A polymer-grafted sheet magnetic powder and its application in polyurethane coatings
By forming an aminosilane anchoring layer on the surface of sheet magnetic powder and performing single-end open-ring grafting, the problem of decreased interlayer adhesion during semi-cured recoating of polyurethane coatings is solved, the interlayer bonding strength and electromagnetic properties are improved, and it is suitable for multi-layer construction of polyurethane coatings.
Patent Information
- Application Number
- CN202611511146.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
In the multi-layer application of polyurethane coatings, the interlayer adhesion decreases during semi-cured recoating, making cracking or peeling more likely. Existing technologies struggle to effectively address the issue of stable bonding between the substrate and the new coating, especially when the substrate contains residual solvents and is not fully cured.
Polymer-grafted sheet-like magnetic powder is used. An aminosilane anchoring layer is formed on the surface of the magnetic powder, and ring-opening grafting is performed with linear polymer chains to form hydroxyl linkages that can participate in polyurethane curing. The functional groups of the outer chain segments do not participate in the isocyanate reaction, ensuring effective bonding between the grafted root and the newly coated resin and reducing the covalent cross-linking constraints of the outer chain segments.
It improves interlayer bonding during semi-cured recoating, reduces the risk of cracking and peeling, maintains the overall performance and electromagnetic response of the coating, and avoids the shortcomings of reducing the degree of curing or increasing free plasticizer components.
Smart Images

Figure CN123107438A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of magnetic powder surface modification and polyurethane microwave absorbing coating technology, and particularly to a polymer-grafted sheet magnetic powder and its application in polyurethane coatings. Background Technology
[0002] With the development of integrated and miniaturized electronic devices and the increasing demand for electromagnetic protection, microwave absorbing coatings not only need to meet electromagnetic parameters and absorption performance requirements, but also need to consider the adaptability to construction, mechanical properties, and reliability of complex component surfaces. Polyurethane resin can be combined with magnetic absorbers to form spray-applied microwave absorbing coatings, and sheet-like iron-based magnetic powder is one type of functional filler. For multi-layer structures formed by multiple spraying, reliable bonding between layers is an important condition for maintaining the overall performance of the coating. Local cracking or interlayer delamination may disrupt the continuity of the coating and affect its reliability.
[0003] The film-forming process of solvent-based two-component polyurethane coatings involves solvent escape and cross-linking reactions between the hydroxyl and isocyanate components. During multi-coat spraying, the substrate may be in a wet, gelled but not fully cured intermediate state before recoating, or fully dried and cured. Under different states, the residual solvent content, degree of cross-linking, chain segment mobility, and solvent resistance of the substrate vary. Whether a substrate is suitable for recoating cannot be determined solely by whether the surface is sticky or by the fixed placement time. In the application of polyurethane microwave absorbing coatings filled with sheet-like iron-based magnetic powder, it was found that continuous spraying while the substrate is still wet, or spraying after the substrate has been fully dried, resulted in relatively good interlayer adhesion; however, when the substrate is in a so-called "semi-dry" intermediate state, the interlayer adhesion after recoating decreases. The semi-cured recoating state of concern in this application refers to a state where the substrate has formed a gel, still contains volatile organic solvents, and is not yet fully cured. Its specific determination should be based on the actual degree of curing and the residual solvent situation.
[0004] To address the above phenomena, the incoordination between the underlying cross-linking and the solvent effect needs to be considered. After the initial cross-linking network is formed in the substrate, the movement of resin segments and their ability to diffuse with the newly coated resin are restricted, but their solvent resistance may not yet be fully established. When recoating solvent enters the near-surface area of the substrate, it may cause swelling and softening, but it may not necessarily restore the gelled resin to its uncured mixed state. Therefore, the substrate may be in a state where it can be disturbed by the solvent, but it is difficult to reform sufficient interfacial bonds.
[0005] During subsequent drying and curing, continued solvent escape and dimensional changes caused by cross-linking reactions can lead to inconsistent shrinkage in the underlayer, recoating layer, and their near-interface regions. When coating deformation is constrained, and the local interface's load-bearing and stress relaxation capabilities are insufficient, stress concentration may occur, promoting cracking or delamination. The dispersion, orientation, and stacking state of the flake powder also need to be considered in conjunction with the actual failure area. Therefore, semi-cured recoating problems cannot be simply attributed to powder-resin incompatibility or insufficient wetting between the two coating surfaces; the interface reconstruction capability after solvent disturbance and subsequent shrinkage stress must also be considered.
[0006] Treating magnetic powders with silane coupling agents is a conventional method to improve the interfacial interaction between powder and resin. The silanol groups generated from silane hydrolysis can condense and interact with the oxide layer or hydroxyl groups on the powder surface, while organic functional groups can further participate in resin interfacial bonding. For example, studies have shown that KH550-modified carbonyl iron powder has improved the dispersion, interfacial compatibility, and tensile properties of specific polyurethane composite films. However, improvements in the mechanical properties of a single-layer composite film cannot directly replace the evaluation of interlayer adhesion after the underlayer has partially cured and is recoated. Simply increasing the amount of coupling agent or improving the degree of local crosslinking cannot fully balance the stability of the underlayer and the near-interfacial bonding ability during recoating.
