A migration-resistant and fade-resistant ink for interior decoration of laminated glass and its preparation method
By introducing reactive pigment-anchored nano-silica migration inhibitors into the decorative inks inside laminated glass, the problems of pigment migration and fading are solved, and the clarity of the pattern and color stability are improved, which is suitable for the migration resistance and fading resistance of laminated glass.
Patent Information
- Application Number
- CN202611369873.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing decorative inks for laminated glass are prone to problems such as pigment migration, pattern smudging, film contamination, and weather fading during hot-pressing and long-term use. Existing improvement measures are difficult to effectively limit the diffusion and migration of pigments and related components and fading under long-term light exposure.
A reactive pigment-anchored nano-silica migration inhibitor is used, which forms a stable bond between the nano-silica core and the silane coupling layer. Combined with pre-anchoring dispersion and vacuum devolatilization processes, this ensures that the pigment particles are stably bonded to the ink curing network, reducing the risk of migration. Furthermore, a low-migration light stabilizer is used to improve the colorfastness.
It effectively reduces the migration of pigments to the interlayer film, improves pattern clarity and color retention, and ensures that the ink has good weather resistance and color retention in the enclosed environment of the interlayer glass.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of inks, specifically relating to a migration-resistant and fade-resistant ink for interior decoration of laminated glass and its preparation method. Background Technology
[0002] Laminated glass, due to its excellent safety, decorative properties, and application adaptability, is widely used in building doors and windows, interior partitions, glass doors, and decorative components. To achieve patterns, colors, and perspective effects, a decorative ink layer is usually applied inside the interlayer. Unlike ordinary surface printing inks, the decorative inks inside laminated glass must not only meet the requirements of printability, adhesion, and color performance during use, but also withstand the effects of the interlayer hot-pressing process and long-term enclosed environment.
[0003] In existing technologies, the migration and weather resistance issues of this type of ink are typically addressed by adding UV absorbers, hindered amine light stabilizers, inorganic fillers or nanofillers, and by adjusting the resin system, crosslinking system, and curing process. While these measures can improve lightfastness, heat resistance, and film-forming properties to some extent, they still have shortcomings: Firstly, some light stabilizers, dispersants, or other low-molecular-weight additives are still prone to migrating to interlayer films such as PVB, EVA, or SGP during hot pressing and long-term use, leading to blurred pattern boundaries, contamination of transparent areas, and color distortion. Secondly, ordinary inorganic fillers or nanofillers mostly exist in a physically dispersed manner, lacking a stable interface with pigment particles and resin networks, making it difficult to effectively limit the diffusion and migration of pigments and related components during hot pressing. Furthermore, although some existing ink systems can improve initial printing results, they are still prone to fading, yellowing, and decreased pattern clarity under long-term light exposure, high temperature, or humid conditions. Summary of the Invention
[0004] To address the shortcomings mentioned in the background art, the present invention aims to provide a migration-resistant and fade-resistant ink for interior decoration of laminated glass and its preparation method. This ink introduces a reactive pigment-anchored nano-silica migration inhibitor, enabling the pigment particles to form a stable bond with the ink curing network. Combined with pre-anchoring dispersion, vacuum devolatilization, and other process steps, it effectively reduces the migration of pigments and low-molecular-weight components to the interlayer film, reduces pattern smudging after hot pressing, and improves the fade resistance and pattern clarity of the ink layer.
[0005] The objective of this invention can be achieved through the following technical solutions: A migration-resistant and fade-resistant ink for interior decoration of laminated glass, comprising the following components by weight: 20-50 parts film-forming resin, 5-30 parts pigment, 1-15 parts crosslinking agent, 0.1-5 parts low-migration light stabilizer, 0.5-8 parts reactive pigment-anchored nano-silica migration inhibitor, 0.1-5 parts photoinitiator, and 5-30 parts dispersion medium; The reactive pigment-anchored nano-silica migration inhibitor includes a nano-silica core, a silane coupling layer connected to the surface of the nano-silica core, and an organic functional layer connected to the silane coupling layer. The organic functional layer contains both pigment-anchoring groups and crosslinkable groups.
