Method for preparing transfer foil and coated laminated material plates

By using thermoplastic polyurethane (meth)acrylate polymer transfer foil, the problems of scratch resistance, weather resistance and carrier material removal of coated laminated material boards have been solved, achieving efficient and low-cost coating preparation.

CN123107526APending Publication Date: 2026-11-17SUP FUNCTIONAL FILM CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202610661301.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve coatings with excellent scratch resistance, chemical resistance, and weather resistance when preparing coated laminated material boards. At the same time, the carrier material is not easy to remove during processing, which affects production efficiency and cost.

Method used

A transfer foil containing thermoplastic polyurethane (meth)acrylate polymer is used. A thermoplastic coating is formed by coating a mixture of resin components and hardener components onto a carrier material. The coating is then dried at high temperature and extruded onto a laminate board to ensure adhesion and stability.

Benefits of technology

It achieves high scratch resistance, weather resistance and chemical resistance on the surface of laminated material boards, while the carrier material does not detach during processing, simplifying the production process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_8
    Figure SMS_8
Patent Text Reader

Abstract

This invention relates to a method for preparing a transfer foil comprising a carrier material and a coating containing a thermoplastic polyurethane (meth)acrylate polymer. The transfer foil allows the formation of a cross-linked polyurethane (meth)acrylate polymer-based coating on a laminated material sheet. The transfer foil is characterized by particularly good abrasion properties, especially particularly high scratch resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing planar materials, such as foils, laminated sheets, etc., wherein the planar material has a cross-linked polyurethane (meth)acrylate coating. The method uses a so-called transfer process, in which a coating composition is applied to the planar material, such as a laminated sheet, not directly but via a carrier material, wherein the coating composition is first applied to the carrier material and a thermoplastic coating is formed there. In a separate working step, the coated carrier material is bonded to the planar material, after which the carrier material is pulled out. Thus, the coating is applied to the planar material indirectly. Background Technology

[0002] Similar transfer methods are known, for example, from patent document DE3545171C1. This disclosure describes an indirect method for manufacturing differentiated surface finishes, wherein a partially cured coating system of a carrier material is partially transferred onto a laminate material and the carrier material is removed after coating. Metal foil, such as aluminum foil, is used as the carrier material. Many different coating systems have been proposed regarding the coatings. As illustrated in the example of this disclosure, the coating is cured on the carrier material by drying. Preferably, the coating system is only partially cured, leaving it with residual reactivity and participating in further chemical reactions occurring during the process (in the subsequent pressing process), resulting in good adhesion to the surface material (substrate).

[0003] DE10318542A1 discloses a method for manufacturing a planar material, such as a film, having a protective layer comprising a coating. The coating is applied to a carrier material and subsequently at least partially cured. A coating containing a substance polymerizable in a free radical and / or ionic manner is used, and the coating applied to the carrier material is at least partially cured by free radical and / or ionic polymerization. The carrier material thus having the coating is bonded to the planar material with the coating surface and then the carrier material is pulled out. According to one embodiment, a mixture consisting of polyurethane acrylate, polyurethane acrylate containing reactive isocyanate groups, and OH-functional acrylate is coated onto a polypropylene film in a stoichiometric ratio with the free isocyanate groups of the addition reaction portion of the polyurethane acrylate, along with a solvent and a photoinitiator. The solvent is evaporated at approximately 100°C and the layer is cured under UV light. An adhesive primer layer is applied to the layer thus obtained. The resulting transfer material is pressed during an extrusion process at 140°C and 30 MPa. Therefore, an HPL material can be produced whose surface has been treated with a carrier film with gloss or matte finish, which has high scratch and abrasion resistance and provides excellent weather resistance.

[0004] DE102007040376A1 relates to a coating, a flexible layered composite having a carrier and a coating layer applied to the carrier, and the use of the layered composite. The coating consists of a mixture of three components in addition to a photoinitiator and additives: a solid polyol binder containing double bonds (A), a solid polyurethane acrylate binder containing NCO groups (B), and a solid polyurethane acrylate binder (C). According to one example, this type of coating composition is applied to a PET film. The resulting layered composite is first dried at room temperature and then cured in an oven at 100°C. The resulting transfer laminate is applied under slight pressure to an aluminum profile pre-formed with a thin PU adhesive layer. The light radiator (1000 to 7000 mJ / cm²) is cooled with Hg. 2 After UV curing, the PET film can be peeled off from the currently painted aluminum profile without any problems.

[0005] WO2017 / 109118A1 describes a laminated material sheet having a surface layer on at least one board surface, the laminated material sheet having a coating containing a crosslinked polyurethane (meth)acrylate polymer as the outermost layer, and its advantages include excellent scratch resistance and weather resistance. Furthermore, a method for preparing a laminated material sheet coated with (meth)acrylate is provided, in which a coating composition is applied directly as a coating onto the surface material for the laminated material sheet. Summary of the Invention

[0006] In view of the foregoing, an object of the present invention is to provide a flexible, cost-effective, and mass-producible method for forming coated substrates, particularly coated laminated material sheets (including HPL sheets, "high-pressure laminates," and CPL sheets, "continuous pressure laminates"). Furthermore, an object of the present invention is to provide a suitable transfer foil by means of which a coating can be applied in a simple manner during sheet manufacturing (pressing). In particular, an object of the present invention is to provide a transfer foil that provides improved scratch resistance, better chemical resistance, and / or improved weather resistance. In particular, another object of the present invention is that the carrier material of the transfer foil remains on the sheet as a protection to the sheet surface until the final processing step (sheet cutting), so that the sheet including the carrier material thereon can be processed (cut).

[0007] Surprisingly, it has been found that the method according to the invention, the transfer foil obtained therefrom, and the transfer coating that can be prepared therefrom achieve at least one of the above-mentioned objectives.

[0008] In a first aspect, the present invention relates to a method for preparing a transfer foil comprising a carrier material and a coating comprising a thermoplastic polyurethane (meth)acrylate polymer, wherein the method comprises the following steps:

[0009] a) Applying a coating composition to a carrier material, wherein the coating composition comprises a resin component and a hardener component.

[0010] The resin component exists as a mixture comprising at least one component A and at least one component B, wherein,

[0011] Component A is a polymerizable (meth)acrylate compound, each molecule of which has at least two groups with (meth)acrylate double bonds and contains no hydroxyl groups.

[0012] Component B is a polymerizable (meth)acrylate compound, each molecule of which has one or more groups with (meth)acrylate double bonds and at least two hydroxyl groups;

[0013] b) Drying the carrier material coated in step a) at elevated temperature, wherein the hydroxyl groups in the resin component react with the isocyanate groups in the curing agent component to form a coating comprising a thermoplastic polyurethane (meth)acrylate polymer having (meth)acrylate double bond groups.

[0014] Therefore, the coating relates to a transferable coating. The term "thermoplastic" is commonly used by those skilled in the art and refers to polymeric materials that are deformable at high temperatures and thus can be processed using thermoplastic processing methods (e.g., extrusion and / or injection molding). The thermoplastic polyurethane (meth)acrylate polymer formed in step (b) has substantially non-crosslinked polymer chains. The coating obtained in step (b) is substantially non-sticky at room temperature and has storage stability at this temperature over a period of several weeks, thereby enabling intermediate storage and transport as well as simple handling during further processing. In the scope of subsequent applications, particularly in the preparation of laminated material sheets (see below), heat treatment is performed at temperatures ranging from 100°C to 210°C and under high pressure, wherein a polymer melt with outstanding adhesive properties is formed, ensuring particularly strong bonding to the respective substrates.

[0015] In a second aspect, the present invention relates to a transfer foil comprising a carrier material and a coating, wherein the coating comprises a thermoplastic polyurethane (meth)acrylate polymer, and the transfer foil is obtained according to a method according to the invention.

[0016] In a third aspect, the present invention relates to a method for preparing a laminated material plate, the laminated material plate comprising:

[0017] Carrier material,

[0018] Coatings of crosslinked polyurethane (meth)acrylate polymers, and

[0019] Core layer,

[0020] The laminated material plate serves as the outermost layer, having the carrier material, and the coating is disposed between the carrier material and the core layer; and

[0021] The method includes the following steps:

[0022] i) Provide a transfer foil comprising a carrier material and a coating containing a thermoplastic polyurethane (meth)acrylate polymer;

[0023] ii) Provide a pressed stack comprising a core layer of material for forming a laminated material sheet and a transfer foil provided in step i) as a surface layer, such that the transfer foil provided in step i) forms an outermost layer on at least one side of the pressed stack, and wherein a carrier material is present on at least one surface of the pressed stack.