[0007] Introducing polymer grafted layers or polymer brushes onto filler surfaces is an existing technological approach. For example, existing technologies employ polymer brush structures made of thermally conductive and electrically insulating composite materials, involving partial curing and retention of reactive groups for subsequent resin reactions. However, using surface grafting of long chains, introducing reactive groups, or staged curing cannot solve the technical problems addressed in this application. For polyurethane recoating systems, if the reactive sites are distributed at multiple points along the outer chain segments, the grafted chains may be subject to multi-point covalent constraints during the curing of the underlying layer; without clear timing control, there is a lack of technical means to retain these sites until the second coating participates in the reaction. The modified layer, while flexible in the initial dispersion stage, cannot guarantee that it will retain the same mobility after the underlying layer has gelled.
[0008] On the other hand, physically blending flexible polymers into coatings results in different interfacial arrangements compared to fixing them to powder surfaces through a defined grafting structure. The solvent migration of free components, their impact on the curing process, and the final properties cannot be simply predicted; for example, in actual production, it is difficult to conclude that a stable powder interfacial structure has been formed solely based on a short-term increase in adhesion. Even with single-end grafting, the lack of along-chain reaction sites on the outer chain segments does not mean they can move freely within the already gelled underlayer; their actual range of motion is still limited by resin compatibility and the surrounding network. Only chain segments located in the recoating influence area and capable of effective contact with the newly coated resin can participate in near-interfacial bonding, rather than assuming that grafted chains at any location within the coating can directly form interlayer connections.
[0009] Therefore, compared to simply pursuing higher coating weight or denser reactive groups, powder surface treatment for semi-cured recoating applications requires a coordinated approach that balances stable anchoring, bottom-layer curing bonding, and the subsequent activity of outer chain segments. The effectiveness should be compared under similar curing levels and residual solvent conditions, considering interlayer strength and failure location to distinguish between genuine interfacial improvement and recoating window shifts caused solely by changes in drying rate. Simultaneously, it is necessary to consider both the target frequency electromagnetic response and the final curing performance of the coating, avoiding achieving apparent improvement by reducing the degree of curing or increasing free plasticizer components. Summary of the Invention
[0010] In view of the aforementioned deficiencies in the prior art, the purpose of this invention is to provide a polymer-grafted sheet-like magnetic powder. This invention addresses how to modify the powder surface, coordinate the stable bonding between the powder and the underlying resin, and ensure effective near-interface bonding during recoating, while retaining the sheet-like morphology of the iron-based magnetic powder and considering the magnetic response in the target frequency band and the final curing performance of the polyurethane coating. This improves the problem of decreased interlayer adhesion when the underlying layer has gelled, still contains residual solvent, and is not fully cured. This invention focuses on the technical problem that the underlying layer may swell and soften after being exposed to recoating solvents, making it difficult to restore sufficient interfacial bonding. It aims to reduce the risk of cracking and peeling caused by near-interface weakening and localized stress concentration during subsequent solvent escape and curing shrinkage, without compromising the final curing degree of the coating or increasing free plasticizer components.
[0011] To achieve the above objectives, the technical solution provided by the present invention is as follows: In a first aspect of the present invention, a polymer-grafted sheet-like magnetic powder is provided, comprising: Flake-shaped iron-based metal magnetic powder and its surface polymer grafted layer; The polymer grafting layer includes an aminosilane anchoring layer and a linear polymer chain. The aminosilane anchoring layer is connected to the surface oxide layer of the magnetic powder through metal-oxygen-silicon bonds. The linear polymer chain is covalently connected to an aminosilane anchoring layer through a chain end, and the connecting part contains a β-hydroxyamine structure formed by the ring-opening reaction of terminal epoxy groups and amino groups. The connecting portion retains the hydroxyl groups that react with the isocyanate groups; outside the connecting portion, the remaining segments of the linear polymer chain and the non-grafted ends do not contain hydroxyl, carboxyl, mercapto, NH-bonded groups, epoxy groups and isocyanate groups, and do not form other covalent connections with the aminosilane anchoring layer.
[0012] The aforementioned polymer grafting layer design includes an aminosilane anchoring structure, a hydroxyl-containing grafting connector, and a linear polymer chain fixed at one end through the connector. The grafting connector participates in the curing and bonding of the polyurethane resin, while the remaining segments of the linear polymer chain and the non-grafted ends do not contain functional groups that react with isocyanate under the curing conditions, thus forming functional partitions between the grafting root and the outer chain segments.
[0013] Preferably, the sheet-like iron-based metal magnetic powder is selected from iron-based soft magnetic alloy sheet-like powder; the iron-based soft magnetic alloy sheet-like powder includes one or more of iron-silicon alloy, iron-aluminum alloy, iron-cobalt alloy, iron-nickel alloy, and their multi-component alloy sheet-like magnetic powders.
[0014] Those skilled in the art can select the powder particle size, flake thickness, and filling amount according to the electromagnetic properties of the target frequency band and the requirements of the spraying application; among them, iron-silicon-aluminum-cobalt alloy flake magnetic powder is a further preferred type of the present invention. The surface treatment process is not aimed at crushing, grinding, or re-flakening; instead, mechanical stirring is used to achieve contact between the powder and the treatment liquid, and to control particle agglomeration and morphological changes.