[0006] More preferably, the film-forming resin is one or more of polyurethane acrylate, epoxy acrylate, polyester acrylate, and hydroxyl acrylic resin; the crosslinking agent is one or more of polyfunctional acrylate, blocked isocyanate, and polyfunctional epoxy resin; and the dispersion medium is one or more of reactive diluent and organic solvent.
[0007] More preferably, the pigment is one or more selected from titanium dioxide, iron oxide red, iron oxide yellow, phthalocyanine blue, phthalocyanine green, quinacridone red, diketopyrrolopyrrole red, and carbon black, and the low-migration light-stabilizing agent is selected from one or more selected from low-migration ultraviolet absorbers, low-migration hindered amine light stabilizers, and antioxidants.
[0008] More preferably, in the reactive pigment-anchored nano-silica migration inhibitor, the pigment anchoring group is selected from one or more of phosphate ester group, phosphonic acid group, and carboxyl group, and the crosslinkable group is selected from one or two of acrylate group and methacrylate group.
[0009] More preferably, the reactive pigment-anchored nano-silica migration inhibitor is prepared by reacting nano-silica, a silane coupling agent containing crosslinkable groups, and an acrylate reactive monomer containing phosphate groups. The silane coupling agent containing crosslinkable groups is 3-methacryloyloxypropyltrimethoxysilane, and the acrylate reactive monomer containing phosphate groups is 2-hydroxyethyl methacrylate phosphate.
[0010] A method for preparing a migration-resistant and fade-resistant ink includes the following steps: S1. Pre-anchoring and dispersing of pigments and reactive pigment-anchored nano-silica migration inhibitors; S2. Add film-forming resin to the system obtained in step S1, and perform grinding dispersion and vacuum devolatilization treatment; S3. Add crosslinking agent, photoinitiator and low migration light stabilizer to the system obtained in step S2, and mix evenly to obtain the migration-resistant and fade-resistant ink.
[0011] More preferably, in step S1, the pre-anchoring dispersion is carried out by first stirring at low speed and then dispersing at high speed; the amount of the reactive pigment anchoring nano silica migration inhibitor added to the ink is 0.5 to 8 parts by weight; and the particle size of the nano silica is 10 to 100 nm.
[0012] More preferably, in step S2, the temperature of the vacuum devolatilization is 40–70°C, the vacuum degree is 0.06–0.09 MPa, and the processing time is 0.5–3 h.
[0013] A method for preparing a reactive pigment-anchored nano-silica migration inhibitor includes the following steps: S101. Disperse nano-silica in an alcohol-water mixture and adjust the pH. S102. Add a silane coupling agent containing crosslinkable groups to the system obtained in step S101 to carry out a surface silanization reaction; S103. Add phosphate ester-containing acrylate reactive monomers to the system obtained in step S102 for graft polymerization, followed by solid-liquid separation, washing, drying, pulverizing and sieving to obtain the reactive pigment-anchored nano silica migration inhibitor.
[0014] More preferably, the silane coupling agent containing crosslinkable groups is 3-methacryloyloxypropyltrimethoxysilane, and the acrylate reactive monomer containing phosphate groups is 2-hydroxyethyl methacrylate phosphate.
