Protective adhesive and its manufacturing method, microdisplay encapsulation method

By using a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica as a protective adhesive material, the problem of incomplete removal of the protective adhesive in the prior art is solved, achieving high reliability and efficient encapsulation of the microdisplay.

CN123107510APending Publication Date: 2026-11-17ZHUHAI HUAHUI INTELLIGENT MFG SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611036440.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing microdisplay packaging methods, the protective adhesive is not completely removed, resulting in low reliability of the microdisplay, complex processes, and low efficiency.

Method used

A mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica is used as a protective adhesive material. The protective adhesive is formed through a specific mixing and dispersion process and is then applied to the display area of ​​the micro-display screen before being removed by immersion in pure water.

Benefits of technology

It improves the reliability of microdisplays, simplifies the process, increases packaging efficiency, and does not damage the display structure, thus avoiding chemical residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107510A_ABST
    Figure CN123107510A_ABST
Patent Text Reader

Abstract

This disclosure provides a protective adhesive and its preparation method, as well as a microdisplay encapsulation method. The protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity and strong adhesion of the protective adhesive film; the diethylene glycol butyl ether optimizes the flowability and coating effect of the protective adhesive; and the fumed silica improves the hardness and scratch resistance of the protective adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of display technology, and in particular to a protective adhesive and its manufacturing method, and a microdisplay encapsulation method. Background Technology

[0002] As the core imaging device of augmented reality terminals, microdisplays have extremely small pixel sizes and require extremely high optical precision. They are highly sensitive to particulate contaminants, chemical corrosion, and mechanical stress during the manufacturing process. In the top-mold encapsulation stage, epoxy encapsulants release tiny particles during high-temperature filling and curing. These particles easily adhere to the display pixel areas of the microdisplay, leading to problems such as bright / dark pixels, decreased optical transmittance, and degraded image quality. This significantly reduces the yield and long-term reliability of the microdisplay.

[0003] Related technologies provide a microdisplay packaging method, which includes creating a protective adhesive in the display area of ​​the microdisplay; encapsulating the microdisplay to expose the protective adhesive coated in the display area of ​​the microdisplay; and removing the protective adhesive using a chemical solvent.

[0004] However, the microdisplay encapsulation methods provided by related technologies do not completely remove the protective adhesive, resulting in low reliability of the microdisplay, and the process is complex and inefficient. Summary of the Invention

[0005] This disclosure provides a protective adhesive and its manufacturing method, as well as a microdisplay encapsulation method, which can improve the reliability of the microdisplay. The technical solution is as follows: On one hand, a protective adhesive is provided, wherein the material of the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether and fumed silica.

[0006] Optionally, the sulfonated polyester resin accounts for 44-48% of the total mass of the protective adhesive, the diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective adhesive, and the fumed silica accounts for 3-5% of the total mass of the protective adhesive.

[0007] On the other hand, a method for manufacturing a protective adhesive is provided, the method comprising: Diethylene glycol butyl ether solvent and sulfonated polyester resin are added to the reaction vessel and dissolved to form a resin solution; The diethylene glycol butyl ether solvent and fumed silica are added to the first dispersion tank to form a dispersion. The resin solution and the dispersion are added to a second dispersion tank and mixed and stirred to form the protective colloid.

[0008] Optionally, the diethylene glycol butyl ether solvent and sulfonated polyester resin are added to the reaction vessel and dissolved to form a resin solution, comprising: Add 70-80% of the total amount of diethylene glycol butyl ether solvent to the reaction vessel and stir the diethylene glycol butyl ether solvent. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total amount of sulfonated polyester resin. The reaction vessel is heated to 60-80°C, and then kept at that temperature and stirred for 2-4 hours. The reactor was allowed to cool naturally to room temperature.

[0009] Optionally, the diethylene glycol butyl ether solvent and the fumed silica are added to the first dispersion tank to form a dispersion comprising: Take 20-30% of the total amount of diethylene glycol butyl ether solvent and add it to the first dispersion tank. The rotation speed of the first dispersion tank is 1000-1500 rpm. Add fumed silica to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total amount of silica. Increase the rotation speed of the first dispersion cylinder to 2500~3000 rpm and disperse for 30~60 minutes; Reduce the rotation speed of the first dispersion tank to 250-350 rpm and stir for 9-11 minutes.

[0010] Optionally, the resin solution and the dispersion are added to a second dispersion tank and mixed and stirred to form the protective colloid, comprising: The resin solution is added to the second dispersion tank, and the resin solution is stirred at a speed of 500~800 rpm. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective adhesive at 35,000 to 45,000 cps; Stir the protective adhesive for 1-2 hours.

[0011] On the other hand, a microdisplay packaging method is provided, the microdisplay packaging method comprising: A protective adhesive is applied to the display area of ​​the microdisplay screen. The protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The non-display area of ​​the micro-display screen is encapsulated. The microdisplay screen is immersed in pure water to remove the protective adhesive.

[0012] Optionally, before applying the protective adhesive to the display area of ​​the microdisplay, the method further includes: The protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is equal to or less than 5μm; the protective colloid is then filtered using a 100-200 mesh nylon filter bag.

[0013] Optionally, the protective adhesive is applied to the display area of ​​the microdisplay, including: The protective adhesive is applied to the display area of ​​the microdisplay using a fully automated precision dispensing or piezoelectric valve spraying process. The thickness of the protective adhesive is 5~20μm, the uniformity of the protective adhesive is less than or equal to 2μm, and the edge of the protective adhesive extends less than or equal to 0.1mm beyond the boundary of the display area of ​​the microdisplay. The microdisplay screen coated with the protective adhesive is placed in a constant temperature chamber and cured for 10 to 30 minutes at a temperature of 100 to 150°C.

[0014] Optionally, immersing the microdisplay in pure water to remove the protective adhesive includes: The microdisplay screen is ultrasonically immersed for 15-60 minutes at a temperature of 50-80℃, an ultrasonic power of 20-50W, and an ultrasonic frequency of 20-40kHz to remove the protective adhesive.

