A water-based anti-slip and wear-resistant colored pavement coating for sidewalks and its preparation method

By combining hydroxypropyl-modified waterborne polyurethane resin with composite ion-exchange modified montmorillonite, a strong cross-linked network is constructed, which solves the problems of difficulty in achieving both anti-slip and wear resistance and insufficient weather resistance in waterborne walkway coatings. This results in a coating effect with high anti-slip, high wear resistance and long-lasting weather resistance, suitable for municipal walkways and scenic greenway projects.

CN123107520APending Publication Date: 2026-11-17GUANGDONG WINDBELL TREE MATERIAL TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611618596.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water-based walkway coatings struggle to balance anti-slip and wear-resistant properties, lack weather resistance, are prone to aggregate detachment, and are susceptible to blistering and pinhole formation, making it difficult to meet the requirements for long-term safety and durability.

Method used

A strong cross-linked network was constructed by using hydroxypropyl-modified waterborne polyurethane resin and composite ion-exchange modified montmorillonite. Combined with compound functional additives and graded anti-slip aggregates, a resin-nanofiller integrated structure was formed, which improved the cross-linking density and mechanical strength of the coating and enhanced its wear resistance and weather resistance.

Benefits of technology

It significantly improves the anti-slip, wear-resistant and weather-resistant properties of the coating, avoids coating cracking, particle loss and shrinkage defects, adapts to the thermal expansion and contraction deformation of the trail, and is suitable for large-scale engineering applications of municipal trails and scenic greenways.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107520A_ABST
    Figure CN123107520A_ABST
Patent Text Reader

Abstract

This invention relates to the field of coating technology, specifically to a water-based anti-slip and wear-resistant colored pavement coating for sidewalks and its preparation method. It consists of two components, A and B, including: Component A: hydroxypropyl-modified waterborne polyurethane resin, deionized water, compounded film-forming aids, defoamer, dispersant, composite pigments and fillers, compounded defoamer, leveling agent, composite ion-exchange modified montmorillonite, associative polyurethane thickener, and nonionic wetting agent; Component B: curing agent and PMA solvent; Construction additives: 80-120 mesh corundum or fused silica anti-slip aggregate. The coating of this invention possesses both high flexibility and high hardness, adapting to the thermal expansion and contraction deformation of sidewalks, exhibiting strong crack resistance, and showing no cracking or particle shedding even after high-frequency foot traffic. The two-component system has a moderate curing speed, is easy to apply, and can be directly coated onto substrates such as concrete and asphalt without complex pretreatment, making it suitable for large-scale engineering applications such as municipal sidewalks, scenic greenways, and community slow-traffic systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, specifically to a water-based anti-slip and wear-resistant colored pavement coating for sidewalks and its preparation method. Background Technology

[0002] With the rapid development of urban slow-traffic systems, scenic walkways, and municipal colored paving, water-based colored pavement coatings are gradually replacing traditional oil-based coatings and colored asphalt, becoming the mainstream material for walkway paving due to their advantages such as environmental friendliness, low VOC content, convenient construction, and adjustable colors. However, in practical applications, existing water-based pavement coatings still have problems such as difficulty in achieving both anti-slip and wear resistance, insufficient weather resistance, easy aggregate detachment, and easy blistering and pinhole formation in the coating. Especially in wet and slippery environments such as rain and snow, high-frequency pedestrian traffic, and long-term UV aging, they are prone to defects such as rapid decrease in the coefficient of friction, wear and tear, fading and powdering, cracking and peeling, making it difficult to meet the long-term safety and durability requirements of walkways.

[0003] While existing technologies have improved water-based pavement coatings, they still have significant limitations: CN116445048A discloses a single-component, fast-drying, colored anti-slip water-based coating, which focuses on solving the problem of thick coatings drying only on the surface and not in the interior. It improves the drying rate by optimizing the resin emulsification system, but it does not build a strong cross-linked network between the resin and filler. The adhesion between the aggregate and the matrix interface is weak, and the particles are prone to falling off after long-term wear. Furthermore, it does not have a structural design for wet anti-slip, and its anti-slip stability is poor in rain and snow environments.

[0004] CN202511776135.1 discloses a waterborne polyurethane asphalt colored pavement protective coating, which uses ion-crosslinked waterborne polyurethane asphalt emulsion to improve adhesion and wear resistance. However, the asphalt component is susceptible to UV aging and degradation, resulting in insufficient long-term weather resistance. Furthermore, the absence of a nano-reinforcing phase limits the coating's hardness and anti-aging properties, making it unsuitable for long-term outdoor use.

[0005] CN114106677A discloses a waterborne coating of polyurethane resin modified with hydroxypropyl distarch phosphate. The hydroxypropyl modification improves the compatibility and stability of the resin, but it does not have a special additive system designed for road coatings. The defoaming, leveling and wetting properties are insufficient, and bubbles and pinholes are easily generated during construction, which affects the smoothness and anti-slip effect of the coating.

[0006] In summary, current water-based walkway coatings generally suffer from core problems such as low cross-linking degree of resin matrix, lack of nano-reinforced fillers, weak aggregate-matrix interface bonding, and poor compatibility of additive systems, making it impossible to simultaneously achieve the comprehensive requirements of high anti-slip, high wear resistance, high weather resistance, and construction stability.

[0007] Therefore, developing a water-based anti-slip and wear-resistant colored pavement coating for sidewalks that combines excellent anti-slip and wear-resistant properties, long-lasting weather resistance, and good workability has significant engineering application value. Summary of the Invention

[0008] The purpose of this invention is to provide a water-based anti-slip and wear-resistant colored pavement coating for sidewalks and its preparation method.

[0009] To achieve the above objectives, the present invention provides the following technical solution: A water-based, anti-slip, and wear-resistant colored pavement coating for sidewalks, composed of two components, A and B, in parts by weight: Component A: 58-62 parts of hydroxypropyl-modified waterborne polyurethane resin, 7.5-8.5 parts of deionized water, 4.5-5.5 parts of compounded film-forming aid, 0.15-0.25 parts of defoamer, 2.0-2.8 parts of dispersant, 16-21 parts of composite pigments and fillers, 0.3-0.5 parts of compounded defoamer, 0.45-0.55 parts of leveling agent, 1.5-2.2 parts of composite ion-exchange modified montmorillonite, 0.25-0.35 parts of associative polyurethane thickener, and 0.15-0.25 parts of nonionic wetting agent; Component B: 21-24 parts curing agent, 7.2-7.8 parts PMA solvent with moisture content <500ppm; Add the following during construction: 8-12 parts of 80-120 mesh corundum or fused silica anti-slip aggregate.