[0015] The beneficial effects of this invention are: This invention provides a migration-resistant and fade-resistant ink for interior decoration of laminated glass and its preparation method. Addressing the problems of pigment migration, pattern smudging, film contamination, and weather fading that easily occur in existing interior decoration inks for laminated glass during hot pressing and long-term use, this invention achieves comprehensive performance improvement through synergistic optimization of material structure design and preparation process. Firstly, this invention introduces a reactive pigment-anchoring nano-silica migration inhibitor. Utilizing the inorganic barrier and hot-press dimensional stabilization effect of the nano-silica core, combined with a silane coupling layer to improve its compatibility with the resin system, and through an organic functional layer containing phosphate ester groups to enhance its interfacial adsorption and anchoring ability on the pigment particle surface, the pigment and related components are more stably distributed within the ink layer, thereby effectively reducing the tendency to migrate towards the laminated film. Secondly, this invention employs a process route of pre-anchoring dispersion, followed by grinding, then devolatilization and the addition of crosslinking and light-stabilizing components. This allows the modifier to preferentially act on the pigment interface and participate in the formation of a more stable film-forming network during subsequent curing, helping to reduce pattern diffusion and edge blurring under hot pressing conditions and improving the clarity of the pattern after hot pressing. Thirdly, the present invention, in conjunction with a low-migration light-stabilized system, reduces the risk of migration of small molecule additives and fading under long-term light exposure while ensuring the printability of the system. This allows the ink to maintain good color retention and weather resistance even in a sealed environment of laminated glass, under high temperature and light conditions. Detailed Implementation
[0016] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0017] In the following examples and comparative examples, the low-migration UV absorber is UV-328, the low-migration hindered amine light stabilizer is Chimassorb 944, and the antioxidant is antioxidant 1010; the dispersion medium includes a reactive diluent and an organic solvent, wherein the reactive diluent is isobornyl acrylate, and the organic solvent is propylene glycol methyl ether acetate.
[0018] Example 1: This invention provides a method for preparing a migration-resistant and fade-resistant ink, comprising the following steps: I. Preparation of Reactive Pigment-Anchored Nano-Silica Migration Inhibitor Weigh 100 parts by weight of nano-silica, add 500 parts by weight of ethanol and 50 parts by weight of deionized water, and sonicate for 20 min. Then, add glacial acetic acid to adjust the pH of the system to 4.2 to obtain a nano-silica dispersion. Separately weigh 12 parts by weight of 3-methacryloyloxypropyltrimethoxysilane, add 50 parts by weight of ethanol and 5 parts by weight of deionized water, pre-hydrolyze at room temperature for 25 min, and then slowly add it dropwise to the above nano-silica dispersion. Stir the reaction at 60°C for 4 h to obtain a silanized nano-silica intermediate. Subsequently, the reaction system is subjected to reduced pressure treatment to remove some water.
[0019] Under nitrogen protection, 18 parts of 2-hydroxyethyl methacrylate phosphate, 0.8 parts of azobisisobutyronitrile, and 45 parts of ethanol were added to the above system, and the reaction was continued at 70°C for 4 hours. After the reaction was completed, the resulting product was subjected to solid-liquid separation, washed three times with ethanol, and then vacuum dried at 60°C for 8 hours. The product was then pulverized and sieved to obtain the reactive pigment-anchored nano-silica migration inhibitor.
[0020] II. Preparation of migration-resistant and fade-resistant inks By weight, 15 parts of phthalocyanine blue pigment, 2 parts of reactive pigment-anchored nano-silica migration inhibitor, 8 parts of isoborneol acrylate, and 5 parts of propylene glycol methyl ether acetate were weighed. The mixture was first stirred at low speed for 10 min, then dispersed at high speed for 30 min to obtain a pre-anchored dispersion system. Subsequently, 35 parts of polyurethane acrylate were added to the above system, and the mixture was ground and dispersed in a sand mill until the fineness was controlled to be less than 10 μm. After grinding, the resulting system was de-devoured at 60℃ and a vacuum of 0.08 MPa for 1 h.
[0021] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 30 minutes, then filtered to obtain the migration-resistant and fade-resistant ink.
[0022] Example 2: This invention provides a method for preparing a migration-resistant and fade-resistant ink, comprising the following steps: I. Preparation of Reactive Pigment-Anchored Nano-Silica Migration Inhibitor By weight, 100 parts of nano-silica were added to 500 parts of ethanol and 50 parts of deionized water, and ultrasonically dispersed for 20 min. The pH of the system was then adjusted to 4.0 with glacial acetic acid to obtain a nano-silica dispersion. Separately, 15 parts of 3-methacryloyloxypropyltrimethoxysilane were added to 50 parts of ethanol and 5 parts of deionized water, and pre-hydrolyzed at room temperature for 30 min. This pre-hydrolyzed silane was then added dropwise to the above nano-silica dispersion, and the mixture was stirred at 60 °C for 4 h to obtain a silanized nano-silica intermediate. The resulting system was then subjected to vacuum dehydration.
