater side of concrete structures.

[0018] Reaction mechanism: The hybrid modification mechanism of PMS and dual-terminated monohydroxy organosilicon described in this invention is as follows (the following reaction formulas are schematic diagrams of the mechanism, which are explanations of the mechanism of non-single polymerization systems; for the sake of brevity, the dual-terminated monohydroxy organosilicon shown in formula (I) is abbreviated as HO in the following text). SiR′ SiR′ OH, in which SiR′ SiR′ (This indicates its flexible silicon-oxygen backbone). (1) PMS aqueous phase hydrolysis reaction: Potassium methylsilicate undergoes hydrolysis in aqueous solution, dissociating potassium ions to generate highly active methylsilanetriol. The system forms a weakly alkaline environment, providing catalytic conditions for subsequent condensation reactions: CH3Si(OK)3+ 3H2O → CH3Si(OH)3+ 3KOH (2) Self-condensation reaction of PMS hydrolysis products: The methylsilanetriol molecules generated by hydrolysis undergo dehydration condensation, initially constructing a rigid inorganic silicon-oxygen framework, which endows the coating film with inorganic material properties such as high hardness, aging resistance, and acid and alkali resistance. nCH3Si(OH)3→ [CH3SiO3 / 2]n + 3n / 2 H2O (3) Hybrid condensation reaction of double-terminated monohydroxy organosilicon with PMS (core modification reaction): The active silanol groups at both ends of the double-terminated monohydroxy organosilicon dehydrate and bond with the hydroxyl groups of methylsilanetriol, covalently attaching the flexible siloxane segments to the rigid inorganic framework to achieve organic-inorganic hybrid modification; since both ends of the organosilicon have active hydroxyl groups, it can continuously participate in condensation in both directions to form a three-dimensional cross-linked structure: CH3Si(OH)3+ HO SiR′ SiR′ OH → CH3Si(OH)2 O SiR′ SiR′ OH + H2O (4) Anchoring reaction of active groups with inorganic powder surface: PMS hydrolysis products and double-terminated monohydroxyl organosilicon condense with the silanol groups on the surface of inorganic powders such as silica sol, quartz sand, and quartz powder, respectively, so that the organic-inorganic hybrid system is firmly anchored to the surface of inorganic filler, improving the density and adhesion of the coating film: Surf OH + HO Si(CH3)(OH)2→ Surf O Si(CH3)(OH)2+ H2O Surf OH + HO SiR′ SiR′ OH → Surf O SiR′ SiR′ OH + H2O (where Surf) OH represents the surface-active silanol groups of inorganic powder. (5) Overall cross-linking network formation reaction: Methylsilanetriol, double-terminated monohydroxy organosilicon, and inorganic powder surface hydroxyl groups undergo a multi-component co-condensation reaction, ultimately constructing a complete organic-inorganic hybrid Si-O-Si cross-linked waterproof network: CH3Si(OH)3+ HO SiR′ SiR′ OH + Surf OH → ( H2O) organic Inorganic hybrid Si O Si cross-linked network + H2O In the aforementioned network: the rigid inorganic skeleton formed by PMS self-condensation endows the coating with high hardness (4H~5H) and water resistance; the flexible siloxane segments of the double-ended monohydroxy organosilicon are embedded in the network through chemical bonding at both ends. When subjected to stress, they buffer and dissipate energy through segment deformation, overcoming the defects of high brittleness and easy cracking of pure PMS inorganic coatings. At the same time, since both ends of the segments are anchored, there is no migration and precipitation problem of physically blended organosilicon, and the toughening effect can be maintained for a long time; during the film formation process, the siloxane segments (especially the side chain alkyl) migrate and accumulate to the coating surface, constructing a low surface energy hydrophobic layer, which further improves the contact angle of the coating and has a high retention rate after immersion in water; the chemical anchoring of the hybrid system and the surface of the inorganic filler enhances the bonding between the filler and the matrix, improves the density of the coating, and simultaneously improves the water penetration resistance and adhesion.

