Articles including corrosion-inhibiting coatings and methods for producing such articles.

By forming a cross-linked inorganic-organic hybrid coating on the surface of a metal substrate, the problem of insufficient adhesion of corrosion-inhibiting coatings is solved, achieving efficient and environmentally friendly corrosion protection, suitable for metal parts in corrosive environments.

CN123107433APending Publication Date: 2026-11-17ETA SA MFG HORLOGERE SUISSE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611187442.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-27
Filing Date
2023-07-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, corrosion-inhibiting coatings have insufficient adhesion, resulting in poor corrosion protection. At the same time, the use of irritating chemicals and complex and expensive deposition methods is environmentally unfriendly.

Method used

A cross-linked inorganic-organic hybrid coating is used to form a corrosion-inhibiting coating through covalent bonding on the substrate surface. The coating is prepared at a moderate temperature using a non-toxic sol-gel method, avoiding the use of irritating chemicals and simplifying the process.

Benefits of technology

It provides excellent corrosion protection, reduces energy consumption and process complexity, while ensuring the environmental friendliness and adhesion of the coating, making it suitable for metal parts in corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107433A_ABST
    Figure CN123107433A_ABST
Patent Text Reader

Abstract

This invention relates to articles comprising a corrosion-inhibiting coating and a method for producing such articles. The invention discloses articles comprising a substrate and a corrosion-inhibiting coating present on at least a portion of the surface of the substrate, wherein the corrosion-inhibiting coating comprises at least one functional group R. 1 Crosslinked inorganic-organic hybrid coating, wherein R 1 Including one or more selected from C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 The coating comprises aryl, amide, amine, mercapto, and epoxy functional groups, substituted with at least one halogen atom, wherein the coating comprises silicon and / or titanium, and is covalently bonded to the metal element or its alloy via oxygen-silicon or oxygen-titanium bonds. The invention further discloses a method for producing such articles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention application with application number "202310916483.9" and the invention title "Article including corrosion-inhibiting coating and method for producing such article". Technical Field

[0002] This invention relates to articles comprising a substrate and a corrosion-inhibiting coating on at least a portion of the surface of the substrate. The invention further relates to methods for producing such articles, and uses of such articles. Background Technology

[0003] One of the main degradation mechanisms of materials or articles containing metals is corrosion. Corrosion can generally be defined as the reaction of a metallic material with its surrounding environment. Both the physical and chemical properties of the material affect the rate of the corrosion reaction. Therefore, it is necessary to slow down (i.e., inhibit) the corrosion reaction. Various methods for preventing corrosion are known.

[0004] For example, elements are known to be used to enrich the surface of a substrate with corrosion-resistant components during the corrosion process to dope metallic substrates.

[0005] Alternatively, corrosion inhibitors are known to be added, which strongly adsorb onto the metal-containing surface of the substrate and thus prevent reaction with oxidants, thereby preventing corrosion formation. Corrosion inhibitors protect the metal substrate by forming a passivating protective film (i.e., a passivation layer). However, commonly used corrosion inhibitors are quite expensive and are considered toxic under current legislation. It is also known to deposit protective coatings on substrate surfaces, particularly in areas requiring corrosion protection, such as areas containing metal. These coatings provide a protective barrier against corrosive environments. However, many conventional corrosion-protective coatings are now considered environmentally harmful, for example, due to the use of compounds deemed toxic under current legislation.

[0006] In recent years, coatings obtained through the sol-gel process have become increasingly interesting. Sol-gel coatings are popular due to their environmental friendliness, high performance, compatibility with existing coating application technologies, and the ease of customizing coating properties on demand.

[0007] In particular, inorganic-organic hybrid coatings obtained via the sol-gel method, such as those known under the registered trademark Ormocer, have attracted considerable interest. These coatings combine the inherent properties of inorganic materials with those of organic polymers. Inorganic-organic hybrids can achieve properties that purely inorganic or organic materials cannot provide. Typically, organic polymer materials possess good elasticity, toughness, formability, and relatively low density, while inorganic materials are generally hard, rigid, and thermally stable. For inorganic-organic hybrid coatings, their properties can be altered and optimized by modifying the inorganic and organic structural units. Due to their inorganic networks, inorganic-organic hybrid polymers can exhibit high mechanical, chemical, and thermal stability in harsh environments.

[0008] The characteristic of inorganic-organic hybrid coatings is that the inorganic and organic structural units are directly connected, i.e., connected at the molecular scale. Therefore, inorganic-organic hybrid coatings are polymers with three-dimensional inorganic and three-dimensional organic networks interconnected by covalent bonds.

[0009] The sol-gel process is a method for producing solid materials from small molecules and is considered a sustainable and non-toxic technology. This method involves converting monomers into a colloidal solution (sol), which acts as a precursor to an integrated network (or gel) of discrete particles or a network of polymers (crosslinked polymers).