[0015] Preferably, the aminosilane anchoring layer is formed by hydrolysis and condensation of 3-aminopropyltriethoxysilane.
[0016] This invention preferably uses 3-aminopropyltriethoxysilane, i.e., KH550, which forms an anchoring structure through silane hydrolysis and condensation, and is connected to the oxide layer on the magnetic powder surface through metal-oxygen-silicon bonds; the anchoring layer may contain silicon-oxygen structures formed by the condensation of the silane itself. This type of aminosilane has a silicon-containing moiety that can bond with inorganic surfaces and a primary amine that can participate in organic reactions, but this scheme does not automatically consider the silane-treated surface as a uniform and complete monolayer.
[0017] Preferably, the linear polymer chain is a copolymer chain of n-butyl acrylate and methyl methacrylate.
[0018] In this invention, the linear polymer is preferably a copolymer of n-butyl acrylate and methyl methacrylate. The selection of chain segment composition and molecular weight ensures compatibility with the polyurethane resin and application solvent to be used. This polymer should have a clearly defined single-terminal epoxy structure and should not be directly replaced by ordinary hydroxyl acrylic resins, double-terminal epoxy polymers, or polymers with multiple epoxy groups randomly distributed along the chain.
[0019] Preferably, the linear polymer chain and the aminosilane anchoring layer have the following connection structure: -NH-CH2-CH(OH)-CH2-OP; In this context, -NH- is connected to the organic chain segment of the aminosilane anchoring layer, and P represents the chain segment in the linear polymer chain excluding the connecting part.
[0020] Based on the above linkage structure, the terminal epoxy group undergoes a ring-opening grafting reaction with the amino group on the magnetic powder surface, forming a β-hydroxyamine structure at the linkage. Taking the primary amine undergoing a single epoxy addition reaction as an example, its local linkage structure is represented as S-NH-CH2-CH(OH)-CH2-OP; where S represents the portion of the aminosilane structure fixed on the powder surface that is connected to the nitrogen atom, and P represents the remaining linear polymer chain segments and inert ends. This linkage method utilizes the epoxy-amine ring-opening reaction to generate the root hydroxyl group, without the need to introduce multiple reactive groups on the outer polymer chain.
[0021] The “single-end grafting” of the present invention refers to a single polymer chain being covalently connected to the anchoring structure on the powder surface through only one end. It does not mean that only one polymer chain can be grafted onto the powder surface, nor does it necessarily mean that each surface amino group undergoes only one addition.
[0022] In a second aspect of the present invention, a method for preparing polymer-grafted sheet-like magnetic powder according to the first aspect of the present invention is provided, comprising the following steps: (1) Hydrolyze aminosilane in an alcohol-water mixture, add sheet-like iron-based metal magnetic powder, and react under stirring conditions to form an aminosilane anchoring layer on the surface of the magnetic powder. (2) Solid-liquid separation and washing to remove unbound silanes and soluble condensates, yielding aminated magnetic powder; (3) Disperse the aminated magnetic powder in an organic solvent that can dissolve the linear polymer to be grafted, and add a linear polymer with only one end of the chain having an epoxy group, so that the end epoxy group reacts with the amino group on the surface of the magnetic powder to undergo a ring-opening grafting reaction. (4) Separate the grafted magnetic powder, wash it with a solvent that can dissolve the ungrafted polymer, wash away the free polymer, and dry it to obtain polymer-grafted sheet magnetic powder.
[0023] Based on actual production conditions or needs, those skilled in the art can select the hydrolysis, reaction and ring-opening grafting reaction parameters in step (1) and step (3). For example, hydrolysis can be carried out at 20~60 ℃ for 10 min~2 h, reaction at 20~60 ℃ for 1~6 h, and ring-opening grafting reaction at 60~90 ℃ for 6~12 h. Specifically, in step (1), aminosilane is added to an alcohol-water mixture and hydrolyzed at room temperature for 20 min. Then, sheet-like iron-based metal magnetic powder is added in batches. After the addition is completed, the reaction is continued at room temperature for 4 h to form an aminosilane anchoring layer on the surface of the magnetic powder. In step (3), the aminated magnetic powder is dispersed in an organic solvent that can dissolve the linear polymer to be grafted. A linear polymer with only one epoxy group at one chain end is added and the reaction is carried out at 80 ℃ for 8 h to allow the terminal epoxy group to undergo a ring-opening grafting reaction with the amino group on the surface of the magnetic powder.
[0024] Preferably, in step (3), the terminal epoxy group of the linear polymer is a glycidyl ether group; the main chain, side chain and other end of the linear polymer do not contain epoxy groups.
[0025] Before grafting, the linear polymer has only one epoxy group at one end of its chain, while the other end is an inert end group that does not react with isocyanate under polyurethane curing conditions. Preferably, the terminal epoxy group is a glycidyl ether group. Apart from this terminal epoxy group, the polymer backbone, side chains, and the other end contain no other epoxy groups, and are free of hydroxyl, carboxyl, mercapto, NH-containing groups, and isocyanate groups. The end group structure is determined by the structure of the raw material and is not used as a substitute for confirming the single-end structure, even if the average epoxy functionality of the polymer sample is close to 1.