[0019] Compared with the prior art, the present invention has the following technical effects: (1) Achieving simultaneous improvement in hardness and flexibility overcomes the inherent contradiction of "hard and brittle" inorganic coatings. This invention constructs a rigid inorganic silicon-oxygen framework through the self-condensation of potassium methylsilicate. At the same time, through the dehydration condensation reaction between the active silanols at both ends of the double-terminated monohydroxy organosilicon and the silanols on the surface of potassium methylsilicate hydrolysis products, silica sol particles and inorganic fillers, flexible silicon-oxygen segments are connected to the rigid framework by Si-O-Si covalent bonds, forming an organic-inorganic hybrid cross-linked network with "rigid framework-flexible segments" synergistic support. Thus, the coating achieves good flexibility and impact resistance while maintaining high hardness: the pencil hardness of Examples 1-4, according to GB / T 6739-2022, are 4H, 5H, 4H, and 4H-5H respectively; no cracks were found when bent 180° around a 3 mm diameter shaft according to GB / T 1731-2020 (the smallest crack-free shaft diameters of Examples 1-4 are 2 mm, 3 mm, 2 mm, and 2 mm respectively); and no cracks or peeling were found after being impacted from a height of 50 cm with a 1 kg hammer according to GB / T 1732-2020. As a control, the unmodified Comparative Example 1 cracked when bent around a 5 mm shaft (the smallest crack-free shaft diameter was 12 mm), with a pencil hardness of only 2H, and showed cracking and peeling upon impact resistance. (2) The flexible segments are anchored at both ends within the cross-linked network, resulting in durable toughening and hydrophobic effects without migration or precipitation issues. In this invention, both ends of the double-ended monohydroxyl organosilicon participate in covalent bonding, making the flexible segments an embedded bridging structure within the network, rather than free chains in physical blends or dangling chains in monofunctional modified systems. Therefore, they do not migrate or precipitate during service. As a control, Comparative Example 5 used organosilicon with the same structure, number-average molecular weight (1000), and dosage (1.0%), but with methyl-terminated hydroxyl groups at both ends. Its initial contact angle was 92.2°, comparable to 91.4° in Example 1. However, after 48 hours of immersion in water, the contact angle of Comparative Example 5 decreased to 78.2° (retention rate 84.8%), and the coating showed local blistering and edge peeling. In contrast, the contact angle of Example 1 only decreased from 91.4° to 88.2° (retention rate 96.5%), and the coating showed no blistering, peeling, or wrinkling. Since the only difference between Comparative Example 5 and Example 1 is whether the two hydroxyl groups at both ends are reactive, this comparative result proves that the durable and stable hydrophobic and toughening effect comes from the chemical bonding and anchoring between the two hydroxyl groups and the inorganic network, rather than the physical existence of the organosilicon component itself. (3) Enhanced interfacial chemical anchoring improves the adhesion between the coating and the substrate, and is suitable for porous, weakly alkaline cement substrates. In this invention, the silica segments migrate and accumulate to the coating surface during the film formation process, constructing a low surface energy hydrophobic layer. The resulting coating has both a high initial contact angle and excellent retention ability. The initial contact angles of Examples 1-4 were 91.4°, 94.3°, 91.4°, and 91.4°, respectively. After immersion in water for 48 hours according to GB / T 1733-1993, the initial contact angles were 88.2°, 90.3°, 88.0°, and 88.3°, respectively. The contact angle retention rates were 96.5%, 95.8%, 96.3%, and 96.6%, respectively, all exceeding 95%. Furthermore, no blistering, peeling, or wrinkling defects were observed after immersion in water for 48 hours. As controls, the retention rates of Comparative Example 3 (composite modifier added all at once) were 87.8%, Comparative Example 4 (pigment and filler pre-dispersion omitted) was 85.6%, and Comparative Example 5 (methyl-terminated organosilicon) was 84.8%, all exhibiting defects such as microcracks, localized blistering, or whitening. This demonstrates that the durability of the hydrophobic effect depends on both the chemical bonding between the modifier and the inorganic network and the density of the system's dispersion. (4) The stepwise dripping and stepwise preparation processes have a synergistic effect with the hybrid modification. In Comparative Example 3, the total amount of potassium methylsilicate and double-terminated monohydroxy organosilicon was exactly the same as in Example 1. Only the two were pre-mixed and then dripped into the alkaline silica sol at one time. The resulting coating had a flexibility of 5 mm, an adhesion grade of 2, a pencil hardness of 3H, and a contact angle retention rate of 87.8% after immersion in water for 48 hours, all of which were significantly worse than those in Example 1 (2 mm, grade 1, 4H, 96.5%). In Comparative Example 4, the pre-dispersion step of pigments and fillers was omitted, and all components were mixed and stirred at one time. The resulting coating had a contact angle retention rate of 85.6%, an adhesion grade of 2, and local blistering and whitening occurred after immersion in water for 48 hours. The above comparison shows that the stepwise dripping and stepwise pre-dispersion of pigments and fillers have a substantial contribution to the uniformity of the hybrid network and the density of the coating. (5) Environmentally friendly and low VOC: Water is used as the dispersion medium and the VOC content meets the national green coating standards. It is suitable for roofs, basements, kitchens and bathrooms and the back surface of concrete structures. Attached Figure Description