[0010] "Hybrid sol-gel coatings: smart and green materials for corrosion mitigation R. Figueira, I. Fontinha, et al., Coatings 2016, 6, 12, disclose a sol-gel coating for corrosion protection of steel, aluminum, and their alloys. This hybrid coating is obtained by copolymerization of various combinations of two selected from tetraethyl orthosilicate (TEOS), 3-(methacryloyloxy)propyltrimethoxysilane (MAPTS), methyltriethoxysilane (MTES), and triisopropoxy(methyl)silane.

[0011] EP 1729892 discloses the production of inorganic-organic hybrid coatings by a sol-gel method, wherein a crosslinked inorganic-organic hybrid coating (a so-called "gel") is obtained by exposing a prepolymer (the so-called "sol") to atmospheric pressure plasma to crosslink it.

[0012] The disadvantages of the aforementioned inorganic-organic hybrid coatings include limited adhesion to the substrate, leading to delamination. Consequently, water and moisture can reach the interface between the coating and the substrate surface, causing corrosion.

[0013] The aforementioned methods, particularly CVD and PVD, suffer from the drawback of requiring operation in controlled environments to avoid contamination, such as working in a glove box filled with inert gases or under reduced pressure. Consequently, these methods are complex and expensive. Electroplating for coating deposition is disadvantageous due to its very low deposition rate and lengthy process, and its environmentally unfriendly nature caused by the use of harsh chemicals. Furthermore, waste treatment steps, particularly for recycling waste and chemicals, are required to mitigate the environmental impact of these methods, further complicating their complexity and cost. Summary of the Invention

[0014] The object of this invention is to overcome one or more of the aforementioned disadvantages. One object of this invention is to provide an article comprising a substrate, said substrate including a corrosion-inhibiting coating having excellent adhesion to said substrate. Another object of this invention is to provide an article comprising a substrate and a coating, wherein said coating provides excellent corrosion protection to said substrate, and wherein said coating is non-toxic.

[0015] Another object of the present invention is to provide a method for producing such articles, wherein the method does not require the use of irritating or toxic compounds, is carried out at moderate temperatures, and does not require long processing times. In other words, the object of the present invention is to provide a method with reduced energy consumption compared to prior art methods.

[0016] According to a first aspect of the invention, an article comprising a substrate as described in the appended claims and a corrosion-inhibiting coating is disclosed.

[0017] The substrate comprises a metallic element and / or an alloy of metallic elements. Advantageously, at least a portion of the surface of the substrate comprises the metallic element and / or its alloy. For example, the metallic element and / or its alloy may be present only on the surface of the substrate. Alternatively, the substrate may consist substantially of the metallic element and / or its alloy.

[0018] Advantageously, the metallic element is iron or copper. Advantageously, the substrate comprises iron, for example, an alloy comprising iron, such as steel. Advantageously, the steel can be any type of steel, particularly any type of steel used for watch components. For example, the iron alloy can be stainless steel or carbon steel. Alternatively or additionally, the substrate comprises copper, for example, an alloy comprising copper, such as brass.

[0019] According to the present invention, a "corrosion-inhibiting coating" refers to a coating present on a substrate that reduces and advantageously prevents corrosion from forming on the surface area of ​​the substrate including such a coating.

[0020] The corrosion-inhibiting coating contains at least one functional group R. 1 Crosslinked inorganic-organic hybrid coating. Advantageously, R 1Includes one or more selected from C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 Functional groups include aryl, amide, amine, ether, mercapto (i.e., thiol), and epoxy groups. Additionally, R... 1 It includes at least one halogen atom. Advantageously, said halogen atom is fluorine, chlorine, bromine, or iodine. When R 1 When two or more halogen atoms are included, they can be the same or different, i.e., a combination of two or more of fluorine, chlorine, bromine, and iodine. The corrosion-inhibiting coating further comprises silicon and / or titanium.

[0021] According to the implementation plan, R 1 It is C1-C 20 Alkyl groups are those having 1 to 20 carbon atoms in their chain. Advantageously, R 1 It has the formula -(CH2) x (CF2) y CF3 C1-C 20 Alkyl groups, where x is between 0 and z-1, y is zx-1, and z is the total number of carbon atoms, i.e., z is between 1 and 20. For example, when R 1 When it is a C8 alkyl group, i.e., z is 8, it can have the formula -(CH2)2(CF2)5CF3 (x is 2 and y is 5).

[0022] Alternatively, R 1 It contains an amide functional group and one or more ether functional groups. For example, R 1 It can be -(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3.

[0023] The crosslinked inorganic-organic hybrid coating is at least partially covalently bonded to a metallic element or alloy thereof of the substrate. "At least partially covalently bonded" means that the coating is bonded to the metallic element or alloy thereof by at least one, and preferably multiple, covalent bonds. Advantageously, when the corrosion-inhibiting coating comprises silicon, the covalent bonds include oxygen-silicon bonds. Advantageously, when the corrosion-inhibiting coating comprises titanium, the covalent bonds include oxygen-titanium bonds.

[0024] Advantageously, the crosslinked inorganic-organic hybrid coating further includes carbon-silicon bonds.