[0024] iii) Extrusion pressing of stacked bodies under increased pressure and temperature, wherein polymerization of (meth)acrylic double bonds of thermoplastic polyurethane polymers occurs in the coating.

[0025] In a fourth aspect, the present invention relates to a laminated material sheet comprising:

[0026] Carrier material,

[0027] Coatings comprising crosslinked polyurethane (meth)acrylate polymers, and

[0028] Core layer,

[0029] The laminated material board serves as the outermost layer and has a carrier material, and the coating is disposed between the carrier material and the core layer.

[0030] And can be obtained according to the method according to the invention, wherein the coating preferably has a scratch resistance of ≥6N according to Section 25 of EN 438-2:2019.

[0031] Furthermore, the obtained laminated material surface preferably exhibits weather resistance according to Section 29 of EN438-2:2019, wherein the gloss change, measured at a 60° angle according to DIN EN ISO2813:2015-02, is at most 3 gloss units after more than 3000 hours. Additionally, it exhibits color stability according to the grayscale standard EN20105-A02 (no change) at grade 5 and / or stain resistance according to Chapter 26 of EN438-2:2019, wherein the surface reaches at least grade 5. Moreover, the coating displays excellent optical properties (no change) at grade 5 according to Sections 14 and 15 of EN438-2:2019. In subsequent cross-sectional adhesion tests according to ISO2400, the coating exhibits very good adhesion properties and a test value of Gt 0-1.

[0032] Finally, in a fifth aspect, the present invention relates to a method for preparing a component, wherein the method comprises the steps i) to iv):

[0033] i) Provide laminated material sheets as described above;

[0034] ii) Optionally process the laminated material sheet;

[0035] iii) Assemble the laminated material sheets in step i) or ii);

[0036] iv) Remove the carrier material.

[0037] In step a) of the method according to the invention, the coated coating composition comprises a resin component, a hardener component, and optional additives.

[0038] The resin component is a mixture comprising at least one component A and at least one component B. In addition to components A and B, the resin component may also contain other monomeric or polymeric components, adhesion promoters, and / or solvents.

[0039] Component A

[0040] Component A is a polymerizable (meth)acrylate compound having at least two groups per molecule bearing (meth)acrylate double bonds and containing no hydroxyl groups. Component A may be formed from a single type of such polymerizable (meth)acrylate compound or may contain multiple different types of such compounds.

[0041] As is commonly used by those skilled in the art, the terms "(meth)acrylic acid" or "(meth)acrylate" are used as abbreviations for methacrylic acid or acrylic acid, or methacrylate or acrylate. Therefore, the term "(meth)acrylate compound" as a general term includes not only compounds having an acrylate group CH2=CH-C(O)-O- as a group bearing an acrylic double bond, but also compounds having a methacrylate group CH2=CCH3-C(O)-O- as a group bearing a (meth)acrylate double bond. The group bearing a (meth)acrylate double bond in the compound of component A is preferably an acrylate group. Each molecule preferably has at least two (meth)acrylate double bonds, preferably two to eighteen, particularly preferably two to ten, and particularly preferably four to eight.

[0042] Furthermore, the compounds of component A differ from those of component B as defined below in that they do not contain hydroxyl groups. Additionally, compounds of component A preferably do not contain -SH and -NH2 groups. Particularly preferably, compounds of component A are those that do not contain any reactive groups other than at least two groups bearing (meth)acrylic double bonds. As will be readily apparent to those skilled in the art, the term "reactive group" here refers to a reaction that may occur between the components of the coating composition; that is, in these particularly preferred compounds of component A, at least two groups bearing (meth)acrylic double bonds, preferably at least two acrylate groups, are the only groups capable of reacting with the other components of the coating composition to form covalent bonds. As will also be understood to those skilled in the art, this applies particularly to the conditions under which the coating composition is subjected during the process according to the method of the invention.

[0043] Preferably, component A comprises a compound selected from formulas A1 and A2, more preferably a mixture comprising compounds of formulas A1 and A2. Particularly preferably, component A consists of compounds of formulas A1 and A2.

[0044] (A1)

[0045] in,

[0046] R 1 and R 3 Each group is independently selected from aliphatic hydrocarbon groups, aliphatic polyether groups, and aliphatic polyester groups.

[0047] R 2 It is an aliphatic hydrocarbon group or an alicyclic hydrocarbon group, and

[0048] n and m are independently 2 to 9, preferably 2 to 4.

[0049] As can be seen from formula A1, each of the m acrylate groups H2C=CH-C(O)-O- is bonded to the group R via an ester bond. 1 The groups are combined, and n acrylate groups are associated with group R. 3 Combine.

[0050] Preferably, R 1 and R 3 The alkyl group is independently selected from straight-chain or branched alkyl groups, preferably branched, and particularly preferably from alkyl groups having 3 to 10, more preferably 3 to 6 carbon atoms. 2 Preferably, it is an alkyl group, which may be open-chain (i.e., straight-chain or branched) or cyclic, or can be combined in open-chain or branched units, and is particularly preferred to have alkyl groups having 3 to 20, more preferably 6 to 12 C atoms.

[0051] Unless otherwise stated, the term "alkyl" or "alkyl group" is not limited to monovalent saturated hydrocarbon groups within the scope of this specification, but may also include groups with higher valences as clearly apparent from the appropriate context. For example, derived from formula A1, such as R... 1 It is provided in its preferred form as an alkyl group with an m+1 valence bond in formula A1 to bond with adjacent groups. This also applies accordingly to other components of the coating composition.

[0052] (A2)

[0053] in,

[0054] R 4 It is an aliphatic hydrocarbon group, and

[0055] o is 2 to 6, preferably 3 to 5.

[0056] Preferably, R 4 It is a straight-chain or branched alkyl group, preferably a branched alkyl group, particularly preferably an alkyl group having 3 to 10, more preferably 3 to 6 C atoms.

[0057] Preferably, the double bond density of component A is 3.0 mol / kg to 12.0 mol / kg, more preferably 4.0 mol / kg to 12.0 mol / kg, and particularly preferably 4.0 mol / kg to 11.0 mol / kg.

[0058] Component B

[0059] Component B is a polymerizable (meth)acrylate compound, each molecule of which has not only one or more groups bearing (meth)acrylate double bonds but also at least two hydroxyl groups. Component B may be formed from a single type of such polymerizable (meth)acrylate compound or may contain multiple different types of such compounds.

[0060] The compound of component B preferably contains acrylate groups, which are (meth)acrylic acid double bonds. Each molecule contains at least two (meth)acrylic acid double bonds, preferably two to nine, and particularly preferably two to four acrylate groups. Furthermore, the compound of component B contains at least two, preferably two to five, and particularly preferably two hydroxyl groups. These hydroxyl groups are typically alcohol hydroxyl groups.

[0061] Preferably, component B comprises a compound of formula B1, and is particularly preferably composed of a compound of formula B1:

[0062] (B1)

[0063] in,

[0064] R 5 Selected from aliphatic hydrocarbon groups, aliphatic polyether groups, and aliphatic polyester groups.

[0065] R 6 and R 7 Each is independently an aliphatic hydrocarbon group or an alicyclic hydrocarbon group, and

[0066] p is 2 to 9, preferably 2 to 4.

[0067] As can be seen from formula B1, each of the p acrylate groups H2C=CH-C(O)-O- is bonded to the group R via an ester bond. 5 The two hydroxyl groups are combined with group R. 7 Combine.

[0068] Preferably, R 5 It is a straight-chain or branched alkyl group, preferably a branched alkyl group, particularly preferably an alkyl group having 3 to 10, more preferably 3 to 6 carbon atoms. R 6 Preferably, it is an alkyl group, which may be open-chain (i.e., straight-chain or branched) or cyclic, or can be combined in open-chain or branched units, and is particularly preferred to have alkyl groups having 3 to 20, more preferably 6 to 12 C atoms. 7 Preferably, it is an alkyl group, which may be open-chain (i.e., straight-chain or branched) or cyclic, or can be combined in open-chain or branched units, particularly preferably a straight-chain or branched alkyl group having 3 to 20, more preferably 3 to 10 C atoms.

[0069] Preferably, the double bond density of component B is from 1.0 mol / kg to 8.0 mol / kg, more preferably from 2.0 mol / kg to 6.0 mol / kg, and particularly preferably from 3.0 mol / kg to 5.0 mol / kg.