[0026] In a third aspect of the present invention, a two-component polyurethane microwave absorbing coating is provided, comprising: Component A and Component B are stored separately; Component A includes a hydroxyl resin, polymer-grafted sheet-like magnetic powder according to the first aspect of the present invention, and an organic solvent; Component B includes a polyisocyanate curing agent.
[0027] In a fourth aspect of the present invention, a method for preparing a polyurethane multilayer microwave absorbing coating is provided, comprising the following steps: The A component and the B component of the two-component polyurethane microwave absorbing coating of the third aspect of the present invention are mixed and sprayed to form a first layer. While the first layer has formed a gel, still contains volatile organic solvents, and has not yet fully cured, the separately mixed components A and B are sprayed onto the surface of the first layer to form the second layer. The first and second layers are then cured to obtain a polyurethane multilayer microwave absorbing coating.
[0028] Preferably, the solvent system used in the second coating layer is soluble in the pre-grafted linear polymer used in the preparation process of polymer-terminated single-end grafted sheet magnetic powder at the recoating temperature.
[0029] Based on the above technical solutions, the design concept and principle of this invention are as follows: This invention is designed around the functional partitioning of the polymer grafted root and outer chain segments. It utilizes an aminosilane anchoring layer to perform ring-opening grafting with a linear polymer containing epoxy groups at one end. This forms hydroxyl groups at the junction that can participate in polyurethane curing, while preventing the remaining chain segments and non-grafted ends from having functional groups that would react with isocyanate under the curing conditions. The core technology of this solution is to reduce the constraint of multi-point covalent cross-linking along the outer chain segments while fixing the root, providing structural conditions for local rearrangement under the action of recoating solvent, interpenetration with the newly coated resin, and subsequent network fixation. This design aims to improve interlayer bonding during semi-cured recoating, not to dissolve the entire cured substrate, nor to consider the use of coupling agents or grafted long chains as sufficient evidence of performance improvement.
[0030] Specifically, this invention employs a synergistic modification scheme of "aminosilane surface anchoring - linear polymer single-end ring-opening grafting - functional partitioning of grafted roots and outer chain segments". First, an aminosilane anchoring layer is formed on the surface of the flake magnetic powder. Then, a linear polymer with only one epoxy group at its end undergoes a ring-opening reaction with the surface amino group, fixing the polymer chain to the powder surface at one end and forming hydroxyl groups at the grafting junction that can participate in polyurethane curing. The remaining chain segments and non-grafted ends do not contain functional groups that react with isocyanate under the curing conditions, allowing the grafted roots to participate in resin network bonding while preventing the outer chain segments from forming multi-point covalent constraints along the chain due to this type of reaction. After washing to remove free polymer and drying, the resulting modified magnetic powder is used in a two-component polyurethane microwave absorbing coating, sprayed in multiple layers and cured further. This structural design aims to provide conditions for local rearrangement, interpenetration, and subsequent physical fixation of the tethered chain segments that can contact the newly coated resin within the recoating influence area, thereby improving interlayer bonding during semi-cured recoating and providing conditions for local stress relaxation. The present invention aims to balance the stable fixation of the root and the limited mobility of the outer chain segments, rather than redissolving the entire glued substrate, nor assuming that the reactive groups on the grafted chain can be automatically retained until the second spraying before participating in the reaction.
[0031] In terms of application, this invention uses polymer-grafted sheet magnetic powder at one end for two-component polyurethane microwave absorbing coatings and multi-layer coatings formed by multiple sprayings. The structural design concept is that the reactive sites at the grafted root participate in the bonding between the powder and the underlying resin, while reducing the constraint of multi-point covalent cross-linking of the outer chain segments. This provides conditions for local rearrangement, interpenetration, and subsequent network fixation of the tethered chain segments that can contact the new coating resin in the recoating area.
[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention uses aminosilane to form an anchoring structure on the surface of sheet-like iron-based metal magnetic powder. Then, a linear polymer with only one epoxy group at its chain end is used for ring-opening grafting with the surface amino group. The powder is then thoroughly washed with a solvent capable of dissolving the free polymer, and the resulting magnetic powder is used for polyurethane layering spraying when the underlying layer has gelled but not fully cured. This combination arranges powder anchoring, root reactivity, and outer chain segment mobility in different structural locations, providing conditions for near-interface bonding during semi-cured recoating.