[0025] The corrosion-inhibiting coating is present on at least a portion of the substrate surface. In other words, the corrosion-inhibiting coating advantageously covers at least a portion of the substrate surface. Advantageously, the corrosion-inhibiting coating is present on the vulnerable portions of the substrate. Alternatively, the corrosion-inhibiting coating is present on or covers the entire surface of the substrate.

[0026] Non-limiting examples of articles of this disclosure include components used in corrosive environments, such as marine components, components of electronic devices such as printed circuit boards, components susceptible to corrosion during storage, or components prone to aesthetic changes, such as color or brightness, due to oxidation or corrosion. Specific examples of articles of this disclosure include clocks and watches, and clock components.

[0027] According to a second aspect of the invention, a method for producing an article comprising a substrate as described in the appended claims and a corrosion-inhibiting coating present on at least a portion of the surface of the substrate is disclosed.

[0028] Advantageously, the article is according to a first aspect of the invention. Advantageously, a substrate as described above is provided. Advantageously, the substrate comprises a metallic element and / or an alloy of metallic elements on at least a portion of its surface. Advantageously, the metallic element and its alloy are as described above.

[0029] The method includes providing a first compound according to formula (I): in M is silicon or titanium. R 1 It contains one or more selected from C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 A functional group consisting of aryl, amide, amine, ether, mercapto (i.e., thiol) and epoxy groups; and containing at least one halogen atom, and R 2 R 3 and R 4 H, C1-C are independent of each other. 20 Alkyl, C1-C 10 Aryl, C1-C 20 alkenyl, C1-C 20 alkylaryl or C1-C 20 Arylalkyl.

[0030] Advantageously, the halogen atom is fluorine, chlorine, bromine, or iodine. When R 1 When two or more halogen atoms are involved, they can be the same or different, i.e., a combination of two or more of fluorine, chlorine, bromine and iodine.

[0031] The method further includes providing a second compound according to formula (II): in M is silicon or titanium. R 5 It is a cross-linkable functional group, and R 6 R 7 and R 8 H, C1-C are independent of each other. 20 Alkyl, C1-C 10 Aryl, C1-C 20 alkenyl, C1-C 20 alkylaryl or C1-C 20 Arylalkyl.

[0032] According to this disclosure, a "crosslinkable functional group" refers to a functional group capable of reacting with other functional groups. During the reaction, covalent bonds are formed, thereby achieving a crosslinked polymer. A crosslinked polymer can be considered as a polymer with a three-dimensional structure.

[0033] Advantageously, R 5 It is a thermally crosslinkable group and / or a photocrosslinkable group. In other words, R 5 It can be thermally crosslinkable, photocrosslinkable, or both.

[0034] According to this disclosure, "thermally crosslinkable groups" refers to groups that are induced and / or undergo R through thermal crosslinking (also known as thermosetting). 5 Crosslinking. Thermosetting is carried out by exposing (thermally) crosslinkable groups and prepolymers containing such crosslinkable groups in this disclosure to elevated temperatures, i.e., by heating the prepolymer.

[0035] According to this disclosure, "photocrosslinkable groups" refers to groups that are induced and / or undergo R through photochemical crosslinking (also known as photochemical curing). 5 Crosslinking. Photochemical curing is carried out by exposing (photo)crosslinkable groups and prepolymers containing such crosslinkable groups in this disclosure to radiation. Advantageously, the radiation includes one or more of infrared (IR) radiation, ultraviolet (UV) radiation, or radiation with a visible light (VIS) wavelength range.

[0036] Advantageously, R 5 It is a functional group selected from epoxy, (meth)acrylate, ester, mercapto, vinyl, and (meth)acrylate urethane. In this disclosure, "(meth)acrylate" means that the functional group can be an acrylate or a methacrylate.

[0037] Advantageously, R 2 R 3 R 4 R 6 R 7 and R 8 H or Cl-C independently of each other 20Alkyl groups, preferably C1-C8 alkyl groups, more preferably C1-C6 alkyl groups, and most preferably C1-C4 alkyl groups. In particular, R 2 R 3 R 4 R 6 R 7 and R 8 They are methyl (-CH3, i.e., C1 alkyl) or ethyl (-C2H5, i.e., C2 alkyl) independently of each other.

[0038] The first compound and the second compound hydrolyze in the presence of water. During hydrolysis, R... 2 R 3 R 4 R 6 R 7 and R 8 The C1-C8 alkyl chain of any one of them is a C1-C8 alkyl chain, which is converted into hydrogen atoms to form a hydroxyl group and a C1-C8 alkyl chain. x H 2x+1 An alcohol molecule with OH radical, where x is R 2 R 3 R 4 R 6 R 7 and R 8 The number of carbon atoms in a C1-C8 alkyl chain (i.e., x is between 1 and 8).

[0039] Subsequently, the first hydrolyzed compound and the second hydrolyzed compound are condensed. After condensation, water is removed. Following condensation, a prepolymer is obtained from the first hydrolyzed compound and the second hydrolyzed compound. The prepolymer contains R as a functional group. 1 and R 5 The prepolymer can be considered a so-called "sol".