[0010] As a further technical solution, the preparation method of the composite ion-exchange modified montmorillonite includes: (1) Purification: Natural sodium-based montmorillonite was prepared into a 4wt% aqueous suspension, mechanically stirred for 12h and allowed to settle for 36h to remove coarse impurities; the upper colloid was centrifuged at 8000rpm×15min, vacuum dried at 60℃ for 24h, and air-jet pulverized to 30-40nm to obtain high-purity montmorillonite. (2) Composite ion gradient exchange: High-purity montmorillonite was added to the composite exchange solution at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. (3) Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. (4) Silane directional grafting: The intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 was added dropwise, accounting for 12% of the mass of montmorillonite; refluxed at 80℃ for 2h, and centrifuged and dried to obtain silane-modified montmorillonite; (5) In-situ anchoring of polyurethane: Silane-modified montmorillonite is dispersed in anhydrous acetone to prepare a 10wt% dispersion; polyurethane prepolymer with molecular weight of 800-1200 and NCO content of 6-8wt% is added; pre-react at 40℃ for 30min, and then heated to 70℃ for 1h; acetone is removed under reduced pressure, vacuum dried at 60℃, and ground to obtain modified montmorillonite.

[0011] As a further technical solution, the composite exchange solution in step (2) is a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2.

[0012] As a further technical solution, in step (5), the mass of the polyurethane prepolymer is 8-12% of the silane-modified montmorillonite, and the NCO / amino molar ratio is controlled to be 1.01–1.03.

[0013] As a further technical solution, the composite pigment and filler is made by mixing weather-resistant iron oxide pigment or chrome green with titanium dioxide at a mass ratio of 1:3.8-4.2; the prepared pigment paste has a solid content of ≥62wt% and a pigment fineness of ≤18μm.

[0014] As a further technical solution, the compound film-forming aid is DPnB:DPM mass ratio = 1:1.4-1.6.

[0015] As a further technical solution, the hydroxypropyl-modified waterborne polyurethane resin is an aliphatic anionic waterborne polyurethane with a hydroxypropyl grafting rate of 15-20 mol%, a hydroxyl value of 55-65 mgKOH / g, a solid content of 44-46 wt%, a glass transition temperature (Tg) of -20 to -10 °C, and a molecular chain containing hydrophilic carboxyl groups that can covalently bond with the amino groups on the modified montmorillonite surface.

[0016] As a further technical solution, the compound defoamer is a defoamer composed of Surfynol MD20 and Surfynol 104E in a mass ratio of 1:1.5 to 2.5; it has both continuous foam suppression and rapid foam breaking functions, which can avoid pinhole defects.

[0017] As a further technical solution, the nonionic wetting agent is Surfynol 104PA, a low-foaming acetylene glycol wetting agent.

[0018] The preparation method of water-based anti-slip and wear-resistant colored pavement coating for sidewalks includes the following complete steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the method described above, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor according to the ratio; stir at 800-1000 rpm for 15 minutes until the system is uniform and free of bubbles. S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2200-2500 rpm for 15 min; transfer to a horizontal sand mill, grind with 0.8-1.2 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1000-1200 rpm for 20 min until there is no agglomeration and the particle size is uniform; S5A component main synthesis: Hydroxypropyl modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added in sequence; dispersed at 1000 rpm for 30 min; S6 viscosity control: Slowly add associative polyurethane thickener at a dropping rate ≤ 0.1 parts / min, adjust the viscosity to 85-90 KU; maintain pH 7.5-8.5, stabilize at 1000 rpm for 30 min; S7 Filter Packaging Component A: Filtered with a 200-mesh precision filter to remove impurities and gel, then sealed in packaging; S8B formulation: Mix Bayhydur 304 curing agent with PMA solvent with a moisture content of <500ppm; stir at 1000rpm for 15min, filter through a 200-mesh filter, and seal in a moisture-proof package; S9 on-site mixing construction: Before construction, measure according to the mass ratio of A:B=100:30; add 80-120 mesh anti-slip aggregate, mix at 1200rpm for 20min; mix and use immediately.

[0019] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention constructs an integrated structure of resin crosslinking, nano-reinforcement, and aggregate anchoring by synergistically combining hydroxypropyl-modified waterborne polyurethane resin, composite ion-exchange modified montmorillonite, compound functional additives, and graded anti-slip aggregates, thereby achieving a comprehensive performance improvement and solving the technical problems of existing technologies such as difficulty in synergistic anti-slip and wear resistance, poor weather resistance, and easy bubbling and particle loss.

[0020] Hydroxypropyl-modified waterborne polyurethane resin: It adopts an aliphatic anionic structure and introduces hydrophilic carboxyl groups through 15-20 mol% hydroxypropyl grafting. This ensures water dispersion stability and allows it to covalently bond with the amino groups on the surface of modified montmorillonite, forming a high-strength cross-linked network. The hydroxyl value of 55-65 mg KOH / g and the glass transition temperature of -20 to -10℃ endow the coating with excellent flexibility and low-temperature crack resistance. It can disperse the frictional stress caused by stepping on the surface, prevent the coating from cracking, and at the same time improve the interfacial bonding strength between the aggregate and the matrix, preventing the aggregate from falling off.

[0021] Composite ion-exchange modified montmorillonite: After multi-step modification through ion gradient exchange, long-chain intercalation and silane grafting, and polyurethane anchoring, it is uniformly dispersed in the resin matrix at the nanoscale to form a layered cross-linked structure. On the one hand, it can physically block ultraviolet rays, reduce resin degradation, and improve weather resistance. On the other hand, it can enhance the hardness and density of the coating, inhibit the propagation of microcracks, and improve the rheological properties of the coating, preventing storage precipitation and construction sagging, thus solving the problems of easy agglomeration and poor compatibility with resin of traditional montmorillonite.

[0022] The compound functional additive system includes: Surfynol MD20 / 104E compound defoamer, which combines continuous foam suppression and rapid foam breaking functions to eliminate air bubbles in coating preparation and application, thus avoiding pinhole defects in the coating; BYK381 leveling agent and Surfynol104PA wetting agent work synergistically to improve the wetting and spreading properties of the coating on the substrate, ensuring a uniform and smooth coating; Polirol DS19 dispersant prevents pigment and filler agglomeration, ensuring color uniformity and system stability; and associative polyurethane thickener precisely adjusts viscosity to suit application requirements.

[0023] Composite pigments and fillers and graded anti-slip aggregates: Weather-resistant iron oxide pigments / chrome green and titanium dioxide are compounded at a ratio of 1:3.8-4.2. Titanium dioxide can shield ultraviolet rays, improve the weather resistance and color stability of the coating, and enhance the hardness of the coating. 80-120 mesh corundum / fused silica aggregates provide surface micro-roughness, with a dry friction coefficient ≥0.85 and a wet friction coefficient ≥0.78, ensuring anti-slip safety in rain and snow environments.