[0020] Figure 1 Comparison of FTIR spectra of PMS-modified silica sol in Examples 1-2 and Comparative Example 1; Figure 2 XRD diffraction patterns of PMS-modified silica sol in Examples 1-2 and Comparative Examples 1-2; Figure 3 Figure 1 shows the test results of the water resistance of inorganic waterproof coatings in Examples 1-2 and Comparative Examples 1-2. Figure 4 Enlarged view of the water resistance test results of inorganic waterproof coatings in Example 2 and Comparative Example 1; Figure 5 Figure 1-2 shows the contact angle test results of inorganic waterproof coatings from Examples 1-2 and Comparative Examples 1-4. Figure 6 Figure 1 shows the adhesion test results of inorganic waterproof coatings in Examples 1-2 and Comparative Examples 1-4. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments and the accompanying drawings. It should be noted that the following embodiments are examples of this invention and are only used to illustrate the invention, not to limit it. Other combinations and various modifications within the scope of this invention can be made without departing from its spirit or scope. Unless otherwise specified, all chemical reagents used in this invention are commercially available analytical grade reagents.

[0022] Raw material composition:

[0023] Instruments used:

[0024] Note: The above-mentioned double-terminated monohydroxy organosilicones A / B / C all have the structure shown in formula (I), where R¹ and R² are chemical bonds, and R… 5 It is n-octyl, m:n=20:1, and prepared according to the method of Preparation Example 1.

[0025] Preparation Example 1: Preparation of α,ω-dihydroxy-terminated alkyl-modified polydimethylsiloxane In a three-necked flask equipped with a stirrer, thermometer, and reflux condenser, octamethylcyclotetrasiloxane (D4) and octylmethyldimethoxysilane were added as comonomers. The molar ratio of D4 to octyl monomer was controlled at 20:1. 0.05-0.2% of an acidic catalyst (concentrated sulfuric acid or acidic clay) was added. The mixture was heated to 60-80°C under nitrogen protection for 4-8 hours to carry out a ring-opening copolymerization reaction. After the reaction was completed, a measured amount of water was added for hydrolysis. The reaction was terminated with an α,ω-dihydroxy end-capping agent (such as water or dihydroxysiloxane oligomer). After neutralization, washing with water, and removal of low-boiling substances under reduced pressure, hydroxyl-terminated octyl-modified polydimethylsiloxane was obtained. The molecular weight was controlled by adjusting the reaction time and the amount of capping agent. The number-average molecular weight of the product was determined by gel permeation chromatography (GPC), and the hydroxyl value was determined by titration. By adjusting the process parameters, two types of organosilicon A with a number-average molecular weight of about 500 (hydroxyl value of 224 mg KOH / g), organosilicon B with a number-average molecular weight of about 1000 (hydroxyl value of 112 mg KOH / g), and organosilicon C with a number-average molecular weight of about 2000 (hydroxyl value of 56 mg KOH / g) were prepared respectively.

[0026] Example 1 Preparation of PMS-modified silica sol: (1) Measure 47.6 g of PMS solution (content 42%), add 52.4 g of deionized water to make up to 20% by mass, mix evenly and then place in an ultrasonic disperser for ultrasonic dispersion for 30 min to obtain 100 g of PMS mother liquor with a mass fraction of 20%; (2) Weigh 1.0 g of double-terminated monohydroxy organosilicon B (R 5 (The emulsion is n-octyl, Mn=1000 g / mol, hydroxyl value is 112 mgKOH / g), 4.0 g of deionized water is added, and ultrasonic emulsification is carried out for 10 min to obtain 5 g of organosilicon emulsion; (3) Weigh 75 g of alkaline silica sol and place it in a reactor. Heat the temperature to 50°C and slowly add 15 g of the above PMS mother liquor (containing 3.0 g of PMS) under magnetic stirring. After the addition is complete, ultrasonically disperse for 15 min. Then slowly add 5 g of organosilicon emulsion (containing 1.0 g of organosilicon) and continue ultrasonically disperse at 50°C for 30 min. Add deionized water to make the total mass 100 g and stir evenly to obtain PMS-modified silica sol (PMS-Si-OS-3 / 1) with an effective PMS content of 3.0% and an effective content of 1.0% of double-terminated monohydroxy organosilicon.

[0027] Preparation of PMS-modified silica sol inorganic waterproof coating: S1: Weigh out 8 g of titanium dioxide, 4 g of talc, 13 g of quartz sand, 20 g of quartz powder, and 2 g of hydroxyethyl cellulose according to the formula. Add the first part of deionized water (16.1 g), which accounts for 70% of the total deionized water, and stir at 800 r / min for 15 min to obtain the pigment and filler slurry.

[0028] S2: Weigh 30 g of the above PMS modified silica sol and slowly add it to the above pigment and filler slurry under stirring conditions. Then add the remaining 30% deionized water (6.9 g) and continue stirring at 1000 r / min for 30 min to obtain the inorganic waterproof coating.