[0015] The beneficial effects of the technical solutions provided in this disclosure are: In this embodiment, the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity of the protective adhesive film and its strong adhesion; the diethylene glycol butyl ether optimizes the flowability and coating effect of the protective adhesive; and the fumed silica improves the hardness and scratch resistance of the protective adhesive. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of this disclosure, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a flowchart of a method for preparing a protective adhesive according to an embodiment of this disclosure; Figure 2 This is a flowchart of another method for preparing a protective adhesive provided in this embodiment; Figure 3 This is a flowchart of a microdisplay packaging method provided in an embodiment of this disclosure; Figure 4This is a flowchart of another microdisplay packaging method provided in this disclosure embodiment; Figure 5 This is a structural schematic diagram of a microdisplay packaging process provided in an embodiment of this disclosure; Figure 6 This is a schematic diagram of another microdisplay packaging process provided in this embodiment of the disclosure; Figure 7 yes Figure 6 A schematic diagram of the back structure of the microdisplay shown; Figure 8 yes Figure 6 Cross-sectional view at point A-A'; Figure 9 yes Figure 6 Cross-sectional view at point B-B'.

[0018] The attached figures are labeled as follows: 100: Circuit board; 101: Display chip; 102: Wire; 103: Reinforcing steel plate; 104: Connector; 105: Solder pad; 106: Encapsulation layer; 1011: CMOS board; 1012: Display panel; 1000: Display area. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in further detail below with reference to the accompanying drawings.

[0020] This disclosure provides a protective adhesive, the material of which is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica.

[0021] In this embodiment, the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity of the protective adhesive film and its strong adhesion; the diethylene glycol butyl ether optimizes the flowability and coating effect of the protective adhesive; and the fumed silica improves the hardness and scratch resistance of the protective adhesive.

[0022] In this embodiment, sulfonated polyester resin accounts for 44-48% of the total mass of the protective colloid, diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective colloid, and fumed silica accounts for 3-5% of the total mass of the protective colloid.

[0023] In this implementation, sulfonated polyester resin accounts for 44-48% of the total mass of the protective adhesive. As the main body for film formation, this proportion can form a continuous and complete protective film layer, which is firmly bonded to the surface of the microdisplay screen and is not prone to peeling or displacement during encapsulation. At the same time, it retains the hydrophilic properties brought by the sulfonated groups, ensuring that it can be dissolved and peeled off by immersion in pure water. Too low a proportion will lead to discontinuous film formation and protective failure; too high a proportion will result in high adhesive viscosity, poor coating leveling, and a decrease in water solubility. Diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective adhesive. As a solvent and rheology modifier, this ratio can precisely control the overall viscosity and evaporation rate of the protective adhesive. It has excellent leveling properties during coating and can evenly cover the display area, avoiding uneven thickness and missed coating defects. At the same time, it improves the resin dispersion and prevents the system from layering and sedimentation. Insufficient dosage can lead to a thick adhesive solution and difficulty in coating; excessive dosage will result in a thin film layer, insufficient mechanical strength, and reduced protective capability. Fumed silica should account for 3-5% of the total mass of the protective adhesive. As a functional filler, this addition significantly improves the hardness, wear resistance, and impact resistance of the film, enhancing its ability to resist friction and compression from encapsulated materials. It can also fine-tune the thixotropy of the adhesive solution, further optimizing the coating effect. Insufficient addition results in inadequate reinforcement, making the film layer easily scratched and damaged; excessive addition significantly increases the system viscosity, easily causing particle and agglomeration problems, and also reduces the water solubility of the film, resulting in residue removal.

[0024] For example, sulfonated polyester resin accounts for 45% of the total mass of the protective colloid, diethylene glycol butyl ether accounts for 50% of the total mass of the protective colloid, and fumed silica accounts for 5% of the total mass of the protective colloid.

[0025] Figure 1 This is a flowchart illustrating a method for preparing a protective adhesive according to an embodiment of this disclosure. See also... Figure 1 The method includes the following steps: S11. Add diethylene glycol butyl ether solvent and sulfonated polyester resin to the reaction vessel and dissolve them to form a resin solution.

[0026] S12. Add the diethylene glycol butyl ether solvent and fumed silica to the first dispersion tank to form a dispersion.

[0027] S13. Add the resin solution and the dispersion to the second dispersion tank, and mix and stir to form the protective gel.

[0028] In this embodiment, the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity of the protective adhesive film and its strong adhesion; the diethylene glycol butyl ether optimizes the flowability and coating effect of the protective adhesive; and the fumed silica improves the hardness and scratch resistance of the protective adhesive.

[0029] Figure 2This is a flowchart illustrating another method for preparing a protective adhesive according to an embodiment of this disclosure. See also... Figure 2 The method includes the following steps: S21. Add diethylene glycol butyl ether solvent and sulfonated polyester resin to the reaction vessel and dissolve them to form a resin solution.

[0030] In this embodiment, 70-80% of diethylene glycol butyl ether solvent is added to the reactor and stirred. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total amount of sulfonated polyester resin, to achieve slow addition. The reactor is heated to 60-80°C and then kept warm and stirred for 2-4 hours. The reactor is then allowed to cool naturally to room temperature and left to stand for later use.

[0031] In this implementation, 70-80% of the total amount of diethylene glycol butyl ether solvent is added to the reactor. Most of the solvent is added in advance and a flow system is formed, which can provide sufficient dispersion medium for the resin, reduce the probability of subsequent contact and agglomeration of solid powder, and thus improve the uniformity of the resin solution. The appropriate ratio of diethylene glycol butyl ether solvent ensures both solubility and prevents insufficient strength of the final protective colloid due to excessive amounts of diethylene glycol butyl ether solvent. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total sulfonated polyester resin volume. This small-batch, multi-stage addition method allows the resin to be fully wetted and gradually dissolved by the solvent, avoiding the resin clumping problem caused by adding all at once. The reactor is heated to 60-80℃ and then kept at this temperature with stirring for 2-4 hours. This temperature range effectively improves the solubility of the sulfonated polyester resin and accelerates the dissolution process. Combined with prolonged heating and stirring, the resin can be completely dissolved, forming a transparent and homogeneous resin solution. The reactor is then allowed to cool naturally to room temperature. Slow cooling allows the internal stress of the solution to be gradually released, preventing resin precipitation caused by sudden temperature changes. After cooling, the resin solution tends to be stable, making it less prone to deterioration during storage and use, thus improving the encapsulation yield of the microdisplay.

[0032] For example, 75% of the total amount of diethylene glycol butyl ether solvent is added to the reactor and the diethylene glycol butyl ether solvent is stirred; sulfonated polyester resin is added to the reactor in batches, each time the amount added is 1 / 6 of the total amount of sulfonated polyester resin; the reactor is heated to 70°C and then kept at that temperature and stirred for 3 hours; the reactor is then allowed to cool naturally to room temperature.