[0024] Hydroxypropyl-modified waterborne polyurethane resin and composite ion-exchange modified montmorillonite form a strongly cross-linked "resin-nanofiller" matrix through covalent bonding, which significantly improves the cross-linking density and mechanical strength of the coating. The wear loss is ≤0.19g, which is more than 45% lower than that of ordinary waterborne polyurethane systems. The compounded additive system solves the performance limitations of single additives, avoids construction defects such as bubbles, pinholes, and sagging, ensures uniform surface roughness of the coating, and provides a stable anchoring interface for anti-slip aggregates. The composite pigments and fillers work synergistically with graded aggregates to improve the weather resistance and color durability of the coating, and to build a hard and wear-resistant skeleton.

[0025] The coating of this invention combines high flexibility and high hardness, adapting to the thermal expansion and contraction deformation of the walkway, exhibiting strong crack resistance, and showing no cracking or particle shedding even after high-frequency foot traffic. The two-component system has a moderate curing speed, simplifies construction, and can be directly applied to substrates such as concrete and asphalt without complex pretreatment, making it suitable for large-scale engineering applications such as municipal walkways, scenic greenways, and community slow-traffic systems. The water-based formula is low in VOCs, environmentally friendly, and non-toxic, aligning with the trend of green building materials development. It combines multiple advantages, including safety, slip resistance, durability, wear resistance, aesthetic appeal, and environmental friendliness, demonstrating significantly superior overall performance compared to existing water-based walkway coatings, and possessing broad market prospects. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the preparation process of a water-based anti-slip and wear-resistant colored pavement coating for sidewalks. Detailed Implementation

[0027] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0028] This invention provides a water-based anti-slip and wear-resistant colored pavement coating for sidewalks, composed of two components, A and B, in parts by weight: Component A: 58-62 parts of hydroxypropyl-modified waterborne polyurethane resin, 7.5-8.5 parts of deionized water, 4.5-5.5 parts of compounded film-forming aid, 0.15-0.25 parts of Tego902W defoamer, 2.0-2.8 parts of PolirolDS19 dispersant, 16-21 parts of composite pigments and fillers, and SurfynolMD20 / 104E compounded defoamer. Component A: 0.3-0.5 parts of agent, 0.45-0.55 parts of BYK381 leveling agent, 1.5-2.2 parts of composite ion exchange modified montmorillonite, 0.25-0.35 parts of associative polyurethane thickener, and 0.15-0.25 parts of nonionic wetting agent; Component B: 21-24 parts of Covestro Bayhydur 304 curing agent and 7.2-7.8 parts of PMA solvent with a moisture content of <500ppm; Construction additives: 8-12 parts of 80-120 mesh corundum or fused silica anti-slip aggregate.

[0029] In this invention, the preparation method of composite ion-exchange modified montmorillonite includes: (1) Purification: Natural sodium-based montmorillonite was prepared into a 4wt% aqueous suspension, mechanically stirred for 12h and allowed to settle for 36h to remove coarse impurities; the upper colloid was centrifuged at 8000rpm×15min, vacuum dried at 60℃ for 24h, and air-jet pulverized to 30-40nm to obtain high-purity montmorillonite. (2) Composite ion gradient exchange: High-purity montmorillonite was added to the composite exchange solution at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. (3) Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. (4) Silane directional grafting: The intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 was added dropwise, accounting for 12% of the mass of montmorillonite; refluxed at 80℃ for 2h, and centrifuged and dried to obtain silane-modified montmorillonite; (5) In-situ anchoring of polyurethane: Silane-modified montmorillonite is dispersed in anhydrous acetone to prepare a 10wt% dispersion; polyurethane prepolymer with molecular weight of 800-1200 and NCO content of 6-8wt% is added; pre-react at 40℃ for 30min, and then heated to 70℃ for 1h; acetone is removed under reduced pressure, vacuum dried at 60℃, and ground to obtain modified montmorillonite.

[0030] In this invention, the composite exchange solution in step (2) is preferably a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2.

[0031] In this invention, the mass of the polyurethane prepolymer in step (5) is preferably 8-12% of the silane-modified montmorillonite, and the NCO / amino molar ratio is controlled to be 1.01–1.03.

[0032] In this invention, the composite pigment and filler are preferably made by mixing weather-resistant iron oxide pigment or chrome green with titanium dioxide at a mass ratio of 1:3.8-4.2; the solid content of the prepared pigment paste is preferably ≥62wt%, and the pigment fineness is preferably ≤18μm.

[0033] In this invention, the preferred ratio of the compounded film-forming aids is DPnB:DPM mass ratio = 1:1.4-1.6.

[0034] In this invention, the hydroxypropyl-modified waterborne polyurethane resin is preferably an aliphatic anionic waterborne polyurethane, with a preferred hydroxypropyl grafting rate of 15-20 mol%, a preferred hydroxyl value of 55-65 mgKOH / g, a preferred solid content of 44-46 wt%, and a preferred glass transition temperature Tg of -20 to -10 °C. The molecular chain contains hydrophilic carboxyl groups, which can covalently bond with the amino groups on the modified montmorillonite surface.

[0035] In this invention, the defoamer is preferably a mixture of Surfynol MD20 and Surfynol 104E in a mass ratio of 1:1.5 to 2.5; it has both continuous foam suppression and rapid foam breaking functions, which can avoid pinhole defects.

[0036] In this invention, the nonionic wetting agent is preferably a low-foaming acetylene glycol wetting agent, Surfynol 104PA.

[0037] The present invention also provides a method for preparing the above-mentioned water-based anti-slip and wear-resistant colored pavement coating for sidewalks, comprising the following complete steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the method described above, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor according to the ratio; stir at 800-1000 rpm for 15 minutes until the system is uniform and free of bubbles. S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2200-2500 rpm for 15 min; transfer to a horizontal sand mill, grind with 0.8-1.2 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1000-1200 rpm for 20 min until there is no agglomeration and the particle size is uniform; S5A Component Main Synthesis: Hydroxypropyl-modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added sequentially; dispersion was carried out at 1000 rpm for 30 min; S6 Viscosity Control: Associative polyurethane thickener was slowly added dropwise at a dropping rate ≤0.1 parts / min to adjust the viscosity to 85-90 KU; pH was maintained at 7.5-8.5, and the mixture was stabilized at 1000 rpm for 30 min. S7 Filtering and Packaging Component A: Filter through a 200-mesh precision filter to remove impurities and gel, then seal in packaging; S8 Component B Preparation: Mix Bayhydur 304 curing agent with PMA solvent containing <500ppm moisture; stir at 1000rpm for 15min, filter through a 200-mesh filter, and seal in moisture-proof packaging; S9 On-site Mixing and Construction: Before construction, measure according to the mass ratio of A:B=100:30; add 80-120 mesh anti-slip aggregate, stir at 1200rpm for 20min; prepare and use immediately.