[0040] The prepolymer is applied to at least a portion of the surface of the substrate. Advantageously, the prepolymer is applied to at least a portion of the surface containing the metallic element and / or its alloy. Application can be performed by methods known in the art, such as casting or immersing the substrate in the prepolymer, spraying the prepolymer onto the substrate, bar coating, or roller-to-roll coating.

[0041] Optionally, the substrate may be cleaned before applying the prepolymer to at least a portion of the substrate (so-called pre-cleaning). Advantageously, pre-cleaning is performed on at least a portion of the surface of the substrate to which the prepolymer is applied. This pre-cleaning can be performed by methods known in the art. Non-limiting examples include grinding and polishing, chemical cleaning, ultrasonic cleaning, sandblasting, plasma treatment or corona treatment (air plasma) at atmospheric or reduced pressure.

[0042] The prepolymer applied to at least a portion of the surface of the substrate is crosslinked. Advantageously, the crosslinking of the prepolymer is achieved through crosslinkable functional groups R. 5 This is achieved through cross-linking.

[0043] When R 5 When the functional group is thermally crosslinkable, the crosslinking is advantageously induced and / or carried out by exposing the prepolymer to a temperature of up to 250°C, advantageously 25°C to 250°C, preferably 50°C to 200°C, more preferably 75°C to 185°C, for example 100°C to 175°C, or 125°C to 160°C.

[0044] When R 5 When the functional group is photocrosslinkable, it is advantageous to induce and / or carry out the crosslinking by exposing the prepolymer to radiation. Advantageously, the radiation is IR radiation or UV radiation or a combination thereof.

[0045] After crosslinking, a corrosion-inhibiting coating is obtained on a portion of the surface of the substrate to which the prepolymer has been applied. The coating is covalently bonded to a metallic element or alloy thereof of the substrate via oxygen-M bonds, wherein M is silicon or titanium.

[0046] The corrosion-inhibiting coating contains at least one functional group R. 1 Cross-linked inorganic-organic hybrid coatings (so-called "gels").

[0047] According to a third aspect of the invention, use of the article according to the first aspect or the article obtained through the second aspect as described in the appended claims is disclosed. Advantageously, the article is used in clocks and watches.

[0048] The present invention discloses the following technical solutions: Option 1. An article comprising a substrate and a corrosion-inhibiting coating present on at least a portion of the surface of the substrate, wherein the substrate comprises a metallic element and / or an alloy of metallic elements, wherein the corrosion-inhibiting coating comprises at least one functional group R. 1 Crosslinked inorganic-organic hybrid coating, wherein R 1 Includes one or more selected from C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 Functional groups including aryl, amide, amine, mercapto, and epoxy groups. Its characteristic is that R 1 Further replaced by at least one halogen atom, characterized in that the crosslinked inorganic-organic hybrid coating comprises silicon and / or titanium, and characterized in that each of the crosslinked inorganic-organic hybrid coatings is covalently bonded to a metal element or its alloy via an oxygen-silicon bond or an oxygen-titanium bond.

[0049] Option 2. The article according to Option 1, wherein the crosslinked inorganic-organic hybrid coating further comprises carbon-silicon bonds.

[0050] Option 3. The article according to any one of the preceding options, wherein the halogen atom is fluorine, chlorine, bromine, iodine or a combination of two or more thereof.

[0051] Option 4. The article according to any one of the preceding options, wherein R 1 It is -(CH2) x (CF2) y CF3, where x is between 0 and z-1, y is zx-1, and z is the number of carbon atoms between 1 and 20.

[0052] Option 5. The article according to Option 4, wherein R 1 It is -(CH2)2(CF2)5CF3.

[0053] Option 6. The article according to any one of Options 1 to 3, wherein R 1 It is -(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3.

[0054] Option 7. The article according to any one of the preceding options, wherein the metallic element is iron or copper.

[0055] Option 8. The article of claim 7, wherein the metallic element is iron, and the substrate comprises steel, preferably carbon steel.

[0056] Option 9. The article of claim 7, wherein the metallic element is copper, and the substrate comprises a copper alloy, preferably brass.

[0057] Option 10. The article according to any one of the preceding options, wherein the article is a watch component.

[0058] Option 11. A method for producing an article comprising a substrate and a corrosion-inhibiting coating present on at least a portion of the surface of said substrate, said article being an article according to any one of the preceding options, wherein the method comprises: - Provide a substrate containing metallic elements and / or alloys of metallic elements. - Provide a first compound according to formula (I) and a second compound according to formula (II). in M is silicon or titanium. R 1 It includes one or more selected from C1-C 20Alkyl, C1-C 20 cycloalkyl, C1-C 10 A functional group comprising aryl, amide, amine, mercapto, and epoxy groups; and including at least one halogen atom. R 5 It is a cross-linkable functional group. R 2 R 3 R 4 R 6 R 7 and R 8 H, C1-C are independent of each other. 20 Alkyl, C1-C 10 Aryl, C1-C 20 alkenyl, C1-C 20 alkylaryl or C1-C 20 Arylalkyl, - Hydrolyze the first compound and the second compound in the presence of water. - The first compound is condensed and hydrolyzed, and the second compound is hydrolyzed, thereby obtaining a compound containing R. 1 and R 5 As a prepolymer of functional groups, - Apply the prepolymer to at least a portion of the surface of the substrate, and - Inducing crosslinkable functional groups R by exposing the prepolymer to one or more of a temperature of up to 250°C, UV radiation, or IR radiation. 5 The crosslinking process yields an article comprising a substrate and a corrosion-inhibiting coating covering at least a portion of the surface of the substrate. The corrosion-inhibiting coating is characterized by containing at least one functional group R. 1 The cross-linked inorganic-organic hybrid coating is characterized in that the cross-linked inorganic-organic hybrid coating is covalently bonded to a metal element or its alloy via oxygen-M bonds.