[0070] The concentration of hydroxyl groups in component B is preferably 1.0 to 5.0 mol / kg, more preferably 2.0 to 4.0 mol / kg, and particularly preferably 2.5 to 3.5 mol / kg.

[0071] The concentration of urethane groups in component B is preferably 1.0 to 5.0 mol / kg, more preferably 2.0 to 4.0 mol / kg, and particularly preferably 2.5 to 3.5 mol / kg.

[0072] Component C

[0073] Furthermore, the resin component used according to the present invention may contain at least one component C, which is a polyurethane prepolymer having at least two hydroxyl groups per molecule, preferably exactly two hydroxyl groups, and is free of isocyanate groups.

[0074] Component C is a polyurethane prepolymer having at least two hydroxyl groups per molecule and being free of isocyanate groups. As will be apparent to those skilled in the art, the hydroxyl groups are typically alcohol hydroxyl groups. The polyurethane prepolymer can be linear or branched. It is preferably formed from a polyisocyanate having 2 to 4, preferably 2, isocyanate groups and a polyol having 2 to 4, preferably 2 or 3 alcohol hydroxyl groups. The polyisocyanate and polyol are preferably aliphatic compounds. The number of subunits formed from the polyisocyanate and the number of subunits formed from the polyol in the polyurethane prepolymer are preferably each 2 to 20, preferably 2 to 9. The number of hydroxyl groups per molecule of the polyurethane prepolymer is preferably at least 2, preferably 2 to 5, particularly preferably 2 to 3, for example 2.

[0075] The polyurethane prepolymer of component C does not contain isocyanate groups. Preferably, component C consists of polyurethane prepolymers that do not contain any other reactive groups besides the at least two hydroxyl groups. As will be appreciated by those skilled in the art, the term "reactive group" here refers to a possible reaction between the components of the coating composition; that is, in these preferred polyurethane prepolymers of component C, the at least two hydroxyl groups are the only groups capable of reacting with the other components of the coating composition to form covalent bonds. As will also be understood by those skilled in the art, this applies particularly to the conditions subjected to the coating composition during the process according to the method of the invention.

[0076] Preferably, component C comprises at least one compound of formula C1 and optionally at least one compound of formula C2. Particularly preferably, component C consists of a polyurethane prepolymer selected from compounds of formulas C1 and C2. A combination of compounds C1 and C2 is preferred.

[0077] (C1)

[0078] in,

[0079] R 8 Each time it appears, it is independently selected from aliphatic hydrocarbon groups, aliphatic polyether groups, and aliphatic polyester groups that can be replaced by one or more hydroxyl groups.

[0080] R 9 Each time they appear, they are independently aliphatic or alicyclic hydrocarbon groups, and

[0081] q is 2 to 9.

[0082] Preferably, all groups R 8 They are the same and all groups R 9 They are the same. Preferably, R 8 It is a straight-chain or branched alkyl group, preferably branched, and particularly preferably an alkyl group having 3 to 10, more preferably 3 to 6 carbon atoms. Alkyl group R 9 It can also be substituted by one or more hydroxyl groups, for example, having 0, 1, or 2 such hydroxyl substituents. R 9 Preferably, it is an alkyl group, which may be open-chain (i.e., straight-chain or branched) or cyclic, or can be combined in open-chain or branched units, and is particularly preferred to have alkyl groups having 3 to 20, more preferably 6 to 12 C atoms.

[0083] (C2)

[0084] in,

[0085] R 8 and R 8a Each time it appears, it is independently selected from aliphatic hydrocarbon groups, aliphatic polyether groups, and aliphatic polyester groups that can be replaced by one or more OH groups.

[0086] R 9 Each time they appear, they are independently aliphatic or alicyclic hydrocarbon groups, and

[0087] q is 2 to 9.

[0088] For formula C2, it is preferred that all groups R are used. 8 and R 8a They are the same and all groups R 9 They are the same. Preferably, the group R 8 and R 8a Each is a straight-chain or branched alkyl group, preferably branched, and particularly preferably an alkyl group having 3 to 10, more preferably 3 to 6 carbon atoms. Group R 8 and R 8a It can also be substituted by one or more hydroxyl groups. Preferably, in R 8 It contains one or two hydroxyl substituents, and in R8a It contains either 0 or 1 hydroxyl substituent. R 9 Preferably, it is an alkyl group, which may be open-chain (i.e., straight-chain or branched) or cyclic, or can be combined in open-chain or branched units, and is particularly preferred to have alkyl groups having 3 to 20, more preferably 6 to 12 C atoms.

[0089] Adhesion promoter

[0090] To improve the adhesion of the coating to the core layer of the laminate, the resin component may contain one or more adhesion promoters.

[0091] Suitable adhesion promoters particularly include compounds that can interact not only with the coating of the laminated sheet but also with the core layer. As the core layer for the laminated sheet, fiber-reinforced phenolic and amino plastic resins are typically used, or paper impregnated therewith and temporarily dried, or temporarily dried fiber pulp or fiberboard made therefrom. The structure of the core layer and the laminated sheet has been known to those skilled in the art and in the prior art for decades and has been standardized according to DIN EN438, ISO 4586, NEMAL D3, and JISK 6902. Therefore, according to the invention, it is preferable to introduce an adhesion promoter that can interact not only with the coating but also with the phenolic and amino plastic resins.

[0092] Suitable adhesion promoters also include monomeric, oligomeric, and polymeric adhesion promoters. Examples of monomeric and oligomeric adhesion promoters are epoxy or oxyethylene functionalized compounds (such as glycidyl ethers), epoxy or oxyethylene functionalized alcohols, (meth)acrylate functionalized alcohols, such as hydroxyethyl acrylate (HEA), methyl hydroxymethyl acrylate (HEMA), methyl hydroxypropyl acrylate (HPMA), pentaerythritol ester (PETIA), glycidyl (meth)acrylate, substances and mixtures thereof that can be synthesized by reacting aliphatic or alicyclic diisocyanates with (meth)acrylate-functionalized aliphatic branched and unbranched alcohols to produce epoxy or oxyethylene functionalized alcohols. Glycidyl ethers are particularly preferred and are commercially available, for example, under the product names GE100 and GE500 from Raschig GmbH.

[0093] Other suitable adhesion promoters are maleic acid derivatives, such as maleic acid, maleic anhydride (MSA), methylmaleic anhydride, maleimide, N-methylmaleimide, maleamide (MSA), N-phenylmaleimide and N-cyclohexylmaleimide, fumaric acid derivatives, methacrylic anhydride, and acrylic anhydride. When using adhesion promoters containing hydroxyl groups, the possible reaction between the hydroxyl groups and the isocyanate groups of the hardener component should be considered (see below), as the amount of the hardener component should be increased accordingly so that the resulting coating is substantially non-sticky after drying.

[0094] Suitable adhesion promoters also include organosilanes having the following structures:

[0095] (RO)3–Si–R'–X

[0096] in,

[0097] R contains an aliphatic hydrocarbon group, preferably an alkyl group or acyl group having 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and particularly preferably methyl, ethyl or acetyl groups;

[0098] R' contains an aliphatic hydrocarbon group, preferably an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms;

[0099] X contains an amino group, an epoxy group, or a (meth)acrylate group.

[0100] As will be apparent to those skilled in the art, the RO group is a hydrolyzable group, typically methoxy, ethoxy, or acetoxy, which can react with water to form a silanol group (Si–OH) and which ultimately bonds to the components of the coating and / or the resin of adjacent layers of the pressed stack. The X group can also react with the components of the coating and / or the resin of adjacent layers of the pressed stack. The corresponding adhesion promoter is, for example, Dynasylan®, commercially available from Evonik Operations GmbH.

[0101] In another embodiment, the adhesion promoter may be an acrylic resin composed of monomers having reactive groups. Examples of suitable reactive groups include hydroxyl, carboxyl, amino, amide, anhydride, imide, and epoxy groups. The acrylic resin may contain one or more of these reactive groups. Examples of monomers having reactive groups are: monomers having hydroxyl groups, such as hydroxyalkyl methacrylate; monomers having carboxyl groups, such as (meth)acrylic acid, (meth)acryloyloxyalkyl carboxylic acid, or aromatic (meth)acryloyloxy carboxylic acid; monomers having amino groups, such as (meth)acrylic acid-aminoalkyl acrylate; monomers having amide groups, such as (meth)acrylic acid-alkylamide alkyl acrylate; anhydride monomers, such as maleic anhydride; maleimide monomers, such as maleimide or alkylmaleimide; and monomers having epoxy groups, such as glycidyl methacrylate.