[0033] In this embodiment of the present disclosure, the diethylene glycol butyl ether solvent is stirred at a speed of 200-300 rpm.

[0034] For example, the diethylene glycol butyl ether solvent was stirred at a speed of 250 rpm.

[0035] It should be noted that the reaction vessel must be sealed during the dissolution process to prevent the resin solution from evaporating and being lost. The final solid content of the resin solution is approximately 50-55%.

[0036] S22. Diethylene glycol butyl ether solvent and fumed silica are added to the first dispersion tank to form a dispersion.

[0037] In this embodiment, 20-30% of the total amount of diethylene glycol butyl ether solvent is added to a first dispersion tank at a rotation speed of 1000-1500 rpm. Fumed silica is added to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total amount of silica, to achieve slow addition. The rotation speed of the first dispersion tank is increased to 2500-3000 rpm to achieve high-speed dispersion for 30-60 minutes. The rotation speed of the first dispersion tank is then reduced to 250-350 rpm, and the mixture is stirred for 9-11 minutes to defoam, and then allowed to stand for later use.

[0038] In this implementation, 20-30% of the total amount of diethylene glycol butyl ether solvent is added to the first dispersion tank. The first dispersion tank rotates at 1000-1500 rpm. This low-to-medium speed operation allows the solvent to form a stable flow field without violent splashing, creating basic conditions for subsequent feeding and avoiding the introduction of a large number of air bubbles at high speeds. Fumed silica is added to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total silica amount. This small-batch, multiple-feeding method allows the fumed silica to gradually contact the solvent and be fully wetted, significantly reducing the risk of fumed silica ignition due to its high surface activity. To address the clumping and difficulty in dispersing of silica, the speed of the first dispersion tank is increased to 2500-3000 rpm, and dispersion is carried out for 30-60 minutes. This high speed generates strong centrifugal force, effectively breaking down the tiny aggregates of fumed silica, allowing the silica to be completely wetted and forming a uniform thixotropic pre-dispersion. Sufficient dispersion time ensures thorough dispersion. The speed of the first dispersion tank is then reduced to 250-350 rpm, and stirring is carried out for 9-11 minutes. Gentle stirring at low speed removes air bubbles trapped during high-speed dispersion, preventing pinholes and pores after coating, and improving the overall quality of the dispersion.

[0039] For example, take 25% of the total amount of diethylene glycol butyl ether solvent and add it to the first dispersion tank. The rotation speed of the first dispersion tank is 1250 rpm. Add fumed silica to the first dispersion tank in batches, with each addition being 1 / 4 of the total amount of silica. Increase the rotation speed of the first dispersion tank to 2700 rpm and disperse for 40 minutes. Reduce the rotation speed of the first dispersion tank to 300 rpm and stir for 10 minutes.

[0040] It should be noted that the dispersion process temperature should be less than or equal to 40℃ to prevent solvent evaporation; after dispersion, the dispersion can be judged by the scraping method, and the dispersion is qualified if there are no obvious particles.

[0041] S23. Add the resin solution and dispersion to the second dispersion tank and mix and stir to form a protective gel.

[0042] In this embodiment, the resin solution is added to the second dispersion tank and stirred at a speed of 500-800 rpm to achieve medium-speed stirring. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective colloid at 35,000-45,000 cps. The protective colloid is stirred for 1-2 hours to adjust the viscosity.

[0043] In this implementation, the resin solution is added to a second dispersion tank and stirred at a speed of 500-800 rpm. The dispersion is then slowly added to the second dispersion tank. This combination of low-to-medium speed and slow addition prevents filler particles from re-agglomerating and reduces bubble formation, ensuring thorough mixing of the resin solution and dispersion. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective adhesive at 35,000-45,000 cps. Lower viscosity results in an excessively thin protective adhesive, reducing the encapsulation and protection capabilities; higher viscosity leads to poor flowability, making it difficult to evenly cover the display area and causing missed coatings and adhesive buildup. The protective adhesive is stirred for 1-2 hours. Prolonged and uniform stirring thoroughly homogenizes the overall adhesive solution, ensuring consistent coating effects and film quality during mass production.

[0044] For example, the resin solution is added to the second dispersion tank and stirred at a speed of 600 rpm. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to keep the viscosity of the protective colloid constant at 25°C. Using the Brookfield HBDV-Ⅱ test, the viscosity is maintained at 40,000 cps. The protective colloid is stirred for 1.5 hours.

[0045] S24. Grind and filter the protective adhesive.

[0046] In this embodiment, the protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is equal to or less than 5μm; the protective colloid is filtered using a 100-200 mesh nylon filter bag to remove impurities and undispersed particles.

[0047] In this implementation, the protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm, and 5μm, respectively, to make the particle size of the protective colloid equal to or less than 5μm. Gradually reducing the roller gap allows for the gradual application of extrusion and shearing action to the colloid, avoiding component damage caused by single high-pressure grinding, and gradually crushing agglomerated particles such as fumed silica. Multiple grinding processes ensure that the particle size is stable and meets the standard, making the protective colloid more uniform. The protective colloid is filtered using a 100-200 mesh nylon filter bag. This mesh size range can effectively trap large particles that are not thoroughly ground, and the purity of the protective colloid after filtration is greatly improved.

[0048] The phrase "grinding the protective colloid 2-3 times with a three-roll mill with roller gaps of 20μm, 10μm and 5μm in sequence" means that the protective colloid passes through the 20μm roller, 10μm roller and 5μm roller of the mill in sequence, repeating 2-3 times.

[0049] For example, the protective colloid is ground twice using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is 5μm; the protective colloid is then filtered using a 150-mesh nylon filter bag.

[0050] S25. The protective adhesive is tested and stored.

[0051] In this embodiment of the disclosure, the detection of the protective adhesive includes: The first step is to test the viscosity of the protective adhesive.

[0052] In this embodiment of the disclosure, the viscosity test includes: under the condition of a temperature of 25°C, the viscosity of the protective adhesive is 35,000~45,000 cps, the fineness of the protective adhesive is less than or equal to 5μm, and the solid (resin + silica) content of the protective adhesive is 47~53%, which is considered qualified.

[0053] The second step is to conduct an appearance test on the protective adhesive.

[0054] In this embodiment of the disclosure, the appearance test includes: the protective adhesive is transparent and uniform, without particles or sediment.