[0038] The coating formulation and preparation process provided by this invention selects a specific resin, modified montmorillonite, and additive system. The synergistic effect of each component can significantly improve the anti-slip performance, wear resistance, weather resistance, and dimensional stability of the road surface coating. At the same time, it is easy to apply, has a moderate curing speed, and is not prone to shrinkage cavities and blistering, making it suitable for large-scale application in colored pavement engineering for sidewalks.

[0039] To further illustrate the present invention, the following embodiments will be described in detail.

[0040] Example 1: (1) Preparation of composite ion-exchange modified montmorillonite: a. Purification: Take natural sodium-based montmorillonite and prepare a 4wt% aqueous suspension. Stir mechanically for 12 hours and let it stand for 36 hours to remove coarse impurities. Centrifuge the upper colloid at 8000 rpm for 15 minutes, vacuum dry at 60℃ for 24 hours, and pulverize it to 30 nm to obtain high-purity montmorillonite. b. Composite ion gradient exchange: High-purity montmorillonite was added to a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2 at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. c. Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. d. Silane-directed grafting: Intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 (12% of the montmorillonite mass) was added dropwise; the mixture was refluxed at 80℃ for 2 hours and then centrifuged and dried to obtain silane-modified montmorillonite. e. In-situ anchoring of polyurethane: Silane-modified montmorillonite was dispersed in anhydrous acetone to prepare a 10wt% dispersion; a polyurethane prepolymer with a molecular weight of 800 and an NCO content of 6wt% was added, the mass of which was 8% of the silane-modified montmorillonite, and the NCO / amino molar ratio was controlled at 1.01; the pre-reaction was carried out at 40℃ for 30 min, and then the temperature was increased to 70℃ for 1 h; the acetone was removed under reduced pressure, and the mixture was dried under vacuum at 60℃ and ground to obtain composite ion-exchange modified montmorillonite, which was then sealed for later use.

[0041] (2) Group A allocation system: By weight: 58 parts hydroxypropyl-modified waterborne polyurethane resin, 7.5 parts deionized water, 4.5 parts compounded film-forming aid, 0.15 parts Tego902W defoamer, 2.0 parts PolirolDS19 dispersant, 16 parts composite pigments and fillers, 0.3 parts SurfynolMD20 / 104E compounded defoamer, 0.45 parts BYK381 leveling agent, 1.5 parts composite ion-exchange modified montmorillonite, 0.25 parts associative polyurethane thickener, and 0.15 parts nonionic wetting agent. Among these: The hydroxypropyl-modified waterborne polyurethane resin is an aliphatic anionic waterborne polyurethane with a hydroxypropyl grafting rate of 15 mol%, a hydroxyl value of 55 mg KOH / g, a solid content of 44 wt%, and a glass transition temperature (Tg) of -20℃. The compound film-forming aid has a DPnB:DPM mass ratio of 1:1.4; The composite pigment and filler is a mixture of weather-resistant iron oxide pigment and titanium dioxide at a mass ratio of 1:3.8, with a pigment paste solid content of 62wt% and a pigment fineness of 18μm. The compound defoamer is a mixture of Surfynol MD20 and Surfynol 104E at a mass ratio of 1:1.5; The nonionic wetting agent is Surfynol 104PA.

[0042] Preparation steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the above method, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor; stir at 800 rpm for 15 min until the system is uniform and free of bubbles; S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2200 rpm for 15 min; transfer to a horizontal sand mill, grind with 0.8 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1000 rpm for 20 min until there is no agglomeration and the particle size is uniform; S5A component main synthesis: Hydroxypropyl modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added in sequence; dispersed at 1000 rpm for 30 min; S6 viscosity control: Slowly add associative polyurethane thickener at a dropping rate ≤ 0.1 parts / min, adjust viscosity to 85 KU; maintain pH 7.5, stabilize at 1000 rpm for 30 min; S7 Filter Packaging Component A: Filtered with a 200-mesh precision filter to remove impurities and gel, then sealed in packaging.

[0043] (3) Group B allocation system: By weight: 21 parts Covestro Bayhydur 304 curing agent, 7.2 parts PMA solvent with moisture content <500ppm. Preparation steps: Mix Bayhydur 304 curing agent and PMA solvent; stir at 1000rpm for 15min, filter through a 200-mesh sieve, and seal in a moisture-proof package.

[0044] (4) On-site mixed construction: Before construction, measure according to the mass ratio of A:B=100:30; add 8 parts of 80-mesh diamond anti-slip aggregate, stir at 1200rpm for 20min; mix and use immediately to obtain the finished water-based anti-slip and wear-resistant colored pavement coating for sidewalks.

[0045] Example 2: (1) Preparation of composite ion-exchange modified montmorillonite: a) Purification: Take natural sodium montmorillonite and prepare a 4wt% aqueous suspension. Stir mechanically for 12 hours and let it stand for 36 hours to remove coarse impurities. Centrifuge the upper colloid at 8000 rpm for 15 minutes, vacuum dry at 60℃ for 24 hours, and pulverize it to 40 nm to obtain high-purity montmorillonite. b. Composite ion gradient exchange: High-purity montmorillonite was added to a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2 at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. c. Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. d. Silane-directed grafting: Intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 (12% of the montmorillonite mass) was added dropwise; the mixture was refluxed at 80℃ for 2 hours and then centrifuged and dried to obtain silane-modified montmorillonite. e. In-situ anchoring of polyurethane: Silane-modified montmorillonite was dispersed in anhydrous acetone to prepare a 10wt% dispersion; a polyurethane prepolymer with a molecular weight of 1200 and an NCO content of 8wt% was added, the mass of which was 12% of the silane-modified montmorillonite, and the NCO / amino molar ratio was controlled at 1.03; the pre-reaction was carried out at 40℃ for 30 min, and then the temperature was increased to 70℃ for 1 h; the acetone was removed under reduced pressure, and the mixture was dried under vacuum at 60℃ and ground to obtain composite ion-exchange modified montmorillonite, which was then sealed for later use.