[0029] Example 2 The difference between this embodiment and Example 1 is that in step (3), 70 g of alkaline silica sol is weighed and placed in a reactor, and 25 g of 20% PMS mother liquor (containing 5.0 g of PMS) is added dropwise. The amount of organosilicon emulsion remains unchanged (containing 1.0 g of organosilicon), thus obtaining a modified silica sol (PMS-Si-OS-5 / 1) with an effective PMS content of 5.0% and an effective content of 1.0% of double-terminated monohydroxy organosilicon. The preparation of the coating in this embodiment is the same as in Example 1.

[0030] Example 3 The difference between this embodiment and Example 1 is that in step (2), double-terminated monohydroxy organosilicon A (number average molecular weight of 500) is used instead of double-terminated monohydroxy organosilicon B. All other operations and raw material amounts are the same as in Example 1, resulting in a hybrid modified silica sol with an effective PMS content of 3.0% and an effective double-terminated monohydroxy organosilicon content of 1.0%. The coating preparation in this embodiment is the same as in Example 1, and the performance of the resulting coating is basically equivalent to that of Example 1.

[0031] Example 4 The difference between this embodiment and Example 1 is that in step (2), double-terminated monohydroxy organosilicon C (number average molecular weight of about 2000) is used instead of double-terminated monohydroxy organosilicon B, and in step (3), the ultrasonic dispersion time after adding the organosilicon emulsion is extended to 45 min. The remaining operations and raw material amounts are the same as in Example 1, and a hybrid modified silica sol with an effective PMS content of 3.0% and an effective double-terminated monohydroxy organosilicon content of 1.0% is obtained. The coating preparation of this embodiment is the same as that of Example 1. The obtained coating showed no abnormalities after immersion in water for 48 h, and the contact angle, adhesion, and pencil hardness were basically the same as those of Example 1.

[0032] Comparative Example 1 The difference between this comparative example and Example 1 is that no PMS mother liquor or silicone emulsion was added. Instead, 75 g of alkaline silica sol was diluted to 100 g with deionized water and ultrasonically dispersed at 50°C for 30 min to obtain unmodified silica sol. The coating preparation of this comparative example was the same as that of Example 1.

[0033] Comparative Example 2 The difference between this comparative example and Example 1 is that in step (3), 5 g of 20% PMS mother liquor (containing 1.0 g of PMS) is added dropwise, while the rest is the same as in Example 1, to obtain a hybrid modified silica sol with an effective PMS content of 1.0% and an effective content of 1.0% of double-terminated monohydroxy organosilicon. The preparation of the coating in this comparative example is the same as in Example 1.

[0034] Comparative Example 3 The difference between this comparative example and Example 1 is that the stepwise dropwise addition process is omitted. 15 g of PMS mother liquor and 5 g of silicone emulsion are pre-mixed and slowly added dropwise to 75 g of alkaline silica sol at 50°C. After the addition is complete, the mixture is ultrasonically dispersed for 60 min, and deionized water is added to bring the total mass to 100 g, resulting in a hybrid modified silica sol with an effective PMS content of 3.0% and an effective content of 1.0% of dual-terminated monohydroxyl silicone. The coating preparation in this comparative example is the same as in Example 1.

[0035] Comparative Example 4 The preparation of the hybrid modified silica sol in this comparative example is the same as in Example 1. The difference between this comparative example and Example 1 is that the pigment and filler pre-dispersion step is omitted. 30 g of hybrid modified silica sol, 8 g of titanium dioxide, 4 g of talc, 13 g of quartz sand, 20 g of quartz powder, 2 g of hydroxyethyl cellulose, and all 23 g of deionized water are added to a container at once and stirred at 1000 r / min for 45 min to obtain the coating.

[0036] Comparative Example 5 The difference between this comparative example and Example 1 is that: methyl-terminated alkyl-modified polydimethylsiloxane (number average molecular weight 1000, structure is the same as that of bi-terminated monohydroxy organosilicon B but the hydroxyl groups at both ends are capped by methyl, and it has no reactivity) is used instead of bi-terminated monohydroxy organosilicon B. All other operations and raw material amounts are the same as in Example 1.

[0037] The PMS-modified silica sol inorganic waterproof coatings prepared in Examples 1-4 and Comparative Examples 1-5 were subjected to the following performance tests: 1. FTIR Testing: The silica sol sample was uniformly coated onto the surface of a polyvinyl chloride (PVC) sheet and allowed to stand at room temperature until all moisture evaporated. The coating was then scraped off, dried in a 60°C oven, and ground. Approximately 1% (by mass) of the sample powder was thoroughly mixed with KBr and pressed into a transparent sheet. Fourier transform infrared spectroscopy was used in the wavenumber range of 400 cm⁻¹. - ¹~4000 cm - ¹Internal scan.