[0102] In another embodiment, the adhesion promoter may be a polyester resin having reactive groups. Examples of suitable reactive groups include hydroxyl, carboxyl, amino, amide, anhydride, imide, and epoxy groups, and ionic groups such as alkylammonium groups. Suitable polyester resins with reactive groups are commercially available from BYK-Chemie GmbH and Worlée-Chemie GmbH.

[0103] In another embodiment, the adhesion promoter may be an etherified or partially etherified amino plastic resin, preferably an etherified or partially etherified melamine-formaldehyde resin (MF resin). Examples are n-butyl, isobutyl, and methylated MF resins. These are available from Prefere Resins Holding GmbH under the names Maprenal® and Resimene®.

[0104] In another embodiment, the adhesion promoter may be an isocyanate derivative wherein the reactivity of the isocyanate group is blocked at room temperature to 120°C. It may be a polyisocyanate having isocyanurate, biuret, urethane, iminooxadiazine dione, carbamate, urea, carbodiimide, and / or urea dione groups. These can be prepared in a conventional and known manner from the diisocyanates described below (i). The corresponding products are known to those skilled in the art and are commercially available, for example, as Desmodur® BL from Covestro AG.

[0105] In addition, the resin component of the coating composition may include at least one solvent. Examples of exemplary solvents include esters such as ethyl acetate, butyl acetate, or 2-butoxyethyl acetate, aliphatic hydrocarbons, alicyclic hydrocarbons and aromatic hydrocarbons, alcohols, glycol ethers, or ketones. The total concentration of components A and B, and if present, component C and / or the adhesion promoter, may be from 50% to 100% by weight based on the total weight of the coating composition.

[0106] To prepare the resin component of the coating composition, components A and B, as well as component C (if present) and / or an adhesion promoter, can be provided and mixed. Alternatively, for example, particularly to provide component A (e.g., a compound of formula A1), component B, and component C, starting products such as polyols, polyisocyanates, and / or compounds with mixed functionalities such as polyacrylates having one or more hydroxyl groups can be mixed, wherein components A, B, and C can be prepared from the above-described composition within the range of the synthesis of the resin component. For example, the resin component can be prepared by one-step or multi-step synthesis at a temperature of 30 to 130°C.

[0107] In the resin composition, based on the total weight of components A to C and the adhesion accelerator, component A is preferably present in an amount of 30.0 to 80.0% by weight, component B is preferably present in an amount of 15.0 to 70.0% by weight, component C is present in an amount of 0.0 to 5.0% by weight, and the adhesion accelerator is present in an amount of 0.0 to 10.0% by weight. Here, the total amount of the components is 100% by weight.

[0108] In a more preferred embodiment, the resin component comprises a component of formula A1 in an amount of 15.0 wt% to 45.0 wt%, a component of formula A2 in an amount of 15.0 wt% to 45.0 wt% (wherein the total amount of A1 and A2 is 30.0 wt% to 80.0 wt%), and a component of formula B1 in an amount of 15.0 wt% to 70.0 wt%. If present, components C1 and C2 are present in a total amount of 0.0 to 5.0 wt%, and an adhesion promoter is present in an amount of 0.0 to 9.0 wt%. Here, the total amount of the components is 100 wt%.

[0109] In one, or even more preferred, embodiment, the resin component comprises, in amounts of 15.0% to 40.0% by weight of component A1, in amounts of 15.0% to 40.0% by weight of component A2 (wherein the total amount of A1 and A2 is 30.0% to 80.0% by weight), in amounts of 25.0% to 60.0% by weight of component B1, in amounts of, if present, in amounts of, 0.0% to 3.0% by weight of components C1 and C2, and in amounts of, 0.0% to 8.0% by weight of adhesive accelerator. Here, the total amount of said components is 100% by weight.

[0110] hardener components

[0111] In addition to the resin component, the coating composition also includes a hardener component, which is at least a bifunctional isocyanate. The isocyanate of the hardener component preferably contains 2 to 4 isocyanate groups. Optionally, the isocyanate groups may have their reactivity blocked at room temperature.

[0112] Preferred examples of the hardener components are as follows (i) to (iii):

[0113] (i) can use formula R 11 -[-N=C=O] s The isocyanate, wherein s is 2 to 4, preferably 2 or 3, and R 11 It is an aliphatic hydrocarbon group or an alicyclic hydrocarbon group, preferably an open-chain (i.e., straight-chain or branched) or cyclic alkyl group, or it can be combined in an open-chain or branched unit, particularly preferably an alkyl group having 3 to 20, more preferably 3 to 12 C atoms.

[0114] Suitable examples of isocyanates are isophorone diisocyanate, 5-isocyano-1-(isocyanomethyl-1,3,3-trimethylcyclohexane), 5-isocyano-1-(2-isocyanoethyl-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyano-1-(3-isocyanopropyl-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyano-(4-isocyanobutyl-1-yl)-1,3,3-trimethylcyclohexane, 1-isocyano-2-(3-isocyanopropyl-1-yl)cyclohexane, 1-isocyano-2-(3-isocyanoethyl-1-yl)cyclohexane, 1- Isocyanate-2-(4-isocyanate-but-1-yl)cyclohexane, 1,2-diisocyanate-cyclobutane, 1,3-diisocyanate-cyclobutane, 1,2-diisocyanate-cyclopentane, 1,3-diisocyanate-cyclopentane, 1,2-diisocyanate-cyclohexane, 1,3-diisocyanate-cyclohexane, 1,4-diisocyanate-cyclohexane, dicyclohexylmethane-2,4'-diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), ethylethylene diisocyanate, trimethylhexane diisocyanate, heptamethylene diisocyanate, methylpentyl diisocyanate Diisocyanate (MPDI), nonane triisocyanate (NTI), or diisocyanates derived from dimer fatty acids as described in WO97 / 49745 and WO97 / 49747, particularly 2-heptyl-3,4-bis(9-isocyanate-nonyl)-1-pentylcyclohexane, or 1,2-, 1,4- or 1,3-bis(isocyanate-methyl)cyclohexane, 1,2-, 1,4- or 1,3-bis(2-isocyanate-ethyl-1-yl)cyclohexane, 1,3-bis(3-isocyanate-propyl-1-yl)cyclohexane, 1,2-, 1,4- or 1,3-bis(4-isocyanate-butyl-1-yl)cyclohexane, or as described in the patent application The trans / trans isomer content described in DE4414032A1, GB1220717A1, DE1618795A1, and DE1793785A1 can reach up to 30% by weight, preferably 25% by weight, and particularly 20% by weight, of liquid bis(4-isocyanate cyclohexyl)methane, preferably isophorone diisocyanate, 5-isocyanate-1-(2-isocyanate ethyl-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyanate-1-(3-isocyanate propyl-1-yl)-1,3,3-trimethylcyclohexane, or 5-isocyanate-1-(4-isocyanate butyl-1-yl)-1,3...3-Trimethylcyclohexane, 1-isocyano-2-(3-isocyano-propyl-1-yl)cyclohexane, 1-isocyano-2-(3-isocyano-ethyl-1-yl)cyclohexane, 1-isocyano-2-(4-isocyano-butyl-1-yl)cyclohexane, or hexamethylene diisocyanate, with hexamethylene diisocyanate being particularly preferred.

[0115] (ii) Oligomers, such as dimers or trimers composed of isocyanates of the formula given below (i). A preferred example of such oligomers is a trimer of hexamethylene diisocyanate.

[0116] (iii) A derivative of the isocyanate described in (i) or (ii), wherein the reactivity of the isocyanate group is blocked at room temperature. It may be a polyisocyanate having isocyanurate, biuret, urethane, iminooxadiazine dione, carbamate, urea, carbodiimide and / or urea dione groups, which are generally prepared from the above diisocyanates in a known manner.

[0117] The ratio of resin component to hardener component in the coating composition (as a ratio of the weight of component A+B+C to the weight of hardener component) is preferably in the range of 100 / 20 to 100 / 40, and particularly preferably in the range of 100 / 25 to 100 / 35.

[0118] Here, it is preferable to select the amounts of components A+B+C relative to the curing agent components such that the hydroxyl groups of component B exist in stoichiometric amounts relative to the free isocyanate groups of the curing agent components.

[0119] In order to provide a coating composition, the resin component and the hardener component are mixed together with optional additives if necessary. After the two components are mixed, the service life of the coating composition is typically in the range of one hour to several hours, for example, between 1 and 3 hours.