[0046] (2) Group A allocation system: By weight: 62 parts hydroxypropyl modified waterborne polyurethane resin, 8.5 parts deionized water, 5.5 parts compounded film-forming aid, 0.25 parts Tego902W defoamer, 2.8 parts PolirolDS19 dispersant, 21 parts composite pigments and fillers, 0.5 parts SurfynolMD20 / 104E compounded defoamer, 0.55 parts BYK381 leveling agent, 2.2 parts composite ion-exchange modified montmorillonite, 0.35 parts associative polyurethane thickener, and 0.25 parts nonionic wetting agent. Among which: The hydroxypropyl-modified waterborne polyurethane resin is an aliphatic anionic waterborne polyurethane with a hydroxypropyl grafting rate of 20 mol%, a hydroxyl value of 65 mg KOH / g, a solid content of 46 wt%, and a glass transition temperature (Tg) of -10℃. The compound film-forming aid has a DPB:DPM mass ratio of 1:1.6; The composite pigment and filler is a mixture of chrome green and titanium dioxide at a mass ratio of 1:4.2, with a pigment solid content of 64wt% and a pigment fineness of 16μm. The compound defoamer is a mixture of Surfynol MD20 and Surfynol 104E at a mass ratio of 1:2.5; The nonionic wetting agent is Surfynol 104PA.

[0047] Preparation steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the above method, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor; stir at 1000 rpm for 15 min until the system is homogeneous and free of bubbles; S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2500 rpm for 15 min; transfer to a horizontal sand mill, grind with 1.2 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1200 rpm for 20 min until there is no agglomeration and the particle size is uniform; S5A component main synthesis: Hydroxypropyl modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added in sequence; dispersed at 1000 rpm for 30 min; S6 viscosity control: Slowly add associative polyurethane thickener at a dropping rate ≤ 0.1 parts / min, adjust viscosity to 90 KU; maintain pH 8.5, stabilize at 1000 rpm for 30 min; S7 Filter Packaging Component A: Filtered with a 200-mesh precision filter to remove impurities and gel, then sealed in packaging.

[0048] (3) Group B allocation system: By weight: 24 parts Covestro Bayhydur 304 curing agent, 7.8 parts PMA solvent with moisture content <500ppm. Preparation steps: Mix Bayhydur 304 curing agent and PMA solvent; stir at 1000rpm for 15min, filter through a 200-mesh sieve, and seal in a moisture-proof package.

[0049] (4) On-site mixed construction Before construction, measure according to the mass ratio of A:B=100:30; add 12 parts of 120 mesh fused silica anti-slip aggregate, stir at 1200 rpm for 20 minutes; mix and use immediately to obtain the finished water-based anti-slip and wear-resistant colored pavement coating for sidewalks.

[0050] Example 3: (1) Preparation of composite ion-exchange modified montmorillonite: a. Purification: Take natural sodium montmorillonite and prepare a 4wt% aqueous suspension. Stir mechanically for 12 hours and let it stand for 36 hours to remove coarse impurities. Centrifuge the upper colloid at 8000 rpm for 15 minutes, vacuum dry at 60℃ for 24 hours, and pulverize it to 35 nm to obtain high-purity montmorillonite. b. Composite ion gradient exchange: High-purity montmorillonite was added to a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2 at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. c. Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. d. Silane-directed grafting: Intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 (12% of the montmorillonite mass) was added dropwise; the mixture was refluxed at 80℃ for 2 hours and then centrifuged and dried to obtain silane-modified montmorillonite. e. In-situ anchoring of polyurethane: Silane-modified montmorillonite was dispersed in anhydrous acetone to prepare a 10wt% dispersion; a polyurethane prepolymer with a molecular weight of 1000 and an NCO content of 7wt% was added, the mass of the prepolymer being 10% of the silane-modified montmorillonite, and the NCO / amino molar ratio was controlled at 1.02; the pre-reaction was carried out at 40℃ for 30 min, and then the temperature was increased to 70℃ for 1 h; the acetone was removed under reduced pressure, and the mixture was dried under vacuum at 60℃ and ground to obtain composite ion-exchange modified montmorillonite, which was then sealed for later use.

[0051] (2) Group A allocation system: By weight: 60 parts hydroxypropyl modified waterborne polyurethane resin, 8.0 parts deionized water, 5.0 parts compounded film-forming aid, 0.20 parts Tego902W defoamer, 2.5 parts PolirolDS19 dispersant, 20 parts composite pigments and fillers, 0.4 parts SurfynolMD20 / 104E compounded defoamer, 0.50 parts BYK381 leveling agent, 2.0 parts composite ion-exchange modified montmorillonite, 0.30 parts associative polyurethane thickener, and 0.20 parts nonionic wetting agent. Among them: The hydroxypropyl-modified waterborne polyurethane resin is an aliphatic anionic waterborne polyurethane with a hydroxypropyl grafting rate of 18 mol%, a hydroxyl value of 60 mg KOH / g, a solid content of 45 wt%, and a glass transition temperature (Tg) of -15℃. The compound film-forming aid has a DPnB:DPM mass ratio of 1:1.5; The composite pigment and filler is a mixture of weather-resistant iron oxide pigment and titanium dioxide at a mass ratio of 1:4.0, with a pigment paste solid content of 63wt% and a pigment fineness of 17μm. The compound defoamer is a mixture of Surfynol MD20 and Surfynol 104E at a mass ratio of 1:2.0; The nonionic wetting agent is Surfynol 104PA.

[0052] Preparation steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the above method, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor; stir at 900 rpm for 15 min until the system is uniform and free of bubbles; S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2350 rpm for 15 min; transfer to a horizontal sand mill, grind with 1.0 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1100 rpm for 20 min until there is no agglomeration and the particle size is uniform; S5A component main synthesis: Hydroxypropyl modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added in sequence; dispersed at 1000 rpm for 30 min; S6 viscosity control: Slowly add associative polyurethane thickener at a dropping rate ≤ 0.1 parts / min, adjust the viscosity to 88KU; maintain pH 8.0 and stabilize at 1000 rpm for 30 min; S7 Filter Packaging Component A: Filtered with a 200-mesh precision filter to remove impurities and gel, then sealed in packaging.

[0053] (3) Group B allocation system: By weight: 22.5 parts Covestro Bayhydur 304 curing agent, 7.5 parts PMA solvent with moisture content <500ppm. Preparation steps: Mix Bayhydur 304 curing agent and PMA solvent; stir at 1000rpm for 15min, filter through a 200-mesh sieve, and seal in a moisture-proof package.

[0054] (4) On-site mixed construction: Before construction, measure according to the mass ratio of A:B=100:30; add 10 parts of 100-mesh diamond anti-slip aggregate, stir at 1200rpm for 20min; mix and use immediately to obtain the finished water-based anti-slip and wear-resistant colored pavement coating for sidewalks.