[0059] Option 12. The method according to Option 11, wherein R 5 It is a functional group selected from epoxy, (meth)acrylate, ester, mercapto, vinyl and (meth)acrylate urethane.

[0060] Option 13. The method according to Option 11 or Option 12, wherein the crosslinking is carried out at a temperature of 50°C to 200°C, preferably 100°C to 175°C.

[0061] Option 14. The method according to any one of Options 11 to 13, wherein R 2 R 3 R 4 R 6 R7 and R 8 Each is independently a C1-C8 alkyl group, preferably a C1-C4 alkyl group.

[0062] Option 15. Use of the article according to any one of Options 1 to 10 in clocks and watches. Attached Figure Description

[0063] Various aspects of the invention will now be described in more detail with reference to the accompanying drawings, wherein like reference numerals denote like features, and wherein: - Figure 1 The invention is schematically represented. - Figure 2 The open-circuit potential values ​​of the substrates coated with the coatings of the present invention and the reference coatings are shown. Detailed Implementation

[0064] Figure 1 The article 1 according to the invention is shown schematically. The article comprises a substrate 2 and a corrosion-inhibiting coating 3 covering at least a portion of the surface of the substrate 2.

[0065] The substrate 2 comprises a metallic element and / or an alloy of metallic elements. Advantageously, at least a portion of the surface of the substrate 2 comprises a metallic element and / or an alloy of the metallic element. Advantageously, at least a portion (e.g., all) of the surface portion comprising the metallic element and / or its alloy is covered by a corrosion-inhibiting coating 3. By doing so, any areas of the substrate susceptible to corrosion during handling, storage, manufacturing, and operation can be effectively protected from corrosion. Advantageously, as... Figure 1 As shown, the entire surface of the substrate 2 is basically covered with a corrosion-inhibiting coating 1.

[0066] Non-limiting examples of metallic elements include iron, copper, aluminum, zinc, silver, gold, tin, manganese, and nickel. The substrate may contain two or more metallic elements and / or alloys thereof. Advantageously, the substrate includes iron and / or copper.

[0067] For example, the substrate may include iron or be primarily composed of iron. For example, when the substrate includes iron, the substrate may include steel or may be steel, such as carbon steel.

[0068] For example, the substrate may include copper or be primarily composed of copper. For example, when the substrate includes copper, the substrate may include brass or bronze, or may be brass or bronze.

[0069] In this invention, "basic composition" refers to the amount of impurities or other components present in the substrate that is advantageously less than 1 wt%, preferably less than 0.5 wt%, more preferably less than 0.1 wt%, for example, below the detection limit of analytical techniques used to determine the composition, such as X-ray photoelectron spectroscopy (XPS).

[0070] Optionally, the substrate may contain additional nonmetallic elements and / or nonmetallic compounds. Non-limiting examples of such nonmetallic elements include phosphorus, or metalloids such as silicon and arsenic. Non-limiting examples of nonmetallic compounds include polytetrafluoroethylene (PTFE), polyethylene, polypropylene, polyurethane, polyamide, polyimide, polyamide-imide, epoxy resins such as FR4, and glass.

[0071] Advantageously, the corrosion-inhibiting coating is an inorganic-organic hybrid coating. Advantageously, the corrosion-inhibiting coating is a cross-linked inorganic-organic hybrid coating. Advantageously, the corrosion-inhibiting coating is at least partially covalently bonded to the substrate surface, particularly to a metallic element, or, when the metallic element is present as an alloy, covalently bonded to a metallic element contained in the alloy. Advantageously, the corrosion-inhibiting coating is covalently bonded to the metallic element through oxygen-containing bonds (e.g., oxygen atoms in the coating covalently bonded to the metallic element).

[0072] Advantageously, the crosslinked inorganic-organic hybrid coating comprises one or more of silicon, titanium, zirconium, aluminum, iron, or boron, preferably silicon and / or titanium. Advantageously, when the crosslinked inorganic-organic hybrid coating comprises silicon and / or titanium, the coating is at least partially covalently bonded to the metal element of the substrate through silicon-oxygen-metal bonds and / or titanium-oxygen-metal bonds.