[0120] Other optional additives that can be added to coating compositions are known to those skilled in the art. Examples that can be used alone or in combination include inhibitors, catalysts, polymerization initiators, light stabilizers, fillers, dyes, pigments, additives that affect gloss, additives that improve the wetting of carrier materials, additives that improve surface uniformity, additives that improve surface smoothness, additives that reduce clogging tendency, solubilizers, flame retardants, UV absorbers, and additives that improve conductivity.

[0121] To further improve abrasion resistance, especially scratch and wear resistance, hard additives such as corundum, alumina, and / or appropriately designed nanoparticles can be included in the coating composition. Additionally, substances that reduce surface energy can be introduced, which can also be combined with suitable microstructured surfaces to mimic the lotus effect.

[0122] Preferably, the coating composition contains one or more polymerization initiators as additives, i.e., compounds that form free radicals when heated, for example, to 130°C or higher. An example of a suitable polymerization initiator is tert-butyl peroxybenzoate. The amount of the additive can be suitably selected by those skilled in the art. Preferably, the coating composition comprises: a resin component, an adhesion promoter component, and a hardener component in a total amount of at least 90% by weight, and optional additives in a total amount of at most 10% by weight, with the total weight of the coating composition as 100% by weight. Here, the dosage refers to solids content, i.e., excluding any solvents that may be present.

[0123] Furthermore, the coating composition may contain one or more light stabilizers. Light stabilizers are generally known and are described in detail, for example, in Hans Zweifel, *Plastics Additives Handbook*, Hanser Press, 5th edition, 2001, page 141 and following pages. Light stabilizers include UV absorbers, UV stabilizers, and free radical scavengers.

[0124] Suitable UV absorbers are exemplary selected from the group consisting of substituted benzophenones, salicylates, cinnamates, oxaloyl aniline, benzoxazinones, benzotriazoles, triazines, or benzylmethylene malonates, wherein benzotriazoles and triazines, and combinations thereof, are particularly preferred. The most well-known representatives of UV stabilizers are sterically hindered amines (hindered amine light stabilizers, HALS).

[0125] Benzotriazole-type UV absorbers typically contain 2-(2'-hydroxyphenyl)benzotriazole. Relevant compounds specifically include 2-(2'-hydroxy-5'-methylphenyl)-benzotriazole, 2-(3',5'-di-tert-butyl-2'-hydroxyphenyl)benzotriazole, 2-(5'-tert-butyl-2'-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-(1,1,3,3-tetramethylbutyl)phenyl)benzotriazole, 2-(3',5'-di-tert-butyl-2'-hydroxyphenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-methylphenyl)-5-chloro-benzotriazole, 2-(3'-sec-butyl-5'-tert-butyl-2'-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-4'-methyl ... 2-(3',5'-di-tert-pentyl-2'-hydroxyphenyl)benzotriazole, 2-(3',5'-bis-(α,α-dimethylbenzyl)-2'-hydroxyphenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)-carbonyl-ethyl]-2'-hydroxyphenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-methoxycarbonyl-ethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl) ... 2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonyl-ethyl)phenyl)benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)carbonyl-ethyl]-2'-hydroxyphenyl)benzotriazole, 2-(3'-dodecyl-2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-isooctyloxycarbonyl-ethyl)phenyl)benzotriazole, 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-benzotriazole-2- [3'-tert-butyl-5'-(2-methoxycarbonyl-ethyl)-2'-hydroxyphenyl]-2H-benzotriazole and polyethylene glycol 300 transesterification product; [R-CH2CH2-COO-CH2CH2-, where R=3'-tert-butyl-4'-hydroxy-5'-2H-benzotriazole-2-ylphenyl, 2'-[2'-hydroxy-3'-(α,α-dimethylbenzyl)-5'-(1,1,3,3-tetramethylbutyl)-phenyl]-benzotriazole; 2'-[2'-hydroxy-3'-(1,1,3,3-tetramethylbutyl)-5'-(α,α-dimethylbenzyl)-phenyl]benzotriazole.Other examples of available benzotriazole-type UV absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-[2-hydroxy-3,5-di(α,α-dimethylbenzyl)phenyl]benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-butyl-5-methylphenyl)-5-chlorobenzotriazole, and 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole. 1-Chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3-sec-butyl-5-tert-butylphenyl)benzotriazole and 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, phenol, 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)]. These compounds are also available, for example, as Tinuvin® 360, Tinuvin® 1130 and Tinuvin® 234 from BASF SE (Ludwigshafen, Germany) and, for example, as Chiguard® 234, Chiguard® 5528, Chiguard® 5431, Chiguard® 5530, Chiguard® 5582 from Chitec Technology Co., Ltd.

[0126] Triazine-type UV absorbers are typically 2-(2-hydroxyphenyl)-1,3,5-triazine derivatives. Preferred 2-(2-hydroxyphenyl)-1,3,5-triazines include, in particular, 2,4,6-tris-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, (dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2,4-bis(2-hydroxy-4-propyloxyphenyl). (2,4-Dimethylphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-octyloxyphenyl)-4,6-bis(4-methylphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-dodecyloxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-tridecyloxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[2-hydroxy [-4-(2-hydroxy-3-butoxypropoxy)phenyl]-4,6-bis(2,4-dimethyl)-1,3,5-triazine, 2-[2-hydroxy-4-(2-hydroxy-3-octyloxypropyloxy)phenyl]-4,6-bis(2,4-dimethyl)-1,3,5-triazine, 2-[4-(dodecyloxy / tridecyloxy-2-hydroxypropoxy)-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine Azine, 2-[2-hydroxy-4-(2-hydroxy-3-dodecyloxypropoxy)phenyl]-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-hexyloxy)phenyl-4,6-diphenyl-1,3,5-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-1,3,5-triazine, 2,4,6-tris[2-hydroxy-4-(3-butoxy-2-hydroxypropoxy)phenyl] Triazine-type UV absorbers, such as 2-(2-hydroxyphenyl)-4-(4-methoxyphenyl)-6-phenyl-1,3,5-triazine, 2-{2-hydroxy-4-[3-(2-ethylhexyl-1-oxy)-2-hydroxypropyloxy]phenyl}-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2,4-bis(4-[2-ethylhexyloxy]-2-hydroxyphenyl)-6-(4-methoxyphenyl)-1,3,5-triazine, can also be used.These compounds are commercially available from BASF SE (Ludwigshafen, Germany) under the trademarks Tinuvin® 1600, Tinuvin® 1577, Tinuvin® 400 or Tinuvin® 1545, and from Chitec Technology Co., Ltd. as Chiguard® 1064, Chiguard® 5400, Chiguard® 5405, Chiguard® 5577, Chiguard® 460, Chiguard® 477, for example.

[0127] Staggered amines, or HALS (hindered amine light stabilizers), are known UV stabilizers. They can be used to suppress aging in paints and plastics, particularly polyolefin plastics (Kunststoffe, 74(1984)10, pp. 620-623; Farbe + Lack, Vol. 96, September 1990, pp. 689-693). The tetramethylpiperidine group present in HALS compounds is responsible for the stabilizing effect. These compounds may be unsubstituted on the piperidine nitrogen or have substitution on the piperidine nitrogen via alkyl or acyl groups. Staggered amines do not absorb in the UV region. They scavenge already formed free radicals, which UV absorbers cannot do. Examples of HALS compounds that have stabilizing properties and can also be used in mixture form are: bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, 8-acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro(4,5)-decane-2,5-dione, bis(2,2,6,6-tetramethyl-4-piperidinyl) succinate, poly(N-β-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidinyl succinate) or bis(N-methyl-2,2,6,6-tetramethyl-4-piperidinyl) sebacate. These compounds were purchased, for example, under the trademarks Tinuvin® 123 and Tinuvin® 292 from BASF SE (Ludwigshafen, Germany) and, for example, as Chiguard® 100, Chiguard® 353, Chiguard® 2285, Chiguard® 101, Chiguard® 106, and Chiguard® 4050 from Chitec Technology Co., Ltd.

[0128] Light stabilizers are typically used in amounts of 0.1 to 10% by weight, preferably 0.5 to 5% by weight, based on the total weight of the coating composition.