[0055] Comparative Example 1: The formulation and preparation method are the same as in Example 3, except that: no composite ion exchange modified montmorillonite is added to component A, the other components and their amounts remain unchanged, the preparation process parameters are completely consistent with those in Example 3, and the same anti-slip aggregate is added during on-site construction to obtain the comparative coating 1.

[0056] Comparative Example 2: The formulation and preparation method are the same as in Example 3, except that the hydroxypropyl modified waterborne polyurethane resin is replaced with ordinary aliphatic waterborne polyurethane (without hydroxypropyl grafting, Tg-15℃, solid content 45wt%), while the other components and dosages remain unchanged. The preparation process parameters are completely consistent with those in Example 3. The same anti-slip aggregate is added during on-site construction to obtain the comparative coating 2.

[0057] Comparative Example 3: The formulation and preparation method are the same as in Example 3, except that the SurfynolMD20 / 104E compound defoamer is replaced with an equal amount of single Surfynol104E defoamer, while the other components and dosages remain unchanged. The preparation process parameters are completely consistent with those in Example 3. The same anti-slip aggregate is added during on-site construction to obtain the comparative coating 3.

[0058] Comparative Example 4: The formulation and preparation method are the same as in Example 3, except that the composite pigments and fillers are replaced with an equal amount of weather-resistant iron oxide pigment (without titanium dioxide compounding), while the other components and amounts remain unchanged. The preparation process parameters are completely consistent with those in Example 3. The same anti-slip aggregate is added during on-site construction to obtain the comparative coating 4.

[0059] test: Test 1: Basic physical properties test (adhesion, abrasion resistance, water resistance, chemical resistance); 1.1 Experimental Objective: The adhesion, abrasion resistance, water resistance, and chemical resistance of the cured coatings of Examples 1-3 and Comparative Examples 1-4 were verified. The technical indicators were as follows: adhesion (concrete ≥1.5MPa, asphalt ≥1.0MPa), abrasion resistance ≤0.03g, no abnormality in water resistance for 240h, and no abnormality in chemical resistance for 72h.

[0060] 1.2 Experimental Principle: Adhesion (pull-out method): After the coating has cured, it is pulled vertically with a pull-out tester to determine the maximum tensile strength between the coating and the substrate.

[0061] Abrasion resistance (Taber wear): CS-17 grinding wheel, 1000g load, 1000 rpm, quality difference before and after abrasion test.

[0062] Water resistance: After immersion in water at room temperature for 240 hours, visually observe for blistering, peeling, and discoloration.

[0063] Chemical resistance: Immersed in gasoline, engine oil, and 10% H2O respectively. 2 SO4 and 10% NaOH solution were used for 72 hours, and visual observation revealed abnormalities.

[0064] 1.3 Test instruments and substrates: Instruments: Coating pull-out adhesion tester, Taber abrasion tester, electronic balance (0.001g), constant temperature water bath, sealed immersion container, magnifying glass. Substrates: C30 concrete blocks (150×150×20mm), AC-13 asphalt blocks (150×150×20mm), tinplate (abrasion-resistant / water-resistant / chemical-resistant). Samples: Coatings from Examples 1-3 and Comparative Examples 1-4.

[0065] 1.4 Test Methods: 1.4.1 Adhesion (pull-out test); 1) The substrate is clean and dry, the coating is applied and a film is formed, the dry film is 1.5mm, and it is cured at room temperature for 7 days; 2) Adhere standard drawn ingots to the coating surface and cure for 24 hours; 3) Apply the pull-out tester at a constant speed, record the maximum tensile force at failure, and calculate the adhesion strength (MPa). 4) Three parallel tests were conducted for each group, and the average value was taken; concrete / asphalt substrates were tested separately.

[0066] 1.4.2 Abrasion resistance (Taber wear) 1) Coating tinplate with paint, dry film thickness 1.5mm, curing for 7 days; 2) Weigh the initial mass m0 using an electronic balance; 3) Taber testing machine: CS-17 wheel, 1000g, 1000 rpm; 4) Clean up the grinding debris and weigh the final mass m1; 5) Wear loss = m0 m1; 3 parallels per group.

[0067] 1.4.3 Water resistance (immersion at room temperature for 240 hours); 1) Coat the tinplate with paint and cure for 7 days; 2) Soak in deionized water at room temperature for 240 hours; 3) Remove and dry, then visually inspect with a magnifying glass for bubbling, peeling, and discoloration; record "pass / fail".

[0068] 1.4.4 Chemical resistance (72h); 1) Coat the tinplate with paint and cure for 7 days; 2) Immerse in: gasoline, engine oil, and 10% H2O respectively. 2 SO4, 10% NaOH; 72 hours at room temperature; 3) Remove and rinse with clean water, dry, and visually inspect for bubbling, peeling, cracking, and discoloration; record "pass / fail".

[0069] 1.5 Experimental Data: (Adhesion: concrete / asphalt; Abrasion resistance: mass loss g; Water resistance / Chemical resistance: √ Pass / × Fail) Table 1 Test results of basic physical properties of coating

[0070] Examples 1-3: Concrete adhesion ≥1.5MPa, asphalt ≥1.0MPa, abrasion ≤0.03g, no abnormalities after 240h of water resistance, and stable after 72h of chemical resistance.

[0071] Comparative Example 1 (Unmodified montmorillonite): Adhesion significantly decreased, abrasion exceeded standards, water resistance caused blistering, and alkali solution detachment. Reason: Modified montmorillonite provides nano-crosslinking reinforcement, improving interfacial adhesion, density, and chemical stability; without it, the interface is weak, the structure is loose, and the physical and chemical properties are comprehensively degraded.

[0072] Comparative Example 2 (Ordinary waterborne polyurethane): Insufficient adhesion, excessive abrasion, and acid discoloration. Reason: Hydroxypropyl-modified polyurethane is covalently bonded to montmorillonite, resulting in high interfacial strength and resistance to acids and alkalis; ordinary resin has weak crosslinking, poor chemical resistance, and is easily damaged at the interface.

[0073] Comparative Example 3 (Single Defoamer): Excessive abrasion and alkaline microbubbles. Reasons: Compound defoamer eliminates microbubble defects, resulting in a dense coating; single defoamer leaves residual microbubbles, causing abrasion stress concentration and alkaline penetration and bubbling.

[0074] Comparative Example 4 (without titanium dioxide): Adhesion was low, abrasion exceeded the standard, and acid resistance showed slight discoloration. Reason: Titanium dioxide enhances hardness and chemical inertness, making it wear-resistant and acid-resistant; with only iron oxide pigment, the hardness is insufficient, and acid corrosion easily causes discoloration.