[0038] 2. XRD Test: The silica sol sample was uniformly coated onto a PVC board and allowed to stand at room temperature until the moisture evaporated naturally. The coating was then scraped off and dried in a 60℃ oven for 3 hours, and ground into a fine powder. XRD analysis was performed using an X-ray diffractometer.

[0039] 3. Water resistance test: According to the national standard GB / T 1733-1993, the coated tinplate sheet was placed in deionized water, submerging two-thirds of the sample area, at a temperature of 23℃±2℃, for 48 hours. After removal, the paint film was observed to see if discoloration, blistering, peeling, or wrinkling occurred.

[0040] 4. Contact angle test: The contact angle was measured using a contact angle measuring instrument with a drop volume of 2 μL, and the contact angle value was calculated.

[0041] 5. Adhesion test: Refer to the national standard GB / T 9286-2021, use a cross-cutting knife to make 6 cutting lines in the horizontal and 6 in the vertical directions, with a line spacing of 3 mm. Use transparent tape to tightly adhere to the cross-cutting area, and rate it from 0 to 5.

[0042] 6. Pencil hardness test: According to national standard GB / T 6739-2022, the hardness is 0.5~1 mm·s. - ¹ Push the test cart at a speed of about 8 mm until the pencil edge leaves a scratch of more than 3 mm on the paint surface, and record the previous level of pencil hardness.

[0043] 7. Flexibility test: Referring to the national standard GB / T 1731-2020, the cured coated samples were bent 180° around shafts with diameters of 2 mm, 5 mm, and 10 mm, respectively. The paint film was observed with a magnifying glass to see if cracks were produced. The flexibility was evaluated by the smallest shaft diameter that did not produce cracks.

[0044] 8. Impact resistance test: According to the national standard GB / T 1732-2020, place the coated sample with the coating film facing up on the base of the impact tester, and drop a 1 kg weight from a height of 50 cm to impact it. Observe whether the paint film cracks or peels off.

[0045] The coating prepared above was applied to the surface of a clean tinplate sheet using a wolf hair brush. The dry film thickness of the coating was controlled to be about 120 μm. After curing at room temperature for 7 days at 23℃ and 60% relative humidity, the coating was tested.

[0046] Experimental Results and Data Analysis: 1. FTIR test results Depend on Figure 1 Analysis revealed that in Comparative Example 1 (unmodified), 2981 cm - The weak absorption peak at ¹ is attributed to the stretching vibration of saturated alkyl CH groups in trace additives in the raw material alkaline silica sol; 1116 cm⁻¹ - The peak at ¹ is the characteristic peak of the Si-O-Si antisymmetric stretching vibration, 805 cm⁻¹. - The peak at position ¹ represents the characteristic peak of the Si-O-Si symmetric stretching vibration, which is a typical skeletal vibrational peak position of alkaline silica sol. In Example 1 (PMS 3% + organosilicon 1%) and Example 2 (PMS 5% + organosilicon 1%), a new peak at 2960 cm⁻¹ appears. - ¹、2900 cm - ¹ The saturated CH stretching vibration peak at position ¹ (corresponding to Si-CH3 and the octyl side chain) and 1270 cm⁻¹ - The characteristic peak of the Si-CH3 symmetric deformation vibration at position ¹ proves that the segments of the double-terminated monohydroxy organosilicon and the alkyl side groups are retained and enriched in the coating after film formation, with the original peak at 2981 cm⁻¹. - The weak absorption at point ¹ is covered by the newly added characteristic absorption mentioned above; at the same time, the Si-O-Si antisymmetric stretching vibration peak in Example 1 shifts to 1108 cm⁻¹. - ¹, In Example 2, the displacement was 1079 cm. - ¹The peak shape is significantly broadened and flattened, and the symmetrical stretching vibration peak shifts to 798 cm⁻¹. -¹ indicates that the reaction between PMS and dihydroxyl-terminated organosilicon and alkaline silica sol becomes more complete with increasing modifier dosage, resulting in a more uniform distribution of Si-O-Si bonds and the formation of a dense amorphous cross-linked network. The appearance, shift, and peak shape changes of the above peaks form a complete chain of evidence, confirming that the hybrid cross-linking effect between PMS, dihydroxyl-terminated organosilicon, and alkaline silica sol gradually strengthens with increasing addition amount.