[0129] Furthermore, the coating composition may contain one or more wetting agents that reduce the surface tension of the coating composition and thereby improve the wetting of the carrier material in step (a). Wetting agents and wetting mechanisms are generally known and are described in detail, for example, in sections 2.1.4.2, 2.2.3, and 3.1.1 of the BASF Coatings Technology Handbook (by Professor Dr. Artur Goldschmidt and Dr. Hans-Joachim Streitberger, Vincentz Publishers, 2002, ISBN 3-87870-324-4).

[0130] Suitable wetting agents include, in particular, siloxane-containing compounds, polyacrylate-based additives, fluorinated surfactants, EO / PO block copolymers, and siloxane-free surfactants based on alcohol alkoxylates. Preferred wetting agents are those that do not adversely interact with the isocyanate or hydroxyl functional groups of polyurethane (meth)acrylate adhesives. Examples include additives containing polydimethylsiloxane, modified acrylate-based polyethers, fluorinated alkyl polyethers, and nonionic surfactants. These additives also help improve leveling properties, reduce pitting, and ensure uniform film formation, and are available, for example, from manufacturers known to those skilled in the art such as BYK-Chemie GmbH (BYK-310, BYK-314, BYK-3765) or Evonik Industries AG (TEGO® WET, TEGO® TWIN).

[0131] The concentration of wetting agent in the coating composition used according to the invention is typically from 0.05% by weight to 2.0% by weight based on the total weight of the coating composition.

[0132] The coating composition is typically liquid at 25°C and normal pressure and has a viscosity, for example, from 100 to 3000 mPas.

[0133] According to the method of the invention, the coating composition is applied as a coating onto the carrier material in step (a). The application of the coating composition can be performed by known methods, such as using a roller or a slit nozzle. Preferably, the coating is applied such that a closed film of the coating composition is formed on the carrier material. The amount applied is preferably between 20 and 150 g / m³. 2 Within the range, particularly preferred is 50 to 100 g / m 2 Within the range.

[0134] In the method according to the invention, smooth, matte, or structured paper, metal foil (especially copper or aluminum foil), and / or plastic film impregnated or coated with a water-repellent agent are preferably used as carrier materials. As plastic films, in particular polyethylene, polypropylene, or polyester films, for example, suitable are PET films, each with a water-repellent (with a release agent) pretreatment or no pretreatment. Composite materials composed of the aforementioned paper and film are also suitable. Preferably, the paper and film are also pretreated with a water-repellent agent on their back side, for example, coated with a release agent such as silicone. Additional microstructuring on the back side aids this effect. This aids in the storage capacity of the product according to the invention by preventing blockage in product rolls or stacks. In a further preferred embodiment, the carrier material is transparent.

[0135] For good transferability of the coating to be transferred onto the target surface (laminated substrate), it is particularly advantageous to coordinate the adhesion between the coating and the carrier material. Therefore, in the method according to the invention, on the one hand, an uncoated carrier material can be used, which, due to its surface tension, does not completely adhere to the coating; on the other hand, the carrier material, such as paper, can be provided with a release agent, such as a stearic acid-based, wax-based, or silicone-based release agent, to produce the desired release properties (the ability of the carrier material to peel off from the fully cured coating). By optimally controlling the release properties, another advantage of the method according to the invention is the possibility that a protective film (laminated foil) subsequently applied to the laminated substrate can generally be eliminated, as these carrier materials remain on the coated laminated substrate during the transfer of the suitable carrier material (base substrate) and are only removed by the end user. When a transparent substrate is used as the carrier material, quality control can be implemented on the surface of the laminated substrate, including impurities such as inclusions or color defects that penetrate the transparent carrier material. The carrier material typically has a thickness of 10 μm to 1000 μm, preferably 20 μm to 300 μm.

[0136] Therefore, the transfer foil of the present invention comprises a carrier material and a coating, wherein the carrier material can be used as a surface forming material on the one hand and as a release medium on the other hand due to the coordination of surface energy, and the coating comprises a thermoplastic polyurethane (meth)acrylate polymer. Optionally, the coating may comprise a substance that can be crosslinked by methods other than free radical or ionic polymerization, such as a base polymer that can be crosslinked by addition or condensation reactions.

[0137] After the coating composition is applied, the transfer foil is dried in the next step (b), wherein a coating comprising a thermoplastic polyurethane (meth)acrylate polymer is formed. As will be apparent to those skilled in the art, the term "drying" refers to the transformation of the coating composition from a liquid state to a state where it is no longer flowable when the surface material is treated at room temperature, preferably at a temperature below 50°C. In this step, any solvent present is completely or partially removed.

[0138] Drying is carried out at elevated temperatures, during which the hydroxyl groups in the resin component react with the isocyanate groups in the hardener component of the coating composition, resulting in the formation of a thermoplastic polyurethane (meth)acrylate polymer with (meth)acrylate double bonds in the coating. Typically, drying is carried out at a temperature of 110°C or lower, preferably in the temperature range of 70 to 100°C. At this temperature, it is ensured that the reaction with the hardener component proceeds at a sufficiently high rate before the (meth)acrylate double bonds have polymerized. As an aid, an inhibitor can be added to the coating composition to prevent the (meth)acrylate double bonds from polymerizing during the drying step, and a catalyst can be added to promote the reaction between the isocyanate groups of the hardener component and the hydroxyl groups of the resin component. In this way, the processability of the coating on a fully automated roll coating machine can be optimally controlled.

[0139] Advantageously, the transfer foil according to the invention has a coating after the drying step, which is corrosion-resistant and has no segments relative to the back of the carrier. The transfer foil can be easily transported, stored, and further processed, and is therefore a valuable intermediate product in the manufacture of laminated material sheets. Typically, the coating after drying has a thickness between 2.0 μm and 1000 μm, preferably between 10 μm and 300 μm.

[0140] The transfer foil according to the invention can, for example, be incorporated into the manufacturing process of a laminated material sheet by placing one or both sides of the transfer foil onto a core layer made of a material impregnated with a synthetic resin, wherein the side of the coating to be transferred is placed on the core layer, the composite is pressed under normal temperature, pressure, and time conditions, and after cooling, the carrier material can be pulled out or retained thereon to protect the sheet surface until final processing (sheet blank). This yields a laminated material sheet whose surface has been treated with the gloss or matte finish of the carrier film, and which exhibits high scratch and abrasion resistance and provides excellent weather resistance.

[0141] After drying the transfer foil, a pressed stack is provided, which contains a core layer material for forming a laminated material sheet and a transfer foil according to the invention as a surface layer. At least on one side, optionally on both sides, the dried transfer foil according to the invention forms the outermost layer of the pressed stack, and a carrier material is disposed on at least one surface, optionally on both surfaces, of the pressed stack.

[0142] The material used to form the core layer of the laminated material sheet comprises one or more, preferably multiple, layers of material impregnated with a curable synthetic resin. Suitable materials are familiar to those skilled in the art. This typically involves planar materials, i.e., materials whose length and width are significantly greater than their thickness, such as foils, sheets, webs of material, or curved portions of material. The layers may be made of the same material or two or more different materials.

[0143] The material used to form the core layer of the laminated material sheet comprises one or more, preferably multiple layers of material impregnated with a curable synthetic resin. Preferably, the number of layers is in the range of 1 to 200, particularly 2 to 120.

[0144] In a particularly preferred embodiment, the material used to form the core layer comprises a decorative layer on at least one side of the outermost layer. Examples of suitable materials for the decorative layer are nonwoven, non-woven fabrics, or woven fabrics made of natural or synthetic organic or inorganic fibers, particularly in the form of webs, sheets, or foils of such materials made of plastics (thermoplastics, thermosetting plastics, or elastomers), metals, wood, stone, glass, or composite materials. A preferred example of a suitable material is paper, for example, in the form of paper webs. Particularly preferred is a paper web impregnated, dyed, or printed with a curable synthetic resin as the material for the decorative layer. The curable synthetic resin used here can be synthetic resins known for their application in laminated sheets, such as phenolic resins (PF resins), melamine-formaldehyde resins (MF resins), urea-formaldehyde resins (UF resins), or mixtures thereof, epoxy resins, polyester resins, thermoplastics, or elastomers. Preferably, phenolic resin (PF resin), melamine-formaldehyde resin (MF resin), urea-formaldehyde resin (UF resin), or a mixture thereof is used as the curable synthetic resin.