[0075] Test 2: Accelerated weathering test (QUV-B / Xenon lamp, color difference ΔE, gloss retention rate, chalking grade); 2.1 Experimental Objective: Evaluation of long-term outdoor weather resistance stability of coating: QUV-B (313nm) or xenon lamp aging for 2000h; test color difference ΔE, gloss retention rate, and chalking grade (according to GB / T1766-2008).

[0076] 2.2 Experimental Principle: QUV-B (313nm): Short-wave ultraviolet + condensation, accelerates photo-oxidative aging; Xenon lamp aging: Simulating full-spectrum sunlight, 2000h; Color difference ΔE: Color difference before and after aging; Gloss retention rate: 100% after 60° gloss aging / initial gloss level; Chalking grade (GB / T1766-2008): Grade 0: No chalking; Grade 5: Severe chalking.

[0077] 2.3 Test instruments and samples: Instruments: QUV-B ultraviolet aging chamber, xenon lamp aging chamber, 60° gloss meter, colorimeter, chalking rating board, tinplate (100×50×1mm). Samples: Coatings from Examples 1-3 and Comparative Examples 1-4.

[0078] 2.4 Test Methods: 1) Coating tinplate with paint, dry film thickness 1.5mm, cured at room temperature for 7 days; 2) Initial test: 60° gloss G0, color difference L0 / a0 / b0; 3) Aging conditions: Xenon lamp aging for 2000 hours (irradiation 0.51W / m²) 2 (60℃, 50%RH); 4) Post-aging tests: 60° gloss G1, color difference L1 / a1 / b1, chalking grade; 5) Calculation: Gloss retention rate = G1 / G0 × 100%; ΔE = √[(ΔL)] 2 +(Δa) 2 +(Δb) 2 6) Three parallel samples are taken for each group, and the average value is taken; the powdering level is recorded directly.

[0079] 2.5 Experimental Data: (Calming grade: GB / T1766-2008; ΔE, gloss retention %) Table 2 Results of accelerated aging test for coating weather resistance

[0080] Examples 1-3 exhibit excellent weather resistance: ΔE≤1.1, gloss retention ≥89%, and grade 0 no chalking; Example 2 demonstrates the strongest anti-aging properties, with the formula suitable for long-term outdoor use without fading, loss of gloss, or chalking.

[0081] Comparative Example 1 (Unmodified montmorillonite): Large ΔE, significantly reduced gloss, and grade 3 chalking. Reason: Modified montmorillonite provides strong UV shielding and thermal stability, inhibiting resin degradation; its absence leads to rapid photo-oxidative aging of the resin, pigment decomposition, and severe chalking.

[0082] Comparative Example 2 (Ordinary waterborne polyurethane): Significant ΔE, low gloss, and grade 2 chalking. Reason: Aliphatic hydroxypropyl modified polyurethane is more resistant to UV radiation; ordinary resin is prone to yellowing and degradation, resulting in a significant decrease in weather resistance.

[0083] Comparative Example 3 (single defoamer): ΔE is too high, gloss is reduced, and grade 1 chalking occurs. Reason: Microbubble defects become aging penetration channels, accelerating aging; compound defoamers ensure density and delay aging.

[0084] Comparative Example 4 (without titanium dioxide): ΔE is higher, gloss is reduced, and it exhibits grade 1 chalking. Reason: Titanium dioxide provides efficient UV shielding, protecting the pigment and resin; with only iron oxide pigment, UV radiation directly corrodes the pigment, resulting in significant fading and aging.

[0085] Experiment 3: Freeze-thaw stability and low-temperature flexibility: 3.1 Experimental Objective: Verify the freeze-thaw stability of the coating emulsion (-5℃, 5 cycles) and the low-temperature flexibility of the coating film (-10℃, φ10mm shaft 180° without cracking), and evaluate its adaptability to low-temperature environments.

[0086] 3.2 Experimental Principle: Freeze-thaw stability: Emulsion frozen at -5℃ → thawed at room temperature, 5 cycles, observe demulsification / layering / precipitation; Low-temperature flexibility: The coating is kept at a constant temperature of -10℃ and bent 180° around a φ10mm shaft. Visual cracking is observed.

[0087] 3.3 Test Instruments and Samples: Instruments: Low-temperature freezer (-10℃ to room temperature), constant temperature low-temperature chamber, φ10mm metal shaft, tinplate, emulsion samples (component A emulsions of Examples 1-3 and Comparative Examples 1-4).

[0088] 3.4 Test methods: 3.4.1 Emulsion freeze-thaw stability (-5℃, 5 cycles) 1) Take 50 mL of component A emulsion and seal it; 2) Cycle: freeze at -5℃ for 12 h → thaw at room temperature for 12 h, which is 1 cycle; repeat 5 times in total; 3) Observe: demulsification, layering, precipitation, clumping; record "qualified / unqualified".

[0089] 3.4.2 Low-temperature flexibility of coating (-10℃, φ10mm shaft) 1) Coat the tinplate with paint, dry film thickness 1.0mm, cure for 7 days; 2) Place at -10℃ for 2 hours; 3) Quickly bend around a φ10mm shaft 180°; 4) Visually inspect for cracks with a magnifying glass; record "pass / fail"; 3 parallel samples per group.

[0090] 3.5 Experimental Data: (Freeze-thaw stability: √ Pass / × Fail; Low-temperature flexibility: √ No cracking / × Cracking) Table 3 Results of freeze-thaw stability and low-temperature flexibility tests of coatings

[0091] Examples 1-3 demonstrate excellent low-temperature performance: the emulsion remains stable after 5 freeze-thaw cycles, and the coating does not crack when bent at -10℃, fully meeting the requirements for construction and use of low-temperature walkways.

[0092] Comparative Example 1 (Unmodified montmorillonite): Emulsion freeze-thaw separation and precipitation, coating low-temperature cracking. Reason: Modified montmorillonite plays a colloidal stabilizing and low-temperature toughening role in the emulsion, resisting freeze-thaw cycles and low-temperature brittleness; without it, the emulsion stability is poor and the coating low-temperature brittleness is high.

[0093] Comparative Example 2 (Ordinary waterborne polyurethane): The emulsion was stable, but the coating edge cracked. Reason: Hydroxypropyl modified polyurethane has a low Tg and good low-temperature toughness; ordinary resin has a high Tg and insufficient low-temperature toughness, making it prone to cracking when bent.

[0094] Comparative Example 3 / 4: The low-temperature performance is qualified, indicating that the defoamer and pigment / filler system has little impact on low-temperature stability, and the core low-temperature performance is determined by the modified montmorillonite and modified polyurethane.