[0055] In this embodiment of the disclosure, the filtered protective adhesive is sealed and filled, and stored in an environment of -5~5°C to prevent the protective adhesive from evaporating and moisture from entering.

[0056] In this embodiment, the protective adhesive is selected from water-soluble polyester or modified polyvinyl alcohol hydrolysate, with a glass transition temperature greater than or equal to 100°C. It can withstand the high temperature of 120~180°C for mold top encapsulation without cracking, melting, or chemical decomposition. Furthermore, the protective adhesive is insoluble in conventional organic solvents and encapsulation additives, and it hydrolyzes rapidly only at room temperature or in warm water. The hydrolysis products are non-toxic, leave no residue, and do not damage the display pixels or optical microstructure.

[0057] Figure 3 This is a flowchart of a microdisplay packaging method provided in an embodiment of this disclosure. See also... Figure 3 The method includes the following steps: S31. The protective adhesive is applied to the display area of ​​the micro-display screen. The protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica.

[0058] S32. The non-display area of ​​the micro-display screen is encapsulated.

[0059] S33. Immerse the micro-display screen in pure water to remove the protective adhesive.

[0060] In this embodiment, the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity and strong adhesion of the protective adhesive film; the diethylene glycol butyl ether optimizes the flowability and coating effect; and the fumed silica enhances the hardness and scratch resistance of the protective adhesive. Applying the protective adhesive to the display area of ​​the microdisplay screen prevents contact with encapsulation materials, protecting the display area from damage. Encapsulating the microdisplay screen exposes the protective adhesive applied to the display area. Relying on the protective adhesive's isolating and protective function, the overall encapsulation can be completed normally, ensuring a stable device encapsulation structure while protecting the display area. This protective adhesive uses sulfonated polyester resin as the main resin, which does not exhibit irreversible chemical cross-linking, and is combined with a water-oil composite material. The compatible diethylene glycol butyl ether constructs internal water-permeable micropores and weakens the interfacial adhesion between the adhesive film and the device. Furthermore, hydrophilic fumed silica is used to regulate the protective adhesive's properties through reversible hydrogen bonding. Upon contact with water, the hydrogen bonds break, and the resin ionizes and disperses. Therefore, immersing the microdisplay in pure water can remove the protective adhesive. Existing technologies often use hydrophobic crosslinked resins such as epoxy and silicone, combined with hydrophobic additives and fillers, to form a dense and stable three-dimensional network waterproof structure after curing. This requires organic solvents for debonding, but the cured protective adhesive is prone to over-crosslinking, and chemical solvents are insufficient, resulting in residue. Therefore, the microdisplay encapsulation method provided in this application offers a simpler and chemical-free process for removing the protective adhesive, without corroding or damaging the microdisplay and display structure. It is environmentally friendly and highly efficient.

[0061] Figure 4 This is a flowchart of another microdisplay packaging method provided in this disclosure. See also... Figure 4 The method includes the following steps: S41 provides a micro display screen.

[0062] The microdisplay includes a circuit board, a display chip, wires, a reinforcing steel plate, and a connector.

[0063] Figure 5This is a structural schematic diagram of a microdisplay packaging process provided in an embodiment of this disclosure. See also... Figure 5 The microdisplay includes: a circuit board 100, a display chip 101, wires 102, a reinforcing steel plate 103, and a connector 104. The display chip 101 is located on the reinforcing steel plate 103. One end of the circuit board 100 is stacked with one end of the reinforcing steel plate 103. The display chip 101 is electrically connected to the circuit board 100 through wires 102. The connector 104 is integrated on the second end of the circuit board 100. The first end and the second end are opposite ends.

[0064] For example, the microdisplay is a micro light-emitting diode (Micro LED) display.

[0065] The microdisplay includes multiple pixels.

[0066] The display chip 101 includes a complementary metal-oxide-semiconductor (CMOS) board 1011 and a display panel 1012 bonded to the CMOS board 1011.

[0067] like Figure 5 As shown, pads 105 are provided on the display chip 101 and the circuit board 100 respectively, and the two ends of the wire 102 are connected to the pads 105 respectively.

[0068] In this embodiment of the disclosure, the display panel 1012 has a display area 1000.

[0069] In this embodiment of the disclosure, the circuit board 100 is a flexible printed circuit board (FPCB).

[0070] In other embodiments, circuit board 100 may also be other circuit boards, such as ceramic-based circuit boards.

[0071] In this embodiment of the disclosure, the CMOS board 1011 is a micro CMOS chip.

[0072] In this embodiment of the disclosure, the conductor 102 is a gold wire.

[0073] In other embodiments, wire 102 may also be other wires, such as copper wire.

[0074] S42. Preprocess the display area of ​​the micro-display screen.

[0075] The display area of ​​the micro-display screen is also known as the display surface or display area (AA area) of the micro-display screen.

[0076] For example, step S42 may include: The first step involves sequentially cleaning the surface of the micro-display screen's display area using plasma cleaning and deionized water cleaning processes.

[0077] In this implementation method, plasma cleaning and deionized water cleaning processes are used sequentially to clean the surface of the micro-display area, which can remove dust, oil, and organic residues from the surface of the micro-display area.

[0078] The second step is to dry the microdisplay screen with nitrogen or at a low temperature below 80°C.

[0079] In this implementation, drying the microdisplay with nitrogen or at a low temperature below 80°C ensures that the surface of the display area is free of impurities and moisture, thus improving the adhesion of subsequent coatings.

[0080] For example, the microdisplay is dried by blowing nitrogen gas.

[0081] S43. Prepare a protective colloid. The protective colloid is made of a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica.

[0082] Table 1 below shows the material pretreatment steps and objectives of the protective adhesive in this embodiment. As can be seen from Table 1, sulfonated polyester resin accounts for 44-48% of the total protective adhesive volume. The moisture content of the sulfonated polyester resin is less than or equal to 0.3%, and the particle size of the sulfonated polyester resin is less than or equal to 10 mm. The purpose is to accelerate the dissolution rate and avoid moisture affecting film formation. Diethylene glycol butyl ether accounts for 48-52% of the total protective adhesive volume. Diethylene glycol butyl ether needs to be filtered to remove mechanical impurities. The moisture content of diethylene glycol butyl ether is less than or equal to 0.1%. The purpose is to ensure solvent purity and prevent resin hydrolysis. Fumed silica accounts for 3-5% of the total protective adhesive volume. Hydrophobic fumed silica is used and dried at 100°C for 2 hours to remove adsorbed water. The purpose is to prevent silica agglomeration and ensure thixotropic effect.