[0047] 2. XRD test results Depend on Figure 2 Analysis revealed that the XRD patterns of the hybrid modified silica sol samples with different modifier contents showed consistent peak shapes and positions, with no new characteristic peaks of the crystal phase appearing. However, the diffraction peak intensity of Example 2 (PMS 5%) was lower than that of Comparative Example 1 (unmodified), and the peak shape was also slightly broadened. This indicates that the addition of the modifier did not cause a change in the crystal phase of the silica sol, but only affected its amorphous microstructure. This suggests that the modification of the silica sol surface by PMS and the dual-terminated monohydroxyl organosilicon is mainly a physical or chemical bonding effect, without inducing a crystal transformation of the silica sol, while possibly having some influence on the aggregation state of the silica sol particles.

[0048] 3. Water resistance test results Figures 3-4 The results show the condition of samples with different coatings after a 48-hour immersion water resistance test. Figure 3 In the figures a, b, c, and d, the coatings of Comparative Example 1 (unmodified), Comparative Example 2 (PMS 1%), Example 1 (PMS 3% + organosilicon 1%), and Example 2 (PMS 5% + organosilicon 1%) are respectively. Figure 4 This is a partial enlarged view of the corresponding samples of Comparative Example 1 and Example 2. It can be seen that the coating surfaces of Comparative Example 1 and Comparative Example 2 have defects such as peeling and rust, which are particularly obvious in the sample of Comparative Example 1, where the integrity of the coating is destroyed. The coatings of Example 1 and Example 2 show good water resistance. From the enlarged view of the sample of Example 2, it can be observed that the edges are slightly yellowed, and the paint film has only minor defects, without obvious peeling or rust.

[0049] Due to the high water absorption rate of the unmodified coating and the low PMS dosage, water molecules can easily penetrate the coating, leading to a decrease in the adhesion between the coating and the tinplate substrate, resulting in peeling. Simultaneously, moisture causes substrate corrosion. In contrast, the coatings in Examples 1 and 2 have lower water absorption rates, and the migration of bi-terminated monohydroxyl organosilicon segments to the coating surface forms a low-surface-energy hydrophobic layer, effectively blocking water molecule intrusion and reducing the damage to coating adhesion and corrosion of the substrate. This indicates that the water resistance of the hybrid Si-O-Si network coating is significantly enhanced after the introduction of PMS and bi-terminated monohydroxyl organosilicon composite modification, resulting in a more prominent protective effect on the substrate.

[0050] After immersion in water for 48 hours, neither Example 1 nor Example 2 showed any defects such as blistering, peeling, or wrinkling. The contact angles remained stable at 88.2° and 90.3°, respectively, with a retention rate greater than 95%. Comparative Example 1 cracked, shed powder, and turned yellow after immersion in water, while Comparative Example 2 showed slight yellowing. This indicates that when the effective content of PMS is between 3% and 5% and the effective content of double-terminated monohydroxyl silicone is 1%, the water resistance of the coating is significantly optimized.

[0051] 4. Contact angle, adhesion, and hardness test results Depend on Figure 5 , Figure 6 As shown in Table 1, the initial contact angles of Examples 1 and 2 reached 91.4° and 94.3°, respectively, which were higher than those of Comparative Example 1 (77.8°) and Comparative Example 2 (89.3°). After soaking in water for 48 hours, they still maintained 88.2° and 90.3°, respectively, with a retention rate of over 95%, significantly better than Comparative Example 3 (87.8%) and Comparative Example 4 (85.6%). Regarding adhesion, Examples 1 and 2 both reached Grade 1 without any abnormalities; Comparative Example 1 was Grade 2 and showed peeling and powdering; Comparative Example 2, although reaching Grade 1, had cracking and powdering defects; Comparative Example 3 and Comparative Example 4 were both Grade 2. Regarding pencil hardness, Examples 1 and 2 reached 4H and 5H, respectively, without scratch defects; Comparative Example 1 and Comparative Example 2 were both 2H; Comparative Example 3 and Comparative Example 4 were both 3H.

[0052] Comparative Example 3 shows that even with the same total amount of PMS and organosilicon, a single addition of the composite modifier cannot achieve uniform coating of the modifier on the particle surface and efficient cross-linking between particles, indicating that the stepwise dropwise addition process makes a substantial contribution to the uniformity of the hybrid network. Comparative Example 4 shows that after removing the pre-dispersion of pigments and fillers, agglomeration defects and capillary pores form inside the coating, allowing water molecules to penetrate along the filler-matrix interface, resulting in a significant deterioration in water resistance and adhesion, indicating a synergistic effect between the stepwise formulation process and the hybrid modifier.