[0095] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A water-based, anti-slip, and wear-resistant colored pavement coating for sidewalks, characterized in that, Composed of two components, A and B, in parts by weight: Component A: 58-62 parts of hydroxypropyl-modified waterborne polyurethane resin, 7.5-8.5 parts of deionized water, 4.5-5.5 parts of compounded film-forming aid, 0.15-0.25 parts of defoamer, 2.0-2.8 parts of dispersant, 16-21 parts of composite pigments and fillers, 0.3-0.5 parts of compounded defoamer, 0.45-0.55 parts of leveling agent, 1.5-2.2 parts of composite ion-exchange modified montmorillonite, 0.25-0.35 parts of associative polyurethane thickener, and 0.15-0.25 parts of nonionic wetting agent; Component B: 21-24 parts curing agent, 7.2-7.8 parts PMA solvent with moisture content <500ppm; Add the following during construction: 8-12 parts of 80-120 mesh corundum or fused silica anti-slip aggregate.

2. The coating according to claim 1, characterized in that, The preparation method of the composite ion-exchange modified montmorillonite includes: (1) Purification: Natural sodium-based montmorillonite was prepared into a 4wt% aqueous suspension, mechanically stirred for 12h and allowed to settle for 36h to remove coarse impurities; the upper colloid was centrifuged at 8000rpm×15min, vacuum dried at 60℃ for 24h, and air-jet pulverized to 30-40nm to obtain high-purity montmorillonite. (2) Composite ion gradient exchange: High-purity montmorillonite was added to the composite exchange solution at a solid-liquid ratio of 1:15 g / mL; pretreatment was performed at 85℃ for 1.5 h, followed by deep treatment at 95℃ for 2 h; washing was continued until Cl-free. - Mg 2+ The residue was dried at 60°C to obtain ion-exchange montmorillonite. (3) Long-chain intercalation compatibilization: Ion-exchange montmorillonite was dispersed in hot water at 65℃ at a mass ratio of 1:10, and dodecyl dimethyl benzyl ammonium chloride was added. The mass ratio of montmorillonite to dodecyl dimethyl benzyl ammonium chloride was 10:1.

5. The mixture was stirred and intercalated at 65℃ for 2 hours, washed with water and dried to obtain intercalated montmorillonite. (4) Silane directional grafting: The intercalated montmorillonite was dispersed in 8wt% anhydrous ethanol at a mass ratio of 1:10, and KH-550 was added dropwise, accounting for 12% of the mass of montmorillonite; refluxed at 80℃ for 2h, and centrifuged and dried to obtain silane-modified montmorillonite; (5) In-situ anchoring of polyurethane: Silane-modified montmorillonite is dispersed in anhydrous acetone to prepare a 10wt% dispersion; polyurethane prepolymer with molecular weight of 800-1200 and NCO content of 6-8wt% is added; pre-react at 40℃ for 30min, and then heated to 70℃ for 1h; acetone is removed under reduced pressure, vacuum dried at 60℃, and ground to obtain modified montmorillonite.

3. The coating according to claim 2, characterized in that, In step (2), the composite exchange solution is a composite exchange solution of 0.5 mol / L NaCl and 0.2 mol / L MgCl2.

4. The coating according to claim 2, characterized in that, In step (5), the mass of the polyurethane prepolymer is 8-12% of the silane-modified montmorillonite, and the NCO / amino molar ratio is controlled to be 1.01–1.

03.

5. The coating according to claim 1, characterized in that, The composite pigments and fillers are made by mixing weather-resistant iron oxide pigments or chrome green with titanium dioxide at a mass ratio of 1:3.8-4.2; the prepared pigment paste has a solid content of ≥62wt% and a pigment fineness of ≤18μm.

6. The coating according to claim 1, characterized in that, The compound film-forming aid has a mass ratio of DPnB:DPM of 1:1.4-1.

6.

7. The coating according to claim 1, characterized in that, The hydroxypropyl-modified waterborne polyurethane resin is an aliphatic anionic waterborne polyurethane with a hydroxypropyl grafting rate of 15-20 mol%, a hydroxyl value of 55-65 mgKOH / g, a solid content of 44-46 wt%, and a glass transition temperature (Tg) of -20 to -10 °C.

8. The coating according to claim 1, characterized in that, The compound defoamer is a defoamer composed of Surfynol MD20 and Surfynol 104E in a mass ratio of 1:1.5 to 2.

5.

9. The coating according to claim 1, characterized in that, The nonionic wetting agent is Surfynol 104PA, a low-foaming acetylene glycol wetting agent.

10. The method for preparing the water-based anti-slip and wear-resistant colored pavement coating for sidewalks according to claim 2, characterized in that, Includes the following complete steps: S1 modified montmorillonite pre-preparation: Prepare composite ion-exchange modified montmorillonite according to the method described above, and seal for later use; S2 base solution preparation: Add deionized water, compound film-forming aid, Tego902W antifoaming agent, and PolirolDS19 dispersant to the reactor according to the ratio; stir at 800-1000 rpm for 15 minutes until the system is uniform and free of bubbles. S3 Pigment Dispersion and Grinding: Add composite pigments and fillers, disperse at high speed of 2200-2500 rpm for 15 min; transfer to a horizontal sand mill, grind with 0.8-1.2 mm zirconium beads, control the material temperature ≤40℃, until the pigment fineness is ≤18μm; S4 modified montmorillonite dispersion: Return the ground slurry to the reactor, add the composite ion exchange modified montmorillonite; stir at 1000-1200 rpm for 20 minutes until there is no agglomeration and the particle size is uniform; S5A component main synthesis: Hydroxypropyl modified waterborne polyurethane resin was slowly added at a low speed of 600 rpm; Surfynol MD20 / 104E compound defoamer, BYK381 leveling agent, and nonionic wetting agent were added in sequence; dispersed at 1000 rpm for 30 min; S6 viscosity control: Slowly add associative polyurethane thickener at a dropping rate ≤ 0.1 parts / min, adjust the viscosity to 85-90 KU; maintain pH 7.5-8.5, stabilize at 1000 rpm for 30 min; S7 Filter Packaging Component A: Filtered with a 200-mesh precision filter to remove impurities and gel, then sealed in packaging; S8B formulation: Mix Bayhydur 304 curing agent with PMA solvent with a moisture content of <500ppm; stir at 1000rpm for 15min, filter through a 200-mesh filter, and seal in a moisture-proof package; S9 on-site mixing construction: Before construction, measure according to the mass ratio of A:B=100:30; add 80-120 mesh anti-slip aggregate, mix at 1200rpm for 20min; mix and use immediately.

Citation Information

Patent Citations

  • Preparation of single-component quick-drying colored antiskid water-based paint and application of paint in slow-moving system

    CN116445048A

  • Waterborne polyurethane asphalt colored pavement protective coating and preparation method thereof