[0033] In the polymer-terminated single-end grafted sheet-like magnetic powder and its preparation process design of the present invention, the terminal epoxy group forms hydroxyl groups at the linker after ring opening, which can react with the isocyanate groups of the polyurethane curing agent; NH-containing groups that may remain in the linker and anchoring layer can also participate in the reaction. Therefore, the root of the grafted chain has the conditions to combine with the coating network, which helps to improve the stability of the powder interface and reduce the uncertainty of free component migration when only a flexible polymer is physically added. The linear polymer does not have functional groups that react with isocyanate under the curing conditions except for the linker, which can reduce the constraint of multi-point covalent cross-linking along the chain on the outer chain segments during the curing of the bottom layer. The tethered chain segments located in the recoating influence zone undergo limited local rearrangement and interpenetration under the combined action of the suitable solvent and the new coating resin, and are physically fixed by the network as the two layers continue to cure, thereby providing conditions for improving interlayer bonding. When the flexibility of polymer chain segments, the amount of grafting, and the compatibility of resin are appropriate, the resulting flexible interface is expected to alleviate the local stress concentration around the flake powder and near the interlayer interface, and reduce the tendency to crack and peel caused by solvent escape and uncoordinated curing shrinkage. Attached Figure Description
[0034] Figure 1 This diagram illustrates the preparation process and grafting structure of polymer-grafted sheet-like magnetic powder. In this diagram, 1 represents the sheet-like magnetic powder and its surface oxide layer; 2 represents the aminosilane anchoring structure; 3 represents the β-hydroxyamine-containing linker; 4 represents the outer linear polymer chain and its inert end; S represents the aminosilane portion fixed to the powder surface, and P represents the outer polymer chain segment and its inert end. Each chain is anchored at only one end; a surface amino group may undergo one or further epoxy addition. The shown linking structure is a schematic of primary amino group addition and does not indicate the presence of only one type of linking or a uniform monolayer on the surface. Figure 2 The figure shows a comparison of electromagnetic parameters of Examples 1-4 and Comparative Example 1 in the range of 0.1-6 GHz, as indicated by the legend; where, from top to bottom, the real part ε′ and the imaginary part ε″ of the relative permittivity are respectively. Figure 3 The figure shows a comparison of the electromagnetic parameters of Examples 1-4 and Comparative Example 1 in the range of 0.1-6 GHz, as indicated by the legend; where, from top to bottom, the real part μ′ and the imaginary part μ″ of the relative permeability are respectively. Figure 4 The images show the fracture surfaces of Examples 1-4 and Comparative Example 1 after the pull-out test, along with the numerical values. The top row, from left to right, represents Examples 1-4, and the bottom row represents Comparative Example 1. Detailed Implementation
[0035] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.
[0036] In the following embodiments, polymer-grafted sheet-like magnetic powder is prepared according to the following specific process under the guidance of the method provided by the present invention: First, aminosilane is hydrolyzed in an alcohol-water mixture. Then, flake-shaped iron-based magnetic powder is added, and under mechanical stirring, the hydrolyzed silane comes into contact with the powder surface to form an anchoring structure. After the reaction, solid-liquid separation is performed, and unbound silane, soluble condensates, and other residues are washed away with a suitable solvent to obtain surface-aminated flake-shaped magnetic powder. The hydrolysis medium is preferably a mixture of ethanol and deionized water; the hydrolysis, feeding, and stirring conditions should balance the silane reaction with the powder stability.
[0037] Subsequently, the aminated magnetic powder is dried and transferred to an organic medium capable of dissolving the terminal epoxy polymer and compatible with the grafting reaction. The terminal epoxy polymer is pre-dissolved and added to the powder dispersion, and ring-opening grafting is performed under mechanical stirring. Candidate media can be xylene or a mixture of xylene and n-butyl acetate, whose solubility and reaction compatibility have been confirmed through actual testing. No polyisocyanate curing agent is added during the grafting stage to avoid the formation of a polyurethane crosslinking network before the powder grafting and washing are completed. After the grafting reaction is complete, the powder is recovered by filtration, centrifugation, or magnetic separation-assisted solid-liquid separation. It is then redispersed and washed using a solvent capable of dissolving the ungrafted polymer to remove free polymer and soluble residues. The washed powder is dried, depolymerized, and sieved to obtain modified magnetic powder. The solvent entering the coating should meet the requirements of the curing system for moisture and reactive impurities, and should not directly introduce alcohol-water residues from the silane treatment or washing stages into the coating.
[0038] In Examples 1-4 and Comparative Example 1, the following measurements were based on 300.0 g of dried iron-based flake alloy powder before treatment, using the same batch of powder. P1 was a proposed random copolymer of monobutyl acrylate and methyl methacrylate with a single-end glycidyl ether base and a target mass ratio of repeating units of 70:30; the other end of the chain was an inert end cap free of active hydrogen. The only difference between P2 and P1 was that the target mass ratio of repeating units was 80:20. The grafting solvent was a mixture S of xylene and monobutyl acetate in a volume ratio of 7:3. Before use, it was confirmed that P1 and P2 were soluble at 25 °C and 80 °C, respectively, and no obvious precipitation was observed after cooling and standing for 24 h. Solvent S was a polyurethane-grade solvent with controlled water content and free of reactive hydroxyl or amino impurities. All four examples retained the same single-end grafting structure and layered construction route. Example 1 was the baseline; Examples 2 and 3 only changed the polymer feed; Example 4 only changed the target copolymer composition.
[0039] Example 1 This embodiment provides a polymer-grafted sheet-like magnetic powder, which is prepared by the following method: (1) Surface treatment with aminosilane: Weigh 300.0 g of sheet-like iron-based magnetic powder. Add 570 mL of anhydrous ethanol and 30 mL of deionized water to a 2 L reaction vessel. Slowly add 3.00 g of KH-550 at room temperature and 300 r / min, and stir for 20 min to hydrolyze. Add the powder in batches, with a feeding time of about 15 min, and maintain room temperature while stirring for 4 h.