[0023] Under nitrogen protection, 20 parts of 2-hydroxyethyl methacrylate phosphate, 1 part of azobisisobutyronitrile, and 50 parts of ethanol were added to the above system, and the reaction was carried out at 70°C for 4 hours. After the reaction was completed, the product was subjected to solid-liquid separation, washed three times with ethanol, and vacuum dried at 60°C for 8 hours. After pulverization and sieving, a reactive pigment-anchored nano-silica migration inhibitor was obtained.
[0024] II. Preparation of migration-resistant and fade-resistant inks By weight, 15 parts of phthalocyanine blue pigment, 3.5 parts of the above-mentioned reactive pigment-anchored nano-silica migration inhibitor, 8 parts of isoborneol acrylate, and 5 parts of propylene glycol methyl ether acetate were taken. The mixture was premixed at low speed for 10 min, then dispersed at high speed for 30 min to prepare a pre-anchored dispersion slurry. Subsequently, 35 parts of polyurethane acrylate were added, and the mixture was ground in a sand mill to control the fineness to less than 10 μm. After grinding, the resulting system was de-devoured at 60℃ and a vacuum of 0.08 MPa for 1 h.
[0025] After the devolatilization process is complete, add 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010, and 5 parts of propylene glycol methyl ether acetate to the system in sequence. Stir and mix for 30 minutes, filter, and obtain migration-resistant and fade-resistant ink.
[0026] Example 3: This invention provides a method for preparing a migration-resistant and fade-resistant ink, comprising the following steps: I. Preparation of Reactive Pigment-Anchored Nano-Silica Migration Inhibitor By weight, 100 parts of nano-silica were weighed and added to 500 parts of ethanol and 50 parts of deionized water. The mixture was ultrasonically dispersed for 20 min, and then glacial acetic acid was added to adjust the pH to 4.5 to obtain a nano-silica dispersion. Separately, 18 parts of 3-methacryloyloxypropyltrimethoxysilane were weighed and added to 50 parts of ethanol and 5 parts of deionized water. After pre-hydrolyzing at room temperature for 35 min, the mixture was slowly added dropwise to the above nano-silica dispersion. The mixture was stirred and reacted at 65°C for 5 h to obtain a silanized nano-silica intermediate. The reaction system was then subjected to reduced pressure to remove some of the water.
[0027] Under nitrogen protection, 22 parts of 2-hydroxyethyl methacrylate phosphate, 1 part of azobisisobutyronitrile, and 50 parts of ethanol were added to the above system, and the reaction was continued at 72°C for 5 hours. After the reaction was completed, the resulting product was subjected to solid-liquid separation, washed four times with ethanol, and then vacuum dried at 60°C for 8 hours. The product was then pulverized and sieved to obtain the reactive pigment-anchored nano-silica migration inhibitor.
[0028] II. Preparation of migration-resistant and fade-resistant inks By weight, 15 parts of phthalocyanine blue pigment, 5 parts of reactive pigment-anchored nano-silica migration inhibitor, 8 parts of isoborneol acrylate, and 5 parts of propylene glycol methyl ether acetate were weighed. The mixture was first stirred at low speed for 12 min, then dispersed at high speed for 30 min to obtain a pre-anchored dispersion system. Subsequently, 35 parts of polyurethane acrylate were added, and the mixture was ground in a sand mill until the fineness was less than 10 μm. The system was then subjected to devolatilization at 65℃ and a vacuum of 0.08 MPa for 1.5 h.
[0029] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.5 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 35 minutes, then filtered to obtain migration-resistant and fade-resistant ink.