[0145] After the stack is pressed, it is pressed under increased pressure and at a temperature higher than the drying temperature, at which the transfer foil according to the invention is dried. The temperature is chosen to be high enough that polymerization of (meth)acrylic double bonds occurs in the dried coating. The pressure used during pressing is typically between 300 and 900 N / cm². 2The pressure is within the range of 3.0 to 9.0 MPa. Those skilled in the art can select and adjust the extrusion pressure accordingly to suit their press system. The temperature is typically above 110°C, preferably in the range of 135 to 210°C. Pressing is typically performed over a period of 30 seconds to 100 minutes.

[0146] If necessary, the pressing can be carried out in a hot press having a surface with a given structure and giving the laminated material sheet a surface structure.

[0147] Preferably, the core layer includes at least one decorative layer disposed on at least one outer side of the core layer.

[0148] According to the present invention, a laminated material plate having a core layer and a surface layer is formed on at least one plate surface, the plate surface having a coating containing a crosslinked polyurethane (meth)acrylate polymer as the outermost layer. The crosslinked polyurethane (meth)acrylate polymer comprises polymeric units linked by urethane bonds and polymeric units linked by carbon-carbon bonds via (meth)acrylate double bonds. Furthermore, the crosslinked polyurethane (meth)acrylate polymer also comprises sub-units formed of a resin having a phenolic or amino plastic backbone, by using an adhesion promoter at the interface with the core layer in the coating composition. Preferably, the coating is composed of a crosslinked polyurethane (meth)acrylate polymer, which, as described above, is formed from a resin component, a hardener component, an adhesion promoter, and optional additives.

[0149] Therefore, according to the present invention, a laminated material sheet is provided having a core layer and a transfer foil on at least one surface, the surface serving as a carrier material with the transfer foil as the outermost layer. If an adhesion promoter is used, the crosslinked polyurethane (meth)acrylate polymer has sub-units at the interface with the core layer, these sub-units being formed by the reaction of the adhesion promoter with a resin having a phenolic or amino plastic backbone. After the carrier material is pulled out, the coating containing the crosslinked polyurethane (meth)acrylate polyurethane polymer exhibits high scratch resistance, and its gloss changes only slightly during weathering. Furthermore, the surface of the obtained laminated material sheet has a stain resistance rating of 5 according to EN 438-2.26:2019, thus allowing for easy removal of graffiti and other dirt (easy to clean). In particular, the surface has a scratch resistance of ≥6N (measured according to EN438-2.25:2019) and a gloss change of no more than 3 gloss units, preferably no more than 2, after 3000 hours by the method of EN438-2.29:2019 (measured according to DINENISO2813:2015-02 at an angle of 60°).

[0150] Furthermore, the coating exhibits excellent optical properties (without variation) according to Sections 14 and 15, Grade 5, of EN438-2:2019. In subsequent cross-sectional adhesion tests according to ISO2400, the coating showed very good adhesion properties and a test value of Gt0-1.

[0151] The adhesion between the sheet material used as the core (core layer) and the coating applied to the carrier material naturally depends on the sheet material used. To achieve this adhesion, the present invention essentially provides two basic mechanisms: on the one hand, using a coating composition comprising a thermoplastic polyurethane (meth)acrylate polymer, which melts under pressure and elevated temperature, resulting in thermoplastic inflow into the existing pores and uneven surfaces of the core layer and thus physically bonds it; on the other hand, optionally additionally including a suitable adhesion promoter, which enables the coating comprising the thermoplastic polyurethane (meth)acrylate polymer to be chemically and additionally bonded to the core layer, or both. In the second case, as mentioned above, an adhesion promoter can be added to the coating composition, enabling targeted adhesion control based on selected physical or chemical properties.

[0152] Compared to direct methods (applying the coating directly to the core layer), the method according to the invention has the following advantages: it is substantially independent of the amount of material to be coated and the finish. In other words, fewer batches can be covered using the method according to the invention. For example, it is possible to apply abrasion-resistant and weather-resistant coatings to multiple smaller batches of material, each with different surface finishes, because the transfer foil according to the invention can not only be easily manufactured in smaller quantities, but can also be used in the same form regardless of batch size and finish.

[0153] The coating is applied in the final step of the laminate production process. Here, the method according to the invention can be implemented in a continuous or discontinuous manner.

[0154] By designing the surface of the carrier material in contact with the coating, decorative properties (such as special structures, colors, matte finishes) and functional properties introduced through micro-roughness, such as ease of cleaning or fingerprint resistance, can be transferred to the coating and thus to the core layer to be coated. Overall, this method offers significant economic advantages because individual components can also have surface protection according to this method, and therefore there are no limitations on larger quantities.

[0155] Furthermore, a particularly advantageous aspect of using the above-described coating composition is that, due to the thermoplastic properties of the thermoplastic polyurethane (meth)acrylate polymer, excellent deformability of the transfer coating is achieved during pressing to form HPL or CPL boards, while simultaneously achieving a high crosslinking density and therefore outstanding durability on the board surface produced in the same process steps. Moreover, the described layers adhere particularly well to each other. This adhesion is not lost under normal thermal, mechanical, or chemical influences.

[0156] During the manufacture of laminated material sheets, the coating of the transfer foil according to the invention ensures excellent chemical and / or mechanical adhesion to the core layer of the laminated material sheet. Therefore, the additional use of adhesive layers commonly found in the prior art can be eliminated.

[0157] Laminated sheets manufactured using the method of the present invention are characterized by particularly good abrasion resistance, especially high scratch resistance and weather resistance. They are suitable for interior applications, but are also particularly preferred for exterior applications, such as wall coverings, roofing elements, or outdoor furniture. The method according to the invention particularly enables combinations of particularly scratch-resistant surfaces with decorative design possibilities, wherein the materials obtained according to the invention are characterized by a particularly long service life. Laminated sheets can be manufactured continuously in the form of webs, but can also be manufactured discontinuously as individual elements.

[0158] The laminated material sheet according to the invention is particularly suitable for manufacturing components, preferably building facade elements, using a method comprising the following steps i) to iv):

[0159] i) Provide laminated material sheets;

[0160] ii) Optionally process the laminated material sheet;

[0161] iii) Assemble the laminated material sheet in step (i) or (ii);

[0162] iv) Remove the carrier material.

[0163] The laminated material sheet provided in step i) can be processed in an optional second step ii). This processing may include, for example, cutting, drilling, milling, punching, edge finishing, introduction of connecting elements, or other machining steps. The processing can be performed automatically or manually and is adapted to the specific requirements of subsequent components or the application site. These processing steps can be omitted once the laminated material sheet provided in step i) already exists in the desired shape and size.

[0164] In step iii), processed or unprocessed laminated material sheets are installed in or on the target component. In applications to building facade elements, this may, for example, involve inserting the sheets into a supporting frame system, applying them to the substructure, or bonding them to a carrier material. The assembly may also include temporary fixing if the carrier material should be removed only after securing it in the next step.

[0165] After assembly, the carrier material is removed in step vi). This can be done by pulling, peeling, or mechanical removal. Removal is preferably performed after assembly to ensure protection of the decorative surface of the laminated material sheet during processing and handling. Therefore, the use of an additional laminating film is not required.

[0166] The method according to the invention enables the reliable manufacturing and assembly of decorative and / or functional components with high surface quality. High durability against weather effects, mechanical loads, and UV radiation is achieved through the use of HPL or CPL panels, emphasizing their suitability as building facade elements. Detailed Implementation

[0167] The present invention will now be described in detail with reference to various embodiments.

[0168] Example

[0169] Explanation of quantities in grams

[0170] Example 1

[0171] Coating composition:

[0172]

[0173] The coating composition was applied to a structured aluminum-laminated paper with a thickness of 100 μm onto its aluminum surface and dried in a hot air drying oven at 100 °C for 5 minutes. The resulting paper-aluminum-coating composite (transfer foil) was then placed in direct contact with the coating surface on a stack consisting of melamine-impregnated decorative paper and phenolic resin-impregnated core paper, and dried together with them at 700 N / cm. 2 It is pressed at 145°C for 10 minutes under pressure to finally cure.

[0174] After cooling, a laminated sheet (HPL) is obtained. The aluminum-laminated paper can be pulled off the laminated sheet with very little force, and the finally cured coating is inseparably bonded to the melamine resin layer of the resulting HPL sheet. Here, the now hard and scratch-resistant coating accepts the surface structure of the aluminum-coated paper.

[0175] Example 2

[0176] Coating composition:

[0177]

[0178] The coating composition was applied by scraping onto a structured silicone release paper with a structured silicone surface, the layer thickness being 100 μm, and dried in a hot air drying oven at 100 °C for 5 minutes. The resulting paper-coating composite (transfer foil) was then placed in direct contact with the coating surface on a stack consisting of melamine resin-impregnated decorative paper and phenolic resin-impregnated core paper, and dried together with them at 700 N / cm. 2 It is pressed at 145°C for 10 minutes under pressure to finally cure.