[0040] (2) Separation and drying: The above slurry was filtered, and the resulting filter cake was redispersed and washed three times with anhydrous ethanol. The powder was vacuum dried at 60 °C, and then kept at 80 °C for 2 h under nitrogen protection to obtain the aminated powder to be used for subsequent grafting.
[0041] (3) Single-end polymer grafting: Take the whole batch of aminated powder obtained in step (2). First, dissolve 3.00 g of P1 in 100 mL of solvent S, add the aminated powder to 500 mL of solvent S and disperse at 300 r / min, slowly add the polymer solution and stir at 80 °C for 8 h, without adding isocyanate curing agent and other crosslinking agents.
[0042] (4) Elution: After cooling to room temperature, filter and redisperse and wash at least 3 times with solvent S. Vacuum dry at 60 °C to obtain the proposed modified powder, namely polymer-terminated plate magnetic powder.
[0043] This embodiment provides an application of the prepared polymer-grafted sheet magnetic powder, which is formulated into a coating and sprayed in layers: Component A was prepared by mixing 200.0 g of polymer-grafted flake magnetic powder, 100.0 g of hydroxyl acrylic resin solution, and 120.0 g of added polyurethane-grade mixed solvent. Component B was prepared by adding 21.0 g of HDI trimer curing agent just before use. After the first layer reached the common recoating condition criteria described below, a second layer was applied using freshly prepared paint and cured further. The mixing, recoating condition, final film thickness, and curing status were recorded. Independent test panels were prepared for evaluation of interlayer adhesion and electromagnetic properties.
[0044] Example 2 This embodiment provides a polymer-grafted sheet-like magnetic powder, which is prepared by the following method: (1) Surface treatment of aminosilane: Weigh 300.0 g of the same batch of raw powder, use 570 mL of anhydrous ethanol, 30 mL of deionized water and 3.00 g of KH-550, and treat according to the feeding sequence, hydrolysis time, temperature, paddle type and rotation speed in Example 1, and react for 4 h.
[0045] (2) Separation and drying: The powder was redispersed and washed three times with 300 mL of anhydrous ethanol each time, as in Example 1, and then subjected to the same vacuum drying and nitrogen protection treatment at 80 °C to obtain the aminated powder.
[0046] (3) Single-end polymer grafting: P1 1.50 g was first dissolved in 100 mL solvent S, and then added to 500 mL solvent S containing aminated powder; the reaction was carried out at 80 °C, 300 r / min, and nitrogen protection for 8 h.
[0047] (4) Elution: Using the same washing liquid volume, washing time, endpoint requirements and drying procedure as in Example 1, polymer single-end grafted sheet magnetic powder was obtained.
[0048] Coating preparation and evaluation: Take 200.0 g of the obtained polymer-grafted sheet magnetic powder, and use the same resin, curing agent, external solvent and their respective amounts as in Example 1 to prepare two coatings according to the common construction procedure; after recording the recoating state, film thickness and final curing state, test according to the common evaluation method.
[0049] Example 3 This embodiment provides a polymer-grafted sheet-like magnetic powder, which is prepared by the following method: (1) Surface treatment of aminosilane: Weigh 300.0 g of the same batch of raw powder, use 570 mL of anhydrous ethanol, 30 mL of deionized water and 3.00 g of KH-550, and treat according to the feeding sequence, hydrolysis time, temperature, paddle type and rotation speed in Example 1, and react for 4 h.
[0050] (2) Separation and drying: The powder was redispersed and washed three times with 300 mL of anhydrous ethanol each time, as in Example 1, and then subjected to the same vacuum drying and nitrogen protection treatment at 80 °C to obtain the aminated powder.
[0051] (3) Single-end polymer grafting: P1 6.00 g was first dissolved in 100 mL solvent S, and then added to 500 mL solvent S containing aminated powder; the reaction was carried out at 80 °C, 300 r / min and nitrogen protection for 8 h.
[0052] (4) Elution: Using the same washing liquid volume, washing time, endpoint requirements and drying procedure as in Example 1, polymer single-end grafted sheet magnetic powder was obtained.
[0053] Coating preparation and evaluation: Take 200.0 g of the obtained polymer-grafted sheet magnetic powder, and use the same resin, curing agent, external solvent and their respective amounts as in Example 1 to prepare two coatings according to the common construction procedure; after recording the recoating state, film thickness and final curing state, test according to the common evaluation method.
[0054] Example 4 This embodiment provides a polymer-grafted sheet-like magnetic powder, which is prepared by the following method: (1) Surface treatment of aminosilane: Weigh 300.0 g of the same batch of raw powder, use 570 mL of anhydrous ethanol, 30 mL of deionized water and 3.00 g of KH-550, and treat according to the feeding sequence, hydrolysis time, temperature, paddle type and rotation speed in Example 1, and react for 4 h.
[0055] (2) Separation and drying: The powder was redispersed and washed three times with 300 mL of anhydrous ethanol each time, as in Example 1, and then subjected to the same vacuum drying and nitrogen protection treatment at 80 °C to obtain the aminated powder.
[0056] (3) Single-end polymer grafting: P2 3.00 g was first dissolved in 100 mL solvent S, and then added to 500 mL solvent S containing aminated powder; the reaction was carried out at 80 °C, 300 r / min, and nitrogen protection for 8 h.