[0073] Advantageously, the inorganic-organic hybrid coating contains at least one functional group R. 1 Advantageously, R 1 Includes or consists of one or more functional groups selected from or composed of the following: C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 Aryl, amide, amine, ether, mercapto (i.e., thiol) and epoxy.

[0074] Favorably, “C1-C 20 "Alkyl" includes alkyl functional groups containing 1 to 20 carbon atoms in the chain. Advantageously, C1-C 20 Alkyl groups are C1-C 12 Alkyl groups, preferably C1-C 10 Alkyl groups, such as C1-C8 alkyl, C1-C6 alkyl, or C1-C4 alkyl.

[0075] Favorably, “C1-C 20 "Cycloalkyl" refers to cycloalkyl functional groups that contain a total of 1 to 20 carbon atoms in the chain.

[0076] Favorably, “C1-C 10 "Aryl" refers to aryl functional groups containing 1 to 10 carbon atoms in the chain. For example, R 1 It may include phenyl functional groups, or it may be C1-C 20 Alkylphenyl.

[0077] Advantageously, when R 1 When amide functional groups are included, R 1 It has the formula -(CH2) a (CF2) b C(O)NH2, where a is between 0 and c-2, b is ca-1, and c is the total number of carbon atoms. Advantageously, c is between 2 and 20, preferably 2 to 10, such as 2 to 8, 2 to 6, or 2 to 4, such as 2, 3, or 4.

[0078] Advantageously, when R 1 When amine functional groups are included, R 1 It has the formula -(CH2) p (CF2) q NH2, wherein p is between 0 and r-1, q is rp-1, and r is the total number of carbon atoms. Advantageously, r is between 1 and 20, preferably 1 to 10, such as 1 to 8, 1 to 6, or 1 to 4, such as 1, 2, 3, or 4.

[0079] Advantageously, when R 1 When it includes a thiol functional group, R 1 It has the formula -(CH2) u (CF2) v SH, where u is between 0 and w-1, v is wu-1, and w is the total number of carbon atoms. Advantageously, w is between 1 and 20, preferably between 1 and 10, such as 1 to 8, 1 to 6, or 1 to 4, such as 1, 2, 3, or 4.

[0080] Advantageously, the inorganic-organic hybrid coating further comprises at least one halogen atom. Advantageously, the halogen atom is fluorine, chlorine, bromine, or iodine. When R 1 When two or more halogen atoms are included, they can be the same or different, i.e., a combination of two or more of fluorine, chlorine, bromine, and iodine. The corrosion-inhibiting coating further comprises silicon and / or titanium.

[0081] Advantageously, R 1 Including C1-C according to formula (III) 20 Alkyl groups or those composed of -(CH2) x (CF2) y CF3(III) in x is between 0 and z-1. y is z-1-x, and z is the number of carbon atoms in the chain, and it is between 0 and 20.

[0082] For example, R 1It could be -(CH2)2(CF2)5CF3, meaning z is 8, x is 2, and y is 5. For example, R 1 It could be -(CH2)5CF3, that is, z is 6, x is 5 and y is 0.

[0083] R 1 It can be C1-C 20 Perfluoroalkyl, i.e., an alkyl group in which all hydrogen atoms are replaced by fluorine atoms, according to -(CF2) y CF3, where in equation (III) x is 0, y is z-1, and z is between 1 and 20. For example, R 1 It can be a C8 perfluoroalkyl, i.e., -(CF2)7CF3 (z = 8, x = 0 and y = 7 in formula (III)), a C6 perfluoroalkyl, i.e., -(CF2)5CF3 (z = 6, x = 0 and y = 5 in formula (III)), or a C4 perfluoroalkyl, i.e. -(CF2)3CF3 (z = 4, x = 0 and y = 3 in formula (III)).

[0084] Advantageously, the coating has a thickness of 1 µm to 20 µm, preferably 1.2 µm to 10 µm, such as 1.5 µm to 5 µm. As will be understood, the optimal coating thickness (among other things) depends on the substrate to be protected, particularly its composition and shape, and the intended use of the article.

[0085] Advantageously, when the substrate comprises iron, such as steel, particularly carbon steel, the coating has a thickness of at least 2 µm, for example at least 2.1 µm, preferably at least 2.2 µm, such as at least 2.3 µm, at least 2.4 µm, or at least 2.5 µm. When the coating has such a thickness, it can provide effective corrosion protection for the substrate.

[0086] Advantageously, when the substrate comprises copper, such as brass or bronze, the coating has a thickness of at least 1 µm, preferably at least 1.2 µm, such as at least 1.3 µm, at least 1.4 µm, or at least 1.5 µm. When the coating has such a thickness, it can provide effective corrosion protection for the substrate.

[0087] Advantageously, when the article is a watch component, i.e., used in a watch, its thickness is advantageously 5 µm or less. As is known in the field of watch components, a thicker coating can affect the function of the watch and may require redesign of the component, which involves significant costs. The inventors have discovered that the article of the present invention (where the coating thickness is at most 5 µm) allows for a significant reduction in corrosion while avoiding the need for redesign.