[0053] It is worth noting that Comparative Example 5 (methyl-terminated organosilicon) achieved an initial contact angle of 92.2°, comparable to or even slightly higher than the examples. This is because methyl-terminated organosilicon also possesses low surface energy alkyl and siloxane segments, providing surface hydrophobicity from the initial state. However, due to the absence of active hydroxyl groups at both ends, it cannot chemically bond with the inorganic network and exists only as a physical blend in the coating. After soaking in water for 48 hours, the contact angle dropped to 78.2°, with a retention rate of only 84.2%, and the coating exhibited localized blistering and edge peeling, indicating that the flexible hydrophobic component had migrated and precipitated. This result demonstrates from the opposite perspective that only by anchoring organosilicon segments to the inorganic network through chemical bonding of bi-terminated hydroxyl groups can a durable and stable hydrophobic and toughening effect be obtained. This is precisely the core basis for the use of bi-terminated monohydroxyl organosilicon as a composite modifier component in this invention.

[0054] 5. Flexibility and impact resistance Comparative Example 1 (purely inorganic) cracked upon bending a shaft of 5 mm or more. Example 1 showed no cracking upon bending a 2 mm shaft 180°, Example 2 showed no cracking upon bending a 3 mm shaft 180°, and Examples 3 and 4 showed no cracking upon bending shafts of 2-5 mm. In the impact resistance test, Comparative Example 1 showed cracking and peeling, while the Examples showed no abnormalities. This set of data is used to demonstrate the flexibility and crack resistance of the coating after covalent embedding of flexible silicon-oxygen segments, which is one of the core effects of this invention.

[0055] 6. Application Testing on Concrete Substrate To further verify the protective effect of the coating of the present invention in actual building scenarios (roofs, basements, and backwater surfaces), the coating prepared in Example 1 was applied to the surface of a standard concrete mortar test block (70 mm × 70 mm × 20 mm, mix ratio of cement:sand:water = 1:2:0.5, standard curing time 28 days), with the dry film thickness controlled at approximately 120 μm. The block was cured at room temperature for 7 days at 23℃ and 60% relative humidity. Tensile bond strength tests were conducted according to JGJ / T 70-2009, and a 48-hour water immersion test was performed according to GB / T 1733-1993. The results showed that the tensile bond strength of the coating in Example 1 on the concrete substrate was 1.2 MPa, and after 48 hours of water immersion, there was no efflorescence, peeling, or flaking on the surface of the test block. The tensile bond strength of Comparative Example 1 (unmodified) was only 0.6 MPa, and after water immersion, the edges of the test block showed obvious efflorescence and localized peeling of the coating. The data shows that the coating of the present invention also has excellent waterproof and protective properties on porous, weakly alkaline cement substrates.

[0056] Table 1. Comparative test data of coating performance in Examples 1-4 and Comparative Examples 1-5

[0057] In summary, this invention, through a combination of "PMS + dual-terminated monohydroxy organosilicon composite hybrid modification + stepwise dripping process + stepwise pre-dispersion of pigments and fillers," retains the core advantage of low VOC in silica sol coatings while simultaneously improving the crosslinking density, packing compactness, water resistance, adhesion, hardness, and flexibility and crack resistance of the coating by utilizing the chemical bonding hybridization of a rigid inorganic framework and flexible siloxane segments. Significant synergistic effects exist among the various technical features, and the technical solution possesses outstanding substantive characteristics and significant progress.

[0058] The present invention can also be implemented in various other ways. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the appended claims.

Claims

1. A PMS-modified silica sol inorganic waterproofing coating, characterized by, By weight, it includes: 28-33 parts PMS modified silica sol; 8-10 parts titanium dioxide; 3-5 parts talc; 12-15 parts quartz sand; 18-22 parts quartz powder; 1-3 parts hydroxyethyl cellulose; and 20-25 parts deionized water. The PMS modified silica sol is prepared by dehydration condensation reaction using alkaline silica sol with a solid content of 25-30% and a pH of 9.0-10.5 as raw material and potassium methylsilicate and double-terminated monohydroxy organosilicon as composite modifiers. Based on the total mass of the PMS-modified silica sol, the effective solids mass fraction of the potassium methylsilicate is 3-5%, the effective solids mass fraction of the double-terminated monohydroxyl organosilicon is 0.5-1.0%, and based on the effective solids, the mass ratio of the potassium methylsilicate to the double-terminated monohydroxyl organosilicon is (1-5):

1. The dual-terminated monohydroxy organosilicon is an alkyl-modified polydimethylsiloxane with both ends capped by hydroxyl groups, having the general formula shown in formula (I): HO-R1-[Si(CH3)2-O] m -[Si(CH3)(R 5 )-O] n -R2-OH formula (I); In formula (I), R1, R2are both chemical bonds; R 5 is a linear alkyl group having 6 to 10 carbon atoms; m, n are number average polymerization degrees (statistical average values), m:n=(15 to 25):1; the number average molecular weight of the double-end monohydroxy organosilicon is 500 to 2000.