[0057] (4) Elution: Using the same washing liquid volume, washing time, endpoint requirements and drying procedure as in Example 1, polymer single-end grafted sheet magnetic powder was obtained.
[0058] Coating preparation and evaluation: Take 200.0 g of the obtained polymer-grafted sheet magnetic powder, and use the same resin, curing agent, external solvent and their respective amounts as in Example 1 to prepare two coatings according to the common construction procedure; after recording the recoating state, film thickness and final curing state, test according to the common evaluation method.
[0059] The above presents representative embodiments of the method of the present invention. Those skilled in the art can make appropriate adjustments based on the process steps and parameter optimization range of the present invention, combined with actual conditions or needs, and all can achieve the basic purpose of the present invention.
[0060] Comparative Example 1 The only difference between this comparative example and Example 1 is that the linear polymer is not added, and the preparation process is as follows: (1) Surface treatment of aminosilane. Weigh 300.0 g of the same batch of raw powder, use 570 mL of anhydrous ethanol, 30 mL of deionized water and 3.00 g of KH-550, hydrolyze for 20 min in the same order, temperature and speed as in Example 1, add powder and react for 4 h.
[0061] (2) Separation and drying. The process was exactly the same as in Example 1, with 300 mL of anhydrous ethanol for redispersing and washing three times for 10 min each time; the same vacuum drying and nitrogen protection treatment at 80 °C were performed.
[0062] (3) Same process without polymer addition. The aminated powder was dispersed in 500 mL of solvent S, and another 100 mL of pure solvent S was added at the same time as in Example 1, without adding P1. The mixture was stirred for 8 h at 80 °C, 300 r / min, and under nitrogen protection. Then the same filtration, washing and drying procedures were followed.
[0063] Coating preparation and layered spraying: Take 200.0 g of the obtained dry powder, use 100.0 g of hydroxyl acrylic resin solution, 120.0 g of external mixed solvent and 21.0 g of HDI trimer curing agent as in Example 1, and make test panels according to the same dispersion, standing, recoating interval, spraying and final curing procedures, and test according to the common evaluation method.
[0064] Test Example 1 The electromagnetic parameters (ε′, ε″, μ′, μ″) of the sample were measured in the range of 0.1 to 6 GHz using a vector network analyzer in conjunction with a suitable coaxial transmission / reflection fixture. Figure 2 , 3 The electromagnetic parameters of Examples 1-4 and Comparative Example 1 in the range of 0.1-6 GHz are presented in a comparative graph. As can be seen from the real part (ε′) curve of the dielectric constant, within the test frequency band shown, the ε′ of Examples 1-4 is lower than that of Comparative Example 1. Specifically, Examples 1 and 4 maintain a lower ε′ over a wider frequency band, Example 2 has a relatively higher ε′, and Example 3 falls somewhere in between.
[0065] The above results indicate that each polymer treatment scheme corresponds to a decrease in the real part of the effective dielectric constant of the tested composite sample, and different feed amounts and copolymer composition targets have different effects on the magnitude of this decrease. As can be seen from the imaginary part curve of the dielectric constant, ε″ in Examples 1-4 is generally slightly lower than that in Comparative Example 1, with a more significant difference in the approximately 2-5 GHz range. As can be seen from the real part curve of the permeability, both Examples 1 and Comparative Example 1 show a decreasing trend of μ′ with increasing frequency, but μ′ in each Example 1 is slightly lower than that in Comparative Example 1 in most of the illustrated frequency bands. As can be seen from the imaginary part curve of the permeability, each Example 1 still retains the main magnetic loss peak around approximately 1 GHz, without any disappearance or significant shift of this peak. Comparing Examples 1 and 2, it can be seen that when the feed amount of P1 is increased from 0.5% to 1.0% of the original powder mass, ε′ decreases further, and ε″ in some mid-frequency bands also decreases further, while the main magnetic loss peak is retained. Comparing Example 3 with Example 1, it can be seen that when the amount of P1 added is further increased to 2.0%, ε′ does not continue to decrease, and μ″ does not show further improvement, indicating that increasing the amount of polymer added does not necessarily lead to a continuous improvement in the combination of electromagnetic parameters. In summary, after further polymer treatment on the basis of the common KH-550 treatment, each example exhibits lower real and imaginary parts of the dielectric constant, while retaining the main magnetic loss peaks and their frequency variation characteristics. Among them, Example 1 shows a good balance between the dielectric reduction effect and the retention of magnetic loss response in the illustrated frequency band, and can be used as a benchmark scheme for further optimization and application verification.
[0066] Test Example 3 The adhesion test was conducted according to the applicable procedure of GB / T 5210-2006 "Paints and Varnishes - Pull-off Method". The maximum tensile force F and the area A at failure were recorded, and the tensile stress was calculated using σ = F / A. F is expressed in N and A in mm. 2 For timing, σ is measured in MPa. Figure 4 The results are the interlayer adhesion test results of Examples 1-4 and Comparative Example 1.
[0067] Under the same experimental conditions, it was shown that adding the polymer treatment step improved the resistance to damage at the target interlayer interface and significantly increased the interlayer adhesion from 5.39 MPa to 9.13 MPa. In Examples 1-4, different polymer feed amounts and copolymer compositions resulted in varying degrees of improvement in interlayer adhesion. Example 1 showed the highest improvement in interlayer adhesion and can serve as a benchmark for further optimization and application verification.