[0088] For example, when the substrate includes iron, such as carbon steel, the coating advantageously has a thickness of 2 µm to 5 µm, preferably 2.2 µm to 5 µm, and more preferably 2.4 µm to 5 µm.

[0089] For example, when the substrate includes copper, such as bronze or brass, the coating advantageously has a thickness of 1 µm to 5 µm, preferably 1.2 µm to 5 µm, for example 1.3 µm to 5 µm, more preferably 1.5 µm to 5 µm. Example

[0090] Two types of substrates are available: carbon steel sheet and brass sheet.

[0091] A reference article was obtained by applying a reference corrosion-inhibiting coating to two substrates. This reference corrosion-inhibiting coating is a halogen-free coating.

[0092] Four different prepolymers according to the present invention were prepared. Detailed information regarding the functional groups is listed in Table 1. Two prepolymers contain fluorinated alkyl groups having the formula -(CH2)2(CF2)5CF3 as functional groups (B1 and B2 in Table 1). Based on the total weight of the respective prepolymers, B1 contains a low proportion of fluorinated alkyl functional groups, and B2 contains a high proportion of fluorinated alkyl functional groups. The other two prepolymers contain functional groups containing amide and ether functional groups, having the formula -(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3 (C1 and C2 in Table 1). Based on the total weight of the respective prepolymers, C1 contains a low proportion of functional groups, and C2 contains a high proportion of functional groups.

[0093] Table 1: Overview of Test Coatings coating Functional groups ratio A Reference halogen-free B1 <![CDATA[-(CH2)2(CF2)5CF3]]> Low B2 <![CDATA[-(CH2)2(CF2)5CF3]]> high C1 <![CDATA[-(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3]]> Low C2 <![CDATA[-(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3]]> high .

[0094] The prepolymer of the present invention is applied to carbon steel and brass substrates by immersing the substrate in the prepolymer and then thermosetting it at 160°C. The coating thickness obtained on the carbon steel substrate is between 1 µm and 3 µm, while the coating thickness obtained on the brass substrate is between 1.5 µm and 2.5 µm.

[0095] It should be noted that all four coatings of the present invention (B1, B2, C1, C2) are transparent and uniformly cover the substrate. Furthermore, it should be noted that coating C2 exhibits greater flexibility (lower rigidity) than coating C1, which helps reduce the risk of defects (e.g., cracks) forming at thicker thicknesses. It should also be noted that coating B2 is easier to clean and exhibits a slightly lower surface energy than coating B1, which contains a lower amount of fluorinated functional groups. Surface energy is measured by measuring the water contact angle according to standard ASTM D5946 and converting the water contact angle to a surface energy value using a known and published conversion table.

[0096] The corrosion protection properties of all five products and the substrate without any corrosion protection were tested in 0.1% NaCl solution by measuring the open-circuit potential (OCP). Higher OCP values ​​indicate better corrosion protection because damage such as short circuits caused by corrosion is significantly reduced. OCP was measured at 24°C using the EC-pen method with a saturated calomel electrode (SCE) as the reference electrode. Results showed... Figure 2 In the OCP value, "uncoated" indicates the substrate without any corrosion protection. The value marked with a triangle 4 represents the OCP value of carbon steel substrate, while the value marked with a circle 5 represents the OCP value of brass substrate.

[0097] from Figure 2 It is clear that all corrosion-inhibiting or corrosion-protecting coatings applied to carbon steel resulted in higher OCP values ​​than the uncoated, unprotected substrate. It is well known that carbon steel without any protection is susceptible to corrosion. Therefore, the results indicate that all coatings provided corrosion protection for the carbon steel substrate. Furthermore, coatings based on epoxy-containing functional groups (C1 and C2) provided better protection than the reference coatings, while alkyl functional groups (B1 and B2) showed slightly lower protection, which was still significant compared to the bare substrate.

[0098] In terms of OCP value, the coating on the brass substrate does not appear to provide significantly improved corrosion protection. However, it should be noted that brass itself is known to possess a certain degree of corrosion resistance, even without any protection. This is evident from the fact that the OCP value of bare brass substrates is significantly higher than that of bare carbon steel substrates. Therefore, from Figure 2 As can be seen, no coating reduces the inherent corrosion protection of the brass substrate. Furthermore, coating B1 exhibits a significantly higher OCP value than the uncoated substrate.

[0099] As a second test for evaluating corrosion protection, the amount of ion release from the substrate was measured. Higher release or leaching of ions contained in the substrate indicates greater damage to the substrate from side effects (such as corrosion reactions).

[0100] An ion release test was performed on the untreated substrate and the coated substrates B1 and C1. The substrates were placed in a 0.9% NaCl solution at 37°C for 7 days. Any released ions were measured by inductively coupled plasma mass spectrometry (ICP-MS).

[0101] Table 2 shows the results for the carbon steel substrates, and Table 3 shows the results for the brass substrates. "<LOD" means that the concentration of released ions is below the limit of detection.