2. The PMS modified silica sol inorganic waterproof coating according to claim 1, characterized in that, The PMS-modified silica sol is prepared by a method comprising the following steps: (1) Mix potassium methylsilicate solution with deionized water to prepare a PMS stock solution with a mass fraction of 15-25%, and disperse it by ultrasonication; (2) The double-terminated monohydroxy organosilicon was mixed with deionized water and ultrasonically emulsified to obtain an organosilicon emulsion; (3) Weigh the alkaline silica sol and place it in a reactor. Heat the temperature to 45-60°C. Add the PMS mother liquor dropwise under stirring. After the addition is complete, ultrasonically disperse for 10-30 min. Then add the organosilicon emulsion dropwise. After the addition is complete, continue ultrasonically disperse for 30-60 min at 45-60°C to allow the potassium methylsilicate hydrolysis product, the double-terminated monohydroxy organosilicon, and the silica sol particles to undergo dehydration condensation reaction on the surface and between the particles. Add deionized water and stir evenly to obtain the PMS modified silica sol.

3. The PMS modified silica sol inorganic waterproof coating according to claim 1, characterized in that, The particle size of the quartz sand is 150 μm to 180 μm, and the particle size of the quartz powder is smaller than that of the quartz sand.

4. The PMS modified silica sol inorganic waterproof coating according to claim 1, characterized in that, The coating is applied to the surface of the substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm. After being immersed in water for 48 hours according to GB / T 1733-1993, the coating has a contact angle ≥88° and a contact angle retention rate ≥95%.

5. The PMS modified silica sol inorganic waterproof coating according to claim 1, characterized in that, The coating is applied to the surface of the substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm. The coating is bent 180° around a 3 mm diameter shaft according to GB / T 1731-2020 without cracking, and the pencil hardness measured according to GB / T 6739-2022 is 4H~5H. Furthermore, it is subjected to an impact of a 1 kg hammer from a height of 50 cm according to GB / T 1732-2020 without cracking or peeling.

6. The PMS modified silica sol inorganic waterproof coating according to claim 1, characterized in that, The coating is applied to the surface of a concrete substrate and cured for 7 days at a temperature of 23°C and a relative humidity of 60% to form a coating with a dry film thickness of 120 μm. The tensile bond strength of the coating, as measured by JGJ / T 70-2009, is ≥1.2 MPa, and after immersion in water for 48 hours according to GB / T 1733-1993, there is no efflorescence or peeling.

7. The method of preparing the PMS-modified silica sol inorganic waterproof coating according to any one of claims 1-6, characterized in that, Includes the following steps: S1: First, mix titanium dioxide, talc, quartz sand, quartz powder, hydroxyethyl cellulose and the first part of deionized water, and stir at a speed of 600~900 r / min for 10~20 min to obtain pigment and filler slurry; S2: Under stirring conditions, the PMS modified silica sol as described in any one of claims 1 to 6 is added to the pigment and filler slurry. After the addition is complete, a second portion of deionized water is added, and stirring is continued at a speed of 800 to 1200 r / min for 30 to 60 min to obtain the PMS modified silica sol inorganic waterproof coating. The total amount of the first part of deionized water and the second part of deionized water is 20 to 25 parts by weight. The PMS-modified silica sol is prepared by a method comprising the following steps: (a) Mix potassium methylsilicate solution with deionized water to prepare a PMS stock solution with a mass fraction of 15-25%, and disperse it by ultrasonication; (b) A silicone emulsion was prepared by mixing a double-terminated monohydroxyl organosilicon with deionized water and ultrasonically emulsifying it. (c) Weigh the alkaline silica sol and place it in a reactor. Heat the temperature to 45-60°C. Under stirring conditions, first add the PMS mother liquor dropwise. After the addition is complete, ultrasonically disperse for 10-30 min. Then add the organosilicon emulsion dropwise. After the addition is complete, continue ultrasonic dispersion at 45-60°C for 30-60 min. This allows the potassium methylsilicate hydrolysis product, the double-terminated monohydroxy organosilicon, and the silica sol particles to undergo a dehydration condensation reaction on the surface and between the particles. Add deionized water and stir until homogeneous to obtain the PMS-modified silica sol.

8. The preparation method of the PMS-modified silica sol inorganic waterproof coating according to claim 7, characterized in that, The amount of deionized water used in the first part is 60-80% of the total amount of deionized water.

9. A method for applying a water repellent coating to a substrate surface, characterized by, include: Apply the PMS modified silica sol inorganic waterproof coating according to any one of claims 1 to 6 to the surface of the substrate, control the dry film thickness to be 100 to 150 μm, and cure at room temperature for 5 to 7 days under the conditions of 20 to 25°C and 50 to 70% relative humidity.

10. The application of the PMS modified silica sol inorganic waterproof coating according to any one of claims 1 to 6 in waterproofing projects for building roofs, basements, kitchens and bathrooms, or the backwater side of concrete structures.