[0083] Table 1

[0084] For example, step S43 may include: The first step involves adding diethylene glycol butyl ether solvent and sulfonated polyester resin to a reaction vessel and dissolving them to form a resin solution.

[0085] In this embodiment, 70-80% of diethylene glycol butyl ether solvent is added to the reactor and stirred. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total amount of sulfonated polyester resin, to achieve slow addition. The reactor is heated to 60-80°C and then kept warm and stirred for 2-4 hours. The reactor is then allowed to cool naturally to room temperature and left to stand for later use.

[0086] In this implementation, 70-80% of the total amount of diethylene glycol butyl ether solvent is added to the reactor. Most of the solvent is added in advance and a flow system is formed, which can provide sufficient dispersion medium for the resin, reduce the probability of subsequent contact and agglomeration of solid powder, and thus improve the uniformity of the resin solution. The appropriate ratio of diethylene glycol butyl ether solvent ensures both solubility and prevents insufficient strength of the final protective colloid due to excessive amounts of diethylene glycol butyl ether solvent. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total sulfonated polyester resin volume. This small-batch, multi-stage addition method allows the resin to be fully wetted and gradually dissolved by the solvent, avoiding the resin clumping problem caused by adding all at once. The reactor is heated to 60-80℃ and then kept at this temperature with stirring for 2-4 hours. This temperature range effectively improves the solubility of the sulfonated polyester resin and accelerates the dissolution process. Combined with prolonged heating and stirring, the resin can be completely dissolved, forming a transparent and homogeneous resin solution. The reactor is then allowed to cool naturally to room temperature. Slow cooling allows for the gradual release of internal stress in the solution, preventing resin precipitation caused by sudden temperature changes. After cooling, the resin solution tends to be stable, making it less prone to deterioration during storage and use, thus improving the encapsulation yield of the microdisplay.

[0087] For example, 75% of the total amount of diethylene glycol butyl ether solvent is added to the reactor and the diethylene glycol butyl ether solvent is stirred; sulfonated polyester resin is added to the reactor in batches, each time the amount added is 1 / 6 of the total amount of sulfonated polyester resin; the reactor is heated to 70°C and then kept at that temperature and stirred for 3 hours; the reactor is then allowed to cool naturally to room temperature.

[0088] In this embodiment of the present disclosure, the diethylene glycol butyl ether solvent is stirred at a speed of 200-300 rpm.

[0089] For example, the diethylene glycol butyl ether solvent was stirred at a speed of 250 rpm.

[0090] It should be noted that the reaction vessel must be sealed during the dissolution process to prevent the resin solution from evaporating and being lost. The final solid content of the resin solution is approximately 50-55%.

[0091] The second step involves adding diethylene glycol butyl ether solvent and fumed silica to the first dispersion tank to form a dispersion.

[0092] In this embodiment, 20-30% of the total amount of diethylene glycol butyl ether solvent is added to a first dispersion tank at a rotation speed of 1000-1500 rpm. Fumed silica is added to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total amount of silica, to achieve slow addition. The rotation speed of the first dispersion tank is increased to 2500-3000 rpm to achieve high-speed dispersion for 30-60 minutes. The rotation speed of the first dispersion tank is then reduced to 250-350 rpm, and the mixture is stirred for 9-11 minutes to defoam, and then allowed to stand for later use.

[0093] In this implementation, 20-30% of the total amount of diethylene glycol butyl ether solvent is added to the first dispersion tank. The first dispersion tank rotates at 1000-1500 rpm. This low-to-medium speed operation allows the solvent to form a stable flow field without violent splashing, creating basic conditions for subsequent feeding and avoiding the introduction of a large number of air bubbles at high speeds. Fumed silica is added to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total silica amount. This small-batch, multiple-feeding method allows the fumed silica to gradually contact the solvent and be fully wetted, significantly reducing the risk of fumed silica ignition due to its high surface activity. To address the clumping and difficulty in dispersing of silica, the speed of the first dispersion tank is increased to 2500-3000 rpm, and dispersion is carried out for 30-60 minutes. This high speed generates strong centrifugal force, effectively breaking down the tiny aggregates of fumed silica, allowing the silica to be completely wetted and forming a uniform thixotropic pre-dispersion. Sufficient dispersion time ensures thorough dispersion. The speed of the first dispersion tank is then reduced to 250-350 rpm, and stirring is carried out for 9-11 minutes. Gentle stirring at low speed removes air bubbles trapped during high-speed dispersion, preventing pinholes and pores after coating, and improving the overall quality of the dispersion.

[0094] For example, take 25% of the total amount of diethylene glycol butyl ether solvent and add it to the first dispersion tank. The rotation speed of the first dispersion tank is 1250 rpm. Add fumed silica to the first dispersion tank in batches, with each addition being 1 / 4 of the total amount of silica. Increase the rotation speed of the first dispersion tank to 2700 rpm and disperse for 40 minutes. Reduce the rotation speed of the first dispersion tank to 300 rpm and stir for 10 minutes.

[0095] It should be noted that the dispersion process temperature should be less than or equal to 40℃ to prevent solvent evaporation; after dispersion, the dispersion can be judged by the scraping method, and the dispersion is qualified if there are no obvious particles.

[0096] The third step is to add the resin solution and dispersion to the second dispersion tank and mix them to form a protective gel.

[0097] In this embodiment, the resin solution is added to the second dispersion tank and stirred at a speed of 500-800 rpm to achieve medium-speed stirring. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective colloid at 35,000-45,000 cps. The protective colloid is stirred for 1-2 hours to adjust the viscosity.

[0098] In this implementation, the resin solution is added to a second dispersion tank and stirred at a speed of 500-800 rpm. The dispersion is then slowly added to the second dispersion tank. This combination of low-to-medium speed and slow addition prevents filler particles from re-agglomerating and reduces bubble formation, ensuring thorough mixing of the resin solution and dispersion. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective adhesive at 35,000-45,000 cps. Lower viscosity results in an excessively thin protective adhesive, reducing the encapsulation and protection capabilities; higher viscosity leads to poor flowability, making it difficult to evenly cover the display area and causing missed coatings and adhesive buildup. The protective adhesive is stirred for 1-2 hours. Prolonged and uniform stirring thoroughly homogenizes the overall adhesive solution, ensuring consistent coating effects and film quality during mass production.