[0102] Table 2: Ion concentrations released from carbon steel substrates in 0.9% NaCl solution at 37°C over 7 days ion Uncoated B1 C1 Al 28.69 µg / cm² <LOD <LOD Si <LOD <LOD <LOD P <LOD <LOD <LOD Mn 9.87 µg / cm² 2.39 µg / cm² 2.70 µg / cm² Fe 4118.16 µg / cm² 816.38 µg / cm² 756.28 µg / cm² Ni <LOD <LOD <LOD Cu <LOD <LOD <LOD Zn <LOD <LOD <LOD Sn <LOD <LOD <LOD Pb 1.78 µg / cm² <LOD <LOD total 4158.50 µg / cm² 818.77 µg / cm² 758.98 µg / cm² .

[0103] It can be clearly seen from Table 2 that the concentrations of iron (Fe) ions and manganese (Mn) ions dissolved from the coated carbon steel substrates into the NaCl solution are significantly reduced when compared with the substrates without any corrosion protection ("uncoated"). In addition, contrary to the uncoated substrates, no release or leaching of any lead (Pb) ions was detected for the coated substrates. This demonstrates the effective protection of the coating of the present invention for carbon steel substrates.

[0104] Table 3: Ion concentrations released from brass substrates in 0.9% NaCl solution at 37°C over 7 days ion Uncoated B1 C1 Al <LOD <LOD <LOD Si <LOD <LOD <LOD P <LOD <LOD <LOD Mn <LOD <LOD <LOD Fe <LOD <LOD <LOD Ni <LOD <LOD <LOD Cu 2.16 µg / cm² <LOD <LOD Zn 143.85 µg / cm² <LOD <LOD Sn <LOD <LOD <LOD Pb 5.33 µg / cm² 0.34 µg / cm² 0.34 µg / cm² total 151.34 µg / cm² 0.34 µg / cm² 0.34 µg / cm² .

[0105] It can be clearly seen from Table 3 that for the coated brass substrates, the main components of brass, copper (Cu) ions and zinc (Zn) ions, do not dissolve from the brass substrates into the NaCl solution, which is contrary to the substrates without any corrosion protection ("uncoated"). This demonstrates the effective protection of the coating of the present invention for brass substrates.

[0106] It should further be noted that brass substrates without any coating change their color or luster within 3 to 5 days of exposure to the atmosphere (sunlight, air). The golden-like color turns into an orange luster. When such brass parts are used in timepieces and are visible from the outside, such changes in hue, luster or color are undesirable changes from an aesthetic point of view. In contrast to uncoated brass, it should be noted that the same substrates coated with the coating according to the present invention do not show any signs of corrosion after several months of exposure to the atmosphere (no visible changes were noted in tests lasting up to 6 months).

[0107] The adhesion strength of coatings B1 and C1 on both types of substrates was measured according to EN ISO 2409 (the so-called "cross-cut test"). All test samples achieved a score of 0, indicating that the edges of the cuts were smooth and none of the squares of the lattice were detached.

[0108] name 1. Products 2. Substrate 3. Corrosion-inhibiting coating 4. OCP value of carbon steel 5. Brass OCP value

Claims

1. An article comprising a substrate and a corrosion-inhibiting coating present on at least a portion of the surface of the substrate, wherein the substrate comprises a metallic element and / or an alloy of metallic elements, and wherein the corrosion-inhibiting coating comprises at least one functional group R. 1 Crosslinked inorganic-organic hybrid coating, wherein R 1 Includes one or more selected from C1-C 20 Alkyl, C1-C 20 cycloalkyl, C1-C 10 Functional groups including aryl, amide, amine, mercapto, and epoxy groups. characterized in that R 1 further substituted by at least one halogen atom, characterized in that the crosslinked inorganic-organic hybrid coating comprises silicon and / or titanium, and in that the crosslinked inorganic-organic hybrid coating is each covalently bound to the metal element or its alloy by an oxygen-silicon bond or an oxygen-titanium bond.

2. The article of claim 1, wherein the crosslinked inorganic-organic hybrid coating further comprises carbon-silicon bonds.

3. The article of claim 1 or 2, wherein the halogen atom is fluorine, chlorine, bromine, iodine or a combination of two or more thereof.

4. The article of manufacture according to claim 1 or 2, wherein R 1 It is -(CH2) x (CF2) y CF3, where x is between 0 and z-1, y is zx-1, and z is the number of carbon atoms between 1 and 20.

5. The article of claim 4, wherein R 1 is -(CH2)2(CF2)5CF3.

6. The article of claim 1 or 2, wherein R 1 is -(CH2)3NHC(O)OCH2CF(CF3)OCF2CF(CF3)O(CF2)2CF3.

7. The article of claim 1 or 2, wherein the metallic element is iron or copper.

8. The article of claim 7, wherein the metallic element is iron, and the substrate comprises steel, preferably carbon steel.

9. The article of claim 7, wherein the metallic element is copper, and the substrate comprises a copper alloy, preferably brass.

10. The article of claim 1 or 2, wherein the article of claim 1 or 2 is a watch component.

Citation Information

Patent Citations

  • Method and apparatus for coating a substrate using dielectric barrier discharge

    EP1729892A1