[0030] Comparative Example 1: This comparative example does not contain reactive pigment-anchored nano-silica migration inhibitors. Weigh out 15 parts by weight of phthalocyanine blue pigment, 8 parts by weight of isoborneol acrylate, and 5 parts by weight of propylene glycol methyl ether acetate. Stir at low speed for 10 min, then disperse at high speed for 30 min to obtain a pre-dispersed system. Next, add 38.5 parts by weight of polyurethane acrylate and grind in a sand mill until the fineness is less than 10 μm. Then, place the system at 60℃ and a vacuum of 0.08 MPa for 1 h for devolatilization.
[0031] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 30 minutes, then filtered to obtain a comparative migration-resistant and fade-resistant ink.
[0032] Comparative Example 2: In this comparative example, unmodified nano-silica was used to replace reactive pigment-anchored nano-silica migration inhibitors. By weight, 15 parts phthalocyanine blue pigment, 3.5 parts unmodified nano-silica, 8 parts isoborneol acrylate, and 5 parts propylene glycol methyl ether acetate were weighed. The mixture was first stirred at low speed for 10 min, then dispersed at high speed for 30 min to obtain a pre-dispersed system. Subsequently, 35 parts polyurethane acrylate were added, and the mixture was ground in a sand mill until the fineness was less than 10 μm. The system was then subjected to desorption at 60℃ and a vacuum of 0.08 MPa for 1 h.
[0033] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 30 minutes, then filtered to obtain a comparative migration-resistant and fade-resistant ink.
[0034] Comparative Example 3: This comparative example uses silane-modified nano-silica to replace reactive pigment-anchored nano-silica migration inhibitors, and the silane-modified nano-silica does not contain an organic functional layer formed by phosphate-containing acrylate reactive monomers. I. Preparation of Silane-Modified Nano-Silica By weight, 100 parts of nano-silica were added to 500 parts of ethanol and 50 parts of deionized water, and ultrasonically dispersed for 20 min. The pH of the system was then adjusted to 4.0 with glacial acetic acid to obtain a uniform dispersion. Separately, 15 parts of 3-methacryloyloxypropyltrimethoxysilane were dissolved in 50 parts of ethanol and 5 parts of deionized water, and pre-hydrolyzed at room temperature for 30 min. This solution was then slowly added to the above nano-silica dispersion, and the reaction was carried out at 60 °C for 4 h to obtain a silane-modified nano-silica intermediate. The system was then subjected to solid-liquid separation, washed three times with ethanol, and vacuum dried at 60 °C for 8 h. Finally, the mixture was pulverized and sieved to obtain the silane-modified nano-silica.
[0035] II. Preparation of migration-resistant and fade-resistant inks By weight, 15 parts of phthalocyanine blue pigment, 3.5 parts of the above-mentioned silane-modified nano-silica, 8 parts of isoborneol acrylate, and 5 parts of propylene glycol methyl ether acetate were weighed. The mixture was first stirred at low speed for 10 min, then dispersed at high speed for 30 min to obtain a pre-dispersed system. Subsequently, 35 parts of polyurethane acrylate were added, and the mixture was ground in a sand mill until the fineness was less than 10 μm. The system was then subjected to desorption at 60℃ and a vacuum of 0.08 MPa for 1 h.
[0036] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 30 minutes, then filtered to obtain a comparative migration-resistant and fade-resistant ink.
[0037] Comparative Example 4: This comparative example uses a common phosphate ester dispersant instead of a reactive pigment-anchoring nano-silica migration inhibitor. By weight, 15 parts phthalocyanine blue pigment, 1 part polyoxyethylene nonylphenyl ether phosphate, 8 parts isoborneol acrylate, and 5 parts propylene glycol methyl ether acetate were weighed. The mixture was first stirred at low speed for 10 min, then dispersed at high speed for 30 min to obtain a pre-dispersed system. Subsequently, 37.5 parts polyurethane acrylate were added, and the mixture was ground in a sand mill until the fineness was less than 10 μm. The system was then subjected to desorption at 60℃ and a vacuum of 0.08 MPa for 1 h.