[0099] For example, the resin solution is added to the second dispersion tank and stirred at a speed of 600 rpm. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to keep the viscosity of the protective colloid constant at 25°C. Using the Brookfield HBDV-Ⅱ test, the viscosity is maintained at 40,000 cps. The protective colloid is stirred for 1.5 hours.

[0100] The fourth step is to grind and filter the protective adhesive.

[0101] In this embodiment, the protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is equal to or less than 5μm; the protective colloid is filtered using a 100-200 mesh nylon filter bag to remove impurities and undispersed particles.

[0102] In this implementation, the protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm, and 5μm, respectively, to make the particle size of the protective colloid equal to or less than 5μm. Gradually reducing the roller gap allows for the gradual application of extrusion and shearing action to the colloid, avoiding component damage caused by single high-pressure grinding, and gradually crushing agglomerated particles such as fumed silica. Multiple grinding processes ensure that the particle size is stable and meets the standard, making the protective colloid more uniform. The protective colloid is filtered using a 100-200 mesh nylon filter bag. This mesh size range can effectively trap large particles that are not thoroughly ground, and the purity of the protective colloid after filtration is greatly improved.

[0103] The phrase "grinding the protective colloid 2-3 times with a three-roll mill with roller gaps of 20μm, 10μm and 5μm in sequence" means that the protective colloid passes through the 20μm roller, 10μm roller and 5μm roller of the mill in sequence, repeating 2-3 times.

[0104] For example, the protective colloid is ground twice using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is 5μm; the protective colloid is then filtered using a 150-mesh nylon filter bag.

[0105] The fifth step is to test and store the protective adhesive.

[0106] In this embodiment of the disclosure, the detection of the protective adhesive includes: The first step is to test the viscosity of the protective adhesive.

[0107] In this embodiment of the disclosure, the viscosity test includes: under the condition of a temperature of 25°C, the viscosity of the protective adhesive is 35,000~45,000 cps, the fineness of the protective adhesive is less than or equal to 5μm, and the solid (resin + silica) content of the protective adhesive is 47~53%, which is considered qualified.

[0108] The second step is to conduct an appearance test on the protective adhesive.

[0109] In this embodiment of the disclosure, the appearance test includes: the protective adhesive is transparent and uniform, without particles or sediment.

[0110] In this embodiment of the disclosure, the filtered protective adhesive is sealed and filled, and stored in an environment of -5~5°C to prevent the protective adhesive from evaporating and moisture from entering.

[0111] In this embodiment, the protective adhesive is selected from water-soluble polyester or modified polyvinyl alcohol hydrolysate, with a glass transition temperature greater than or equal to 100°C. It can withstand the high temperature of 120~180°C for mold top encapsulation without cracking, melting, or chemical decomposition. Furthermore, the protective adhesive is insoluble in conventional organic solvents and encapsulation additives, and it hydrolyzes rapidly only at room temperature or in warm water. The hydrolysis products are non-toxic, leave no residue, and do not damage the display pixels or optical microstructure.

[0112] S44. Apply protective adhesive to the display area of ​​the microdisplay screen.

[0113] For example, step S44 may include: The first step involves applying a protective adhesive to the display area of ​​the micro-display screen using a fully automated precision dispensing or piezoelectric valve spraying process. The thickness of the protective adhesive is 5~20μm, the uniformity of the protective adhesive is less than or equal to 2μm, and the edge of the coating extends less than or equal to 0.1mm beyond the boundary of the display area.

[0114] In this implementation, a fully automated precision dispensing or piezoelectric valve spraying process is adopted. The automated equipment dispenses adhesive with precision and operates stably, eliminating human error compared to manual coating and adapting to large-scale mass production. Piezoelectric valve spraying provides excellent atomization and high dispensing control accuracy, adapting to different forms of micro-displays and significantly improving coating efficiency and consistency. The protective adhesive thickness is 5~20μm. Insufficient thickness results in a thin protective adhesive that is prone to breakage. Excessive thickness not only increases raw material costs but also makes curing and adhesive removal more difficult, easily leaving adhesive residues that contaminate the device. Furthermore, the release film can only absorb a thickness of less than or equal to 30μm during molding. If the protective adhesive is too thick, there is a risk of adhesive overflow into the display area during molding. The uniformity of the protective adhesive is less than or equal to 2μm, with minimal thickness deviation. This prevents protective gaps due to local thinness or internal stress due to local thickness, ensuring stable protection throughout the encapsulation process. The coating edge extends less than or equal to 0.1mm beyond the display area boundary, completely covering the edge of the display area and eliminating blind spots in protection.

[0115] The phrase "the coating edge extends beyond the display area boundary" means that the coating completely covers the display area and extends beyond the edge of the display area.

[0116] For example, a fully automated precision dispensing or piezoelectric valve spraying process is used to apply protective adhesive to the display area of ​​the microdisplay screen. The protective adhesive has a thickness of 10 μm, a uniformity of 2 μm, and the coating edge extends 0.1 mm beyond the boundary of the display area.

[0117] In other embodiments, the protective adhesive can also be applied to the display area of ​​the microdisplay using screen printing or doctor blade coating.

[0118] The second step is to place the micro-display screen coated with protective adhesive in a constant temperature chamber and cure it for 10 to 30 minutes at a temperature of 100 to 150°C.

[0119] In this implementation, a temperature of 100-150℃ rapidly removes residual solvent from the adhesive layer, promoting the formation of a stable solid film from the sulfonated polyester resin. This temperature range is gentle, preventing burns or aging of the light-emitting chip and surrounding structures, balancing curing effectiveness with device safety. Lower temperatures result in incomplete solvent evaporation, leading to a softer, more easily deformed film. Excessively high temperatures can cause thermal damage to the device. Curing for 10-30 minutes allows the protective adhesive coating to transform from a liquid to a solid state, forming a high-temperature resistant, impact-resistant, and highly dense physical protective film that can withstand the high-temperature environment of mold top encapsulation and does not chemically react with the molding compound.

[0120] For example, the microdisplay screen coated with protective adhesive was placed in a constant temperature chamber and cured for 20 minutes at a temperature of 125°C.

[0121] exist Figure 5In the structure shown, protective adhesive is applied to the display area 1000 of the microdisplay, covering the entire display area 1000.

[0122] S45. Perform encapsulation processing on the micro-display screen.

[0123] For example, step S45 may include: The first step is to encapsulate the micro-display using a transfer molding process. The encapsulation temperature is 120~180℃, the encapsulation pressure is 5~15MPa, and the initial curing time is 30~90 seconds.