[0179] After cooling, a laminated sheet (HPL) is obtained. The silicone release paper can be pulled out of the laminated sheet with very little force, and the finally cured coating is inseparably bonded to the melamine resin layer of the resulting sheet. Here, the now hard and scratch-resistant coating accepts the surface structure of the silicone release paper.

[0180] Example 3

[0181] Coating composition:

[0182]

[0183] The coating composition was applied onto a smooth polyester film to a thickness of 100 μm and dried in a hot air drying oven at 100 °C for 5 minutes for pre-crosslinking. The resulting foil-coating composite (transfer foil) was then placed in direct contact with the coating surface on a stack consisting of melamine-impregnated blue decorative paper and phenolic resin-impregnated core paper, and subjected together with them to a temperature of 700 N / cm. 2 The paper is pressed at 140°C for 10 minutes under pressure to achieve final curing. To simulate smudging the decorative paper with a pencil, approximately 1×1mm marks are made on the decorative paper beforehand.

[0184] As the structure provider, in the pressing steps listed above, an extrusion die with a wood-porous appearance is pressed together with the polyester foil. After cooling, a laminate sheet (HPL) is obtained, from which the polyester foil can be pulled out with very little force, and the finally cured coating is inseparably bonded to the melamine resin layer of the resulting decorative paper. Here, the now hard and scratch-resistant coating accepts the surface structure of the extrusion die. Before the polyester foil is pulled out, the marks applied to the decorative paper with a pencil before pressing can be clearly identified through the transparent polyester foil.

Claims

1. A method for preparing a transfer foil, the transfer foil comprising a carrier material and a coating comprising a thermoplastic polyurethane (meth)acrylate polymer, wherein, The method includes the following steps: a) Applying a coating composition to a carrier material, wherein the coating composition comprises a resin component and a hardener component. The resin component exists as a mixture comprising at least one component A and at least one component B. Component A is a polymerizable (meth)acrylate compound, each molecule of which has at least two groups with (meth)acrylate double bonds and contains no hydroxyl groups. Component B is a polymerizable (meth)acrylate compound, each molecule of which has one or more groups with (meth)acrylate double bonds and at least two hydroxyl groups; b) Drying the carrier material coated in step a) at an elevated temperature, wherein the hydroxyl groups in the resin component react with the isocyanate groups in the hardener component to form a coating of a thermoplastic polyurethane (meth)acrylate polymer containing groups having (meth)acrylate double bonds.

2. The method according to claim 1, wherein, Component A contains no other reactive groups except for groups with (meth)acrylic acid double bonds.

3. The method according to claim 1 or 2, wherein, The polymerizable (meth)acrylate compound of component A comprises a compound of formula A1: (A1) in, R 1 and R 3 are each, independently of one another, selected from aliphatic hydrocarbon radicals, aliphatic polyether radicals and aliphatic polyester radicals, R 2 is an aliphatic or cycloaliphatic hydrocarbon group, and n and m are each independently 2 to 9.

4. The method according to at least one of claims 1 to 3, wherein, The polymerizable (meth)acrylate compound of component A comprises a compound of formula A2: (A2) in, R 4 It is an aliphatic hydrocarbon group, and o is 2 to 6.

5. The method according to at least one of claims 1 to 4, wherein, The polymerizable (meth)acrylate compound of component B comprises a compound of formula B1: (B1) in, R 5 Selected from aliphatic hydrocarbon groups, aliphatic polyether groups, and aliphatic polyester groups. R 6 and R 7 Each is independently an aliphatic hydrocarbon group or an alicyclic hydrocarbon group, and p is 2 to 9.

6. The method according to at least one of claims 1 to 5, wherein, The resin component further comprises at least one component C, said component C being a polyurethane prepolymer having at least two hydroxyl groups per molecule, preferably exactly two hydroxyl groups, and being free of isocyanate groups; and Wherein, the polyurethane prepolymer of component C preferably contains no other reactive groups besides hydroxyl groups, and The polyurethane prepolymer of component C preferably includes at least one compound of formula C1. (C1) in, R 8 Each time it appears, it is independently selected from aliphatic hydrocarbon groups that can be replaced by one or more hydroxyl groups; aliphatic polyether groups and aliphatic polyester groups; R 9 Each time they appear, they are independently aliphatic or alicyclic hydrocarbon groups; and q is 2 to 9; and / or Preferably, it comprises at least one compound of formula C2. (C2) in, R 8 and R 8a Each time it appears, it is independently selected from aliphatic hydrocarbon groups that can be replaced by one or more OH groups; aliphatic polyether groups and aliphatic polyester groups; R 9 Each time they appear, they are independently aliphatic or alicyclic hydrocarbon groups; and q is 2 to 9.

7. The method according to at least one of claims 1 to 6, wherein, The resin component also contains at least one adhesion promoter.

8. The method according to at least one of claims 1 to 7, wherein, The resin component comprises, based on the total weight of the resin component. 30.0 to 80.0% by weight of component A, 15.0 to 70.0% by weight of component B, 0.0 to 5.0% by weight of the component C, and 0.0 to 10.0% by weight of the adhesion promoter.

9. The method according to at least one of claims 1 to 8, wherein, The drying in step (b) is carried out at a temperature of 110°C or lower.

10. The method according to at least one of claims 1 to 9, wherein, The carrier material has a surface that imparts a structure.

11. A transfer foil comprising a carrier material and a coating comprising a thermoplastic polyurethane (meth)acrylate polymer, and the transfer foil being obtainable by the method according to at least one of claims 1 to 10.

12. The transfer foil according to claim 11, wherein, A separation layer is arranged between the coating containing thermoplastic polyurethane (meth)acrylate polymer and the carrier material.

13. A method for preparing a laminated material sheet, the laminated material sheet comprising: Carrier material, Coatings comprising crosslinked polyurethane (meth)acrylate polymers, and Core layer, Wherein, the laminated material plate serves as the outermost layer having the carrier material, and the coating is disposed between the carrier material and the core layer; and The method includes the following steps: i) Provide the transfer foil according to claim 11 or 12; ii) Provide a pressed stack comprising a core layer of material for forming a laminated material sheet and a transfer foil provided in step i) as a surface layer, such that the transfer foil provided in step i) forms an outermost layer on at least one side of the pressed stack, and wherein the carrier material is present on at least one surface of the pressed stack; iii) The compressed stack is extruded under increased pressure and temperature, wherein polymerization of the (meth)acrylic double bonds of the thermoplastic polyurethane polymer occurs in the coating.

14. A laminated material sheet, comprising: Carrier material, Coatings comprising crosslinked polyurethane (meth)acrylate polymers, and Core layer, The laminated material board serves as the outermost layer, having the carrier material, and the coating is disposed between the carrier material and the core layer. And can be obtained by the method according to claim 13, wherein the coating preferably has According to Section 29 of EN438-2:2019, the weather resistance, wherein after more than 3000 hours, the change in gloss measured at a 60° angle according to DIN EN ISO2813:2015-02 is a maximum of 3 gloss units; and / or Color stability of grade 5 (no change) according to grayscale standard EN20105-A02 and / or stain resistance according to section 26 of EN438-2:2019, wherein the surface achieves at least grade 5; and / or According to Sections 14 and 15 of EN438-2:2019, optical properties of grade 5 (no change), wherein the coating shows a test value of Gt 0-1 in a subsequent cross-sectional adhesion test according to ISO2400.

15. A method for preparing a component, wherein, The method includes the following steps: i) Provide a laminated material sheet according to claim 14; ii) Optionally process the laminated material sheet; iii) Assemble the laminated material sheets in step i) or ii); iv) Remove the carrier material.

Citation Information

Patent Citations

  • varnish, flexible layered composite with a carrier and a layer of varnish applied thereto and their use

    DE102007040376A1

  • Process for the production of flat materials provided with a protective layer containing a lacquer and transfer film therefor

    DE10318542A1

  • liquid mixtures of 4,4'-mcthylene bis(cyclohexyl isocyanate) isomers

    DE1618795A1

  • 4,4'-Methylene-bis(CYCLOHEXYLISOCYANATE) ISOMERIC MIXTURE

    DE1793785A1

  • Process for producing laminate sheets, films and the like provided with a surface finish and transfer films for carrying out the process

    DE3545171C1