[0038] After devolatilization, 6 parts of trimethylolpropane triacrylate, 1 part of 1-hydroxycyclohexylphenyl ketone, 1 part of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 0.6 parts of UV absorber UV-328, 0.4 parts of polymeric hindered amine light stabilizer Chimassorb 944, 0.2 parts of antioxidant 1010 and 5 parts of propylene glycol methyl ether acetate were added to the system. The mixture was stirred and mixed for 30 minutes, then filtered to obtain a comparative migration-resistant and fade-resistant ink.
[0039] Performance testing Inks were prepared according to Examples 1-3 and Comparative Examples 1-4, and standard line patterns with a width of 0.50 mm were printed on the same glass substrate. The dry film thickness was controlled at 10±2 μm. After being treated under the same pre-curing conditions, the inks were laminated with a PVB interlayer film with a thickness of 0.38 mm and hot-pressed at 120 ℃ and 0.8 MPa for 30 min to obtain interlayer samples. The paint film samples used for performance testing were prepared according to GB / T 1727-2021 "General Preparation Method of Paint Film", and the film thickness was measured according to GB / T 13452.2-2008 "Determination of Film Thickness of Paints and Varnishes".
[0040] (1) Migration distance: The composite sandwich sample was placed at 60 ℃ for 168 h. After taking it out, the sample was cut along the edge of the pattern and the maximum distance of the pigment diffusion to the outside of the pattern boundary or to the direction of the film was measured under a stereomicroscope. The unit is μm. Five parallel samples were tested in each group and the average value was taken.
[0041] (2) Change rate of line width after hot pressing: The standard line width W0 before hot pressing and the line width W1 after hot pressing are measured respectively. The result is calculated according to the formula line width change rate = (W1 - W0) / W0 × 100%. Five positions are measured for each group and the average value is taken.
[0042] (3) Color difference ΔE after aging: Each sample was aged for 500 h under a xenon lamp according to GB / T 1865-2009 "Artificial climate aging and artificial radiation exposure to filtered xenon arc radiation for paints and varnishes". The color before and after aging was measured according to GB / T 11186-2025 "Method for measuring the color of coatings" and the color difference ΔE was calculated.
[0043] The results are shown in the table below.
[0044] Table 1. Comprehensive performance analysis of inks from the examples and comparative examples.
[0045] As shown in the table, the migration distance, linewidth change rate after hot pressing, and color difference ΔE after aging of Examples 1-3 are significantly lower than those of Comparative Examples 1-4, indicating that the ink of the present invention has significant advantages in terms of migration resistance, pattern retention after hot pressing, and fading resistance. Among them, Example 2 has the best overall performance, indicating that the structural design and addition amount of the reactive pigment-anchored nano-silica migration inhibitor are in a better balance. The migration inhibitor provided by the present invention provides inorganic barrier and hot pressing dimensional stability through the nano-silica core, improves its compatibility with the resin system through the silane coupling layer, and enhances its interfacial anchoring ability on the surface of pigment particles through the organic functional layer containing phosphate ester groups. At the same time, it participates in the formation of ink curing network by relying on the surface crosslinkable structure, thereby fixing the pigment and related components more stably within the ink layer. Comparative Example 1 showed the worst results, indicating that the pigment was more prone to migration and diffusion during hot pressing and subsequent storage when the modifier was absent. Although Comparative Examples 2 and 3 introduced nano-silica or silane-modified silica, they still could not achieve effective interface fixation due to the lack of a complete pigment anchoring functional layer. Comparative Example 4 used a common phosphate ester dispersant, which could improve the dispersion state to some extent, but it could not form a stable structure that combined barrier, anchoring and cross-linking fixation functions. Therefore, its overall performance was still significantly lower than that of the present invention.
[0046] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0047] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.