[0124] For example, the encapsulation temperature is 150°C, the encapsulation pressure is 10 MPa, and the initial curing time is 50 seconds.

[0125] The second step is to bake the epoxy encapsulant at a temperature of 160~180℃ for 4~5 hours to allow it to fully cure.

[0126] For example, baking at 170°C for 4.5 hours.

[0127] In this implementation, the protective adhesive layer completely blocks the contamination and erosion of the display area by encapsulation particles, additives, and adhesive debris, improving the yield rate by 25%.

[0128] Figure 6 This is a structural schematic diagram of another microdisplay packaging process provided in this embodiment of the disclosure. Figure 7 yes Figure 6 The diagram shows the back structure of the microdisplay. Figure 8 yes Figure 6 Cross-sectional view at point A-A' Figure 9 yes Figure 6 Cross-sectional view at point B-B'. See also Figures 6 to 9 ,exist Figure 5 Based on this, an encapsulation layer 106 is fabricated, which covers the display chip 101 and exposes the protective adhesive 2000. The encapsulation layer 106 also covers the wires 102.

[0129] In addition, connectors 104 are arranged on both sides of circuit board 100.

[0130] In this embodiment of the disclosure, the purpose of packaging is to protect the CMOS chip and wires, as well as to provide support and protection for the subsequent assembly of the optical engine lens.

[0131] S46. Immerse the micro-display screen in pure water to remove the protective adhesive.

[0132] In this step, the aforementioned protective adhesive is completely removed.

[0133] For example, step S46 may include: ultrasonically immersing the microdisplay screen for 15 to 60 minutes at a temperature of 50 to 80°C, an ultrasonic power of 20 to 50W, and an ultrasonic frequency of 20 to 40kHz to remove the protective adhesive.

[0134] In this implementation, sulfonated polyester resin is used as the main resin for the protective adhesive, eliminating irreversible chemical cross-linking. It is combined with diethylene glycol butyl ether, which is compatible with both water and oil, to construct internal water-permeable micropores and weaken the interfacial adhesion between the adhesive film and the device. Furthermore, hydrophilic fumed silica is added to regulate the protective adhesive's properties through reversible hydrogen bonding. Upon contact with water, the hydrogen bonds break, and the resin ionizes and disperses. Therefore, the protective adhesive rapidly undergoes hydrolysis and swelling reactions upon contact with pure water, causing the protective adhesive coating to spontaneously dissolve and detach from the display area surface. The pure water immersion process can be supplemented with low-frequency ultrasonic vibration to further shorten the debonding time, improve the thoroughness of adhesive removal in complex microstructure areas, and ensure that the ultrasonic parameters do not damage the microdisplay screen or leads.

[0135] For example, ultrasonic immersion was performed for 40 minutes at a temperature of 60°C, an ultrasonic power of 30W, and an ultrasonic frequency of 30kHz.

[0136] S47. Clean and dry the micro display screen.

[0137] For example, step S47 may include: The first step is to rinse the micro-display screen with deionized water spray.

[0138] In this implementation, deionized water is used to spray and rinse the microdisplay screen, which can remove trace amounts of colloidal residue from the microdisplay screen.

[0139] The second step is to dry the product by blowing it with nitrogen or by drying it at a low temperature of 50~70℃.

[0140] For example, drying is achieved by blowing with nitrogen gas.

[0141] In this embodiment of the disclosure, the microdisplay can be applied to augmented reality (AR) devices.

[0142] In this embodiment, the complex process of basic adhesive removal is eliminated, and degumming can be completed simply by soaking in pure water, resulting in high production efficiency and suitability for automated mass production. The raw material cost of the protective adhesive is lower than that of other protective coatings, eliminating the need for recycling and solvent loss, significantly reducing equipment energy consumption and waste liquid treatment costs, and resulting in low overall process costs. No harmful solvents are used throughout the process, and no volatile waste gas or toxic waste liquid is generated. The protective adhesive and hydrolysis products are non-toxic and harmless, complying with national environmental protection production standards, ensuring a safe working environment. The protective adhesive has strong density, completely blocking contamination from encapsulation particles. Pure water degumming is thorough, leaving no adhesive residue or chemical corrosion, and does not damage the optical performance of the display area. The encapsulation yield is 20% to 30% higher than that provided by related technologies. The parameters for protective adhesive application, curing, and degumming are easy to control, with low requirements for operating environment temperature and humidity, strong process stability, and adaptability to the mold top encapsulation needs of AR micro-displays of different sizes and types.

[0143] In this embodiment of the disclosure, a protective adhesive is provided, the material of which is a mixture of sulfonated polyester resin, diethylene glycol butyl ether and fumed silica.

[0144] In this embodiment, the protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The sulfonated polyester resin ensures the integrity and strong adhesion of the protective adhesive film; the diethylene glycol butyl ether optimizes the flowability and coating effect; and the fumed silica improves the hardness and scratch resistance. Applying the protective adhesive to the display area of ​​the microdisplay screen prevents contact with encapsulation materials, protecting the display area from damage. Encapsulating the microdisplay screen exposes the protective adhesive applied to the display area. Relying on the protective effect of the adhesive, the overall encapsulation can be completed normally, ensuring a stable device encapsulation structure while protecting the display area. This protective adhesive uses sulfonated polyester resin as the main resin, which does not have irreversible chemical crosslinking, and is combined with a water- and oil-compatible diethylene glycol butyl ether. Ethylene glycol butyl ether constructs internal water-permeable micropores and weakens the interfacial adhesion between the adhesive film and the device. Hydrophilic fumed silica is then used to regulate the protective adhesive's properties through reversible hydrogen bonding. Upon contact with water, the hydrogen bonds break, and the resin ionizes and disperses. Therefore, immersing the microdisplay in pure water can remove the protective adhesive. Existing technologies often use hydrophobic crosslinking resins such as epoxy and silicone, combined with hydrophobic additives and fillers, to form a dense and stable three-dimensional network waterproof structure after curing. Pure water cannot penetrate and decompose this structure, typically requiring organic solvents for debonding. However, the cured protective adhesive is prone to over-crosslinking, and chemical solvents lack sufficient dissolving power, resulting in adhesive residue. Therefore, the microdisplay encapsulation method provided in this application offers a simpler and chemical-free process for removing the protective adhesive, without corroding or damaging the microdisplay and display structure. It is environmentally friendly and highly efficient.