[0068] In summary, this invention employs aminosilane to treat the surface of flake-shaped iron-based metal magnetic powder, followed by ring-opening grafting with a flexible polymer containing an epoxy group at one end and an inert end group at the other. The modified magnetic powder is then obtained through washing and drying. The grafted root forms hydroxyl groups that can participate in polyurethane curing, while the outer chain segments do not contain functional groups that react with isocyanates under the curing conditions, thus avoiding multi-point covalent cross-linking along the chain. This magnetic powder, used in polyurethane microwave absorbing coatings, improves interlayer bonding during semi-cured recoating of the underlying layer through root reaction fixation and local rearrangement, interpenetration, and subsequent curing fixation of the outer chain segments under the action of recoating solvent. It also alleviates interfacial stress concentration and has excellent application prospects.
[0069] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.
Claims
1. A polymer-grafted sheet-like magnetic powder, characterized in that, include: Flake-shaped iron-based metal magnetic powder and its surface polymer grafted layer; The polymer grafting layer includes an aminosilane anchoring layer and a linear polymer chain. The aminosilane anchoring layer is connected to the surface oxide layer of the magnetic powder through metal-oxygen-silicon bonds. The linear polymer chain is covalently connected to an aminosilane anchoring layer through a chain end, and the connecting part contains a β-hydroxyamine structure formed by the ring-opening reaction of terminal epoxy groups and amino groups. The connecting portion retains the hydroxyl groups that react with the isocyanate groups; outside the connecting portion, the remaining segments of the linear polymer chain and the non-grafted ends do not contain hydroxyl, carboxyl, mercapto, NH-bonded groups, epoxy groups and isocyanate groups, and do not form other covalent connections with the aminosilane anchoring layer.
2. The polymer-grafted sheet-like magnetic powder according to claim 1, characterized in that: The sheet-like iron-based metal magnetic powder is selected from iron-based soft magnetic alloy sheet-like powder; the iron-based soft magnetic alloy sheet-like powder includes one or more of iron-silicon alloy, iron-aluminum alloy, iron-cobalt alloy, iron-nickel alloy and their multi-component alloy sheet-like magnetic powders.
3. The polymer-grafted sheet-like magnetic powder according to claim 1, characterized in that: The aminosilane anchoring layer is formed by hydrolysis and condensation of 3-aminopropyltriethoxysilane.
4. The polymer-grafted sheet-like magnetic powder according to claim 1, characterized in that: The linear polymer chain is a copolymer chain of n-butyl acrylate and methyl methacrylate.
5. The polymer-grafted sheet-like magnetic powder according to claim 1, characterized in that, The linear polymer chain and the aminosilane anchoring layer have the following connection structure: -NH-CH2-CH(OH)-CH2-OP; where -NH- is connected to the organic segment of the aminosilane anchoring layer, and P represents the segment in the linear polymer chain excluding the connecting part.
6. A method for preparing polymer-grafted sheet-like magnetic powder as described in any one of claims 1 to 5, characterized in that, include: (1) Hydrolyze aminosilane in an alcohol-water mixture, add sheet-like iron-based metal magnetic powder, and react under stirring conditions to form an aminosilane anchoring layer on the surface of the magnetic powder. (2) Solid-liquid separation and washing to remove unbound silanes and soluble condensates, yielding aminated magnetic powder; (3) Disperse the aminated magnetic powder in an organic solvent that can dissolve the linear polymer to be grafted, add a linear polymer with only one end of the chain having an epoxy group, and under stirring conditions, allow the end epoxy group to undergo a ring-opening grafting reaction with the amino group on the surface of the magnetic powder. (4) Separate the grafted magnetic powder, wash it with a solvent that can dissolve the ungrafted polymer, wash away the free polymer, and dry it to obtain polymer-grafted sheet magnetic powder.
7. The method for preparing polymer-grafted sheet-like magnetic powder according to claim 6, characterized in that: In step (3), the terminal epoxy group of the linear polymer is a glycidyl ether group; the main chain, side chain and other end of the linear polymer do not contain epoxy groups.
8. A two-component polyurethane microwave absorbing coating, characterized in that, include: Component A and Component B are stored separately; Component A includes a hydroxyl resin, polymer-terminated sheet magnetic powder as described in any one of claims 1 to 5, and an organic solvent; Component B includes a polyisocyanate curing agent.
9. A method for preparing a polyurethane multilayer microwave absorbing coating, characterized in that, Includes the following steps: The A component and B component of the two-component polyurethane microwave absorbing coating as described in claim 8 are mixed and sprayed to form a first layer. While the first layer has formed a gel, still contains volatile organic solvents, and has not yet fully cured, the separately mixed components A and B are sprayed onto the surface of the first layer to form the second layer. The first and second layers are then cured to obtain a polyurethane multilayer microwave absorbing coating.
10. The method for preparing the polyurethane multilayer microwave absorbing coating according to claim 9, characterized in that: The solvent system used in the second coating layer is soluble in the pre-grafted linear polymer used in the preparation of polymer-grafted sheet magnetic powder at the recoating temperature.