Claims
1. A migration-resistant and fade-resistant ink for interior decoration of laminated glass, characterized in that, By weight, it includes the following components: 20-50 parts film-forming resin, 5-30 parts pigment, 1-15 parts crosslinking agent, 0.1-5 parts low migration light stabilizer, 0.5-8 parts reactive pigment-anchored nano silica migration inhibitor, 0.1-5 parts photoinitiator, and 5-30 parts dispersion medium. The reactive pigment-anchored nano-silica migration inhibitor includes a nano-silica core, a silane coupling layer connected to the surface of the nano-silica core, and an organic functional layer connected to the silane coupling layer. The organic functional layer contains both pigment-anchoring groups and crosslinkable groups.
2. The migration-resistant and fade-resistant ink according to claim 1, characterized in that, The film-forming resin is one or more of polyurethane acrylate, epoxy acrylate, polyester acrylate, and hydroxyl acrylic resin; the crosslinking agent is one or more of polyfunctional acrylate, blocked isocyanate, and polyfunctional epoxy resin; and the dispersion medium is one or more of reactive diluent and organic solvent.
3. The migration-resistant and fade-resistant ink according to claim 1, characterized in that, The pigment is one or more of titanium dioxide, iron oxide red, iron oxide yellow, phthalocyanine blue, phthalocyanine green, quinacridone red, diketonepyrrolopyrrole red, and carbon black; the low-migration light-stabilizing agent is selected from one or more of low-migration ultraviolet absorbers, low-migration hindered amine light stabilizers, and antioxidants.
4. The migration-resistant and fade-resistant ink according to claim 1, characterized in that, In the reactive pigment-anchored nano silica migration inhibitor, the pigment anchoring group is selected from one or more of phosphate ester group, phosphonic acid group, and carboxyl group, and the crosslinkable group is selected from one or two of acrylate group and methacrylate group.
5. The migration-resistant and fade-resistant ink according to claim 1, characterized in that, The reactive pigment-anchored nano silica migration inhibitor is prepared by reacting nano silica, a silane coupling agent containing crosslinkable groups, and an acrylate reactive monomer containing phosphate groups. The silane coupling agent containing crosslinkable groups is 3-methacryloyloxypropyltrimethoxysilane, and the acrylate reactive monomer containing phosphate groups is 2-hydroxyethyl methacrylate phosphate.
6. A method for preparing the migration-resistant and fade-resistant ink according to any one of claims 1-5, characterized in that, Includes the following steps: S1. Pre-anchoring and dispersing of pigments and reactive pigment-anchored nano-silica migration inhibitors; S2. Add film-forming resin to the system obtained in step S1, and perform grinding dispersion and vacuum devolatilization treatment; S3. Add crosslinking agent, photoinitiator and low migration light stabilizer to the system obtained in step S2, and mix evenly to obtain the migration-resistant and fade-resistant ink.
7. The preparation method according to claim 6, characterized in that, In step S1, the pre-anchoring dispersion is carried out by first stirring at low speed and then dispersing at high speed; the amount of the reactive pigment anchoring nano silica migration inhibitor added to the ink is 0.5 to 8 parts by weight; the particle size of the nano silica is 10 to 100 nm.
8. The preparation method according to claim 6, characterized in that, In step S2, the vacuum devolatilization temperature is 40–70°C, the vacuum degree is 0.06–0.09 MPa, and the processing time is 0.5–3 h.
9. A method for preparing a reactive pigment-anchored nano-silica migration inhibitor, characterized in that, Includes the following steps: S101. Disperse nano-silica in an alcohol-water mixture and adjust the pH. S102. Add a silane coupling agent containing crosslinkable groups to the system obtained in step S101 to carry out a surface silanization reaction; S103. Add phosphate ester-containing acrylate reactive monomers to the system obtained in step S102 for graft polymerization, followed by solid-liquid separation, washing, drying, pulverizing and sieving to obtain the reactive pigment-anchored nano silica migration inhibitor.
10. The preparation method according to claim 9, characterized in that, The silane coupling agent containing crosslinkable groups is 3-methacryloyloxypropyltrimethoxysilane, and the acrylate reaction monomer containing phosphate groups is 2-hydroxyethyl methacrylate phosphate.