[0145] In the embodiments disclosed herein, sulfonated polyester resin accounts for 44-48% of the total mass of the protective colloid, diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective colloid, and fumed silica accounts for 3-5% of the total mass of the protective colloid.

[0146] In this implementation, sulfonated polyester resin accounts for 44-48% of the total mass of the protective adhesive. As the main body for film formation, this proportion can form a continuous and complete protective film layer, which is firmly bonded to the surface of the microdisplay screen and is not prone to peeling or displacement during encapsulation. At the same time, it retains the hydrophilic properties brought by the sulfonated groups, ensuring that it can be dissolved and peeled off by immersion in pure water. Too low a proportion will lead to discontinuous film formation and protective failure; too high a proportion will result in high adhesive viscosity, poor coating leveling, and a decrease in water solubility. Diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective adhesive. As a solvent and rheology modifier, this ratio can precisely control the overall viscosity and evaporation rate of the protective adhesive. It has excellent leveling properties during coating and can evenly cover the display area, avoiding uneven thickness and missed coating defects. At the same time, it improves the resin dispersion and prevents the system from layering and sedimentation. Insufficient dosage can lead to a thick adhesive solution and difficulty in coating; excessive dosage will result in a thin film layer, insufficient mechanical strength, and reduced protective capability. Fumed silica should account for 3-5% of the total mass of the protective adhesive. As a functional filler, this addition significantly improves the hardness, wear resistance, and impact resistance of the film, enhancing its ability to resist friction and compression from encapsulated materials. It can also fine-tune the thixotropy of the adhesive solution, further optimizing the coating effect. Insufficient addition results in inadequate reinforcement, making the film layer easily scratched and damaged; excessive addition significantly increases the system viscosity, easily causing particle and agglomeration problems, and also reduces the water solubility of the film, resulting in residue removal.

[0147] For example, sulfonated polyester resin accounts for 45% of the total mass of the protective colloid, diethylene glycol butyl ether accounts for 50% of the total mass of the protective colloid, and fumed silica accounts for 5% of the total mass of the protective colloid.

[0148] The above description is merely an optional embodiment of this disclosure and is not intended to limit this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.

Claims

1. A protective adhesive, characterized in that, The protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica.

2. The protective adhesive according to claim 1, characterized in that, The sulfonated polyester resin accounts for 44-48% of the total mass of the protective colloid, the diethylene glycol butyl ether accounts for 48-52% of the total mass of the protective colloid, and the fumed silica accounts for 3-5% of the total mass of the protective colloid.

3. A method for preparing a protective adhesive, characterized in that, The method for preparing the protective adhesive includes: Diethylene glycol butyl ether solvent and sulfonated polyester resin are added to the reaction vessel and dissolved to form a resin solution; The diethylene glycol butyl ether solvent and fumed silica are added to the first dispersion tank to form a dispersion. The resin solution and the dispersion are added to a second dispersion tank and mixed and stirred to form the protective colloid.

4. The method for preparing the protective adhesive according to claim 3, characterized in that, The diethylene glycol butyl ether solvent and sulfonated polyester resin are added to a reaction vessel and dissolved to form a resin solution, comprising: Add 70-80% of the total amount of diethylene glycol butyl ether solvent to the reaction vessel and stir the diethylene glycol butyl ether solvent. Sulfonated polyester resin is added to the reactor in batches, with each addition not exceeding 1 / 5 of the total amount of sulfonated polyester resin. The reaction vessel is heated to 60-80°C, and then kept at that temperature and stirred for 2-4 hours. The reactor was allowed to cool naturally to room temperature.

5. The method for preparing the protective adhesive according to claim 3, characterized in that, The diethylene glycol butyl ether solvent and the fumed silica are added to the first dispersion tank to form a dispersion comprising: Take 20-30% of the total amount of diethylene glycol butyl ether solvent and add it to the first dispersion tank. The rotation speed of the first dispersion tank is 1000-1500 rpm. Add fumed silica to the first dispersion tank in batches, with each addition being less than or equal to 1 / 3 of the total amount of silica. Increase the rotation speed of the first dispersion cylinder to 2500~3000 rpm and disperse for 30~60 minutes; Reduce the rotation speed of the first dispersion tank to 250-350 rpm and stir for 9-11 minutes.

6. The method for preparing the protective adhesive according to claim 3, characterized in that, The resin solution and the dispersion are added to a second dispersion tank and mixed and stirred to form the protective colloid, comprising: The resin solution is added to the second dispersion tank, and the resin solution is stirred at a speed of 500~800 rpm. The dispersion is then slowly added to the second dispersion tank. Diethylene glycol butyl ether is added to the second dispersion tank to control the viscosity of the protective adhesive at 35,000 to 45,000 cps; Stir the protective adhesive for 1-2 hours.

7. A microdisplay packaging method, characterized in that, The microdisplay packaging method includes: A protective adhesive is applied to the display area of ​​the microdisplay screen. The protective adhesive is a mixture of sulfonated polyester resin, diethylene glycol butyl ether, and fumed silica. The non-display area of ​​the micro-display screen is encapsulated. The microdisplay screen is immersed in pure water to remove the protective adhesive.

8. The microdisplay packaging method according to claim 7, characterized in that, Before applying the protective adhesive to the display area of ​​the microdisplay, the method further includes: The protective colloid is ground 2-3 times using a three-roll mill with roller gaps of 20μm, 10μm and 5μm respectively, so that the particle size of the protective colloid is equal to or less than 5μm; the protective colloid is then filtered using a 100-200 mesh nylon filter bag.

9. The microdisplay packaging method according to claim 7 or 8, characterized in that, Applying a protective adhesive to the display area of ​​the microdisplay includes: The protective adhesive is applied to the display area of ​​the microdisplay using a fully automated precision dispensing or piezoelectric valve spraying process. The thickness of the protective adhesive is 5~20μm, the uniformity of the protective adhesive is less than or equal to 2μm, and the edge of the protective adhesive extends less than or equal to 0.1mm beyond the boundary of the display area of ​​the microdisplay. The microdisplay screen coated with the protective adhesive is placed in a constant temperature chamber and cured for 10 to 30 minutes at a temperature of 100 to 150°C.

10. The microdisplay packaging method according to claim 7 or 8, characterized in that, Immersing the microdisplay screen in pure water to remove the protective adhesive includes: The microdisplay screen is ultrasonically immersed for 15-60 minutes at a temperature of 50-80℃, an ultrasonic power of 20-50W, and an ultrasonic frequency of 20-40kHz to remove the protective adhesive.